A production process for polyethylene polyamines and related catalysts and their preparation methods

By combining core-shell structured catalysts with molecular sieve membrane distillation towers, the problems of selectivity and high energy consumption in the production of polyethylene polyamines have been solved, achieving high selectivity and low energy consumption in the production of polyethylene polyamines, thus improving product quality and environmental friendliness.

CN123102408APending Publication Date: 2026-11-17常州市龙鹏化工有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611250068.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-18
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing polyethylene polyamine production processes are difficult to control in terms of product selectivity, and it is difficult to balance catalyst activity, stability and selectivity. The reaction and separation processes are energy-intensive and also pose problems of equipment corrosion and environmental pollution.

Method used

A core-shell catalyst is used, with the core consisting of a Co-Ni alloy and acidic sites of HZSM-5, and the outer shell grafted with basic sites. High selectivity and high efficiency separation are achieved through a combination of molecular sieve membrane and distillation column separation technology.

Benefits of technology

It improves the selectivity and purity of linear polyethylene polyamines, reduces energy consumption and equipment investment, simplifies the separation process, reduces by-product generation and equipment corrosion, and improves product quality and environmental friendliness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This invention relates to the field of chemical synthesis technology, specifically disclosing a production process for polyethylene polyamines and related catalysts and their preparation methods. The production process for polyethylene polyamines includes the following steps: (1) The catalyst is mixed and diluted with an equal volume of inert quartz sand and then fed into a tubular reactor in a segmented manner. A mixture of ammonia and hydrogen is introduced into the tubular reactor for initial activation, and then the reactor is pretreated with pure ammonia to fully amination the catalyst surface; (2) Dichloroethane, liquid ammonia, and hexamethylenetetramine are thoroughly mixed. Unreacted ammonia is separated from the effluent, and the liquid product enters a turbulent contact tower to remove residual chloride ions, resulting in a dechlorinated crude amine solution; (3) The dechlorinated crude amine solution is passed sequentially through an MFI molecular sieve membrane and an FAU molecular sieve membrane. The retentate is transported to a distillation column for purification to obtain polyethylene polyamines. This process is green and environmentally friendly, and can produce polyethylene polyamines with high selectivity and high efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of chemical synthesis technology, and more specifically, to a production process for polyethylene polyamines and related catalysts and their preparation methods. Background Technology

[0002] Polyethylene polyamines, mainly including ethylenediamine (EDA), diethylenetriamine (DETA), triethylenetetramine (TETA), tetraethylenepentamine (TEPA), and their homologues, are an important class of aliphatic nitrogen-containing organic compounds. As key chemical raw materials and intermediates for fine chemicals, they are widely used in epoxy resin curing agents, pesticides, pharmaceuticals, dyes, chelating agents, lubricant additives, and the synthesis of polymer materials, with market demand continuing to grow.

[0003] Currently, the mainstream industrial method for producing polyethylene polyamines is the dichloroethane (EDC) ammonolysis process. This process typically uses liquid ammonia and EDC as raw materials, and the ammonolysis reaction is carried out under high temperature and pressure. The reaction system is extremely complex, involving multiple parallel-series reaction steps such as dechlorination, amination, condensation, and cyclization. The reaction products are widely distributed; in addition to the target linear polyethylene polyamine, a large number of cyclic byproducts, such as piperazine (PIP) and aminoethylpiperazine (AEP), are inevitably generated.

[0004] The prominent technical challenges faced by existing technologies are mainly concentrated in the following three aspects:

[0005] Product selectivity is difficult to control, especially the suppression of cyclic byproducts: existing catalyst systems (such as metal oxides, phosphates, molecular sieves, or their modifications) often struggle to precisely control the reaction pathway. Because cyclic amines such as piperazines are thermodynamically relatively stable, many catalysts tend to promote intramolecular cyclization reactions, leading to excessively high selectivity for byproducts such as PIP (often exceeding 10%, or even higher), severely crowding out the yield of linear polyamines (especially high-value-added TETA and TEPA). Traditional methods often rely on macroscopic means such as increasing the ammonia / chlorine ratio and adjusting reaction conditions to suppress cyclization, but these methods have limited effectiveness and significantly increase energy consumption and separation costs.

[0006] Achieving a balance between catalyst activity, stability, and selectivity is challenging: homogeneous catalysts (such as organic amines) exhibit high activity but suffer from problems like separation difficulties, equipment corrosion, and environmental pollution. Heterogeneous catalysts face even greater challenges.

[0007] Acidic catalysts (such as zeolite molecular sieves) have strong C-Cl bond activation ability and high initial activity, but their strong acidic sites are very likely to induce deep cyclization of intermediates such as EDA, resulting in low selectivity of linear amines and rapid deactivation due to carbon deposition.

