A catalyst support and its modification method and application
By doping Ni2+ or Co2+ into the TiO2 support to form oxygen vacancies, the problem of easy corrosion of the catalyst under high acidity conditions was solved, resulting in a catalyst with high specific surface area and thermal stability, which improved the catalytic activity and stability of biomass oil hydrodeoxygenation.
Patent Information
- Application Number
- CN202611221538.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-12
- Publication Date
- 2026-11-17
AI Technical Summary
Existing catalyst supports are prone to corrosion under high acidity and high water vapor partial pressure conditions, leading to a decrease in specific surface area and rapid deactivation, making long-term stable operation impossible. In particular, they exhibit poor catalytic activity during the hydrodeoxygenation of biomass oil.
By replacing Ti4+ in the TiO2 lattice with doped elements Ni2+ or Co2+ to form oxygen vacancies, a catalyst support is prepared by co-precipitation. Combined with forming agents such as silica sol, the doped elements are uniformly embedded to form a high specific surface area and thermal stability.
Under highly acidic conditions, the catalyst support exhibits high activity and long lifetime, effectively suppressing the transformation of the anatase phase to the rutile phase, maintaining high specific surface area and thermal stability, and achieving efficient hydrodeoxygenation reaction.
Smart Images

Figure CN123102369A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of catalyst technology, specifically to a catalyst support, its modification method, and its application. Background Technology
[0002] In the hydrodeoxygenation (HDO) process of biomass oils or high-acid oils, Ni(Co)-MoS2 / Al2O3 is currently the most widely used commercial catalyst. However, under the strongly acidic and high water vapor partial pressure conditions of the reaction, alumina supports are prone to corrosion and hydration reactions, leading to a sharp decrease in the specific surface area of the catalyst and even pulverization, resulting in rapid catalyst deactivation. This not only increases production costs but also makes it difficult to achieve long-term stable operation of the production process. To solve these problems, titanium dioxide (TiO2), with its excellent chemical stability and resistance to acid and alkali corrosion, is considered a highly promising alternative support. TiO2 exists in two main crystalline phases: the metastable anatase phase and the thermodynamically stable rutile phase. The highly active anatase phase irreversibly transforms into the rutile phase during high-temperature calcination (usually >400℃), accompanied by severe grain sintering, resulting in a rapid decrease in its specific surface area, thus rendering it unusable as a catalyst support. Existing technologies have reported a composite supported catalyst, NiMo / Al2O3-TiO2, which exhibits high catalytic activity in the hydrodesulfurization of traditional petroleum fractions. However, when applied to the hydrodeoxygenation of biomass carboxylic acids and oils with high acidity and high oxygen content, this catalyst system still has significant drawbacks: on the one hand, although the TiO2 component in the support is corrosion-resistant, it inevitably undergoes a transformation from anatase to rutile phase during high-temperature roasting, resulting in a significant decrease in specific surface area, making it difficult to balance high specific surface area and high thermal stability; on the other hand, the Al2O3 component still undergoes corrosion and hydration reactions in strongly acidic reaction environments, causing catalyst structural collapse and rapid activity decay. Therefore, this composite support strategy fails to fundamentally solve the key problem of poor catalyst stability in the hydrodeoxygenation process of high-acid biomass. Summary of the Invention
[0003] This application provides a catalyst support, its modification method, and its application to solve the problems of titanium dioxide-based catalyst supports exhibiting decreased specific surface area and poor thermal stability during high-temperature calcination, resulting in poor catalytic activity when applied to the hydrodeoxygenation of highly acidic biomass.
[0004] In a first aspect, this application provides a catalyst support comprising titanium dioxide and a dopant element. The dopant element, based on the mass of the titanium dioxide, has a content of 0.5 wt%-10 wt%, and the dopant element includes at least one of nickel or cobalt. The dopant element is intercalated into the titanium dioxide lattice in ionic form, heterovalently substituting Ti. 4+ It creates oxygen vacancies at the site.
[0005] In one optional embodiment, the content of the dopant element is 2wt%-8wt% based on the mass of titanium dioxide. When the dopant content is within this preferred range, the specific surface area retention rate of the support after calcination at 600°C can be maintained at an excellent level of about 90%, exhibiting optimal overall performance.
[0006] In one optional embodiment, when the dopant element is nickel, the nickel content is 3wt%-5wt% based on the mass of titanium dioxide; when the dopant element is cobalt, the cobalt content is 2wt%-6wt% based on the mass of titanium dioxide.
