A dry treatment method for kaolin-based coal gangue sludge and coal gangue-based non-fired bricks

By using a dry processing method, combined with dry granular additive mixing, mechanical crushing, screening, and air classification, the problem of continuous crushing and component separation of kaolin-based coal gangue mud was solved, achieving efficient resource utilization and high-strength production of non-fired bricks.

CN123102478APending Publication Date: 2026-11-17ZICHANG TAIRUI NEW ENVIRONMENTALLY FRIENDLY BUILDING MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611464409.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-20
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In the process of resource utilization, kaolin-based coal gangue mud is difficult to continuously crush and effectively separate light fine powder and heavy particles due to its high viscosity and high moisture content, resulting in equipment blockage and low separation efficiency, which affects its large-scale utilization.

Method used

A dry processing method is adopted, which involves mechanical crushing, screening and air classification after mixing with dry granular additives. This avoids the addition of water and utilizes the dry additives to adsorb free water and form a physical isolation layer, thereby achieving continuous crushing and component separation of coal gangue sludge.

Benefits of technology

It has achieved continuous mechanical crushing and effective component separation of kaolin-based coal gangue sludge, improved separation efficiency, ensured the quality and compressive strength of raw materials for non-fired bricks, and realized the full resource utilization of coal gangue sludge.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123102478A_ABST
    Figure CN123102478A_ABST
Patent Text Reader

Abstract

This invention discloses a dry processing method for kaolin-based coal gangue sludge and a coal gangue-based non-fired brick. The method includes: mixing hydrated kaolin-based coal gangue sludge with dry granular additives at a mass ratio of 1:0.5-2 to obtain a mixture; mechanically crushing the mixture without introducing external moisture to obtain crushed material; sieving the crushed material to obtain oversize and undersize materials, and returning the oversize material to the mechanical crushing process; and air-classifying the undersize material to separate light fine powder and heavy particles. This avoids the re-agglomeration of kaolin upon contact with water, solves the problem of continuous dry crushing and component separation of highly viscous coal gangue sludge, and realizes continuous dry crushing and dry component separation of highly viscous coal gangue sludge. The coal gangue-based non-fired brick is made with heavy particles as fine aggregate, light fine powder as fine powder filler, and cement, quicklime, gypsum, and sodium sulfate added.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of coal gangue resource utilization technology, and particularly relates to a dry treatment method for kaolin-based coal gangue mud and coal gangue-based non-fired bricks. Background Technology

[0002] Coal gangue sludge, generated during coal gangue washing, is one of the main solid wastes in the coal industry. Its resource utilization typically requires the effective separation of light fine powder from heavy particles so that they can be used as building material raw materials. For kaolin-based coal gangue sludge, which is mainly composed of clay minerals such as kaolinite and montmorillonite, its high water content and strong adhesion present key challenges in achieving continuous and stable crushing and component separation.

[0003] In related technologies, the treatment of coal gangue slime typically employs wet jigging or mechanical filtration dewatering followed by stockpiling. During wet separation, kaolin-based coal gangue slime easily rehydrates, expands, and agglomerates upon contact with water, reverting to a clay-like state, making effective separation difficult. Mechanically dewatered coal gangue slime retains a high water-holding capacity, resulting in a long natural drying period. However, if conventional dry crushing equipment is used to process coal gangue slime with high moisture content, the material's high adhesiveness easily adheres to the inner wall of the crushing chamber and the screen plates, causing equipment blockage and hindering continuous operation. Furthermore, the methods for effectively separating light fine powder and heavy particles in coal gangue slime under dry conditions are not yet perfect, limiting the component-based utilization of kaolin-based coal gangue slime.

[0004] The aforementioned problems hinder the continuous crushing process and the effective separation of light fine powder and heavy particles in the resource utilization of kaolin-based coal gangue slime, thus affecting the large-scale utilization of coal gangue washing byproducts. Therefore, it is necessary to provide a dry processing technology that can continuously crush kaolin-based coal gangue slime and effectively separate light fine powder and heavy particles without introducing external moisture. Summary of the Invention

[0005] The purpose of this invention is to provide a dry treatment method for kaolin-based coal gangue mud and coal gangue-based non-fired bricks, so as to solve the technical problems in the prior art that high-viscosity coal gangue mud is easy to re-agglomerate when it comes into contact with water, has strong viscosity, and is difficult to continuously mechanically crush and utilize in different grades.