[0008] Basic catalysts (such as supported alkaline earth metal oxides) are beneficial for promoting the condensation chain growth of amines, but they have weak initial activation ability for EDC, require high reaction temperature and pressure, and the basic sites are easily lost in the reaction medium, resulting in poor stability. Most existing catalysts only focus on a single function (acidic or basic) and lack the synergistic catalytic ability for the entire reaction chain of "dechlorination activation-amination-linear condensation".

[0009] High energy consumption in reaction and separation processes: To obtain the target product, existing processes typically rely on multi-stage tubular reactors and complex high-vacuum precision distillation sequences. Due to the close boiling points of the products and the presence of azeotropes, the separation and purification process is energy-intensive, and the high-temperature, long-duration distillation process may cause thermal decomposition or color deepening (high chroma) of some products, affecting product quality. Summary of the Invention

[0010] To address the shortcomings of existing technologies, the present invention aims to provide a production process for polyethylene polyamines, as well as related catalysts and their preparation methods.

[0011] To achieve the above objectives, the present invention provides the following technical solution:

[0012] A catalyst for producing polyethylene polyamines, wherein the raw materials, by weight, comprise the following components:

[0013] ZSM-5 molecular sieve 100-120 parts, cobalt nitrate 5-15 parts, nickel nitrate 6-10 parts, citric acid 8-12 parts, anhydrous ethanol 50-100 parts, boehmite 10-20 parts, tetraethyl orthosilicate 15-30 parts, phosphoric acid 20-35 parts, tetraethylammonium hydroxide 40-70 parts, 3-aminopropyltriethoxysilane 2-8 parts, ammonium fluoride 0.5-2 parts, toluene 200-400 parts, deionized water 600-1200 parts.

[0014] Furthermore, the method for preparing the catalyst includes the following steps:

[0015] S1. Weigh each raw material component according to the weight percentage;

[0016] S2. Add ZSM-5 molecular sieve to 1 / 3 of the deionized water and stir and mix under a water bath at 60~80℃ to obtain a suspension.

[0017] S3. Cobalt nitrate, nickel nitrate and citric acid are added to 1 / 3 of the volume of deionized water, and anhydrous ethanol is added. After stirring evenly, the mixture is slowly added dropwise to the suspension. The mixture is stirred and refluxed under a water bath at 70~85℃ for 6~12h. After filtration and washing, the mixture is dried at 100~120℃. Then, it is calcined in air at 450~550℃ at a rate of 2~4℃ / min for 4~6h to obtain the oxide precursor.

[0018] S4. Place the oxide precursor in an atmosphere furnace and heat it to 500-600℃ in a pure hydrogen stream at a rate of 4-6℃ / min. Reduce it for 3-5 hours and then cool it to room temperature to obtain the catalyst core.

[0019] S5. Add boehmite and phosphoric acid to the remaining 1 / 3 of the deionized water, stir until clear, then add tetraethyl orthosilicate, tetraethylammonium hydroxide and ammonium fluoride in sequence, stir evenly to obtain the mother liquor;

[0020] S6. Add the catalyst core to the mother liquor, ultrasonically disperse for 30-60 min, and age at room temperature for 12-24 h to obtain a mixture;

[0021] S7. Place the mixture in a tubular reactor and crystallize it at 160~190℃ for 24~72h. After filtration, washing and drying, the catalyst precursor is obtained.

[0022] S8. Disperse the catalyst precursor in toluene solvent, add 3-aminopropyltriethoxysilane, reflux at 110~130℃ for 6~12h under nitrogen protection, filter and wash, calcine at 350~450℃ for 2~4h under nitrogen atmosphere, and cool to room temperature to obtain the catalyst.

[0023] Furthermore, in step S4, the space velocity of the pure hydrogen gas stream is 1000~2000 h⁻¹. -1 .

[0024] Furthermore, the power of ultrasonic dispersion in step S6 is 400~600W.

[0025] Furthermore, the production process of the polyethylene polyamine includes the following steps:

[0026] (1) After the catalyst is mixed and diluted with an equal volume of 40-60 mesh inert quartz sand, it is added to the tubular reactor for reaction by segmented feeding. First, a mixture of ammonia and hydrogen is introduced into the tubular reactor and the temperature is raised to 350-450℃ at 3-5℃ / min for reduction and activation for 2-4 hours. Then, pure ammonia is switched and pretreated at 250-300℃ for 1-2 hours to fully amination the catalyst surface.

[0027] (2) Dichloroethane, liquid ammonia and hexamethylenetetramine are thoroughly mixed at a mass ratio of 10:40~80:1~2. After being vaporized in a preheater, the mixture is transported to a tubular reactor for reaction. The effluent is first condensed at a low temperature of -10~10℃ to separate unreacted ammonia. The liquid product enters a turbulent contact tower containing nano-calcium oxide suspended particles, where residual chloride ions are deeply removed to <10ppm at 50~80℃ to obtain dechlorinated crude amine liquid.

[0028] (3) The crude amine solution after dechlorination is passed through an MFI molecular sieve membrane at 80~120℃ and a vacuum of 1~5kPa on the back side of the membrane to selectively separate ethylenediamine and water. The retentate is passed through an FAU molecular sieve membrane at 100~140℃ to selectively separate diethylenetriamine and triethylenetetramine.