[0007] Secondly, this application also provides a method for modifying the above-mentioned catalyst support, comprising the following steps: in the presence of a dispersant, a dopant and a titanium source are subjected to a co-precipitation reaction, a precursor is obtained by solid-liquid separation, and the precursor is calcined to obtain a catalyst support; wherein the dopant includes at least one of a nickel source or a cobalt source.
[0008] In one optional embodiment, the dispersant includes at least one of polyethylene glycol, polyvinylpyrrolidone, and hexadecyltrimethylammonium bromide, preferably polyethylene glycol; the titanium source includes at least one of tetrabutyl titanate, titanium oxysulfate, and titanium tetrachloride; the nickel source includes at least one of nickel nitrate, nickel sulfate, and nickel chloride; the cobalt source includes at least one of cobalt nitrate, cobalt sulfate, and cobalt chloride; the modification method further includes the steps of mixing, molding, drying, and calcining the catalyst support, binder, and additives.
[0009] In one optional embodiment, the polyethylene glycol has a molecular weight of 400-10000; the amount of dispersant is 0.5wt%-5wt% based on the total weight of the dopant and titanium source; the mass of the auxiliary agent is 0.5wt%-5wt% based on the mass of the catalyst support; the pH value of the coprecipitation reaction is 7-10; before solid-liquid separation, the mixture after the coprecipitation reaction is stirred for 2-3 hours and aged for 12-24 hours; the calcination temperature of the precursor is 350℃-450℃, and the calcination time is 3-5 hours; the calcination temperature of the catalyst support and auxiliary agent mixture is 500℃-600℃, and the calcination time is 3-5 hours; the binder includes silica sol; the auxiliary agent includes at least one of guar gum powder, polyvinyl alcohol, and methylcellulose.
[0010] Thirdly, this application provides a catalyst comprising the catalyst support and active component described above.
[0011] In one optional embodiment, the active component includes molybdenum; the catalyst has a specific surface area greater than 150 m². 2 / g, compressive strength greater than 100N / cm.
[0012] In one optional embodiment, the catalyst is obtained by an equal-volume impregnation method, in which a solution containing a molybdenum source is impregnated onto a catalyst support, dried, and calcined. In one optional embodiment, the active component is MoO3, and the active component is a catalyst with a mass of 10-30 wt%.
[0013] Fourthly, the catalyst provided in this application can be applied to the hydrodeoxygenation of oxygen-containing compounds.
[0014] In one optional embodiment, the acid value of the oxygen-containing compound is ≥10 mg KOH / g. The oxygen-containing compound includes at least one of highly acidic oils, biomass pyrolysis oils, waste cooking oils, and acidified palm oils.
[0015] The technical solution of this application has the following advantages: 1. This application provides a catalyst support based on titanium dioxide, using ions with ionic radii slightly larger than Ti. 4+ Ni 2+ or Co 2+ As a dopant element, Ti in a six-coordinate environment 4+ The effective ionic radius of Shannon is 0.605 Å, Ni 2+ It is 0.69 Å, Co 2+ With a spin of 0.745 Å, when these divalent ions partially replace the tetravalent titanium ions in the TiO2 lattice, oxygen vacancies are simultaneously generated in the lattice to maintain charge balance. This lattice contraction / expansion distortion caused by heterovalent substitution, in synergy with oxygen vacancy defects, inhibits the transformation of the anatase phase to the rutile phase from multiple levels, thereby improving the thermal stability of the catalyst support: (a) it increases the atomic rearrangement energy barrier required for local phase transitions; (b) the coordination unsaturated environment formed around the oxygen vacancies pins the lattice interface, hindering grain boundary migration; and (c) the change in surface energy makes the anatase phase more thermodynamically stable. Meanwhile, this application precisely limits the content of doping elements to 0.5 wt%-10 wt%. Doping amounts within this range can generate a sufficient density of oxygen vacancy defects, effectively inhibiting the transformation of the anatase phase to the rutile phase and excessive grain growth, while avoiding a significant reduction in the specific surface area of the support due to the formation of a separated phase from excessive doping.
[0016] 2. The catalyst support provided in this application has a doping element content of 2wt%-8wt% based on the mass of titanium dioxide. When the doping content is 2wt%-8wt%, a more ideal balance can be achieved between suppressing phase transition and maintaining a high specific surface area, resulting in a catalyst support with both higher specific surface area and better thermal stability.