[0006] To solve the above-mentioned technical problems, the present invention provides a dry treatment method for kaolin-based coal gangue sludge, comprising the following steps: S1. Mix the kaolin-based coal gangue mud in a hydrated state with dry granular additives at a mass ratio of 1:0.5-2 to obtain a mixture; S2. The mixture is mechanically crushed without introducing external moisture to obtain crushed material; S3. Screen the crushed material to obtain the oversize and undersize material, and return the oversize material to be mechanically crushed; S4. The sieved material is classified by air separation to obtain light fine powder and heavy particles.

[0007] Preferably, the dry particulate admixture includes at least one of fine sand and dust collector dust.

[0008] Preferably, the moisture content of the kaolin-based coal gangue mud in the water-containing state is 15-25%, the particle size of the fine sand is 0.1-5mm, the moisture content of the fine sand is ≤20%, and the moisture content of the dust from the dust collector is ≤8%.

[0009] Preferably, mechanical crushing specifically involves crushing the mixture to a particle size of less than 3 mm to obtain crushed material.

[0010] Preferably, the crushed material is screened by passing it through a 3mm screen to obtain oversize and undersize material.

[0011] Preferably, the process of air classifying the undersize material involves feeding the undersize material into a classifier and having the classifier perform air classification on the undersize material at a frequency of 28-35Hz.

[0012] Preferably, the light fine powder has a particle size of 0.01-0.5 mm and a bulk density of 0.6-0.9 g / cm³. 3 The heavy particles have a particle size of 0.5-3 mm and a bulk density of 1.2-1.6 g / cm³. 3 .

[0013] The present invention also provides a coal gangue-based non-fired brick, comprising: 45-55 parts fine aggregate, 25-35 parts fine powder filler, 10-18 parts cement, 2-5 parts quicklime, 1-2 parts gypsum, and 0.3-0.8 parts sodium sulfate; wherein the fine aggregate and fine powder filler are heavy particles and light fine powder obtained by any of the above-mentioned dry processing methods of kaolin-based coal gangue mud.

[0014] Preferably, the mass ratio of fine aggregate, fine powder filler, cement, quicklime, gypsum and sodium sulfate is 55:25:15:3:1.5:0.5.

[0015] Preferably, the fine aggregate is fine sand obtained by classifying kaolin-based coal gangue mud through a hydrocyclone screen, and the fine powder filler is dust obtained by classifying kaolin-based coal gangue mud through a dust collector.

[0016] Compared with the prior art, the beneficial effects of the present invention are: This invention's process does not introduce any external moisture, fundamentally avoiding the problem of kaolin re-agglomeration upon contact with water. By mixing wet coal slime with dry auxiliary materials, highly viscous coal gangue slime achieves continuous mechanical crushing. Combined with a screening loop for cyclic crushing and air classification, it realizes the dry separation and utilization of each component of the coal gangue slime. This invention limits the mass ratio range of coal gangue slime to dry auxiliary materials, ensuring that the dry auxiliary materials fully absorb free water and coat the coal gangue slime particles, preventing crushing blockage, while also avoiding excessive burden on air classification due to excessive auxiliary materials, thus balancing crushing continuity and air classification efficiency. The moisture content of the coal gangue slime is limited to 15-25%, allowing the overall moisture content after mixing to be adjusted to the range required for mechanical crushing. This avoids excessive moisture causing blockage in the crushing chamber or insufficient moisture leading to poor dispersion, ensuring the continuity and stability of dry crushing.