[0029] (4) The retentate from the FAU molecular sieve membrane is transported to a distillation column for distillation and purification to obtain polyethylene polyamine;

[0030] The catalyst is the catalyst prepared by the above preparation method.

[0031] Furthermore, in step (1), the space velocity of the ammonia and hydrogen mixture is 500~1000 h⁻¹. -1 The volume ratio of ammonia to hydrogen is 95:5.

[0032] Furthermore, in step (1), the space velocity of pure ammonia is 200~400 h⁻¹. -1 .

[0033] Furthermore, the reaction conditions in step (2) are a temperature of 200~280℃, a pressure of 6.0~10.0MPa, and a weight hourly space velocity of 0.8~1.5h. -1 .

[0034] Furthermore, the conditions for distillation purification in step (4) are a pressure of 0.5~5.0 kPa and a bottom temperature of 150~200℃.

[0035] In summary, this application includes at least the following beneficial effects:

[0036] This invention utilizes a core-shell structured catalyst to produce polyethylene polyamines. The basic sites grafted onto the outer shell efficiently activate ammonia molecules, forming a high-concentration, highly active ammonia atmosphere and initially adsorbing EDC. The Co-Ni alloy in the core synergistically works with the acidic sites of HZSM-5 to strongly activate the C-Cl bonds of EDC, completing rapid dechlorination and initial CN bond formation. The resulting linear small-molecule amine can return to the shell pores, undergoing controlled intermolecular condensation near the basic sites, continuously growing into DETA, TETA, etc., while avoiding deep cyclization at strong acid centers. This ordered spatial and functional division of labor allows the overall selectivity of the linear polyethylene polyamine to be stably expected to reach over 90%, and the product chain length distribution can be controlled within a certain range by adjusting the basicity of the shell.

[0037] Meanwhile, the dense shell encapsulates the highly active Co-Ni alloy nanoparticles, effectively preventing their migration and aggregation in the high-temperature reaction environment. Shape selectivity reduces the formation of cyclic macromolecular byproducts, which are precursors to pore blockage and carbon deposition. The core-shell structure limits the excessive residence of byproducts at active sites. Furthermore, the shell provides some barrier effect against chloride ions or ammonium chloride generated during the reaction, mitigating their erosion and poisoning of the core metal active centers, thus effectively extending the catalytic activity and lifespan of the catalyst. Due to the highly dispersed and synergistic effect of the catalyst active centers, ultra-high conversion rates can be achieved under moderate pressure and temperature, reducing equipment investment and safety risks associated with high-pressure reactors. High selectivity greatly simplifies the product composition in the reaction solution, significantly reducing the load on subsequent separation systems. This greatly simplifies the separation process and reduces energy consumption. Because the content of cyclic byproducts is extremely low, the ultra-precision, high-reflux-ratio distillation column required for separating PIP and DETA / TETA with similar boiling points in traditional processes is avoided, significantly reducing the complexity and energy consumption of the separation sequence. The product contains high-purity linear amines with a light color, reducing subsequent refining steps such as decolorization and improving product quality. The catalyst is a heterogeneous system, with no metal ion dissolution, making it easy to separate and recover. This avoids the equipment corrosion and wastewater treatment problems associated with homogeneous catalysts, making the process more environmentally friendly. Detailed Implementation

[0038] It should be noted that, where there is no conflict, the embodiments and features described in this application can be combined with each other. The present invention will now be described in detail with reference to the embodiments.

[0039] It should be noted that, unless otherwise specified, all technical and scientific terms used in this application have the same meaning as commonly understood by one of ordinary skill in the art to which this application pertains.

[0040] This invention provides a production process for polyethylene polyamines, as well as related catalysts and their preparation methods, wherein:

[0041] A process for producing polyethylene polyamine includes the following steps:

[0042] (1) Weigh out the following components by weight: 100-120 parts of ZSM-5 molecular sieve, 5-15 parts of cobalt nitrate, 6-10 parts of nickel nitrate, 8-12 parts of citric acid, 50-100 parts of anhydrous ethanol, 10-20 parts of boehmite, 15-30 parts of tetraethyl orthosilicate, 20-35 parts of phosphoric acid, 40-70 parts of tetraethylammonium hydroxide, 2-8 parts of 3-aminopropyltriethoxysilane, 0.5-2 parts of ammonium fluoride, 200-400 parts of toluene, and 600-1200 parts of deionized water.

[0043] (2) Add ZSM-5 molecular sieve to 1 / 3 of the volume of deionized water and stir and mix under water bath conditions of 60~80℃ to obtain a suspension;

[0044] (3) Add cobalt nitrate, nickel nitrate and citric acid to 1 / 3 of the deionized water, add anhydrous ethanol, stir evenly, and slowly add dropwise to the suspension. Stir and reflux for 6-12 hours under water bath conditions of 70-85℃. After filtration and washing, dry at 100-120℃. Then, in an air atmosphere, heat to 450-550℃ at 2-4℃ / min and calcine for 4-6 hours to obtain the oxide precursor.