[0017] 3. This application provides a method for modifying a catalyst support, in which doping is performed via co-precipitation in the presence of a dispersant. This method enables uniform mixing of dopant ions with the titanium source at the atomic level, ensuring Ni... 2+ or Co 2+ The efficient embedding of the TiO2 lattice, rather than just enriching it on the surface, maximizes the effect of oxygen vacancies and lattice stress generated by heterovalent doping on suppressing phase transitions. The resulting support exhibits high activity, good stability, and long service life under high acid conditions.
[0018] 4. This application provides a method for modifying a catalyst support, wherein the dispersant is preferably polyethylene glycol. On the one hand, the ether groups (-O-) and hydroxyl groups (-OH) on its molecular chain can be adsorbed on the surface of newly formed nanoparticles, forming a steric hindrance protective layer, effectively preventing particle agglomeration, thereby obtaining an ultrafine, highly dispersed precursor powder, laying the foundation for the large specific surface area of the final support; on the other hand, the hydroxyl groups on the polyethylene glycol molecular chain can coordinate with the dopant elements nickel or cobalt. This coordination effect helps nickel or cobalt ions to be more uniformly embedded in the titanium dioxide lattice, avoiding local enrichment or phase separation, thereby further enhancing the structural uniformity and thermal stability of the support.
[0019] 5. This application provides a method for modifying a catalyst support, using silica sol as a molding binder. Silica sol not only ensures the mechanical strength of the molded body, but also possesses extremely stable chemical properties, preventing damage to the support under strongly acidic conditions. Combined with organic additives such as guar gum powder, it can improve the plasticity of the molded material, making the molding process smoother, and the additives completely decompose during calcination, leaving no harmful residues.
[0020] 6. This application provides a catalyst comprising the above-described support and a molybdenum-containing active component supported thereon. The support prepared in this application not only possesses high specific surface area and high hydrothermal stability, but also exhibits Ni content that has migrated from or remains in the crystal lattice on its surface. 2+ / Co 2+ Species (forming NiO) x or CoO x Clusters can act as Lewis acid sites, generating strong electrostatic and coordination interactions, effectively anchoring molybdate anions (such as Mo7O). 24 6- MoO4 2-This "anchoring effect" inhibits the agglomeration and crystal growth of MoO3 during subsequent calcination, promotes the formation of a highly intrinsically active Ni-Mo-S (Type II) phase after sulfidation, and improves the dispersion and catalytic efficiency of the active component. Simultaneously, the formed dense MoS2 capping layer acts as a physical barrier, protecting the dopants in the support from leaching and loss by the acidic medium. This achieves a dual synergistic effect of structural stability and catalytic enhancement between the support and the active component, resulting in a catalyst exhibiting excellent hydrodeoxygenation activity and long-term stability.
[0021] 7. This application provides the application of the above-mentioned catalyst in the hydrodeoxygenation of highly acidic oils. The catalyst exhibits a high deoxygenation rate and saturated alkane yield for highly acidic oils, and maintains excellent stability after 1000 hours of continuous operation, far exceeding that of traditional catalysts. Attached Figure Description
[0022] To more clearly illustrate the technical solutions in the specific embodiments of this application or the prior art, the drawings used in the description of the specific embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of this application. For those skilled in the art, other drawings can be obtained from these drawings without creative effort.
[0023] Figure 1 The XRD patterns are of the catalyst supports prepared in Examples 1-6 and Comparative Examples 1-3 of this application. Figure 2 This is a microstructure image of the catalyst support prepared in Example 1 of this application, wherein, Figure 2 In the image, A is the SEM image of the catalyst support prepared in Example 1. Figure 2 B in the image is the HRTEM image of the catalyst support prepared in Example 1; Figure 3 The microstructure images of the catalysts provided in Application Examples 1 and 2 of this application are shown in the following figures. Figure 3 C is a TEM image of the catalyst prepared using Example 1. Figure 3 D in the figure represents the TEM image of the catalyst prepared using Example 13; Figure 4 Comparison of the 1000-hour operational stability of the catalyst provided in Application Example 1 and a commercial catalyst. Detailed Implementation
[0024] The following embodiments are provided to better understand this application. However, the following embodiments do not constitute a limitation on the content and scope of protection of this application. Any product that is the same as or similar to this application, derived by anyone under the guidance of this application or by combining the features of this application with other prior art, falls within the scope of protection of this application.
[0025] Unless otherwise specified, all experimental steps or conditions in the examples were performed according to conventional experimental procedures and conditions in the art. Reagents or instruments whose manufacturers are not specified are all commercially available products.
