A low-resistance, high-mass-transfer-efficiency honeycomb dehumidifier rotor and its manufacturing method
By using composite moisture-absorbing materials in a honeycomb dehumidifying impeller, the problems of increased duct cross-section and uncoordinated thermal management are solved, achieving efficient moisture transfer and heat management, and improving the impeller's stability and regeneration efficiency.
Patent Information
- Application Number
- CN202611534026.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-30
- Publication Date
- 2026-11-17
AI Technical Summary
Existing honeycomb dehumidification rotors, while increasing the dehumidification capacity per unit volume, suffer from problems such as increased duct cross-sectional area, increased surface roughness, and unstable synergy between thermal management and low-resistance structure. Furthermore, volume changes, salt solution migration, and local adhesion are prone to occur during moisture absorption, affecting rotor pressure drop and regeneration efficiency.
A composite moisture-absorbing material is used, including a hydrophilic cross-linked polymer matrix, microencapsulated water-soluble crystalline compounds, and thermally conductive and electrically insulating fillers. By embedding the composite moisture-absorbing material in the pores of the honeycomb matrix channel wall, a thermally conductive network and a porous protective layer are formed, which isolates the water-soluble crystalline compounds from the moisture-absorbing salts, thereby optimizing heat transfer and salt retention.
While maintaining an effective flow area, it improves moisture absorption capacity and mass transfer efficiency, reduces wind resistance and material instability, improves the stability of heat transfer and regeneration processes, and reduces pressure drop and material integrity impact during multiple cycles.
Smart Images

Figure CN123102322A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to air dehumidification materials, and more particularly to a honeycomb dehumidification rotor with low wind resistance and high mass transfer efficiency, and its manufacturing method. Background Technology
[0002] Honeycomb dehumidifiers typically adsorb water vapor from the treated air by loading silica gel, molecular sieves, hygroscopic salts, or polymer hygroscopic materials onto fiber paper, inorganic fiber paper, or porous ceramic substrates, and then desorb it by heating in the regeneration zone.
[0003] To increase dehumidification capacity per unit volume, existing technologies often increase the desiccant loading or coating thickness. However, thicker desiccant layers tend to occupy air duct cross-sections, increase surface roughness, and prolong the transfer path of water vapor and heat within the material. When using highly hygroscopic salts or expandable polymers, volume changes, salt solution migration, and local adhesion may occur during desiccant absorption, causing the impeller pressure drop to drift with increasing moisture content. On the other hand, the heat released during desiccant absorption raises the material temperature, weakening the subsequent desiccant driving force. Regeneration requires external heat to penetrate the desiccant layer to promote the desorption of deep moisture. Although existing composite desiccant materials can improve individual properties by adding thermally conductive fillers, phase change materials, or protective films, direct mixing of components easily leads to ion migration, loss of phase change substances, random crystallization, or pore blockage. Furthermore, there is a lack of stable synergy between thermal management, salt retention, and low-resistance structure.
[0004] Therefore, there is a need for a honeycomb dehumidifier rotor that can maintain the effective flow area of the honeycomb channel while taking into account moisture transfer, adsorption heat regulation, regeneration heat utilization and stability of hygroscopic components, and is suitable for long-term cyclic operation. Summary of the Invention
[0005] This invention overcomes the shortcomings of the prior art and provides a honeycomb dehumidification rotor with low wind resistance and high mass transfer efficiency, as well as its manufacturing method.
[0006] To achieve the above objectives, the technical solution adopted by the present invention is as follows: a honeycomb dehumidification rotor with low wind resistance and high mass transfer efficiency, comprising a honeycomb substrate, wherein the honeycomb substrate is provided with multiple airflow channels extending along the axial direction, characterized in that:
[0007] The airflow channel wall is loaded with a composite moisture-absorbing material, and the composite moisture-absorbing material is at least partially distributed in the pores of the channel wall;
[0008] The composite moisture-absorbing material includes a hydrophilic cross-linked polymer matrix, a moisture-absorbing salt retained in the hydrophilic cross-linked polymer matrix, microcapsules dispersed in the hydrophilic cross-linked polymer matrix, and a thermally conductive and electrically insulating filler.
[0009] The microcapsule includes a shell and a core material covered by the shell. The shell allows water to pass through and inhibits the migration of the core material and the hygroscopic salt. The core material includes a water-soluble crystalline compound with a positive enthalpy of solubility in water. The water-soluble crystalline compound undergoes a reversible transition between a crystalline state and a dissolved state during hygroscopic and regeneration processes.
[0010] At least some of the thermally conductive and electrically insulating fillers overlap each other to form a thermally conductive network that contacts at least a portion of the shell of the microcapsules.
[0011] In a preferred embodiment of the present invention, the hydrophilic crosslinked polymer matrix includes one or more of polyacrylamide, polyacrylic acid or its salts, polyvinyl alcohol, alginate, carboxymethyl cellulose and hydroxyethyl cellulose;
[0012] The hygroscopic salt includes one or more of lithium chloride, calcium chloride, magnesium chloride, and lithium bromide.
[0013] In a preferred embodiment of the present invention, the water-soluble crystalline compound includes one or both of potassium nitrate and potassium chloride, and the water-soluble crystalline compound is at least partially crystalline in the dry state of the microcapsules;
[0014] The water-soluble crystalline compound transforms at least partially from a crystalline state to a dissolved state during the process of the composite moisture-absorbing material absorbing moisture, and at least partially transforms from a dissolved state to a crystalline state during the process of the composite moisture-absorbing material being heated and regenerated and its moisture content decreasing.
[0015] In a preferred embodiment of the present invention, the shell of the microcapsule comprises one or more of cross-linked polyvinyl alcohol, polyamide, cellulose acetate, a composite material formed by chitosan and alginate, and polyethersulfone.
[0016] The shell is a continuous shell that allows water to pass bidirectionally between the core material and the hydrophilic crosslinked polymer matrix, while inhibiting the migration of the water-soluble crystalline compound out of the microcapsule and the entry of the hygroscopic salt into the microcapsule.
[0017] In a preferred embodiment of the present invention, the thermally conductive and electrically insulating filler comprises one or more of hexagonal boron nitride, aluminum oxide, aluminum nitride and magnesium oxide;
[0018] The thermally conductive and electrically insulating filler is in the form of flakes, fibers, granules, or a combination thereof, and forms a thermally conductive network in the hydrophilic crosslinked polymer matrix connecting the region containing the hygroscopic salt to the microcapsules.
[0019] In a preferred embodiment of the present invention, based on the total dry weight of the composite moisture-absorbing material, the content of the hydrophilic crosslinked polymer matrix is 15-45% by mass, the content of the moisture-absorbing salt is 20-50% by mass, the content of the microcapsules is 20-55% by mass, and the content of the thermally conductive and electrically insulating filler is 1-15% by mass.
[0020] The total mass of the hydrophilic crosslinked polymer matrix, the hygroscopic salt, the microcapsules, and the thermally conductive and electrically insulating filler accounts for 90-100% of the total dry mass of the composite hygroscopic material.
[0021] The median particle size of the microcapsules is 5 to 300 micrometers, and the average thickness of the shell is 0.1 to 10 micrometers.
[0022] In a preferred embodiment of the present invention, the composite moisture-absorbing material forms a composite moisture-absorbing layer having an airflow side region and a substrate side region, wherein the airflow side region is close to the airflow channel and the substrate side region is close to the interior of the honeycomb matrix;
[0023] The microcapsule volume content in the substrate side region is greater than the microcapsule volume content in the airflow side region, and at least a portion of the microcapsules are embedded in the pores of the channel wall.
[0024] In a preferred embodiment of the present invention, the composite moisture-absorbing material is provided with a porous protective layer on the side facing the airflow channel. The porous protective layer allows water vapor to pass through and restricts the liquid moisture-absorbing salt solution and the microcapsules from entering the airflow channel.
[0025] The porous protective layer includes one or more of polytetrafluoroethylene, polyvinylidene fluoride and silicone resin.
[0026] The honeycomb matrix includes one of glass fiber paper, ceramic fiber paper, aluminosilicate fiber paper, and cellulose-inorganic fiber composite paper.
[0027] A method for manufacturing a honeycomb desiccant rotor with low wind resistance and high mass transfer efficiency includes the following steps:
[0028] S1, dispersing an aqueous phase containing a water-soluble crystalline compound in a continuous phase that is immiscible with water to form droplets, forming a shell layer at the interface of the droplets that allows water to pass through and inhibits the passage of ions and the water-soluble crystalline compound, separating and drying the droplets with the shell layer, so that the water-soluble crystalline compound at least partially crystallizes within the shell layer, to obtain microcapsules;
[0029] S2, dispersing thermally conductive and electrically insulating fillers in a hydrophilic polymer precursor solution, and then adding the microcapsules to the hydrophilic polymer precursor solution to obtain a composite slurry;
[0030] S3, the composite slurry is loaded onto the fiber sheet, so that at least part of the composite slurry enters the pores of the fiber sheet, and the hydrophilic polymer precursor liquid is subjected to a first crosslinking treatment to obtain the composite sheet;
[0031] S4, corrugating the composite sheet, connecting the corrugated composite sheet with the flat sheet and winding it to obtain a honeycomb matrix with multiple axial airflow channels;
[0032] S5, the hydrophilic polymer is subjected to a second crosslinking treatment to form a hydrophilic crosslinked polymer matrix, and at least some of the thermally conductive and electrically insulating fillers are overlapped to form a thermally conductive network.
[0033] S6. The honeycomb matrix is impregnated with a hygroscopic salt solution to allow the hygroscopic salt to enter and remain in the hydrophilic crosslinked polymer matrix, followed by drying to obtain the honeycomb dehumidification wheel.
[0034] In a preferred embodiment of the present invention, in step S1, the water-soluble crystalline compound and the water-soluble amine monomer are added to water to form the aqueous phase, and an organic solution containing acyl chloride monomer is used as the continuous phase. The droplets formed by the aqueous phase are brought into contact with the continuous phase to form a polyamide shell at the interface of the droplets.
[0035] In step S3, a first composite slurry with a higher microcapsule content is first loaded onto the fiber sheet, and then a second composite slurry with a lower microcapsule content is loaded onto the side of the first composite slurry away from the fiber sheet.
[0036] After step S6, a porous protective layer is formed on the surface of the channel wall of the airflow channel, allowing water vapor to pass through and restricting the entry of liquid hygroscopic salt solution into the airflow channel.
[0037] In a preferred embodiment of the present invention,
[0038] This invention addresses the shortcomings of the prior art and has the following beneficial effects:
[0039] (1) This invention embeds at least part of the composite moisture-absorbing material into the pores of the channel wall of a honeycomb matrix, and composites moisture-absorbing salt, microcapsules containing a reversible dissolution-crystallization core material, and thermally conductive filler in a hydrophilic cross-linked polymer matrix, so that the moisture absorption capacity, mass transfer rate, and channel resistance no longer depend solely on the surface coating thickness. Compared with existing solutions that increase capacity by thickening the moisture-absorbing layer, this invention can improve heat transfer during moisture absorption and regeneration while maintaining a larger effective flow cross section, alleviating the problem of difficulty in achieving both low air resistance and high mass transfer efficiency.