[0045] (4) Place the oxide precursor in an atmosphere furnace and heat it at a space velocity of 1000~2000 h⁻¹. -1 In a pure hydrogen gas stream, the temperature is increased to 500-600℃ at 4-6℃ / min, and the reduction is carried out for 3-5 hours. The temperature is then cooled to room temperature to obtain the catalyst core.

[0046] (5) Add boehmite and phosphoric acid to the remaining 1 / 3 of the deionized water, stir until clear, then add tetraethyl orthosilicate, tetraethylammonium hydroxide and ammonium fluoride in sequence, stir evenly to obtain the mother liquor;

[0047] (6) Add the catalyst core to the mother liquor, ultrasonically disperse it at a power of 400~600W for 30~60min, and age it at room temperature for 12~24h to obtain a mixture;

[0048] (7) The mixture is placed in a tubular reactor and crystallized at 160~190℃ for 24~72h. After filtration, washing and drying, the catalyst precursor is obtained.

[0049] (8) The catalyst precursor is dispersed in toluene solvent, 3-aminopropyltriethoxysilane is added, and under nitrogen protection, the mixture is refluxed at 110~130℃ for 6~12h. After filtration and washing, it is calcined at 350~450℃ for 2~4h under nitrogen atmosphere and cooled to room temperature to obtain the catalyst.

[0050] (9) After diluting the catalyst with an equal volume of 40-60 mesh inert quartz sand, add it to the tubular reactor for reaction in stages, first at a rate of 500-1000 h. -1 A mixture of ammonia and hydrogen gas, with a volume ratio of 95:5, is introduced into the tubular reactor at a space velocity of 3-5℃ / min to 350-450℃ for reduction activation for 2-4 hours. Then, pure ammonia gas is introduced and the gas is heated at a speed of 200-400℃ / min for 200-400 hours. -1 The space velocity is increased, and the catalyst is pretreated at 250~300℃ for 1~2h to fully amination of the catalyst surface;

[0051] (10) Dichloroethane, liquid ammonia, and hexamethylenetetramine are thoroughly mixed at a mass ratio of 10:40~80:1~2, vaporized in a preheater, and then transported to a tubular reactor. The mixture is heated at a temperature of 200~280℃, a pressure of 6.0~10.0MPa, and a weight hourly space velocity of 0.8~1.5h. -1 The reaction is carried out under the following conditions. The effluent is first condensed at a low temperature of -10~10℃ to separate unreacted ammonia. The liquid product enters a turbulent contact tower containing nano calcium oxide suspended particles, where residual chloride ions are deeply removed to <10ppm at 50~80℃ to obtain dechlorinated crude amine liquid.

[0052] (11) The crude amine solution after dechlorination is passed through an MFI molecular sieve membrane at 80~120℃ and a vacuum of 1~5kPa on the back side of the membrane to selectively separate ethylenediamine and water. The retentate is passed through an FAU molecular sieve membrane at 100~140℃ to selectively separate diethylenetriamine and triethylenetetramine.

[0053] (12) The retentate of the FAU type molecular sieve membrane is transported to the distillation column and purified under reduced pressure of 0.5~5.0 kPa and a bottom temperature of 150~200℃ to obtain polyethylene polyamine.

[0054] The technical solutions provided by the present invention will be described in detail below with reference to the embodiments, but they should not be construed as limiting the scope of protection of the present invention.

[0055] Example 1

[0056] The production process of polyethylene polyamine in this embodiment includes the following steps:

[0057] (1) Weigh out the following components by weight: 100 parts of ZSM-5 molecular sieve, 5 parts of cobalt nitrate, 6 parts of nickel nitrate, 8 parts of citric acid, 50 parts of anhydrous ethanol, 10 parts of boehmite, 15 parts of tetraethyl orthosilicate, 20 parts of phosphoric acid, 40 parts of tetraethylammonium hydroxide, 2 parts of 3-aminopropyltriethoxysilane, 0.5 parts of ammonium fluoride, 200 parts of toluene, and 600 parts of deionized water.

[0058] (2) Add ZSM-5 molecular sieve to 1 / 3 of the volume of deionized water and stir and mix under a water bath at 60°C to obtain a suspension;

[0059] (3) Cobalt nitrate, nickel nitrate and citric acid were added to 1 / 3 of the deionized water and anhydrous ethanol was added. After stirring evenly, the mixture was slowly added dropwise to the suspension. The mixture was stirred and refluxed for 6 hours under a water bath at 70°C. After filtration and washing, the mixture was dried at 100°C and then calcined at 450°C for 4 hours in an air atmosphere at a rate of 2°C / min to obtain the oxide precursor.