[0026] Example 1 This embodiment provides a method for modifying a catalyst support, with the specific steps and parameters as follows: 1. Dissolve 100g tetrabutyl titanate and 8.5g nickel nitrate hexahydrate in 500mL anhydrous ethanol, add 2.0g polyethylene glycol (PEG-2000), and stir until homogeneous; At 800 rpm, the mixed solution was slowly added dropwise to 500 mL of deionized water. The pH of the mixed solution was adjusted to 8.5 with ammonia water to induce a co-precipitation reaction. After stirring for 2 hours, the mixture was allowed to stand and age for 12 hours to obtain the slurry. 2. The obtained slurry is filtered to separate the solid and liquid. The solid precipitate is washed with deionized water until neutral and dried at 110°C for 12 hours to obtain the precursor of the carrier material. The dried precursor was calcined at 450°C for 4 hours to obtain nickel-modified TiO2 nanopowder.
[0027] 3. Mix 100g of the above nano powder, 30g of silica sol (solid content of 20%), and 2g of guar gum powder, add an appropriate amount of deionized water and knead to form a plastic mud ball. Extrude the mud ball into strips (diameter 1.5mm), dry at 110℃ for 6 hours, and then calcine at 550℃ for 4 hours to obtain the catalyst carrier of this embodiment.
[0028] The catalyst support prepared in this example was determined by inductively coupled plasma optical emission spectrometry (ICP-OES). The nickel content was 4.8 wt% based on the mass of titanium dioxide.
[0029] Example 2 This embodiment provides a method for modifying a catalyst support, with the specific steps and parameters as follows: (1) Dissolve 120g of titanium oxysulfate (titanium source) and 1.7g of nickel nitrate hexahydrate in 600mL of deionized water, add 4.8g of polyethylene glycol (PEG-6000), and stir until homogeneous. Under vigorous stirring, adjust the pH to 9.0 with ammonia water to induce a coprecipitation reaction. Continue stirring for 3 hours, then allow to stand for 24 hours to age.
[0030] (2) The obtained slurry was filtered to separate the solid and liquid phases. The solid precipitate was washed with deionized water until neutral and dried at 100°C for 10 hours to obtain the precursor of the carrier material. The dried precursor was calcined at 450°C for 3 hours to obtain nickel-modified TiO2 nanoparticles.
[0031] (3) Mix 100g of the above nano powder, 25g of silica sol (30% solid content of silica sol) and 1.5g of polyvinyl alcohol, add an appropriate amount of deionized water and knead to form a plastic clay.
[0032] (4) The mud lumps are extruded into strips (2.0 mm in diameter), dried at 100°C for 8 hours, and then calcined at 500°C for 5 hours to obtain the catalyst support of this embodiment.
[0033] The catalyst support prepared in this example was determined by inductively coupled plasma optical emission spectrometry (ICP-OES). The nickel content was 0.9 wt% based on the mass of titanium dioxide.
[0034] Example 3 This embodiment provides a method for modifying a catalyst support, with the specific steps and parameters as follows: (1) Dissolve 90g of titanium tetrachloride (titanium source) and 16.2g of nickel nitrate hexahydrate in 450mL of ice water, add 1.8g of polyethylene glycol (PEG-10000), and stir until homogeneous. Under vigorous stirring, adjust the pH to 8.0 with ammonia water to induce a coprecipitation reaction. Continue stirring for 2 hours, then allow to stand and age for 18 hours.
[0035] (2) The obtained slurry was filtered to separate the solid and liquid phases. The solid precipitate was washed with deionized water until neutral and dried at 90°C for 15 hours to obtain the precursor of the carrier material. The dried precursor was calcined at 350°C for 5 hours to obtain nickel-modified TiO2 nanoparticles.
[0036] (3) Mix 100g of the above nano powder, 35g of silica sol (solid content 25%) and 2.5g of methylcellulose, add an appropriate amount of deionized water and knead to form a plastic clay.
[0037] (4) The mud lumps are extruded into strips (1.8 mm in diameter), dried at 90°C for 10 hours, and then calcined at 600°C for 3 hours to obtain the catalyst support of this embodiment.
[0038] The catalyst support prepared in this example was determined by inductively coupled plasma optical emission spectrometry (ICP-OES). The nickel content was 9.5 wt% based on the mass of titanium dioxide.