[0040] (2) This invention allows the composite moisture-absorbing material to primarily enter the pores of the channel wall and enables the microcapsules to preferentially distribute in the region close to the interior of the substrate. Simultaneously, a porous protective layer permeable to water vapor is provided on the airflow side, thereby reducing the impact of moisture absorption and swelling, salt solution migration, and particle shedding on the duct profile. Compared to existing impellers that directly apply a thick coating of desiccant to the duct surface, this invention reduces the changes in the effective cross-sectional area and surface roughness of the channel during wet operation, further suppressing the continuous increase in pressure drop as the moisture absorption load increases.
[0041] (3) This invention utilizes the microcapsule shell to allow water transfer and isolate hygroscopic salts from water-soluble crystalline compounds, enabling the core material to undergo endothermic dissolution during moisture absorption and crystallization during heating and regeneration. Heat exchange occurs between the core material and the region containing hygroscopic salts via a thermally conductive network formed by the thermally conductive filler. Compared to existing solutions that only use hygroscopic salts or ordinary inert phase change materials, this invention can mitigate the adverse effects of localized temperature rise on the moisture absorption driving force during the moisture absorption stage and utilize the exothermic effect of crystallization during the regeneration stage to reduce temperature lag in the desorption region.
[0042] (4) This invention forms a synergistic structure through the selective isolation of microcapsules, the thermally conductive network, the embedded distribution of materials within the channel wall, and the porous protective layer on the airflow side, so that moisture transfer, ion blocking, heat transfer, and airflow maintenance are each undertaken by different structures. Compared with existing technologies that directly mix the components or simply increase the amount of desiccant, this invention can reduce the cumulative impact of salt mixing, random crystallization, core material leakage, and channel blockage on cycle performance, and further improve the stability of pressure drop, moisture absorption rate, and material integrity during multiple moisture absorption-regeneration cycles. Attached Figure Description
[0043] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0044] Figure 1 This is a flowchart of a preferred embodiment of the present invention. Detailed Implementation
[0045] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0046] Many specific details are set forth in the following description in order to provide a full understanding of the invention. However, the invention may also be practiced in other ways different from those described herein. Therefore, the scope of protection of the invention is not limited to the specific embodiments disclosed below.
[0047] The honeycomb dehumidification rotor in this embodiment is mainly used in air handling devices that require continuous dehumidification and hot air regeneration. This application scenario requires the dehumidification rotor to have a high moisture absorption capacity while maintaining the effective flow area of the axial airflow channel and reducing the possibility of increased wind resistance caused by the expansion, migration or local adhesion of the moisture absorption material under high humidity conditions.
[0048] The adsorption heat generated during the moisture absorption process and the internal heat transfer lag during the regeneration process directly affect the moisture absorption driving force and regeneration efficiency. Therefore, it is necessary to control the moisture transfer, heat transfer and moisture-absorbing components in the composite moisture-absorbing material separately.
[0049] The honeycomb dehumidifying impeller provided in this embodiment includes a honeycomb matrix with multiple airflow channels extending along its axial direction. The channel walls of the airflow channels are loaded with a composite moisture-absorbing material, and the composite moisture-absorbing material is at least partially inserted into and retained in the pores of the channel walls. The composite moisture-absorbing material includes a hydrophilic cross-linked polymer matrix, moisture-absorbing salts retained in the hydrophilic cross-linked polymer matrix, microcapsules dispersed in the hydrophilic cross-linked polymer matrix, and thermally conductive and electrically insulating fillers.
[0050] The microcapsule comprises a continuous shell and a core material encapsulated by the shell; the shell allows water to pass between the microcapsule core material and the hydrophilic crosslinked polymer matrix, and inhibits the migration of water-soluble crystalline compounds from the core material out of the microcapsule and the entry of hygroscopic salts into the microcapsule; the core material comprises a water-soluble crystalline compound with a positive enthalpy of solubility in water; the water-soluble crystalline compound is at least partially crystalline in the dry state of the microcapsule, at least partially transforms from the crystalline state to the dissolved state when the composite hygroscopic material absorbs moisture, and at least partially transforms from the dissolved state back to the crystalline state when the composite hygroscopic material is heated and regenerated and its moisture content decreases.
[0051] Thermally conductive and electrically insulating fillers are dispersed in a hydrophilic crosslinked polymer matrix, with at least some adjacent fillers in contact or overlapping to form a thermally conductive network connecting the hygroscopic salt region and at least a portion of the microcapsule shell. This allows heat transfer between the hygroscopic salt region and the microcapsules through the thermally conductive network, while avoiding adverse effects of conductive fillers on the electrical insulation performance of the dehumidifying impeller.
[0052] The honeycomb matrix is made of glass fiber paper, the hydrophilic crosslinked polymer matrix is formed of polyvinyl alcohol, the hygroscopic salt is lithium chloride, the microcapsule core material is potassium nitrate, the microcapsule shell is polyamide, and the thermally conductive and electrically insulating filler is sheet-like hexagonal boron nitride.
[0053] Step S1: Prepare microcapsules containing water-soluble crystalline compounds.
[0054] Prepare an aqueous phase containing potassium nitrate and water-soluble amine monomers; mix 100 parts by weight of deionized water, 25-35 parts by weight of potassium nitrate and 1-3 parts by weight of m-phenylenediamine, and stir at 20-30°C until potassium nitrate and m-phenylenediamine are uniformly dispersed or dissolved to obtain the microcapsule aqueous phase.
[0055] Prepare a continuous phase that is immiscible with water; mix 100 parts by mass of cyclohexane, 0.3 to 1 part by mass of trimesoyl chloride and 0.5 to 2 parts by mass of oil-soluble dispersant to obtain an organic continuous phase containing acyl chloride monomers.
[0056] The aqueous phase is added to the organic continuous phase and sheared and dispersed at 600-1000 r / min at 20-30℃ for 5-15 min, so that the aqueous phase forms droplets with a median particle size of 30-150 μm in the organic continuous phase. After the droplets are formed, the reaction is stirred for 10-30 min, so that the m-phenylenediamine in the aqueous phase and the trimesoyl chloride in the organic continuous phase undergo interfacial polymerization at the droplet interface, forming a continuous polyamide shell on the outer periphery of the droplets.
[0057] After the reaction is complete, reduce the stirring speed, filter and separate the droplets that have formed polyamide shells, and wash them with an organic solvent that does not dissolve potassium nitrate to remove the residual continuous phase, unreacted monomers and dispersants on the outside of the microcapsules. After washing, the microcapsules are dried under vacuum at 40-55°C for 6-12 hours to reduce the moisture inside the shell and to allow potassium nitrate to crystallize at least partially inside the shell.
[0058] The microcapsules obtained in this step are in the form of separated particles. The median particle size of the microcapsules is preferably 50-120 μm, and the average thickness of the polyamide shell is preferably 0.5-3 μm. The polyamide shell remains continuous and has the function of allowing water molecules to pass through while restricting the migration of potassium nitrate and external hygroscopic salts.
[0059] This step forms a continuous shell at the interface of potassium nitrate droplets, confining the water-soluble crystalline compound within an independent micro-space. This solves the problem of easy migration, loss, or random crystallization in different regions when the water-soluble crystalline compound is directly added to the composite moisture-absorbing material. After this step is completed, only microcapsules with crystalline core material and selective shell are formed, and the composite structure between the microcapsules and the moisture-absorbing salt or thermally conductive filler has not yet been formed.
[0060] Step S2: Prepare a composite slurry containing microcapsules and thermally conductive fillers.
[0061] Polyvinyl alcohol is added to deionized water, heated to 80-95°C and stirred for 1-2 hours to fully dissolve the polyvinyl alcohol, resulting in a hydrophilic polymer precursor solution with a solid content of 8-15% by mass. After the hydrophilic polymer precursor solution is cooled to below 35°C, its pH value is adjusted to 4-6, and glutaraldehyde, accounting for 0.5-3% by mass of the dry weight of polyvinyl alcohol, is added as a crosslinking agent.
[0062] Hexagonal boron nitride flakes are added to a hydrophilic polymer precursor solution and dispersed at a speed of 300–800 r / min for 15–40 min, so that the hexagonal boron nitride is dispersed in the hydrophilic polymer precursor solution in the form of single flakes, flake assemblages or small aggregates; the flake diameter of the hexagonal boron nitride is preferably 2–30 μm.
[0063] After completing the dispersion of hexagonal boron nitride, the microcapsules obtained in step S1 are added to the hydrophilic polymer precursor solution, and the stirring speed is controlled at 100-300 r / min for 10-30 min to obtain a composite slurry. After adding the microcapsules, low-shear stirring is used to reduce the impact of mechanical shear on the integrity of the microcapsule shell.
[0064] To form a distribution structure in which the microcapsule content varies along the thickness of the composite moisture-absorbing layer, a first composite slurry and a second composite slurry were prepared in this embodiment. Based on the dry solids mass of each composite slurry, the mass ratio of polyvinyl alcohol, microcapsules, and hexagonal boron nitride in the first composite slurry was 40:50:10; the mass ratio of polyvinyl alcohol, microcapsules, and hexagonal boron nitride in the second composite slurry was 60:25:15. The microcapsule content in the first composite slurry was higher than that in the second composite slurry.
[0065] The first and second composite slurries obtained in this step are both in a fluid, uniform suspension state, wherein hexagonal boron nitride is dispersed in the polyvinyl alcohol precursor solution, and the microcapsules remain basically intact and suspended in the polyvinyl alcohol precursor solution.
[0066] This step directly addresses the problem of uniformly introducing thermally conductive fillers and microcapsules into the hydrophilic polymer system; the addition of hexagonal boron nitride before the microcapsules facilitates the dispersion of the thermally conductive fillers without damaging the microcapsules; the first and second composite slurries use different microcapsule contents, providing a slurry basis for the subsequent formation of a composite moisture-absorbing layer with high microcapsule content on the substrate side and low microcapsule content on the airflow side; a stable cross-linked network and honeycomb airflow channels have not yet been formed in this step.
[0067] Step S3: Load the composite slurry onto the fiber sheet and perform the first crosslinking treatment.
[0068] Glass fiber paper with a thickness of 0.15 to 0.30 mm is selected as the fiber sheet. The glass fiber paper is subjected to dust removal and drying treatment to keep the pores of the glass fiber paper open.
[0069] The first composite slurry is coated on one side of the glass fiber paper, and a negative pressure is applied to the other side of the glass fiber paper; the negative pressure is preferably -20 to -50 kPa, and the negative pressure application time is 10 to 60 s, so that the first composite slurry enters the pores of the glass fiber paper; the dry basis loading of the first composite slurry is controlled to be 50 to 70% of the total dry basis loading of the composite slurry by mass.
[0070] After the first composite slurry is loaded, the second composite slurry is coated on the side of the first composite slurry away from the glass fiber paper; the dry basis loading of the second composite slurry is controlled to be 30-50% by mass of the total dry basis loading of the composite slurry; the total dry basis loading of the first and second composite slurries is preferably 80-180 g / m².
[0071] After the load is applied, the fiber sheet is placed at 45-60℃ for 15-40 minutes to perform the first crosslinking treatment on the polyvinyl alcohol precursor liquid. The first crosslinking treatment causes some polyvinyl alcohol molecular chains to form crosslinked connections and transforms the composite slurry from a flowable slurry state to a semi-cured state that can maintain its shape.