[0060] (4) Place the oxide precursor in an atmosphere furnace and heat it at a space velocity of 1000 h⁻¹. -1 In a pure hydrogen gas stream, the temperature was increased to 500℃ at 4℃ / min, and the reduction was carried out for 3 hours. The mixture was then cooled to room temperature to obtain the catalyst core.

[0061] (5) Add boehmite and phosphoric acid to the remaining 1 / 3 of the deionized water, stir until clear, then add tetraethyl orthosilicate, tetraethylammonium hydroxide and ammonium fluoride in sequence, stir evenly to obtain the mother liquor;

[0062] (6) Add the catalyst core to the mother liquor, ultrasonically disperse it at 400W for 30min, and age it at room temperature for 12h to obtain a mixture;

[0063] (7) The mixture was placed in a tubular reactor and crystallized at 160°C for 24 hours. After filtration, washing and drying, the catalyst precursor was obtained.

[0064] (8) The catalyst precursor was dispersed in toluene solvent, 3-aminopropyltriethoxysilane was added, and the mixture was refluxed at 110°C for 6 h under nitrogen protection. After filtration and washing, the mixture was calcined at 350°C for 2 h under nitrogen atmosphere and cooled to room temperature to obtain the catalyst.

[0065] (9) After diluting the catalyst with an equal volume of 40-mesh inert quartz sand, add it to the tubular reactor for reaction in stages, first at a rate of 500 h⁻¹. -1 A mixture of ammonia and hydrogen gas with a volume ratio of 95:5 was introduced into the tubular reactor at a space velocity of 3℃ / min to 350℃ for reduction and activation for 2 hours. Then, pure ammonia gas was introduced and the reaction was carried out at a speed of 200 h / min. -1 The space velocity was increased, and the catalyst was pretreated at 250°C for 1 hour to fully amination the catalyst surface.

[0066] (10) Dichloroethane, liquid ammonia, and hexamethylenetetramine are thoroughly mixed at a mass ratio of 10:40:1, vaporized in a preheater, and then transported to a tubular reactor. The mixture is heated at 200°C, 6 MPa, and a weight hourly space velocity of 0.8 h⁻¹. -1 The reaction is carried out under the following conditions. The effluent is first condensed at -10℃ to separate unreacted ammonia. The liquid product enters a turbulent contact tower containing nano-calcium oxide suspended particles, where residual chloride ions are deeply removed to <10ppm at 50℃ to obtain dechlorinated crude amine liquid.

[0067] (11) The crude amine solution after dechlorination was passed through an MFI molecular sieve membrane at 80°C and a vacuum of 1 kPa on the back side of the membrane to selectively separate ethylenediamine and water. The retentate was passed through an FAU molecular sieve membrane at 100°C to selectively separate diethylenetriamine and triethylenetetramine.

[0068] (12) The retentate of the FAU molecular sieve membrane is transported to the distillation column and purified at a bottom temperature of 150°C under reduced pressure of 0.5 kPa to obtain polyethylene polyamine.

[0069] Example 2

[0070] The production process of polyethylene polyamine in this embodiment includes the following steps:

[0071] (1) Weigh out the following components by weight: 110 parts of ZSM-5 molecular sieve, 10 parts of cobalt nitrate, 8 parts of nickel nitrate, 10 parts of citric acid, 75 parts of anhydrous ethanol, 15 parts of boehmite, 25 parts of tetraethyl orthosilicate, 30 parts of phosphoric acid, 55 parts of tetraethylammonium hydroxide, 5 parts of 3-aminopropyltriethoxysilane, 1 part of ammonium fluoride, 300 parts of toluene, and 900 parts of deionized water.

[0072] (2) Add ZSM-5 molecular sieve to 1 / 3 of the volume of deionized water and stir and mix under a water bath at 70°C to obtain a suspension;

[0073] (3) Cobalt nitrate, nickel nitrate and citric acid were added to 1 / 3 of the deionized water and anhydrous ethanol was added. After stirring evenly, the mixture was slowly added dropwise to the suspension. The mixture was stirred and refluxed for 9 hours under a water bath at 80°C. After filtration and washing, the mixture was dried at 110°C and then calcined at 500°C for 5 hours in an air atmosphere at a rate of 3°C / min to obtain the oxide precursor.

[0074] (4) Place the oxide precursor in an atmosphere furnace and heat it at a space velocity of 1500 h⁻¹. -1 In a pure hydrogen gas stream, the temperature was increased to 550℃ at 5℃ / min, and the reduction was carried out for 4 hours. The catalyst core was then cooled to room temperature.

[0075] (5) Add boehmite and phosphoric acid to the remaining 1 / 3 of the deionized water, stir until clear, then add tetraethyl orthosilicate, tetraethylammonium hydroxide and ammonium fluoride in sequence, stir evenly to obtain the mother liquor;

[0076] (6) Add the catalyst core to the mother liquor, ultrasonically disperse it at 500W for 45min, and age it at room temperature for 18h to obtain a mixture;

[0077] (7) The mixture was placed in a tubular reactor and crystallized at 175°C for 48 hours. After filtration, washing and drying, the catalyst precursor was obtained.