[0039] Example 4 This embodiment provides a method for modifying a catalyst support. The specific steps and parameters are the same as in Example 1, except that cobalt nitrate is used instead of nickel nitrate.
[0040] Example 5 This embodiment provides a method for modifying a catalyst support. The specific steps and parameters are the same as in Example 1, except that in step 1, the amount of nickel nitrate hexahydrate is reduced from 8.5g to 4.17g, and 4.33g of cobalt nitrate hexahydrate is added.
[0041] The catalyst support prepared in this example was determined by inductively coupled plasma optical emission spectrometry (ICP-OES). The cobalt content was 2.5 wt%, the nickel content was 2.4 wt%, and the total dopant content was 4.9 wt%, based on the mass of titanium dioxide.
[0042] Example 6 This embodiment provides a method for modifying a catalyst support. The specific steps and parameters are the same as in Example 1, except that an equal mass of polyvinylpyrrolidone is used instead of polyethylene glycol.
[0043] Examples 7-12 This embodiment provides a catalyst support modification method. The specific steps and parameters are the same as in Example 1. The difference is that in step 1, the amount of nickel nitrate hexahydrate is adjusted so that the Ni content in the final product is approximately 0.5wt%, 1wt%, 3wt%, 5wt%, 8wt%, and 10wt% of the titanium dioxide mass. The amount of nickel nitrate hexahydrate corresponding to the target Ni content is 0.89g, 1.77g, 5.31g, 8.85g, 14.17g, and 17.71g, respectively.
[0044] Comparative Example 1 This comparative example provides a method for modifying a catalyst support. The specific steps and parameters are the same as in Example 1. The difference is that step 1 does not contain nickel nitrate hexahydrate, that is, 100g of tetrabutyl titanate is directly dissolved in 500mL of anhydrous ethanol; the remaining steps are the same as in Example 1.
[0045] Comparative Example 2 This comparative example provides a method for modifying a catalyst support. The specific steps and parameters are the same as in Example 1. The difference is that in step 1, the amount of nickel nitrate hexahydrate is adjusted to 21.25g, so that the Ni content in the final product is about 12wt% of the mass of titanium dioxide.
[0046] Comparative Example 3 This comparative example provides a catalyst support modification method. The specific steps and parameters are the same as in Example 1, except that equimolar (based on ion valence state correction) copper nitrate trihydrate is used instead of nickel nitrate hexahydrate, so that the Cu content in the final product is 4.8 wt% of the titanium dioxide mass. Copper is chosen as a comparison to illustrate that with similar radius dimensions (Cu... 2+ It has a six-coordinate radius of 0.73 Å, but it is not easy to form equivalent or variable valence ions with stable oxygen vacancies, and thus cannot achieve a synergistic stabilizing effect.
[0047] Application Example 1-15 This application example provides a method for preparing a catalyst, with the specific steps and parameters as follows: Ammonium molybdate solution was impregnated onto the catalyst supports prepared in Examples 1-12 and Comparative Examples 1-3 using an equal-volume impregnation method to obtain intermediates. The MoO3 loading on each intermediate was controlled to be 18 wt%. The intermediates were dried at 110 °C and then calcined at 450 °C for 4 h to obtain the catalyst.
[0048] The catalyst was subjected to sulfidation treatment at 400℃ with a gas mixture containing 10% H2S / H2 for 2 hours to obtain a sulfidated catalyst for later use.
[0049] Experimental Example 1: Testing of Crystal Phase and Texture Properties of Support The catalyst supports prepared in Examples 1-6 and Comparative Examples 1-3 were characterized by XRD, and the specific surface area, average pore size, pore volume, and compressive strength of each catalyst support were measured. The results are shown in the figure. Figure 1 See Table 1.
[0050] Among them, the specific surface area, average pore size and pore volume were measured using a fully automatic specific surface area and pore size analyzer, and the compressive strength was measured according to the industry standard HG / T 2782-2024.
[0051] The catalyst supports prepared in Examples 1-6 and Comparative Examples 1-3 were treated with water vapor at 180°C and 0.8 MPa for 100 h, and their specific surface area and compressive strength were measured again. The results are shown in Table 1.
[0052] The specific surface area retention rate and compressive strength retention rate of the catalyst support were calculated. Wherein, specific surface area retention rate = specific surface area of catalyst support after hydrothermal treatment / specific surface area of catalyst support before hydrothermal treatment × 100%; Compressive strength retention rate = (compressive strength of catalyst support after hydrothermal treatment / compressive strength of catalyst support before hydrothermal treatment) × 100%.