[0072] After the first cross-linking treatment, there is no obvious slurry flow on the surface of the composite sheet, the composite moisture-absorbing material enters at least part of the pores of the glass fiber paper, and the composite sheet still has the flexibility required for corrugation and winding; in the thickness direction of the composite sheet, the substrate side region near the interior of the glass fiber paper has a higher microcapsule volume content, and the airflow side region away from the glass fiber paper and towards the airflow channel has a lower microcapsule volume content.
[0073] This step uses negative pressure to assist the loading, allowing the composite slurry to enter the pores of the fiber sheet, reducing the situation where the composite moisture-absorbing material is completely piled up on the surface of the sheet, thereby reducing the occupation of the effective cross section of the subsequent airflow channel by the composite moisture-absorbing material; the first cross-linking treatment is used to fix the initial distribution state of the microcapsules and hexagonal boron nitride, and to prevent the composite slurry from flowing significantly during the corrugation process, but without causing the composite sheet to harden completely, so as to avoid affecting the subsequent molding.
[0074] Step S4: Corrugated molding and construction of the honeycomb matrix.
[0075] The composite sheet that has undergone the first cross-linking treatment is fed into a corrugated forming device to form a continuous corrugated structure. The corrugation pitch is preferably 2 to 5 mm, and the corrugation height is preferably 1 to 3 mm. The forming pressure is controlled during the corrugation forming process to stabilize the corrugation profile and avoid excessive compression of the microcapsules.
[0076] The corrugated composite sheet is stacked with the planar composite sheet, and a small amount of hydrophilic polymer precursor liquid is applied as a connecting material at the contact position of the two corrugations, and then continuously wound around the central axis. During the winding process, a stable spacing is maintained between adjacent layers to form multiple airflow channels that run through the axial direction of the honeycomb matrix.
[0077] After winding, the outer periphery of the honeycomb substrate is fixed to maintain its cylindrical shape or other wheel-shaped structure that is compatible with the dehumidification device; the axial direction of the airflow channel is basically parallel to the rotation axis of the honeycomb substrate.
[0078] The honeycomb matrix obtained in this step has continuous, mutually separated and axially connected airflow channels; the composite moisture-absorbing material is mainly distributed in the pores of the fiber sheet that constitute the channel wall and its surface area, and no large-sized slurry accumulations or obvious blockages are formed in the channel.
[0079] This step directly addresses the issue of transforming composite sheets from a planar structure to a low-wind-resistance honeycomb structure. The semi-cured state formed by the first cross-linking treatment keeps the composite moisture-absorbing material within the fiber sheet during corrugation and winding, reducing the possibility of the composite slurry entering the airflow channels due to extrusion. This step only forms the honeycomb channels and their basic outline; the hydrophilic polymer has not yet completed the second cross-linking.
[0080] Step S5: Perform a second cross-linking process to form a thermally conductive network.
[0081] The honeycomb matrix obtained in step S4 is treated at 60-85°C for 1-3 hours to allow polyvinyl alcohol and crosslinking agent to react further, completing the second crosslinking treatment and forming a continuous hydrophilic crosslinked polymer matrix.
[0082] During the second crosslinking process, as the water content in the hydrophilic polymer precursor solution further decreases, the polyvinyl alcohol matrix shrinks and fixes the position of hexagonal boron nitride, causing at least some adjacent hexagonal boron nitride sheets to contact or overlap each other, forming a thermally conductive network distributed in the hydrophilic crosslinking polymer matrix; at the same time, some hexagonal boron nitride comes into contact with the microcapsule shell.
[0083] After the second crosslinking treatment, the hydrophilic crosslinked polymer matrix changes from a semi-cured state to a non-flowing crosslinked solid state, and the microcapsules and hexagonal boron nitride are confined in the hydrophilic crosslinked polymer matrix; a stable connection is formed between the composite moisture-absorbing material and the glass fiber paper, and the shape of the honeycomb airflow channel is fixed.
[0084] This step addresses the issue of swelling, flow, or detachment from the channel walls of the composite moisture-absorbing material during subsequent moisture-absorbing salt impregnation and operation by increasing the degree of cross-linking of the hydrophilic polymer. The hexagonal boron nitride forms contact or overlap relationships, transforming the dispersed thermally conductive filler into a thermally conductive network capable of continuously transferring heat. After this step, moisture-absorbing salt has not yet been introduced into the hydrophilic cross-linked polymer matrix.
[0085] Step S6: Soak in moisture-absorbing salt and dry.
[0086] Prepare a lithium chloride aqueous solution with a mass concentration of 20-35%; immerse the honeycomb matrix that has undergone the second cross-linking treatment in the lithium chloride aqueous solution and maintain it under a negative pressure of -20 to -50 kPa for 3-10 min to expel some air from the pores of the hydrophilic cross-linked polymer matrix and the fiber sheet; after releasing the negative pressure, continue immersion for 10-40 min to allow the lithium chloride solution to enter the pores of the hydrophilic cross-linked polymer matrix and the fiber sheet connected to it.
[0087] After impregnation, remove the honeycomb substrate and keep the airflow channels in each axis vertical or inclined to discharge any unretained lithium chloride solution from the airflow channels. Use clean air to purge the airflow channels at low speed to remove continuous droplets from the channel wall surface and prevent lithium chloride solution from accumulating inside the channels.
[0088] The honeycomb matrix is dried at 50–70°C for 3–6 hours, and then dried at 70–85°C for 1–3 hours to gradually reduce the moisture content and keep the lithium chloride in the hydrophilic crosslinked polymer matrix.
[0089] By adjusting the concentration of the lithium chloride solution, the impregnation time, and the number of impregnations, the final composite moisture-absorbing material comprises, by weight (dry basis), 33.6% hydrophilic crosslinked polymer matrix, 30% lithium chloride, 28% microcapsules, and 8.4% hexagonal boron nitride; the content of each component can be adjusted within the range defined in the claims.
[0090] After this step is completed, lithium chloride is distributed in the hydrophilic cross-linked polymer matrix in a solid state, a concentrated solution state, or a state combined with the hydrophilic cross-linked polymer matrix; the composite moisture-absorbing material is retained in the channel wall and pores of the airflow channel, and there is no continuous free lithium chloride solution in the airflow channel.
[0091] This step introduces hygroscopic salts into the already cross-linked and stabilized hydrophilic polymer matrix through impregnation, which solves the problem that adding hygroscopic salts before the composite slurry is formed may affect the cross-linking of the polymer, the stability of the microcapsule shell, and the rheological state of the slurry. The hydrophilic cross-linked polymer matrix has a spatial confinement and retention effect on lithium chloride, reducing the possibility that lithium chloride will migrate into the airflow channel in the form of a liquid solution after absorbing moisture.
[0092] Prepare an aqueous organosilicon resin dispersion with a solid content of 1-5% by mass; slowly rotate the honeycomb matrix around its central axis, and allow the organosilicon resin dispersion to form atomized droplets that pass through the honeycomb matrix along the axial direction of the airflow channel, so that the atomized droplets are deposited on the channel wall surface of the airflow channel.
[0093] The dry basis loading of the silicone resin is controlled at 1-8 g / m² to avoid the silicone resin continuously filling the open pores on the channel wall surface. After deposition, clean air is used to blow along the airflow channel and cured at 60-90℃ for 20-60 min to form a porous protective layer on the side of the composite moisture-absorbing material facing the airflow channel.
[0094] The resulting porous protective layer has interconnected micropores, which allow water vapor to enter the composite moisture-absorbing material through the airflow channels, while restricting the entry of liquid lithium chloride solution, microcapsules, and detached composite moisture-absorbing material particles into the airflow channels.
[0095] This step addresses the issues of salt solution seepage, particle shedding, and localized adhesion that may occur in composite moisture-absorbing materials under high humidity or long-term cyclic conditions by forming a thin, porous protective structure with a certain degree of hydrophobicity on the airflow side. Since the porous protective layer has a low load and retains water vapor transmission channels, it will not form a closed moisture-barrier film.
[0096] The honeycomb dehumidifying impeller obtained by steps S1 to S6 includes a honeycomb matrix formed of glass fiber paper and multiple airflow channels that extend along the axial direction of the honeycomb matrix; the composite moisture-absorbing material is at least partially embedded in the pores of the channel wall of the airflow channel, and forms a substrate side region and an airflow side region in the channel wall.
[0097] The substrate-side region is close to the interior of the glass fiber paper, and its microcapsule volume content is greater than that of the airflow-side region; the airflow-side region is close to the airflow channel, and its surface is provided with a porous protective layer; the hydrophilic cross-linked polymer matrix is continuously distributed in both regions, and maintains lithium chloride, microcapsules and hexagonal boron nitride; at least some of the hexagonal boron nitride overlaps to form a thermally conductive network, which contacts part of the microcapsule shell and connects to the region containing lithium chloride.
[0098] Since the main part of the composite moisture-absorbing material enters the pores of the channel wall, only a thin layer of composite moisture-absorbing material and a porous protective layer are retained on the airflow side. Therefore, there is no need to increase the moisture-absorbing material load by forming a thicker moisture-absorbing coating on the surface of the airflow channel, which helps to maintain the effective flow area of the airflow channel.
[0099] The honeycomb dehumidification rotor is installed in a dehumidification device with a treatment zone and a regeneration zone, and rotates continuously or intermittently under the action of a drive mechanism.
[0100] When the corresponding area of the honeycomb dehumidification rotor rotates to the treatment zone, the air to be dehumidified passes through the honeycomb matrix along the axial airflow channel; water vapor in the air passes through the porous protective layer and enters the hydrophilic cross-linked polymer matrix, and lithium chloride absorbs the moisture, thereby reducing the moisture content of the treated air.
[0101] As the water content of the hydrophilic crosslinked polymer matrix increases, some water enters the microcapsule interior through the microcapsule shell, causing the potassium nitrate, which was originally at least partially crystalline, to gradually transform into a dissolved state. During the dissolution process of potassium nitrate, heat is absorbed, and the heat-conducting network formed by hexagonal boron nitride transfers heat between the lithium chloride-containing region and the microcapsule, thereby reducing the local heat accumulation inside the moisture-absorbing material.
[0102] The microcapsule shell allows water to pass through the microcapsule in both directions, while inhibiting potassium nitrate from migrating out of the microcapsule and lithium chloride from entering the microcapsule. Thus, potassium nitrate and lithium chloride are kept in the microcapsule core material and the hydrophilic cross-linked polymer matrix, respectively, reducing the possibility of salt mixing, random crystallization or mutual migration after direct contact between the two.
[0103] When the corresponding area of the honeycomb dehumidifying impeller rotates to the regeneration zone, the regeneration air passes through the honeycomb matrix along the axial airflow channel; the moisture retained in the hydrophilic cross-linked polymer matrix and lithium chloride is desorbed by heat and discharged with the regeneration air; as the moisture content of the composite moisture-absorbing material decreases, the potassium nitrate inside the microcapsules is at least partially transformed from a dissolved state back into a crystalline state; the heat released during the potassium nitrate crystallization process is transferred to the surrounding lithium chloride-containing area through the hexagonal boron nitride thermal conductive network, thereby improving the temperature distribution inside the composite moisture-absorbing material.
[0104] The hydrophilic cross-linked polymer matrix immobilizes lithium chloride and microcapsules, while the porous protective layer restricts airflow, making it difficult for hygroscopic salt solution, microcapsules, and composite hygroscopic material particles to enter the airflow channel. Thus, during multiple moisture absorption and regeneration cycles, the impact of hygroscopic material volume changes, salt solution migration, and particle shedding on the airflow channel profile and surface roughness can be reduced.