[0017] This invention selects fine sand and / or dust from dust collectors as dry auxiliary materials. These materials utilize their large surface area to adsorb free water and coat particles, preventing re-adhesion, while simultaneously enabling the recycling of fine sand and dust collector dust. The fine sand particle size is limited to 0.1-5mm, allowing it to form a stable physical isolation layer on the surface of coal gangue sludge particles. The moisture content of the fine sand is limited to ≤20%, and the moisture content of the dust collector dust is limited to ≤8%, ensuring that the auxiliary materials have sufficient water absorption capacity and preventing the crushing equipment from becoming clogged due to excessive moisture.

[0018] This invention crushes the mixture to below 3mm, allowing the coal gangue mud agglomerates to fully disintegrate and the dry auxiliary materials to fully mix with the coal gangue mud particles, providing suitable particle size conditions for air classification; a 3mm screen is set for screening and the material on the screen is returned for recycling and crushing, ensuring that the particle size of the material entering the air classification is uniform and avoiding the mixing of large particles, which would reduce the separation accuracy of light fine powder and heavy particles.

[0019] This invention utilizes air classification at 28-35Hz to carry out light fine powders while allowing heavy particles to settle. This avoids fine powders from mixing with heavy particles and affecting the aggregate gradation of the non-fired bricks, while also preventing excessive blowing of heavy particles into the light fine powders, thus avoiding material waste. Furthermore, by limiting the classifier frequency to 30-32Hz, the air classification airflow velocity is kept more stably within the separation range, improving the purity and yield of the light fine powders and heavy particles, and ensuring the stability of the raw material quality for non-fired bricks.

[0020] This invention specifies that the light fine powder has a particle size of 0.01-0.5 mm and a bulk density of 0.6-0.9 g / cm³. 3 The heavy particles have a particle size of 0.5-3 mm and a bulk density of 1.2-1.6 g / cm³. 3 This process ensures that both materials possess the required fineness, density, and particle size characteristics for fillers and aggregates, respectively. After air classification, the lightweight fine powder is used as filler to fill the voids in the aggregate and improve the density of the brick, while the heavy particles are used as aggregate to form a skeleton structure to bear the load. This achieves the synergistic utilization of air-classified products and effectively improves the compressive strength of the non-fired bricks. Attached Figure Description

[0021] To more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings used in the embodiments will be briefly introduced below. It should be understood that the following drawings only show some embodiments of the present invention and should not be regarded as a limitation on the scope. For those skilled in the art, other related drawings can be obtained based on these drawings without creative effort.

[0022] Figure 1 A process flow diagram of the dry treatment method for kaolin-based coal gangue mud provided in the embodiments of this application. Detailed Implementation

[0023] In the description of this application, "multiple" means at least two, such as two, three, etc., unless otherwise explicitly specified. All directional indications (such as up, down, left, right, front, back, top, bottom, etc.) in the embodiments of this application are only used to explain the relative positional relationships and movement of the components in a specific posture (as shown in the figures). If the specific posture changes, the directional indication will also change accordingly. Furthermore, the terms "comprising" and "having," and any variations thereof, are intended to cover non-exclusive inclusion. For example, a process, method, system, product, or IoT terminal that includes a series of steps or units is not limited to the listed steps or units, but may optionally include steps or units not listed, or may optionally include other steps or units inherent to these processes, methods, products, or IoT terminals.

[0024] Furthermore, the reference to "embodiment" herein means that a particular feature, structure, or characteristic described in connection with an embodiment may be included in at least one embodiment of this application. The appearance of this phrase in various places throughout the specification does not necessarily refer to the same embodiment, nor is it a separate or alternative embodiment mutually exclusive with other embodiments. It will be explicitly and implicitly understood by those skilled in the art that the embodiments described herein can be combined with other embodiments.

[0025] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0026] like Figure 1 As shown, the present invention provides a dry treatment method for kaolin-based coal gangue sludge, comprising the following steps: Step 1: Mix the kaolin-based coal gangue mud in a hydrated state with dry granular additives at a mass ratio of 1:0.5-2 to obtain the mixture.