[0053] Table 1 Basic properties of catalyst support
[0054] like Figure 1 As shown, all samples exhibited characteristic diffraction peaks of the anatase phase TiO2 at 2θ = 25.3°, 37.8°, 48.0°, 53.9°, and 55.1°, corresponding to the (101), (004), (200), (105), and (211) crystal planes, respectively. Comparative Example 1 (undoped TiO2) showed a distinct rutile phase (110) characteristic peak at 2θ = 27.4°, and its rutile phase content was approximately 25% according to semi-quantitative analysis, consistent with the data in Table 1. Examples 1 and 3-6 showed no obvious diffraction peaks at 2θ = 27.4°, proving that they were pure anatase phases; Example 2 (Ni doping amount 0.9wt%) showed only a very weak rutile characteristic peak at this position, indicating that the phase transition suppression effect was slightly weaker at low doping amounts but still significantly better than that of the undoped samples. Comparative Example 2 (Ni doping 12wt%) showed a NiO (200) characteristic peak at 2θ=43.3°, confirming that excessive doping led to the formation of NiO segregated phases; Comparative Example 3 (Cu doping) showed a significantly higher intensity rutile characteristic peak at 2θ=27.4° than all Ni / Co doped samples, further proving that Cu²⁺… + It cannot effectively suppress the transformation of the anatase phase to the rutile phase.
[0055] The microstructure of the carrier obtained in Example 1 is as follows Figure 2 As shown in the SEM images, the carrier is composed of uniformly sized nanoparticles with an average particle size of approximately 20-30 nm. No obvious aggregation is observed, and abundant mesoporous structures are formed between the particles. This is consistent with the 185.3 nm particle size recorded in Table 1. 2 / g high specific surface area and 0.48cm 3 The pore volume of / g is consistent with the phase, and the lattice stripes with a spacing of 0.35nm are clearly visible in the HRTEM image, which corresponds to the (101) crystal plane of the anatase phase TiO2. No lattice stripes of the (110) crystal plane (0.32nm) of the rutile phase or the NiO phase were observed, which proves that Ni ions have been uniformly embedded in the TiO2 lattice and have not formed an independent oxide phase. The support maintains the complete pure anatase crystal phase structure.
[0056] Furthermore, according to Figure 1As shown in Table 1, the catalyst supports provided in Examples 1-3, under the same calcination temperature, almost maintained a pure anatase phase or contained only trace amounts of rutile phase, proving that nickel doping effectively suppressed the phase transition. Example 2, due to its lower nickel content, showed a slightly weaker but still significant suppression effect. Examples 4-6, through cobalt doping or changing the dispersant, also obtained a pure anatase phase and high specific surface area, demonstrating the universality of the technical solution. In stark contrast, Comparative Example 1, with its undoped TiO2 support, exhibited obvious rutile diffraction peaks; Comparative Example 2, due to its nickel content exceeding the upper limit, although suppressing the phase transition, showed NiO separation phases, leading to a decrease in specific surface area and intensity; Comparative Example 3, using copper doping, showed a much weaker ability to suppress the phase transition than nickel / cobalt, because Cu... 2+ Without generating an equal amount of stable oxygen vacancies, an effective pinning and energy barrier effect cannot be formed.
[0057] After hydrothermal treatment, the specific surface area retention rate and compressive strength retention rate of all embodiments reached over 88%, while the comparative examples were all below 84%, proving that the doped and modified carrier has excellent hydrothermal stability.
[0058] Experimental Example 2: Thermal Stability Test of Carriers with Different Doping Elements and Contents The catalyst supports provided in Examples 7-12 and Comparative Example 2 of this application were calcined at 600°C for 3 hours. The changes in crystal phase composition and specific surface area of each support after calcination were measured, and the results are shown in Table 2.