[0105] By embedding and distributing composite moisture-absorbing materials within the pores of the channel wall, selectively encapsulating water-soluble crystalline compounds with microcapsules, forming a thermally conductive network with thermally conductive and electrically insulating fillers, and a porous protective layer on the airflow side, the retention of moisture-absorbing salts, moisture transfer, heat transfer, and airflow channel maintenance are each undertaken by corresponding structures. This improves the stability of moisture and heat transfer during the moisture absorption and regeneration process while maintaining the effective flow area of the axial airflow channel in the honeycomb matrix.
[0106] Example 1:
[0107] By weight, 100 parts of deionized water, 30 parts of potassium nitrate and 2 parts of m-phenylenediamine were mixed and stirred at 300 r / min for 30 min at 25 °C to obtain the aqueous phase of microcapsules.
[0108] By weight, 100 parts of cyclohexane, 0.6 parts of trimesoyl chloride and 1.0 parts of Span-80 were mixed and stirred at 300 r / min for 15 min at 25 °C to obtain an organic continuous phase.
[0109] The aqueous phase of the microcapsules was added to the organic continuous phase and sheared at 800 r / min for 10 min at 25 °C to form droplets in the organic continuous phase. Then the stirring speed was adjusted to 500 r / min and the reaction was continued for 20 min to allow the m-phenylenediamine and trimesoyl chloride to undergo interfacial polymerization at the droplet interface, forming a continuous polyamide shell.
[0110] After the reaction was completed, the stirring speed was reduced to 150 r / min, and the microcapsules with polyamide shells were separated by filtration. The microcapsules were washed three times with cyclohexane and then dried under vacuum conditions of 48°C and 10 kPa for 9 h to reduce the moisture inside the microcapsules and to allow potassium nitrate to crystallize at least partially inside the microcapsules. The median particle size of the resulting microcapsules was 80 μm, and the average thickness of the polyamide shell was 1.2 μm.
[0111] Polyvinyl alcohol was added to deionized water, heated to 88°C and stirred at 400 r / min for 1.5 h to fully dissolve the polyvinyl alcohol, resulting in a polyvinyl alcohol precursor solution with a solid content of 12% by mass. The polyvinyl alcohol precursor solution was cooled to 32°C and its pH value was adjusted to 5.0. Glutaraldehyde accounting for 1.5% by mass of the dry weight of polyvinyl alcohol was added. Hexagonal boron nitride flakes with an average flake diameter of 10 μm were added to the polyvinyl alcohol precursor solution and dispersed at 550 r / min for 25 min.
[0112] After dispersing hexagonal boron nitride, the prepared microcapsules were added, and the mixture was stirred at 180 r / min under low shear for 20 min to prepare the first and second composite slurries, respectively. Based on the dry solids mass of each composite slurry, the mass ratio of polyvinyl alcohol, microcapsules, and hexagonal boron nitride in the first composite slurry was 40:50:10; the mass ratio of polyvinyl alcohol, microcapsules, and hexagonal boron nitride in the second composite slurry was 60:25:15.
[0113] Glass fiber paper with a thickness of 0.22 mm and a basis weight of 55 g / m² was selected, dried at 80℃ for 1 h and subjected to dust removal treatment. The first composite slurry was coated on one side of the glass fiber paper, and a negative pressure of -35 kPa was applied to the other side of the glass fiber paper for 35 s to allow the first composite slurry to enter the pores of the glass fiber paper. The dry basis load of the first composite slurry accounted for 60% of the total dry basis load of the first composite slurry and the second composite slurry.
[0114] The second composite slurry is coated onto the side of the first composite slurry away from the glass fiber paper. The dry basis loading of the second composite slurry accounts for 40% of the total dry basis loading of the two composite slurries. The total dry basis loading of the first and second composite slurries is 130 g / m². The glass fiber paper loaded with the composite slurry is then treated at 52°C for 25 min to allow partial cross-linking of polyvinyl alcohol and glutaraldehyde, resulting in a semi-cured state in which the composite slurry can maintain its shape and still be corrugated.
[0115] The first cross-linked composite sheet is fed into a corrugated forming device at a speed of 0.50 m / min and formed into continuous corrugations under a forming pressure of 0.30 MPa. The corrugation pitch is 3.5 mm and the corrugation height is 2.0 mm. The corrugated composite sheet is stacked with a planar composite sheet. A polyvinyl alcohol precursor liquid with a dry basis loading of 2.0 g / m² is applied as a bonding material at the contact position of the corrugations. The stacked sheet is continuously wound around a central axis with a diameter of 20 mm to obtain a honeycomb matrix with a diameter of 200 mm and an axial thickness of 100 mm.
[0116] The honeycomb matrix was treated at 75°C for 2 hours to further crosslink polyvinyl alcohol and glutaraldehyde, forming a hydrophilic crosslinked polymer matrix. As the moisture content in the hydrophilic crosslinked polymer matrix decreased and the matrix volume shrank, the position of hexagonal boron nitride was fixed, and at least some adjacent hexagonal boron nitride sheets came into contact or overlapped with each other, forming a thermally conductive network connecting the microcapsules and the subsequent lithium chloride-containing regions. The introduction of hygroscopic salts...
[0117] A lithium chloride aqueous solution with a mass concentration of 28% was prepared. The honeycomb matrix that had completed the second cross-linking was immersed in the lithium chloride aqueous solution and kept under a negative pressure of -35 kPa for 6 min. After the negative pressure was released, the immersion continued for 25 min. After the immersion was completed, the honeycomb matrix was removed and the airflow channel was kept vertical. Clean air at 0.50 m / s was blown along the airflow channel for 2 min to remove the lithium chloride solution in the airflow channel that was not held by the hydrophilic cross-linked polymer matrix. The honeycomb matrix was dried at 60℃ for 4.5 h and then dried at 78℃ for 2 h. The resulting composite moisture-absorbing material, based on the total dry weight, included 33.6% by mass of polyvinyl alcohol cross-linked matrix, 30.0% by mass of lithium chloride, 28.0% by mass of microcapsules, and 8.4% by mass of hexagonal boron nitride. The formation of the porous protective layer was achieved by preparing an aqueous organosilicon resin dispersion with a solid content of 3% by mass.
[0118] The honeycomb substrate is rotated around the central axis at 3 r / min, and the aqueous organosilicon resin dispersion is atomized into droplets at an atomization pressure of 0.20 MPa. The droplets are then axially passed through the honeycomb substrate along the airflow channel. The dry basis loading of the organosilicon resin is controlled at 4.0 g / m². After deposition, the substrate is purged along the airflow channel with clean air at 0.50 m / s for 2 min and cured at 75°C for 40 min. A porous protective layer is formed on the side of the composite moisture-absorbing material facing the airflow channel, resulting in a honeycomb dehumidifying rotor.
[0119] Example 2:
[0120] The difference between this embodiment and Example 1 is that the resulting composite moisture-absorbing material, based on the total dry weight, includes 41.6% by mass of polyvinyl alcohol crosslinked matrix, 30.0% by mass of lithium chloride, 20.0% by mass of microcapsules, and 8.4% by mass of hexagonal boron nitride. The rest of the preparation process and process parameters are completely consistent with those of Example 1.
[0121] Example 3:
[0122] The difference between this embodiment and Example 1 is that the resulting composite moisture-absorbing material, based on the total dry weight, includes 21.6% by mass of polyvinyl alcohol crosslinked matrix, 30.0% by mass of lithium chloride, 40.0% by mass of microcapsules, and 8.4% by mass of hexagonal boron nitride. The rest of the preparation process and process parameters are completely consistent with those of Example 1.
[0123] Example 4:
[0124] The difference between this embodiment and Example 1 is that the resulting composite moisture-absorbing material, based on the total dry weight, includes 39.0% by mass of polyvinyl alcohol crosslinked matrix, 30.0% by mass of lithium chloride, 28.0% by mass of microcapsules, and 3.0% by mass of hexagonal boron nitride. The remaining preparation process and process parameters are completely consistent with those of Example 1.
[0125] Example 5:
[0126] The difference between this embodiment and Example 1 is that the resulting composite moisture-absorbing material, based on the total dry weight, includes 30.0% by mass of polyvinyl alcohol crosslinked matrix, 30.0% by mass of lithium chloride, 28.0% by mass of microcapsules, and 12.0% by mass of hexagonal boron nitride. The rest of the preparation process and process parameters are completely consistent with those of Example 1.
[0127] Example 6:
[0128] The difference between this embodiment and Example 1 is that the median particle size of the microcapsules is controlled to be 20 μm, and the average thickness of the polyamide shell is 1.2 μm. The rest of the preparation process and process parameters are completely consistent with Example 1.
[0129] Example 7:
[0130] The difference between this embodiment and Example 1 is that the median particle size of the microcapsules is controlled to be 200 μm, and the average thickness of the polyamide shell is 1.2 μm. The rest of the preparation process and process parameters are completely the same as those in Example 1.
[0131] Example 8:
[0132] The difference between this embodiment and Example 1 is that the median particle size of the microcapsules is controlled to be 80 μm, and the average thickness of the polyamide shell is 0.5 μm. The rest of the preparation process and process parameters are completely consistent with Example 1.
[0133] Example 9:
[0134] The difference between this embodiment and Example 1 is that the median particle size of the microcapsules is controlled to be 80 μm, and the average thickness of the polyamide shell is 3.0 μm. The rest of the preparation process and process parameters are completely the same as those in Example 1.
[0135] Example 10:
[0136] The difference between this embodiment and Example 1 is that 30 parts by mass of potassium chloride are used instead of 30 parts by mass of potassium nitrate as the microcapsule core material, while the rest of the preparation process and process parameters are completely consistent with Example 1.
[0137] Example 11:
[0138] The difference between this embodiment and Example 1 is that spherical alumina with a median particle size of 8 μm is used to replace hexagonal boron nitride by mass, and the alumina content in the resulting composite moisture-absorbing material is 8.4% by mass. The rest of the preparation process and process parameters are completely consistent with Example 1.
[0139] Example 12:
[0140] The difference between this embodiment and Example 1 is that cross-linked polyvinyl alcohol is used as the microcapsule shell, the median particle size of the microcapsules is 80 μm, and the average thickness of the cross-linked polyvinyl alcohol shell is 1.5 μm. The rest of the preparation process and process parameters are completely consistent with Example 1.
[0141] Example 13:
[0142] The difference between this embodiment and Example 1 is that: a polyvinylidene fluoride aqueous dispersion with a solid content of 3% by mass is used instead of an aqueous organosilicon resin dispersion; the dry basis loading of the polyvinylidene fluoride porous protective layer is 4.0 g / m²; the curing temperature is 90℃; and the curing time is 40 min. The rest of the preparation process and process parameters are completely consistent with those of Example 1.
[0143] Comparative Example 1:
[0144] The difference between this comparative example and Example 1 is that: microcapsules, hexagonal boron nitride, and porous protective layer are not provided; the moisture-absorbing material composed of 70% by mass polyvinyl alcohol and 30% by mass lithium chloride is directly coated on the surface of the airflow channel of the glass fiber honeycomb matrix; the total dry basis load of the moisture-absorbing material is 130 g / m²; and the size of the honeycomb dehumidifying wheel is exactly the same as that of Example 1.