[0078] (8) The catalyst precursor was dispersed in toluene solvent, 3-aminopropyltriethoxysilane was added, and the mixture was refluxed at 120°C for 8 hours under nitrogen protection. After filtration and washing, the mixture was calcined at 400°C for 3 hours under nitrogen atmosphere and cooled to room temperature to obtain the catalyst.

[0079] (9) After diluting the catalyst with an equal volume of 50-mesh inert quartz sand, add it to the tubular reactor for reaction in stages, first at a rate of 750 h. -1 A mixture of ammonia and hydrogen gas with a volume ratio of 95:5 was introduced into the tubular reactor at a space velocity of 4℃ / min to 400℃ for reduction and activation for 3 hours. Then, pure ammonia gas was introduced and the reaction was carried out at a speed of 300℃ / min. -1 The space velocity was increased, and the catalyst was pretreated at 275℃ for 1.5 h to allow for full amination of the catalyst surface;

[0080] (10) Dichloroethane, liquid ammonia, and hexamethylenetetramine are thoroughly mixed at a mass ratio of 10:60:1.5, vaporized in a preheater, and then transported to a tubular reactor. The mixture is heated at 240°C, 8 MPa, and a weight hourly space velocity of 1.2 h⁻¹. -1 The reaction is carried out under the following conditions. The effluent is first condensed at 0°C to separate unreacted ammonia. The liquid product enters a turbulent contact tower containing nano-calcium oxide suspended particles, where residual chloride ions are deeply removed to <10ppm at 65°C to obtain dechlorinated crude amine liquid.

[0081] (11) The crude amine solution after dechlorination was passed through an MFI molecular sieve membrane at 100°C and a vacuum of 3 kPa on the back side of the membrane to selectively separate ethylenediamine and water. The retentate was passed through an FAU molecular sieve membrane at 120°C to selectively separate diethylenetriamine and triethylenetetramine.

[0082] (12) The retentate of the FAU type molecular sieve membrane is transported to the distillation column and purified at a bottom temperature of 175°C under reduced pressure of 2.5 kPa to obtain polyethylene polyamine.

[0083] Example 3

[0084] The production process of polyethylene polyamine in this embodiment includes the following steps:

[0085] (1) Weigh out the following components by weight: 120 parts of ZSM-5 molecular sieve, 15 parts of cobalt nitrate, 10 parts of nickel nitrate, 12 parts of citric acid, 100 parts of anhydrous ethanol, 20 parts of boehmite, 30 parts of tetraethyl orthosilicate, 35 parts of phosphoric acid, 70 parts of tetraethylammonium hydroxide, 8 parts of 3-aminopropyltriethoxysilane, 2 parts of ammonium fluoride, 400 parts of toluene, and 1200 parts of deionized water.

[0086] (2) Add ZSM-5 molecular sieve to 1 / 3 of the deionized water and stir and mix under water bath conditions at 80°C to obtain a suspension;

[0087] (3) Cobalt nitrate, nickel nitrate and citric acid were added to 1 / 3 of the deionized water and anhydrous ethanol was added. After stirring evenly, the mixture was slowly added dropwise to the suspension. The mixture was stirred and refluxed for 12 hours under a water bath at 85°C. After filtration and washing, the mixture was dried at 120°C and then calcined at 550°C for 6 hours in an air atmosphere at a rate of 4°C / min to obtain the oxide precursor.

[0088] (4) Place the oxide precursor in an atmosphere furnace and heat it at a space velocity of 2000 h⁻¹. -1 In a pure hydrogen gas stream, the temperature was increased to 600℃ at 6℃ / min, and the reduction was carried out for 5 hours. The mixture was then cooled to room temperature to obtain the catalyst core.

[0089] (5) Add boehmite and phosphoric acid to the remaining 1 / 3 of the deionized water, stir until clear, then add tetraethyl orthosilicate, tetraethylammonium hydroxide and ammonium fluoride in sequence, stir evenly to obtain the mother liquor;

[0090] (6) Add the catalyst core to the mother liquor, ultrasonically disperse it at 600W for 60min, and age it at room temperature for 24h to obtain a mixture;

[0091] (7) The mixture was placed in a tubular reactor and crystallized at 190°C for 72 h. After filtration, washing and drying, the catalyst precursor was obtained.

[0092] (8) The catalyst precursor was dispersed in toluene solvent, 3-aminopropyltriethoxysilane was added, and the mixture was refluxed at 130°C for 12 h under nitrogen protection. After filtration and washing, the mixture was calcined at 450°C for 4 h under nitrogen atmosphere and cooled to room temperature to obtain the catalyst.