[0059] Table 2 Thermal stability test of carriers with different doping elements and contents
[0060] As shown in Table 2, the content of doping elements has a regular effect on the thermal stability of the carrier. The overall trend is that with the increase of doping amount, the performance first increases and then slowly decreases, exhibiting a volcano-shaped curve. Specific analysis is as follows: When the doping concentration was 0.5 wt% (Example 7), the rutile phase content decreased significantly from 25.8% in undoped TiO2 (Comparative Example 1) to 8.3%, and the specific surface area retention rate increased significantly from 69.7% to 87.9%, proving that only a very small amount of Ni is needed. 2+ Doping can produce a considerable phase transition suppression effect. When the doping amount increases to 1-8 wt% (Examples 8-11), the rutile phase content further decreases to below 1.7% until it disappears completely, and the specific surface area retention rate is close to or exceeds 90%, reaching an optimal level of 92.2%-93.7% in the range of 3-5 wt%. When the doping amount reaches 10 wt% (Example 12), although the formation of the rutile phase can still be completely suppressed, the local lattice distortion is intensified due to the doping amount approaching the solid solution limit of the TiO2 lattice, resulting in a slight decrease in the initial specific surface area compared to the optimal value (165.3 m). 2 / g), after calcination at 600℃, the specific surface area retention rate was 86.3%, which was still nearly 17 percentage points higher than that of the undoped support. When the doping amount was further increased to 12wt% (Comparative Example 2), the excess Ni 2+ The inability to fully embed into the crystal lattice resulted in the formation of a separated NiO phase, causing the initial specific surface area to plummet to 145.8 m². 2 / g, and the thermal stability is significantly deteriorated.
[0061] In summary, compared to undoped TiO2, the 0.5-10 wt% doping range specified in this application can significantly suppress the transformation from anatase to rutile phase, and increase the specific surface area retention rate after calcination at 600℃ from 69.7% to over 86.3%, thus comprehensively achieving the goal of improving the thermal stability of the TiO2 support. Among these, the overall performance is better when the doping content is 2-8 wt%, and optimal when it is 3-5 wt%.
[0062] Experimental Example 3: Evaluation of Catalyst Activity and Stability The catalysts provided in Example 1 and Application Example 13 were characterized at the microscopic level, and the specific surface area and compressive strength of the supports provided in Application Examples 1-13 were determined in accordance with the method of Experimental Example 1. Using a hexadecane solution containing 30 wt% oleic acid as raw material, the mixture was prepared at 290 °C, 6 MPa hydrogen pressure, a hydrogen-to-oil ratio of 800, and a space velocity of 1.0 h⁻¹. -1 Under the specified conditions, a hydrodeoxygenation reaction was carried out in the presence of a catalyst. The products were quantitatively analyzed by gas chromatography to obtain the deoxygenation rate of oleic acid (calculated as (amount of oleic acid before hydrodeoxygenation - amount of oleic acid after hydrodeoxygenation) / amount of oleic acid before hydrodeoxygenation × 100%) and the yield of the fully hydrogenated product, octadecane. The catalysts used were Application Examples 1-6, Application Examples 13-15, and a commercial catalyst (Ni-Mo / Al₂O₃, nickel content 3.0 wt%, Mo content 21.0 wt%). The relative change rate of activity of each catalyst over 24 hours was recorded.
[0063] Relative change rate of activity = , In the formula, x 24 x is the oleic acid deoxygenation rate after the catalyst has been running continuously for 24 hours, and x0 is the initial oleic acid deoxygenation rate after the reaction reaches steady state.
[0064] In addition, 1000 hours of continuous operation tests were conducted on both use case 1 and the commercial catalyst, and the results are shown in the table. Figure 4 .
[0065] Table 3 Catalyst properties and catalytic activity results
[0066] For the microscopic characterization of the catalysts provided in Use Case 1 and Application Example 13, please refer to [reference needed]. Figure 3 As can be seen, in Application Example 1 (using the support of Example 1 of this application), the MoS2 active phase is uniformly dispersed on the support surface in the form of short sheets, with a sheet length of about 5-10 nm and a main number of 2-5 layers. Figure 3 The structure described in the text (C) is typical of highly intrinsically active Type II Ni-Mo-S phases. In stark contrast, in Application Example 13 (using the undoped support of Comparative Example 1), the MoS2 sheets exhibit severe agglomeration, with sheet lengths increasing to 20-30 nm and the number of layers reaching 5-10. Figure 3 The results show that the NiO on the support surface of this application exhibits large MoS2 aggregates in some areas (D), directly demonstrating the presence of NiO on the support surface. x The anchoring effect of the clusters on molybdate effectively inhibits the agglomeration and crystal growth of MoO3 during calcination, and promotes the formation of highly active Type II phase.