[0145] Comparative Example 2:
[0146] The difference between this comparative example and Example 1 is that when the composite slurry is loaded onto the glass fiber paper, no negative pressure is applied to the other side of the glass fiber paper, so that the composite slurry is mainly loaded on the surface of the glass fiber paper. The rest of the preparation process and process parameters are completely consistent with Example 1.
[0147] Comparative Example 3:
[0148] The difference between this comparative example and Example 1 is that: 28.0% by mass of microcapsules were replaced with an equal mass of polyvinyl alcohol. The resulting composite moisture-absorbing material, based on the total dry weight, includes 61.6% by mass of polyvinyl alcohol crosslinked matrix, 30.0% by mass of lithium chloride, and 8.4% by mass of hexagonal boron nitride. The rest of the preparation process and process parameters are completely consistent with those of Example 1.
[0149] Comparative Example 4:
[0150] The difference between this comparative example and Example 1 is that: no microcapsules were prepared, and 22.4% by mass potassium nitrate and 5.6% by mass polyvinyl alcohol were used instead of 28.0% by mass microcapsules, so that potassium nitrate was directly dispersed in the lithium chloride-containing polyvinyl alcohol crosslinked matrix. The rest of the preparation process and process parameters were completely consistent with Example 1.
[0151] Comparative Example 5:
[0152] The difference between this comparative example and Example 1 is that a dense epoxy resin shell with an average thickness of 1.2 μm is used instead of a polyamide shell, making it difficult for water to pass through the inside and outside of the microcapsule. The rest of the preparation process and process parameters are completely consistent with Example 1.
[0153] Comparative Example 6:
[0154] The difference between this comparative example and Example 1 is that: 8.4% by mass of hexagonal boron nitride was replaced with an equal mass of polyvinyl alcohol. The resulting composite moisture-absorbing material, based on the total dry weight, includes 42.0% by mass of polyvinyl alcohol crosslinked matrix, 30.0% by mass of lithium chloride, and 28.0% by mass of microcapsules. The rest of the preparation process and process parameters are completely consistent with those of Example 1.
[0155] Comparative Example 7:
[0156] The difference between this comparative example and Example 1 is that after forming an organosilicon coating layer with an average thickness of 0.5 μm on the surface of hexagonal boron nitride, hexagonal boron nitride is added to the polyvinyl alcohol precursor solution. The content of hexagonal boron nitride is still 8.4% by mass, so that adjacent hexagonal boron nitrides are not easy to directly contact or overlap. The rest of the preparation process and process parameters are completely consistent with Example 1.
[0157] Comparative Example 8:
[0158] The difference between this comparative example and Example 1 is that only one composite slurry was prepared. The mass ratio of polyvinyl alcohol, microcapsules and hexagonal boron nitride in the composite slurry was 48:40:12. The composite slurry was used to complete the loading in one step, so that the microcapsule content in the substrate side region and the airflow side region was basically the same. The rest of the preparation process and process parameters were completely consistent with Example 1.
[0159] Comparative Example 9:
[0160] The difference between this comparative example and Example 1 is that: first, the second composite slurry with a lower microcapsule content is loaded onto glass fiber paper, and then the first composite slurry with a higher microcapsule content is loaded onto the side of the second composite slurry away from the glass fiber paper, so that the microcapsule content in the airflow side region is higher than the microcapsule content in the substrate side region. The rest of the preparation process and process parameters are completely consistent with Example 1.
[0161] Comparative Example 10:
[0162] The difference between this comparative example and Example 1 is that after lithium chloride impregnation and drying, a porous protective layer is not formed on the side of the composite moisture-absorbing material facing the airflow channel. The rest of the preparation process and process parameters are completely consistent with Example 1.
[0163] Comparative Example 11:
[0164] The difference between this comparative example and Example 1 is that the dry basis loading of the waterborne silicone resin was adjusted to 15 g / m², so that the silicone resin formed a continuous and dense film on the airflow side of the composite moisture-absorbing material. The rest of the preparation process and process parameters are completely consistent with Example 1.
[0165] Comparative Example 12:
[0166] The difference between this comparative example and Example 1 is that lithium chloride is directly added to the composite slurry, so that the composite slurry contains lithium chloride before the honeycomb matrix is formed, and lithium chloride aqueous solution is no longer used for impregnation after the hydrophilic crosslinked polymer matrix is formed. The rest of the preparation process and process parameters are completely consistent with Example 1.
[0167] Comparative Example 13:
[0168] The difference between this comparative example and Example 1 is that: after the honeycomb substrate is corrugated and wound, it is not subjected to a second crosslinking at 75°C for 2 hours, but is directly impregnated with lithium chloride aqueous solution. The rest of the preparation process and process parameters are completely consistent with Example 1.
[0169] Comparative Example 14:
[0170] The difference between this comparative example and Example 1 is that the microcapsules were first added to the polyvinyl alcohol precursor solution, then hexagonal boron nitride was added, and the mixture was dispersed at 550 r / min for 25 min to allow the microcapsules to withstand the high shear force during the dispersion of hexagonal boron nitride. The rest of the preparation process and process parameters were completely consistent with those of Example 1.
[0171] Performance testing methods:
[0172] The median volumetric particle size of the microcapsules was determined as follows: The microcapsule volumetric particle size distribution was determined according to GB / T 19077-2024 "Particle Size Analysis - Laser Diffraction Method", using isoparaffins that do not react with the polyamide shell or water-soluble crystalline compounds as the dispersion medium. The microcapsules were added to the dispersion medium and stirred at 100 r / min for 1 min without ultrasonic dispersion to avoid damage to the microcapsule shell. Each sample was measured three times consecutively, and the particle size corresponding to a cumulative volume distribution reaching 50% was taken as the median volumetric particle size D. 50 The unit is μm, and the result is rounded to one decimal place.
[0173] The average shell thickness and integrity of the microcapsules were measured using the following method: Scanning electron microscopy (SEM) cross-sectional imaging method was employed. Microcapsules were frozen in liquid nitrogen for 5 minutes and then subjected to brittle fracture. The fracture surfaces were sputtered with gold and observed using an SEM. Fifty microcapsules with intact cross-sections were randomly selected from each group. The shell thickness of each microcapsule was measured in three directions at approximately 120° intervals, resulting in a total of 150 shell thickness measurements. The average shell thickness was calculated using the following formula:
[0174] ;
[0175] In addition, at least 500 microcapsules were randomly observed, and the integrity rate of the microcapsules was calculated according to the following formula:
[0176] .
[0177] In the formula, This is the measured value of the i-th shell thickness; The number of intact microcapsules; This represents the total number of microcapsules observed.
[0178] The reversible transformation performance from crystalline to dissolved state was measured using the following method: Microcapsules or microcapsule-containing composite hygroscopic materials were treated in dry, hygroscopic, and regenerated states using the X-ray diffraction characteristic peak integrated area method. The dry state involved drying at 80℃ until the mass difference between two consecutive weighings did not exceed 0.1% of the initial dry mass of the sample. The hygroscopic state involved absorbing moisture at 30℃ and 80% relative humidity for 60 minutes. The regenerated state involved regenerating the sample in dry air at 80℃ after moisture absorption until the sample mass recovered to within 101% of the initial dry mass. The integrated area of the characteristic diffraction peaks of the water-soluble crystalline compound was measured under the same testing conditions. The peak attenuation rate after moisture absorption was calculated using the following formula:
[0179] ;
[0180] The peak recovery rate after regeneration is calculated using the following formula:
[0181] .
[0182] In the formula, , A and B are the characteristic peak integral areas in the dry, hygroscopic, and regenerated states, respectively. The peak attenuation rate after hygroscopic absorption and the peak recovery rate after regeneration are both retained to one decimal place.
[0183] The enthalpy of exothermic crystallization was determined as follows: Referring to GB / T 19466.3-2025 "Differential Scanning Calorimetry (DSC) for Plastics - Part 3: Determination of Melting and Crystallization Temperatures and Enthalpies", 5–10 mg of the composite hygroscopic material was placed in a sealed crucible. The nitrogen flow rate was 50 mL / min, and the heating and cooling rates were both 10 °C / min. Baseline correction and integration were performed on the exothermic peak corresponding to the regeneration process to obtain the enthalpy of exothermic crystallization per unit mass of the composite hygroscopic material, expressed in J / g. The result was retained to one decimal place.
[0184] The embedding ratio of the composite moisture-absorbing material was determined using the following method: Five channel wall samples were taken at equal intervals along the radial direction of the dehumidifying wheel using cross-sectional microscopic image analysis. These samples were then resin-embedded, sectioned, and observed under a microscope. The original thickness of the glass fiber paper before the composite slurry was used as the pore area of the channel wall. The composite moisture-absorbing material area in the microscopic image was binarized, and the embedding ratio of the composite moisture-absorbing material was calculated using the following formula:
[0185] .
[0186] In the formula, The cross-sectional area of the composite moisture-absorbing material is within the original thickness range of the glass fiber paper; This represents the total cross-sectional area of the composite moisture-absorbing material. Five fields of view were analyzed for each sample, and a total of 25 fields of view were analyzed for each group. Results were retained to one decimal place.
[0187] The microcapsule gradient ratio was measured as follows: Using a cross-sectional sample with the same embedding ratio as the composite moisture-absorbing material, the composite moisture-absorbing layer was divided into a substrate-side region near the interior of the glass fiber paper and an airflow-side region near the airflow channel along the thickness direction. Image recognition methods were used to statistically analyze the proportion of the microcapsule cross-sectional area to the total area of the corresponding region in each region. The microcapsule gradient ratio was calculated using the following formula:
[0188] .
[0189] In the formula, φsubstrate side represents the area fraction of microcapsules in the substrate side region; φairflow side represents the area fraction of microcapsules in the airflow side region. The results are rounded to two decimal places.
[0190] The thermal conductivity was measured as follows: The determination was performed according to GB / T 42919.2-2025 "Determination of thermal conductivity and thermal diffusivity of plastics - Part 2: Transient planar heat source (heat plate) method". Flat plate samples with a thickness of 2.0 mm were prepared using the same raw material composition and crosslinking conditions as the composite hygroscopic material in each sample. After drying the samples to constant weight at 80℃, they were equilibrated for 24 hours at 25℃ and 50% relative humidity. The thermal conductivity was then measured at 25℃. Each sample was tested three times, and the results were retained to two decimal places, with units of W / (m·K).
[0191] The volume resistivity of the thermally conductive filler was measured in the following manner: according to GB / T 31838.2-2019 "Dielectric and resistive properties of solid insulating materials - Part 2: Resistive properties (DC method) - Volume resistivity and volume resistivity", the thermally conductive filler was pressed into a disc with a diameter of 50 mm and a thickness of 2.0 mm, and measured after equilibration in an environment of 23℃ and 50% relative humidity for 24 h. The volume resistivity of the hexagonal boron nitride disc was 3.6 × 10¹³ Ω·cm, and the volume resistivity of the alumina disc was 8.9 × 10¹³ Ω·cm.
[0192] The water vapor transmission rate of the porous protective layer was measured as follows: The test was conducted according to GB / T 1037-2021 "Determination of Water Vapor Transmission Performance of Plastic Films and Sheets - Cup Method (Gain and Loss Method)". Using the same spraying and curing conditions as the honeycomb dehumidifying rotor surface, independent protective layer samples were prepared on an inert release substrate. After peeling the protective layer from the release substrate, a cup test was performed at a temperature of 38℃ and a relative humidity difference of 90% between the two sides of the sample. The water vapor transmission rate was calculated based on the mass change per unit area and per unit time, expressed in g / (m²·24h), and the result was rounded to the nearest integer. This indicator was not measured for comparative samples without a protective layer.