[0027] This invention, through extensive experimentation, has found that when the mass ratio of coal gangue sludge to dry additives is less than 1:0.5, the dry additives are insufficient to effectively reduce the overall viscosity of the mixture, and the crushing equipment will still experience blockage. When the ratio is greater than 1:2, the dry additives are excessive, resulting in an excessively high proportion of fine sand and dust in the mixture, which reduces the efficiency of subsequent air classification and also leads to a relatively insufficient cementitious material and reduced brick strength in the non-fired bricks due to the excessively high proportion of fine aggregates. Therefore, the range of 1:0.5-2 is the optimal process range verified by experiments in this invention.

[0028] Step 2: The mixture obtained in Step 1 is mechanically crushed without introducing any external moisture to obtain crushed material.

[0029] After step one, the moisture content of the mixture is reduced to 12-18%, and the viscosity is significantly reduced, so it can be crushed using a conventional hammer crusher or impact crusher.

[0030] Step 3: Screen the crushed material obtained in Step 2 to obtain the oversize and undersize material, and return the oversize material for mechanical crushing.

[0031] Step 4: The sieved material is air-separated to obtain light fine powder and heavy particles.

[0032] Dry processing refers to the process of mixing, crushing, screening, and air classification without adding additional process water to the material. This excludes moisture inherent in the raw materials and does not exclude circulating cooling water in the equipment cooling system that does not come into contact with the material. Dry granular additives can adsorb some of the free water in kaolin-based coal gangue slurry and form a physical barrier on the particle surface, thereby reducing the adhesion of the mixture and allowing the mechanical crushing and screening processes to proceed continuously. The oversize material is returned to the crushing stage to control the particle size within a set range, while air classification uses airflow to carry out light, fine powder and allow heavy particles to settle, achieving dry separation of the two types of products.

[0033] Furthermore, the hydrated kaolin-based coal gangue mud is first mixed with dry granular additives. The dry granular additives can adsorb some free water and form a granular isolation layer on the surface of the coal gangue mud agglomerates, thus dispersing the agglomerates into smaller particles under crushing, impact, and shearing action. Since subsequent screening and air classification are carried out without introducing external moisture, the dispersed fine kaolin particles do not revert to a clay-like state due to rehydration, thereby enabling continuous particle size control and component separation.

[0034] In the above method, the moisture content of the kaolin-based coal gangue sludge can be controlled at 15-25%, and the dry granular additives can include at least one of fine sand and dust from a dust collector. The particle size of the fine sand can be 0.1-5 mm, and the moisture content of the fine sand can not exceed 20%, while the moisture content of the dust from the dust collector can not exceed 8%. When the mass ratio of kaolin-based coal gangue sludge to dry granular additives is 1:1, the moisture content of the mixture can be adjusted to 12-18%, balancing crushing continuity and air classification efficiency. Mechanical crushing can crush the mixture to a particle size of less than 3 mm. After the crushed material is screened through a 3 mm screen, the oversize material that does not meet the size requirements is returned for further crushing. The purpose of crushing to less than 3 mm is to fully disintegrate the coal gangue sludge agglomerates and to fully mix the dry additives with the coal gangue sludge particles, while providing suitable particle size conditions for subsequent air classification. Experiments show that when the crushed particle size is >3 mm, the air classification efficiency decreases significantly.

[0035] After the undersize material enters the air classifier, the classifier frequency can be set to 28-35Hz, or even further to 30-32Hz, to separate light fine powder and heavy particles. When the wind speed is below 28Hz, the light fine powder cannot be effectively separated, and a large amount of fine powder is mixed with the heavy particles, resulting in an imbalance in the aggregate gradation and a decrease in density of the non-fired bricks. When the wind speed is above 35Hz, some heavy particles are excessively blown into the light fine powder, causing material waste and a decrease in classification accuracy. Therefore, 28-35Hz is the optimal wind speed range for this invention, as verified by experiments.