[0067] As shown in Table 3, all embodiments of this application exhibit extremely high initial deoxygenation rates and yields of the fully hydrogenated product, octadecane, with minimal activity degradation over 24 hours. In contrast, the catalysts provided in the comparative examples show significantly poorer activity and stability. Particularly noteworthy is that while the commercial catalysts demonstrate acceptable initial deoxygenation rates and octadecane yields, their activity declines severely over 24 hours, due to corrosion of the support. The results of the 1000-hour continuous operation stability test are as follows... Figure 4 As shown in the figure, the horizontal axis represents the reaction time (h), and the vertical axis represents the oleic acid deoxidation rate (%). The catalyst provided in Application Example 1 achieved an initial deoxidation rate of 99.8%. Throughout the 1000-hour operation, the deoxidation rate showed a slow decreasing trend, remaining at 97.3% after 1000 hours, with a decrease of only 2.5%. Furthermore, the catalyst particles remained intact after the reaction, with no obvious pulverization, and the compressive strength retention rate exceeded 95%. In contrast, while the commercial Ni-Mo / Al2O3 catalyst also achieved an initial deoxidation rate of 99.2%, its deoxidation rate plummeted to below 72% after 200 hours of operation and further decreased to below 50% after 300 hours, completely losing its industrial application value. This comparative result strongly confirms the excellent stability of the catalyst in this application under harsh conditions of high acidity and high water vapor partial pressure.
[0068] Obviously, the above embodiments are merely illustrative examples for clear explanation and are not intended to limit the implementation. Those skilled in the art will recognize that other variations or modifications can be made based on the above description. It is neither necessary nor possible to exhaustively list all possible implementations here. However, obvious variations or modifications derived therefrom are still within the scope of protection of this application.
Claims
1. A catalyst support, characterized in that, It includes titanium dioxide and doping elements, wherein the content of the doping elements is 0.5wt%-10wt% based on the mass of titanium dioxide, and the doping elements include at least one of nickel or cobalt.
2. The catalyst support according to claim 1, characterized in that, The content of the doping element is 2wt%-8wt% based on the mass of titanium dioxide.
3. The catalyst support according to claim 2, characterized in that, When the doping element is nickel, the nickel content is 3wt%-5wt% based on the mass of titanium dioxide. And / or, when the doping element is cobalt, the cobalt content is 2wt%-6wt% based on the mass of titanium dioxide.
4. A method for modifying the catalyst support according to any one of claims 1-3, characterized in that, The process includes the following steps: in the presence of a dispersant, a dopant and a titanium source are co-precipitated, a precursor is obtained by solid-liquid separation, and the precursor is calcined to obtain a catalyst support; the dopant includes at least one of a nickel source or a cobalt source.
5. The modification method according to claim 4, characterized in that, The dispersant includes at least one of polyethylene glycol, polyvinylpyrrolidone, and hexadecyltrimethylammonium bromide; And / or, the titanium source includes at least one of tetrabutyl titanate, titanium oxysulfate, and titanium tetrachloride; And / or, the nickel source includes at least one of nickel nitrate, nickel sulfate, and nickel chloride; And / or, the cobalt source includes at least one of cobalt nitrate, cobalt sulfate, and cobalt chloride; And / or, the modification method further includes the steps of mixing, molding, drying, and calcining the catalyst support, binder, and additives.
6. The modification method according to claim 5, characterized in that, The dispersant is polyethylene glycol; And / or, the dispersant is 0.5wt%-5wt% of the catalyst support mass; And / or, the auxiliary agent is 0.5wt%-5wt% of the catalyst support mass; And / or, the pH value of the coprecipitation reaction is 7-10; And / or, before solid-liquid separation, stir the mixture after co-precipitation reaction for 2-3 hours and age it for 12-24 hours; And / or, the temperature of the calcination precursor is 350℃-450℃, and the calcination time is 3h-5h; And / or, the temperature for calcining the catalyst support and additive mixture is 500℃-600℃, and the calcination time is 3h-5h; And / or, the adhesive includes silica sol; And / or, the additives include at least one of guar gum powder, polyvinyl alcohol, and methylcellulose.
7. A catalyst, characterized in that, It includes a support and an active component, wherein the support includes a catalyst support prepared by a modification method of the catalyst support according to any one of claims 1-3 or the catalyst support according to any one of claims 4-6.
8. The catalyst according to claim 7, characterized in that, The active component includes molybdenum; And / or, the specific surface area of the catalyst is greater than 150 m². 2 / g, compressive strength greater than 100N / cm.
9. The catalyst according to claim 8, characterized in that, The catalyst preparation method includes the following steps: using an equal-volume impregnation method, impregnating a solution containing a molybdenum source onto a catalyst support, drying, and calcining; And / or, the active component is a catalyst with a mass of 10wt%-30wt%.