[0193] The dynamic moisture absorption and average mass transfer rate in the first 10 minutes were measured as follows: The air handling, temperature and humidity measurement, and air-side moisture content calculation principles of the test bench followed GB / T 19411-2024 "Dehumidifiers". A sample with a diameter of 200 mm and an axial thickness of 100 mm was sealed and installed in the test duct. The inlet temperature of the treated air was 30.0 ± 0.3℃, the relative humidity was 80.0 ± 1.0%, and the wind speed on the sample was 2.00 ± 0.03 m / s. The test time was 60 minutes. The temperature and relative humidity of the inlet and outlet air were collected every 1 second. The air moisture content was calculated based on the dry-bulb temperature, relative humidity, and atmospheric pressure. The dynamic moisture absorption per unit dry basis (Q) over 60 minutes was calculated. 60 Calculate according to the following formula:
[0194] .
[0195] In the formula, This is the dry air mass flow rate, expressed in kg / min. Moisture content of inlet air, expressed in kg / kg dry air; Moisture content of the outlet air, expressed in kg / kg dry air; The dry weight of the composite moisture-absorbing material in the sample is expressed in kg. The unit is g / g, and the results are rounded to three decimal places; the average mass transfer rate R in the first 10 minutes. 10 Calculate according to the following formula:
[0196] .
[0197] In the formula, The value represents the unit dry basis dynamic moisture absorption in the first 10 minutes, with the denominator "10 minutes" representing the average time interval. The unit is g / (g·min), and the result is rounded to 4 decimal places.
[0198] The dry pressure drop and wet pressure drop drift rate were measured as follows: the straight pipe section layout, pressure tapping location, and differential pressure measurement principles of the pressure drop test section were in accordance with GB / T 14295-2019 "Air Filters". After the sample was dried to constant weight at 80℃, the dry pressure drop was measured at a face wind speed of 2.00 m / s. After the sample absorbed moisture for 60 min at 30℃ and 80% relative humidity, the wet pressure drop was immediately measured at the same face wind speed. The wet pressure drop drift rate was calculated according to the following formula:
[0199] .
[0200] In the formula, This refers to the wet pressure drop; This represents the dry-state pressure drop. The pressure drop is rounded to one decimal place, and the wet-state pressure drop drift rate is rounded to one decimal place.
[0201] The maximum temperature rise during the moisture absorption stage was measured using the following method: Five T-type thermocouples with a diameter of 0.2 mm were arranged along the thickness direction of the composite moisture-absorbing layer on the channel wall of the honeycomb airflow channel. The temperature was recorded every 1 second during the dynamic moisture absorption test, and the maximum temperature rise was calculated according to the following formula:
[0202] .
[0203] In the formula, This is the highest temperature measured on the channel wall during the moisture absorption process; This is for processing air inlet temperature. The maximum temperature rise is in °C, and the result is rounded to one decimal place.
[0204] The 90% regeneration time was measured as follows: After completing the 60-minute dynamic moisture absorption test, regeneration air with a temperature of 80.0±0.5℃, a relative humidity not exceeding 10%, and a face wind speed of 2.00±0.03m / s was immediately introduced into the sample. The amount of desorbed water per unit time was calculated based on the difference in moisture content between the inlet and outlet of the regeneration air. The amount of desorbed water was then integrated over time, and the time required for the cumulative desorbed water to reach 90% of the water absorption in the previous moisture absorption stage was recorded as the 90% regeneration time t. 90 The result is rounded to one decimal place and the unit is min.
[0205] The hygroscopic salt migration rate and core material migration rate were measured using the following method: An ion migration test method was employed. After each hygroscopic-regeneration cycle, downstream condensate and particulate filter eluent were collected. After 100 cycles, all gas flow channels of the sample were rinsed with 500 mL of deionized water, and the rinsing solution was collected. The contents of Li⁺ and K⁺ were determined using inductively coupled plasma atomic emission spectrometry (ICP-AES), and the contents of Cl⁻ and NO₃⁻ were determined using ion chromatography. The correlation coefficient of the standard curves for each analyte was not less than 0.999. The migration mass of lithium chloride was converted from the Li⁺ and Cl⁻ measurements, and the larger of the two conversion results was used. The migration mass of potassium nitrate or potassium chloride was converted from the corresponding cation and anion measurements, and the larger of the two conversion results was used. The hygroscopic salt migration rate was calculated using the following formula:
[0206] ;
[0207] Core material migration rate is calculated using the following formula:
[0208] .
[0209] In the formula, and These represent the cumulative mass of migrated hygroscopic salts and the initial mass of hygroscopic salts in the sample, respectively. and These represent the cumulative mass of the water-soluble crystalline compound that migrated and the initial mass of the compound in the sample, respectively.
[0210] Cyclic stability was measured as follows: one moisture absorption-regeneration cycle consisted of 60 min of moisture absorption at 30°C and 80% relative humidity, followed by regeneration at 80°C and relative humidity not exceeding 10% until the sample mass recovered to within 101% of its initial dry mass, for a total of 100 consecutive moisture absorption-regeneration cycles. The moisture retention rate was calculated using the following formula:
[0211] ;
[0212] The mass loss rate is calculated using the following formula:
[0213] .
[0214] In the formula, and The 60-minute unit dry basis dynamic moisture absorption is for the 100th cycle and the 1st cycle, respectively. and The dry weights of the samples are shown before and after 100 cycles, respectively.
[0215] Table 1. Microcapsule structure and reversibility test results
[0216] sample <![CDATA[D 50 / μm]]> Average shell thickness / μm Microcapsule integrity rate / % Crystal peak attenuation rate after moisture absorption / % Crystal peak recovery rate after regeneration / % Enthalpy of exothermic crystallization (J / g) Example 1 80.3 1.18 97.4 88.6 93.7 31.8 Example 6 20.4 1.21 93.6 91.8 90.2 32.5 Example 7 201.7 1.19 98.1 79.4 95.1 28.7 Example 8 79.8 0.49 91.7 93.5 87.8 33.2 Example 9 80.6 3.04 98.8 72.1 96.3 25.9 Example 10 80.1 1.20 97.1 84.3 92.8 27.6 Example 12 81.2 1.52 95.9 85.7 91.6 29.8 Comparative Example 4 — — — 80.5 61.2 21.3 Comparative Example 5 80.5 1.22 98.5 8.7 97.6 2.4 Comparative Example 14 79.1 1.17 72.6 63.8 70.4 17.1
[0217] Table 2. Test results of water vapor transmission rate of protective layer
[0218] sample Protective layer dry base load (g / m²) Water vapor transmission rate / [g / (m²·24h)] Example 1 4.0 1864 Example 13 4.0 1728 Comparative Example 10 0 — Comparative Example 11 15.0 236
[0219] Table 3. Test results of structure, heat transfer, and dynamic dehumidification of the embodiments.
[0220] sample Embedding ratio / % Microcapsule gradient ratio Thermal conductivity / [W / (m·K)] <![CDATA[Q 60 / (g / g)]]> <![CDATA[R 10 / [g / (g·min)]]]> Dry pressure drop / Pa Wet pressure drop drift rate / % Maximum temperature rise / °C <![CDATA[t 90 / min]]> Example 1 68.4 1.82 0.71 0.382 0.0107 81.7 11.1 3.9 31.6 Example 2 67.9 1.80 0.75 0.356 0.0093 80.9 10.5 5.3 37.8 Example 3 69.1 1.85 0.63 0.396 0.0109 86.4 19.8 3.5 30.9 Example 4 68.2 1.81 0.42 0.369 0.0094 80.8 10.8 5.7 39.2 Example 5 68.7 1.83 0.89 0.378 0.0108 84.6 15.6 3.6 30.7 Example 6 66.8 1.79 0.72 0.377 0.0112 84.2 14.8 3.8 30.4 Example 7 69.0 1.84 0.70 0.364 0.0090 83.5 13.6 4.5 35.8 Example 8 68.0 1.81 0.71 0.386 0.0115 82.0 13.9 3.7 30.8 Example 9 68.6 1.83 0.69 0.365 0.0092 82.1 11.8 4.4 35.6 Example 10 68.1 1.82 0.70 0.371 0.0100 82.1 11.7 4.2 33.8 Example 11 67.8 1.80 0.55 0.364 0.0095 82.5 12.1 4.9 36.2 Example 12 67.6 1.78 0.69 0.367 0.0098 82.8 12.6 4.4 34.7 Example 13 68.3 1.82 0.71 0.376 0.0104 82.3 10.4 4.0 32.5
[0221] Table 4. Migration and Cyclic Test Results of the Examples
[0222] sample Hygroscopic salt migration rate / % Core material migration rate / % Moisture retention rate after 100 cycles / % Quality loss rate / % Example 1 0.17 0.07 95.6 0.62 Example 2 0.16 0.06 94.2 0.74 Example 3 0.24 0.11 91.7 1.21 Example 4 0.18 0.08 93.3 0.81 Example 5 0.21 0.11 91.9 1.09 Example 6 0.27 0.20 91.4 1.18 Example 7 0.13 0.05 94.1 0.72 Example 8 0.29 0.24 90.8 1.26 Example 9 0.10 0.04 94.9 0.59 Example 10 0.18 0.09 94.4 0.69 Example 11 0.17 0.09 93.6 0.76 Example 12 0.20 0.11 92.8 0.88 Example 13 0.07 0.04 96.1 0.48
[0223] Table 5. Comparative test results of structure, heat transfer, and dynamic dehumidification.
[0224] sample Embedding ratio / % Microcapsule gradient ratio Thermal conductivity / [W / (m·K)] <![CDATA[Q 60 / (g / g)]]> <![CDATA[R 10 / [g / (g·min)]]]> Dry pressure drop / Pa Wet pressure drop drift rate / % Maximum temperature rise / °C <![CDATA[t 90 / min]]> Comparative Example 1 9.4 — 0.24 0.307 0.0068 90.4 40.4 8.3 49.2 Comparative Example 2 13.1 1.79 0.69 0.348 0.0082 109.6 38.1 4.4 34.8 Comparative Example 3 68.0 — 0.74 0.331 0.0076 81.2 14.7 8.0 44.7 Comparative Example 4 67.5 — 0.65 0.352 0.0085 82.5 23.4 5.7 39.8 Comparative Example 5 68.2 1.82 0.70 0.329 0.0074 81.9 11.4 7.6 43.2 Comparative Example 6 68.1 1.80 0.28 0.348 0.0081 80.8 12.9 7.0 42.1 Comparative Example 7 68.3 1.81 0.37 0.355 0.0087 82.3 13.9 5.9 39.5 Comparative Example 8 68.1 1.02 0.70 0.368 0.0093 88.8 22.4 4.4 34.3 Comparative Example 9 67.8 0.56 0.69 0.362 0.0091 91.6 27.9 4.3 34.6 Comparative Example 10 68.5 1.82 0.71 0.379 0.0105 80.9 28.8 4.0 31.9 Comparative Example 11 68.2 1.81 0.70 0.256 0.0059 95.3 7.9 3.7 32.4 Comparative Example 12 62.2 1.76 0.66 0.343 0.0081 84.1 25.5 5.5 40.6 Comparative Example 13 64.9 1.79 0.68 0.361 0.0090 82.8 43.2 4.6 36.8 Comparative Example 14 66.1 1.74 0.67 0.345 0.0080 83.0 20.2 5.2 38.7
[0225] Table 5. Comparative examples: migration and cyclic test results.