[0036] After air classification, the particle size of the light fine powder can be 0.01-0.5 mm, and the bulk density can be 0.6-0.9 g / cm³. 3 The main components are dust from dust collectors, fine coal slime particles, and a small amount of fine gangue powder, with a moisture content of ≤8% and a low calorific value; the particle size of the heavy particles can be 0.5-3mm, and the bulk density can be 1.2-1.6g / cm³. 3 The main components are fine sand and dehydrated particles, with a moisture content of ≤5%, exhibiting high particle strength and good gradation characteristics. Lightweight fine powder can be used as fine powder filler in non-fired bricks, while heavy particles can be used as fine aggregate. After both are incorporated into the non-fired brick batching system, the fine powder fills the voids between the aggregates, and the heavy particles form a skeletal structure, improving the density and load-bearing capacity of the brick.

[0037] In one specific embodiment provided in this application, a mass ratio of 1:0.5-2 means that the actual feed mass of kaolin-based coal gangue slurry in its hydrated state is 1 part, and the actual feed mass of dry granular additives is 0.5-2 parts. For example, the mass ratio of kaolin-based coal gangue slurry in its hydrated state to dry granular additives can be 1:0.5, 1:0.6, 1:0.7, 1:0.8, 1:0.9, 1:1.0, 1:1.1, 1:1.2, 1:1.3, 1:1.4, 1:1.5, 1:1.6, 1:1.7, 1:1.8, 1:1.9, or 1:2.0. This mass ratio can be controlled by a belt scale, screw weighing scale, or silo weighing module, or it can be weighed in batches before entering the mixing device.

[0038] When the mass ratio of hydrated kaolin-based coal gangue slime to dry granular additives is less than 1:0.5, the amount of dry granular additives is insufficient to fully adsorb the free water in the coal gangue slime, and it is also difficult to form a continuous particle separation effect on the surface of the coal gangue slime particles. The mixture may still exhibit strong adhesion, and material may easily stick or clog the screen in the crushing chamber and screening surface. When the mass ratio is higher than 1:2, the proportion of dry granular additives is too high, increasing the total amount of material entering the air classification and the probability of particle collisions. The separation interface between light fine powder and heavy particles widens, and some particles that could be used as aggregate may be entrained in the light fine powder, or some fine powder may remain in the heavy particles, resulting in a decrease in classification efficiency. Controlling the mass ratio at 1:0.5-2 is beneficial for achieving a balance between crushing continuity and air classification load.

[0039] Moisture content can be determined using the drying loss-on-weight method. Specifically, take a representative sample of approximately 100 grams, spread it evenly in a desiccator or metal tray, and dry it at 105±5℃ until the difference between two consecutive weighings is no greater than 0.1% of the initial sample mass. The moisture content is calculated as W = [mass before drying - mass after drying] / mass before drying × 100%. This method can be used to determine the moisture content of coal gangue mud, fine sand, dust collector dust, light fine powder, and heavy particles. If the sample contains volatile components that are not moisture, the test temperature and drying time can be checked in conjunction with the source of the raw materials; however, consistent test conditions should be used in comparative tests within the same batch.

[0040] Particle size can be determined by sieving, laser particle size analysis, or a combination of both. For particles in the 0.5-5 mm range, dry sieving or mechanical vibrating sieving using standard sieves can be used. After sieving, the particle size range is determined based on the mass ratio of particles passing through the corresponding sieve openings. For light fine powders in the 0.01-0.5 mm range, laser particle size analyzers can be used for testing. Alternatively, the upper limit can be controlled using a 0.5 mm sieve, and then the volume distribution can be obtained using a laser particle size analyzer. In this article, particle sizes of 0.01-0.5 mm or 0.5-3 mm generally refer to the main particle distribution within this range; in continuous industrial production, a small amount of deviation between adjacent particle sizes is permissible due to sampling, sieving boundaries, or irregular particle morphology.

[0041] Bulk density can be determined using the constant-volume container method. Specifically, a graduated cylinder or metal container with a known volume V can be used. First, weigh the empty container to a mass m0. Then, fill the container with the material to be tested under natural drop conditions. After filling, level the container with a ruler along the rim to avoid artificial compaction. Next, weigh the total mass of the container and the material to a mass m1. The bulk density ρ = [m1 - m0] / V. If the moisture content of the material fluctuates significantly, the moisture content should be recorded simultaneously with the bulk density measurement to evaluate whether the batch of products meets the grading requirements.