[0093] (9) After diluting the catalyst with an equal volume of 60-mesh inert quartz sand, add it to the tubular reactor for reaction in stages, starting with a 1000h reaction. -1 A mixture of ammonia and hydrogen gas with a volume ratio of 95:5 was introduced into the tubular reactor at a space velocity of 5℃ / min to 450℃ for reduction activation for 4 hours. Then, pure ammonia gas was introduced and the gas was heated at 400℃ / min. -1 The space velocity was increased, and the catalyst was pretreated at 300℃ for 2 hours to fully amination the catalyst surface.

[0094] (10) Dichloroethane, liquid ammonia, and hexamethylenetetramine are thoroughly mixed at a mass ratio of 10:80:2, vaporized in a preheater, and then transported to a tubular reactor. The mixture is heated at 280°C, 10 MPa, and a weight hourly space velocity of 1.5 h⁻¹. -1 The reaction is carried out under the following conditions. The effluent is first condensed at a low temperature of 10°C to separate unreacted ammonia. The liquid product enters a turbulent contact tower containing nano-calcium oxide suspended particles, where residual chloride ions are deeply removed to <10ppm at 80°C to obtain dechlorinated crude amine liquid.

[0095] (11) The crude amine solution after dechlorination was passed through an MFI molecular sieve membrane at 120°C and a vacuum of 5 kPa on the back side of the membrane to selectively separate ethylenediamine and water. The retentate was passed through an FAU molecular sieve membrane at 140°C to selectively separate diethylenetriamine and triethylenetetramine.

[0096] (12) The retentate of the FAU type molecular sieve membrane is transported to the distillation column and purified at a bottom temperature of 200°C under reduced pressure of 5.0 kPa to obtain polyethylene polyamine.

[0097] Experimental Example

[0098] The products from Examples 1-3 were selected as samples for testing, including product color, dichloroethane conversion, total amine selectivity, and piperazine selectivity. The specific test results are shown in Table 1.

[0099] Table 1: Test Results of Examples 1-3

[0100]

[0101] As shown in Table 1, the polyethylene polyamines prepared by the method of the present invention in Examples 1-3 all achieved a dichloroethane conversion rate greater than 99.5% and a total amine selectivity greater than 94%. This indicates that the production of polyethylene polyamines using a core-shell structured catalyst utilizes the highly efficient activation of ammonia molecules by the basic sites grafted onto the outer shell, forming a high-concentration, highly active ammonia atmosphere and initially adsorbing EDC. The Co-Ni alloy in the core synergistically with the acidic sites of HZSM-5 to strongly activate the C-Cl bonds of EDC, completing rapid dechlorination and initial CN bond formation. The generated linear small molecule amines can return to the shell pores, undergoing controlled intermolecular condensation near the basic sites, and continuously growing into DETA, TETA, etc., while avoiding deep cyclization at the strong acid center. This ordered division of space and function enables a dichloroethane conversion rate of over 99% and a total amine selectivity of over 94%, and the product chain length distribution can be controlled within a certain range by adjusting the basicity of the shell.

[0102] Meanwhile, the dense shell encapsulates the highly active Co-Ni alloy nanoparticles, effectively preventing their migration and aggregation in the high-temperature reaction environment. Shape selectivity reduces the formation of cyclic macromolecular byproducts, which are precursors to pore blockage and carbon deposition. The core-shell structure limits the excessive residence of byproducts at active sites. Furthermore, the shell provides some barrier effect against chloride ions or ammonium chloride generated during the reaction, mitigating their erosion and poisoning of the core metal active centers, thereby effectively extending the catalyst's catalytic activity and lifespan. Due to the highly dispersed and synergistic effects of the catalyst's active centers, ultra-high conversion rates can be achieved under moderate pressure and temperature, reducing equipment investment and safety risks associated with high-pressure reactors. High selectivity greatly simplifies the product composition in the reaction solution, significantly reducing the load on subsequent separation systems. This greatly simplifies the separation process and reduces energy consumption. Because the content of cyclic byproducts is extremely low, the ultra-precision, high-reflux-ratio distillation column required for separating PIP and DETA / TETA with similar boiling points in traditional processes is avoided, significantly reducing the complexity and energy consumption of the separation sequence. The product contains high-purity linear amines with a light color, reducing subsequent refining steps such as decolorization and improving product quality. The catalyst is a heterogeneous system, with no metal ion dissolution, making it easy to separate and recover. This avoids the equipment corrosion and wastewater treatment problems associated with homogeneous catalysts, making the process more environmentally friendly.

[0103] Therefore, the production process of polyethylene polyamine, as well as the related catalyst and its preparation method provided by this invention, have good application effects and broad market prospects.

[0104] Based on the above-described preferred embodiments of the present invention, and through the foregoing description, those skilled in the art can make various changes and modifications without departing from the inventive concept. The technical scope of this invention is not limited to the contents of the specification, but must be determined according to the scope of the claims.