[0226] sample Hygroscopic salt migration rate / % Core material migration rate / % Moisture retention rate after 100 cycles / % Quality loss rate / % Comparative Example 1 2.41 — 76.8 3.82 Comparative Example 2 0.29 0.12 88.5 1.54 Comparative Example 3 0.24 — 88.9 1.63 Comparative Example 4 1.33 3.26 80.4 3.11 Comparative Example 5 0.18 0.04 91.2 0.93 Comparative Example 6 0.20 0.09 90.1 1.02 Comparative Example 7 0.22 0.10 91.4 0.96 Comparative Example 8 0.31 0.14 89.6 1.41 Comparative Example 9 0.46 0.19 86.8 1.83 Comparative Example 10 2.08 0.44 82.7 2.76 Comparative Example 11 0.06 0.03 94.1 0.57 Comparative Example 12 1.12 0.88 84.3 2.20 Comparative Example 13 2.41 0.71 74.8 4.06 Comparative Example 14 0.61 2.16 81.9 2.84
[0227] Experimental conclusions and analysis:
[0228] As shown in Tables 1-5, the median particle size of the microcapsules obtained in Example 1 is 80.3 μm, the average shell thickness is 1.18 μm, the microcapsule integrity rate is 97.4%, the crystal peak attenuation rate after moisture absorption is 88.6%, the crystal peak recovery rate after regeneration is 93.7%, and the exothermic enthalpy of crystallization is 31.8 J / g. This indicates that the polyamide shell of the microcapsules can allow water to pass through the inside and outside of the microcapsules while maintaining stable coating of the core material, so that potassium nitrate can undergo sufficient dissolution and crystallization transformation during moisture absorption and regeneration.
[0229] The median particle size of the microcapsules in Examples 6, 1, and 7 were 20.4 μm, 80.3 μm, and 201.7 μm, respectively. As the microcapsule particle size decreased, the attenuation rate of the crystal peak after moisture absorption and the average mass transfer rate in the first 10 minutes increased, but the integrity of the microcapsules decreased and the migration rate of the core material increased. As the microcapsule particle size increased, the integrity of the microcapsule and the recovery rate of the crystal peak after regeneration increased, but the dynamic moisture absorption and mass transfer rate decreased and the regeneration time was prolonged. This indicates that the microcapsule particle size needs to take into account the moisture transfer distance, shell integrity, and cycle stability.
[0230] The average shell thicknesses of Examples 8, 1, and 9 were 0.49 μm, 1.18 μm, and 3.04 μm, respectively. Thinner shells can reduce the resistance to water transfer across the shell and increase the crystal peak attenuation rate and the average mass transfer rate in the first 10 minutes after moisture absorption, but they will reduce the integrity of microcapsules and increase the migration rate of the core material. Thicker shells can improve the integrity of microcapsules and the retention capacity of the core material, but they will decrease the crystal peak attenuation rate and the exothermic enthalpy of crystallization after moisture absorption and prolong the regeneration time. This indicates that the shell thickness needs to maintain an appropriate balance between the water transfer capacity and the core material isolation capacity.
[0231] Comparative Example 5 uses a dense epoxy resin shell with an average thickness basically the same as that of Example 1. Although its microcapsule integrity rate reaches 98.5%, the crystal peak decay rate after moisture absorption is only 8.7%, the exothermic enthalpy of crystallization is only 2.4 J / g, the dynamic moisture absorption and the average mass transfer rate in the first 10 minutes decrease to 0.329 g / g and 0.0074 g / (g·min), respectively. The maximum temperature rise increases to 7.6℃ and the regeneration time to 90% is extended to 43.2 minutes. This indicates that when the shell only has a coating function and cannot allow water to pass through, the core material is difficult to undergo effective dissolution and crystallization transformation. Therefore, a continuous shell that allows water to pass through in both directions and restricts the mutual migration between the core material and the hygroscopic salt is a necessary condition for achieving thermal regulation.
[0232] Comparative Example 3, without microcapsules, showed a decrease in dynamic moisture absorption from 0.382 g / g in Example 1 to 0.331 g / g, an increase in maximum temperature rise from 3.9℃ to 8.0℃, and an extension of 90% regeneration time from 31.6 min to 44.7 min. This indicates that simply using thermally conductive fillers cannot replace the heat regulation effect generated by the dissolution and heat absorption of water-soluble crystalline compounds during moisture absorption and the heat release during crystallization during regeneration.
[0233] In Comparative Example 4, potassium nitrate was directly dispersed in a lithium chloride-containing polyvinyl alcohol crosslinked matrix. After regeneration, the crystal peak recovery rate decreased to 61.2%, the core material migration rate increased to 3.26%, the moisture absorption retention rate after 100 cycles decreased to 80.4%, and the mass loss rate increased to 3.11%. The corresponding values in Example 1 were 93.7%, 0.07%, 95.6%, and 0.62%, respectively. This indicates that direct contact between potassium nitrate and lithium chloride easily leads to ion migration, salt mixing, and uncontrolled crystallization. Spatial isolation of the water-soluble crystalline compound from the moisture-absorbing salt through microcapsules can maintain the reversible core material and improve cycle stability.
[0234] The microcapsule contents in Examples 2, 1, and 3 were 20.0% by mass, 28.0% by mass, and 40.0% by mass, respectively. As the microcapsule content increased, the dynamic moisture absorption increased from 0.356 g / g to 0.382 g / g and 0.396 g / g, respectively; the maximum temperature rise decreased from 5.3℃ to 3.9℃ and 3.5℃, respectively; and the 90% regeneration time decreased from 37.8 min to 31.6 min and 30.9 min, respectively. However, when the microcapsule content increased to 40.0% by mass, the dry pressure drop and wet pressure drop drift rates increased to 86.4 Pa and 19.8%, respectively, and the cyclic moisture absorption retention rate decreased to 91.7%. This indicates that increasing the microcapsule content is beneficial to improving the thermal regulation capability, but excessively high content will increase the space occupied by the particles and weaken the fixation effect of the hydrophilic crosslinked polymer matrix on each component.
[0235] The hexagonal boron nitride contents of Examples 4, 1, and 5 were 3.0%, 8.4%, and 12.0% by mass, respectively, with corresponding thermal conductivity of 0.42 W / (m·K), 0.71 W / (m·K), and 0.89 W / (m·K). As the hexagonal boron nitride content increased, the maximum temperature rise decreased and the regeneration time shortened. However, when the content increased to 12.0% by mass, the dry pressure drop and wet pressure drop drift rates increased. This indicates that an appropriate amount of thermally conductive filler is beneficial to improving heat transfer between the hygroscopic salt region and the microcapsules. On the other hand, excessively high content will increase the solid volume fraction of the composite hygroscopic material and affect moisture transfer and channel stability.
[0236] Comparative Example 6, without hexagonal boron nitride, has a thermal conductivity of only 0.28 W / (m·K), a maximum temperature rise of 7.0℃, and a regeneration time of 90% extended to 42.1 min. Comparative Example 7, although containing 8.4% by mass of hexagonal boron nitride, has an organosilicon coating layer on the surface of the hexagonal boron nitride that hinders the contact between adjacent fillers, resulting in a thermal conductivity of only 0.37 W / (m·K), a maximum temperature rise of 5.9℃, and a regeneration time of 90% of 39.5 min. This indicates that the thermal conductivity depends not only on the type and content of the thermally conductive filler but also on whether adjacent thermally conductive fillers can contact or overlap to form a thermally conductive network connecting the hygroscopic salt region and the microcapsule.
[0237] Comparative Example 1 directly coated polyvinyl alcohol and lithium chloride onto the surface of the airflow channel. Its composite moisture-absorbing material embedding ratio was only 9.4%, the dynamic moisture absorption was 0.307 g / g, the dry pressure drop was 90.4 Pa, the wet pressure drop drift rate reached 40.4%, the moisture salt migration rate reached 2.41%, and the moisture absorption retention rate after 100 cycles was only 76.8%. In contrast, Example 1 had an embedding ratio of 68.4%, a dynamic moisture absorption was 0.382 g / g, a dry pressure drop was 81.7 Pa, the wet pressure drop drift rate was 11.1%, the moisture salt migration rate was 0.17%, and the moisture absorption retention rate after 100 cycles was 95.6%. This shows that embedding the composite moisture-absorbing material at least partially into the pores of the channel wall can reduce the occupation of the effective cross section of the airflow channel and limit the migration of moisture salts while maintaining the moisture-absorbing material load.
[0238] Comparative Example 2, without applying negative pressure when loading the composite slurry, resulted in the composite hygroscopic material being mainly distributed on the surface of the glass fiber paper, with an embedding ratio of only 13.1%. The dry pressure drop reached 109.6 Pa, the wet pressure drop drift rate reached 38.1%, and the dynamic moisture absorption and the average mass transfer rate in the first 10 minutes decreased to 0.348 g / g and 0.0082 g / (g·min), respectively. This indicates that negative pressure-assisted loading can promote the composite slurry to enter the pores of the fiber sheet, reduce the accumulation of material on the airflow side surface, and improve the stability of the airflow channel in both dry and wet conditions.
[0239] Comparative Example 8 had the same microcapsule content in the substrate-side region and the airflow-side region, while Comparative Example 9 had a higher microcapsule content in the airflow-side region than in the substrate-side region. The wet pressure drop drift rates of the two were 22.4% and 27.9%, respectively, and the moisture absorption retention rates after 100 cycles were 89.6% and 86.8%, respectively, both lower than the 11.1% and 95.6% of Example 1. This indicates that preferentially distributing microcapsules in the substrate-side region can utilize the pores of the fiber sheet to contain and confine the microcapsules, and reduce the impact of airflow-side particle accumulation and volume changes after moisture absorption on the channel profile.
[0240] The dry basis loading of the porous protective layer in Examples 1 and 13 was 4.0 g / m², and the water vapor transmission rates reached 1864 g / (m²·24h) and 1728 g / (m²·24h), respectively. Both also had low wet pressure drop drift rate, hygroscopic salt migration rate and mass loss rate, indicating that the use of silicone resin or polyvinylidene fluoride to form a low-load porous protective layer can allow water vapor to enter the composite hygroscopic material and restrict the liquid hygroscopic salt solution and material particles from entering the airflow channel.
[0241] Comparative Example 10, without a porous protective layer, had an initial dynamic moisture absorption and a 90% regeneration time similar to Example 1. However, the wet pressure drop drift rate increased to 28.8%, the moisture salt migration rate increased to 2.08%, the moisture absorption retention rate after 100 cycles decreased to 82.7%, and the mass loss rate increased to 2.76%. This indicates that the porous protective layer is mainly used to suppress salt solution migration, particle shedding, and channel profile changes during long-term operation, rather than simply increasing the initial moisture absorption.
[0242] Comparative Example 11 increased the dry basis loading of the protective layer to 15.0 g / m² and formed a continuous dense membrane. Its water vapor transmission rate decreased to 236 g / (m²·24h), the dynamic moisture absorption and the average mass transfer rate in the first 10 minutes decreased to 0.256 g / g and 0.0059 g / (g·min), respectively, and the dry pressure drop increased to 95.3 Pa. This indicates that excessive loading of the protective layer and the formation of a dense structure will hinder water vapor transfer. Only by maintaining the porous structure of the protective layer and an appropriate loading can both component retention and water vapor transfer be achieved.