[0042] Dry granular additives may include at least one of fine sand and dust collector dust. Fine sand has a relatively large particle size, which can form physical gaps between coal gangue mud particles, reducing the probability of direct contact and re-agglomeration between mud particles. Dust collector dust has a finer particle size and a larger specific surface area, which can adsorb and disperse free water and participate in the subsequent filling of non-fired bricks with fine powder. Fine sand and dust collector dust can be used alone or mixed in a certain proportion.

[0043] During the mixing process, the dry granular additives can be added to the mixing device first, followed by the kaolin-based coal gangue slurry containing moisture, or both can be metered and added simultaneously. To improve material uniformity, the mixing time can be controlled between 2 and 10 minutes; the mixer speed can be determined according to the equipment specifications, as long as the dry granular additives and coal gangue slurry are in full contact and over-compaction is avoided. The mixed material should be in the form of loose granules or small clumps, able to clump together when squeezed by hand but disperse easily upon light touch or drop, and there should be no large amount of free water on the surface.

[0044] The overall moisture content of the mixture can be controlled between 12-18%. If the overall moisture content is too high, the impact energy within the crusher will be absorbed by the viscous agglomerates, and the material will easily accumulate at the screen plate and discharge port. If the overall moisture content is too low, the surface of the coal gangue mud agglomerates may not be uniformly coated by the dry granular additives, and dust will increase during crushing and conveying, leading to a higher load on subsequent air separation. By controlling the moisture content of the coal gangue mud, the moisture content of the dry granular additives, and their mass ratio, the overall moisture content of the mixture can be kept within a suitable range for mechanical crushing and screening.

[0045] When mechanically crushing a mixture without introducing external moisture, a hammer crusher can be used. The rotor speed, hammer gap, and screen aperture of the hammer crusher can be adjusted according to the throughput and material moisture content. Taking the processing of kaolin-based coal gangue mud with a moisture content of approximately 20-22% as an example, after the mixture enters the hammer crusher, the impact of the hammers breaks up the coal gangue mud agglomerates. Fine sand particles play a grinding and isolating role during the collision process, while dust from the dust collector adheres to the moist surface, reducing the re-agglomeration of fine particles after crushing. This crushing process does not require spraying water into the crushing chamber or adding wetting agents.

[0046] The crushed material from mechanical crushing then enters the screening device. The oversize material from screening is returned to mechanical crushing, while the undersize material enters the air classification system. The return of oversize material to mechanical crushing can be achieved via a return belt, screw conveyor, or bucket elevator. With the return channel in place, particles whose size does not yet meet the air classification requirements will not directly enter the air classification device, but will circulate between crushing and screening until they can pass through the screen. This cycle transforms particle size control from a single crushing operation to a crushing-screening closed loop, reducing particle size fluctuations caused by variations in the size of the feed cake.

[0047] This invention also provides a coal gangue-based non-fired brick, the raw materials of which, by weight, include: 45-55 parts fine aggregate, 25-35 parts fine powder filler, 10-18 parts cement, 2-5 parts quicklime, 1-2 parts gypsum, and 0.3-0.8 parts sodium sulfate. The fine aggregate can be derived from heavy particles obtained by classifying kaolin-based coal gangue sludge, and the fine powder filler can be derived from light fine powder obtained by classifying kaolin-based coal gangue sludge. In one formulation, the mass ratio of fine aggregate, fine powder filler, cement, quicklime, gypsum, and sodium sulfate can be 55:25:15:3:1.5:0.5. Under this formulation, the heavy particles provide the skeleton, the light fine powder fills the voids, the cement provides the cementing effect, and the quicklime, gypsum, and sodium sulfate together form an alkali-sulfur composite activating system, promoting early strength development and activating the potential activity of the fine-grained gangue.