Claims

1. A catalyst for producing polyethylene polyamines, characterized in that, The raw materials, by weight, include the following components: ZSM-5 molecular sieve 100-120 parts, cobalt nitrate 5-15 parts, nickel nitrate 6-10 parts, citric acid 8-12 parts, anhydrous ethanol 50-100 parts, boehmite 10-20 parts, tetraethyl orthosilicate 15-30 parts, phosphoric acid 20-35 parts, tetraethylammonium hydroxide 40-70 parts, 3-aminopropyltriethoxysilane 2-8 parts, ammonium fluoride 0.5-2 parts, toluene 200-400 parts, deionized water 600-1200 parts.

2. A method for preparing the catalyst as described in claim 1, characterized in that, Includes the following steps: S1. Weigh each raw material component according to the weight percentage; S2. Add ZSM-5 molecular sieve to 1 / 3 of the deionized water and stir and mix under a water bath at 60~80℃ to obtain a suspension. S3. Cobalt nitrate, nickel nitrate and citric acid are added to 1 / 3 of the volume of deionized water, and anhydrous ethanol is added. After stirring evenly, the mixture is slowly added dropwise to the suspension. The mixture is stirred and refluxed under a water bath at 70~85℃ for 6~12h. After filtration and washing, the mixture is dried at 100~120℃. Then, it is calcined in air at 450~550℃ at a rate of 2~4℃ / min for 4~6h to obtain the oxide precursor. S4. Place the oxide precursor in an atmosphere furnace and heat it to 500-600℃ in a pure hydrogen stream at a rate of 4-6℃ / min. Reduce it for 3-5 hours and then cool it to room temperature to obtain the catalyst core. S5. Add boehmite and phosphoric acid to the remaining 1 / 3 of the deionized water, stir until clear, then add tetraethyl orthosilicate, tetraethylammonium hydroxide and ammonium fluoride in sequence, stir evenly to obtain the mother liquor; S6. Add the catalyst core to the mother liquor, ultrasonically disperse for 30-60 min, and age at room temperature for 12-24 h to obtain a mixture; S7. Place the mixture in a tubular reactor and crystallize it at 160~190℃ for 24~72h. After filtration, washing and drying, the catalyst precursor is obtained. S8. Disperse the catalyst precursor in toluene solvent, add 3-aminopropyltriethoxysilane, reflux at 110~130℃ for 6~12h under nitrogen protection, filter and wash, calcine at 350~450℃ for 2~4h under nitrogen atmosphere, and cool to room temperature to obtain the catalyst.

3. The method for preparing a catalyst according to claim 2, characterized in that, In step S4, the space velocity of the pure hydrogen gas stream is 1000~2000 h⁻¹. -1 .

4. The method for preparing a catalyst according to claim 2, characterized in that, The power of ultrasonic dispersion in step S6 is 400~600W.

5. A production process for polyethylene polyamines, characterized in that, Includes the following steps: (1) After the catalyst is mixed and diluted with an equal volume of 40-60 mesh inert quartz sand, it is added to the tubular reactor for reaction by segmented feeding. First, a mixture of ammonia and hydrogen is introduced into the tubular reactor and the temperature is raised to 350-450℃ at 3-5℃ / min for reduction and activation for 2-4 hours. Then, pure ammonia is switched and pretreated at 250-300℃ for 1-2 hours to fully amination the catalyst surface. (2) Dichloroethane, liquid ammonia and hexamethylenetetramine are thoroughly mixed at a mass ratio of 10:40~80:1~2. After being vaporized in a preheater, the mixture is transported to a tubular reactor for reaction. The effluent is first condensed at a low temperature of -10~10℃ to separate unreacted ammonia. The liquid product enters a turbulent contact tower containing nano-calcium oxide suspended particles, where residual chloride ions are deeply removed to <10ppm at 50~80℃ to obtain dechlorinated crude amine liquid. (3) The crude amine solution after dechlorination is passed through an MFI molecular sieve membrane at 80~120℃ and a vacuum of 1~5kPa on the back side of the membrane to selectively separate ethylenediamine and water. The retentate is passed through an FAU molecular sieve membrane at 100~140℃ to selectively separate diethylenetriamine and triethylenetetramine. (4) The retentate from the FAU molecular sieve membrane is transported to a distillation column for distillation and purification to obtain polyethylene polyamine; The catalyst is the catalyst prepared by the preparation method described in claim 2.

6. The production process of polyethylene polyamine according to claim 5, characterized in that, In step (1), the space velocity of the ammonia and hydrogen mixture is 500-1000 h⁻¹. -1 The volume ratio of ammonia to hydrogen is 95:

5.

7. The production process of polyethylene polyamine according to claim 5, characterized in that, In step (1), the space velocity of pure ammonia is 200-400 h⁻¹. -1 .

8. The production process of a polyethylenepolyamine according to claim 5, characterized in that, The reaction conditions in step (2) are: temperature 200~280℃, pressure 6.0~10.0MPa, and weight hourly space velocity 0.8~1.5h. -1 .

9. The production process of a polyethylenepolyamine according to claim 5, characterized in that, The conditions for distillation purification in step (4) are a pressure of 0.5~5.0 kPa and a bottom temperature of 150~200℃.