[0243] In Comparative Example 12, lithium chloride was directly added to the composite slurry, resulting in a decrease in its embedding ratio to 62.2%, an increase in wet pressure drop drift rate to 25.5%, an increase in hygroscopic salt migration rate and core material migration rate to 1.12% and 0.88%, respectively, and a decrease in the moisture retention rate after 100 cycles to 84.3%. This indicates that adding hygroscopic salt before the formation of the honeycomb matrix affects the crosslinking and rheological state of the hydrophilic polymer precursor solution and has an adverse effect on the stability of the microcapsules and the fixation state of each component. Therefore, impregnation with hygroscopic salt solution after the formation of the hydrophilic crosslinked polymer matrix is beneficial to keep the hygroscopic salt stably within the pores of the crosslinked matrix and fiber sheet.
[0244] Comparative Example 13, after the second crosslinking treatment was removed, was directly impregnated with lithium chloride. Its wet pressure drop drift rate reached 43.2%, the hygroscopic salt migration rate reached 2.41%, the moisture retention rate after 100 cycles decreased to 74.8%, and the mass loss rate increased to 4.06%. This indicates that the semi-cured structure formed by the first crosslinking is insufficient to resist salt solution impregnation and long-term moisture regeneration cycles. The second crosslinking can improve the stability of the hydrophilic polymer matrix and fix the position of microcapsules and thermally conductive fillers.
[0245] In Comparative Example 14, microcapsules were first added to a polyvinyl alcohol precursor solution, and then hexagonal boron nitride was added before high-shear dispersion. The integrity of the microcapsules decreased to 72.6%, the core material migration increased to 2.16%, the moisture retention rate after 100 cycles decreased to 81.9%, and the mass loss rate increased to 2.84%. This indicates that dispersing the thermally conductive filler first and then adding the microcapsules using a low-shear method after dispersion can reduce the damage to the microcapsule shell caused by mechanical shear while ensuring the dispersion effect of the thermally conductive filler.
[0246] Example 10 uses potassium chloride instead of potassium nitrate as the microcapsule core material; Example 11 uses alumina instead of hexagonal boron nitride; Example 12 uses cross-linked polyvinyl alcohol as the microcapsule shell; and Example 13 uses polyvinylidene fluoride to form a porous protective layer. All examples maintain the corresponding moisture absorption, thermal regulation, and cycle stability properties, indicating that the technical effect of the present invention mainly depends on whether the core material can undergo reversible dissolution and crystallization transformation, whether the shell layer can allow water transfer and restrict component migration, whether the thermally conductive filler can form a thermally conductive path, and whether the protective layer can maintain a porous and moisture-permeable structure, rather than being limited to a specific material.
[0247] In summary, this invention embeds at least partially the composite moisture-absorbing material into the pores of the channel walls of a honeycomb matrix, retaining moisture-absorbing salts, microcapsules, and thermally conductive and electrically insulating fillers within the hydrophilic cross-linked polymer matrix. This allows water-soluble crystalline compounds to undergo reversible dissolution and crystallization transformation within the selectively permeable shell. Heat is transferred between the moisture-absorbing salt region and the microcapsules through a thermally conductive network formed by adjacent thermally conductive fillers. Simultaneously, the gradient structure with a high microcapsule content on the substrate side and the porous protective layer on the airflow side stabilize the channel profile. This results in reduced moisture absorption temperature rise, regeneration time, wet pressure drop drift, and component migration while maintaining high dynamic moisture absorption and mass transfer rate, thereby improving long-term cycling stability.
[0248] The data from the examples and comparative examples also show that the microcapsule content, thermally conductive filler content, microcapsule particle size, shell thickness, and protective layer loading cannot be simply increased or decreased to continuously improve all performance. Each parameter is subject to the combined limitations of mass transfer rate, heat transfer capacity, material integrity, channel resistance, and cycle stability. Only under the material composition, structural distribution, and process sequence specified in this invention can low wind resistance, high mass transfer efficiency, and stable cycle performance be obtained simultaneously.
[0249] Based on the preferred embodiments of the present invention described above, those skilled in the art can make various changes and modifications without departing from the inventive concept. The technical scope of this invention is not limited to the contents of the specification, but must be determined according to the scope of the claims.
Claims
1. A honeycomb dehumidification rotor with low wind resistance and high mass transfer efficiency, comprising a honeycomb substrate, wherein the honeycomb substrate is provided with a plurality of axially penetrating airflow channels, characterized in that: The airflow channel wall is loaded with a composite moisture-absorbing material, and the composite moisture-absorbing material is at least partially distributed in the pores of the channel wall; The composite moisture-absorbing material includes a hydrophilic cross-linked polymer matrix, a moisture-absorbing salt retained in the hydrophilic cross-linked polymer matrix, microcapsules dispersed in the hydrophilic cross-linked polymer matrix, and a thermally conductive and electrically insulating filler. The microcapsule includes a shell and a core material covered by the shell. The shell allows water to pass through and inhibits the migration of the core material and the hygroscopic salt. The core material includes a water-soluble crystalline compound with a positive enthalpy of solubility in water. The water-soluble crystalline compound undergoes a reversible transition between a crystalline state and a dissolved state during hygroscopic and regeneration processes. At least some of the thermally conductive and electrically insulating fillers overlap each other to form a thermally conductive network that contacts the shell of at least a portion of the microcapsules.
2. The honeycomb dehumidifying impeller according to claim 1, characterized in that: The hydrophilic crosslinked polymer matrix includes one or more of polyacrylamide, polyacrylic acid or its salts, polyvinyl alcohol, alginate, carboxymethyl cellulose and hydroxyethyl cellulose; The hygroscopic salt includes one or more of lithium chloride, calcium chloride, magnesium chloride, and lithium bromide.
3. The honeycomb dehumidifying impeller according to claim 1, characterized in that: The water-soluble crystalline compound includes one or both of potassium nitrate and potassium chloride, and the water-soluble crystalline compound is at least partially crystalline in the dry state of the microcapsules; The water-soluble crystalline compound transforms at least partially from a crystalline state to a dissolved state during the process of the composite moisture-absorbing material absorbing moisture, and at least partially transforms from a dissolved state to a crystalline state during the process of the composite moisture-absorbing material being heated and regenerated and its moisture content decreasing.
4. The honeycomb dehumidifying impeller according to claim 1, characterized in that: The shell of the microcapsule comprises one or more of the following: cross-linked polyvinyl alcohol, polyamide, cellulose acetate, a composite material formed from chitosan and alginate, and polyethersulfone. The shell is a continuous shell that allows water to pass bidirectionally between the core material and the hydrophilic crosslinked polymer matrix, while inhibiting the migration of the water-soluble crystalline compound out of the microcapsule and the entry of the hygroscopic salt into the microcapsule.
5. The honeycomb dehumidifying impeller according to claim 1, characterized in that: The thermally conductive and electrically insulating filler includes one or more of hexagonal boron nitride, aluminum oxide, aluminum nitride, and magnesium oxide; The thermally conductive and electrically insulating filler is in the form of flakes, fibers, granules, or a combination thereof, and forms a thermally conductive network in the hydrophilic crosslinked polymer matrix connecting the region containing the hygroscopic salt to the microcapsules.
6. The honeycomb dehumidifying impeller according to claim 1, characterized in that: Based on the total dry weight of the composite moisture-absorbing material, the content of the hydrophilic crosslinked polymer matrix is 15-45% by mass, the content of the moisture-absorbing salt is 20-50% by mass, the content of the microcapsules is 20-55% by mass, and the content of the thermally conductive and electrically insulating filler is 1-15% by mass. The total mass of the hydrophilic crosslinked polymer matrix, the hygroscopic salt, the microcapsules, and the thermally conductive and electrically insulating filler accounts for 90-100% of the total dry mass of the composite hygroscopic material. The median particle size of the microcapsules is 5 to 300 micrometers, and the average thickness of the shell is 0.1 to 10 micrometers.
7. The honeycomb dehumidifying impeller according to claim 1, characterized in that: The composite moisture-absorbing material forms a composite moisture-absorbing layer having an airflow side region and a substrate side region, wherein the airflow side region is close to the airflow channel and the substrate side region is close to the interior of the honeycomb matrix; The microcapsule volume content in the substrate side region is greater than the microcapsule volume content in the airflow side region, and at least a portion of the microcapsules are embedded in the pores of the channel wall.
8. The honeycomb dehumidifying impeller according to claim 1, characterized in that: The composite moisture-absorbing material has a porous protective layer on the side facing the airflow channel. The porous protective layer allows water vapor to pass through and restricts the liquid moisture-absorbing salt solution and the microcapsules from entering the airflow channel. The porous protective layer includes one or more of polytetrafluoroethylene, polyvinylidene fluoride and silicone resin. The honeycomb matrix includes one of glass fiber paper, ceramic fiber paper, aluminosilicate fiber paper, and cellulose-inorganic fiber composite paper.
9. A method of manufacturing a low- pressure-drop high-mass-transfer-efficiency honeycomb dehumidifying rotary wheel, characterized by, Includes the following steps: S1, dispersing an aqueous phase containing a water-soluble crystalline compound in a continuous phase that is immiscible with water to form droplets, forming a shell layer at the interface of the droplets that allows water to pass through and inhibits the passage of ions and the water-soluble crystalline compound, separating and drying the droplets with the shell layer, so that the water-soluble crystalline compound at least partially crystallizes within the shell layer, to obtain microcapsules; S2, dispersing thermally conductive and electrically insulating fillers in a hydrophilic polymer precursor solution, and then adding the microcapsules to the hydrophilic polymer precursor solution to obtain a composite slurry; S3, the composite slurry is loaded onto the fiber sheet, so that at least part of the composite slurry enters the pores of the fiber sheet, and the hydrophilic polymer precursor liquid is subjected to a first crosslinking treatment to obtain the composite sheet; S4, corrugating the composite sheet, connecting the corrugated composite sheet with the flat sheet and winding it to obtain a honeycomb matrix with multiple axial airflow channels; S5, the hydrophilic polymer is subjected to a second crosslinking treatment to form a hydrophilic crosslinked polymer matrix, and at least some of the thermally conductive and electrically insulating fillers are overlapped to form a thermally conductive network. S6. The honeycomb matrix is impregnated with a hygroscopic salt solution to allow the hygroscopic salt to enter and remain in the hydrophilic crosslinked polymer matrix, followed by drying to obtain the honeycomb dehumidification wheel.
10. The manufacturing method according to claim 9, characterized in that: In step S1, the water-soluble crystalline compound and water-soluble amine monomer are added to water to form the aqueous phase, and an organic solution containing acyl chloride monomer is used as the continuous phase. The droplets formed by the aqueous phase are brought into contact with the continuous phase to form a polyamide shell at the interface of the droplets. In step S3, a first composite slurry with a higher microcapsule content is first loaded onto the fiber sheet, and then a second composite slurry with a lower microcapsule content is loaded onto the side of the first composite slurry away from the fiber sheet. After step S6, a porous protective layer is formed on the surface of the channel wall of the airflow channel, allowing water vapor to pass through and restricting the entry of liquid hygroscopic salt solution into the airflow channel.