[0048] In coal gangue-based non-fired bricks, the fine aggregate, fine powder filler, cement, quicklime, gypsum, and sodium sulfate are not simply mixed together. Heavy particles provide the main skeleton, while lightweight fine powder fills the voids and provides micro-silica-alumina components that can be reacted with in an alkaline environment. Cement provides the basic hydration products, quicklime increases alkalinity, and gypsum and sodium sulfate provide sulfate ions to participate in the early formation of hydration products. These components work together to create a structure in the pressed brick blank during curing that combines aggregate support, fine powder filling, and cementitious bonding.

[0049] The functions of each component in non-fired bricks are as follows: Fine aggregate (45-55 parts): Fine sand sieved using a hydrocyclone, with a particle size of 0.5-3mm. It serves as the skeleton material of the brick body, providing compressive strength support. If the fine aggregate content is too low (<45 parts), the brick body lacks a rigid skeleton and its strength is insufficient; if the content is too high (>55 parts), the fine powder filler is relatively insufficient, increasing the porosity of the brick body and decreasing its density.

[0050] Fine powder filler (25-35 parts): Uses dust from a dust collector, with a particle size <0.5mm. Its function is to fill the voids between fine aggregates, increasing the density of the brick; and to participate in the hydration reaction, reacting with cement and quicklime to form hydrated calcium silicate gel, thus increasing the strength of the brick. When the content is less than 25 parts, the filling is insufficient, resulting in high porosity of the brick; when the content is greater than 35 parts, the aggregate is relatively reduced, leading to increased brick shrinkage.

[0051] Cement (10-18 parts): The main cementing material, it reacts with water to form hydrated calcium silicate gel, which binds the aggregate and filler into a whole. When the cement content is less than 10 parts, the cementing effect is insufficient, and the brick strength is difficult to meet the standard; when it is more than 18 parts, the cost increases and the drying shrinkage is greater.

[0052] Quicklime (2-5 parts): An alkaline activator that generates calcium hydroxide upon addition of water, raising the pH of the system to 12-13, breaking the Si-O and Al-O bonds on the surface of coal gangue particles, and releasing active silica and aluminum components to participate in the hydration reaction. Simultaneously, the exothermic hydration of quicklime can promote early strength development.

[0053] Gypsum (1-2 parts): A sulfate activator that reacts with tricalcium aluminate in cement to form ettringite, which has micro-expansion properties and can compensate for the drying shrinkage of bricks, preventing cracking. When the gypsum content is less than 1 part, the shrinkage compensation effect is insufficient; when it is more than 2 parts, excessive sulfate may lead to later expansion damage.

[0054] Glauber's salt (0.3-0.8 parts): an early strength activator. Its sulfate ions can accelerate the cement hydration process and improve the early strength of bricks. Glauber's salt, quicklime, and gypsum form an "alkali-sulfur" composite activating system. The three work synergistically to produce an activating effect of "1+1+1>3".

[0055] In this invention, quicklime, gypsum, and sodium sulfate constitute an "alkali-sulfur" composite activating system. Their synergistic mechanism is as follows: quicklime provides an alkaline environment (pH>12), disrupting the surface structure of coal gangue particles and releasing active silica and aluminum; sodium sulfate provides sulfate ions, accelerating cement hydration and promoting early strength development; gypsum provides calcium ions and sulfate ions, reacting with tricalcium aluminate to form ettringite, compensating for shrinkage. All three are indispensable. Experiments show (see Table 1): using only cement and aggregate (without the composite activator), the 28-day compressive strength is only 8.9 MPa; after adding the complete composite activator system, the 28-day compressive strength can reach 15.6 MPa, an increase of 75%. This demonstrates that the synergistic activating effect of "quicklime + gypsum + sodium sulfate" is the key technical feature of this invention for achieving high strength performance in its non-fired bricks.

[0056] The present invention will be further described below with reference to specific embodiments and comparative examples, but the present invention is not limited to these embodiments.

[0057] Example 1 Take 100 kg of kaolin-based coal gangue mud with a moisture content of 22%, mix it with 50 kg of fine sand and 50 kg of dust from a dust collector (mass ratio 1:1), and feed it into a hammer crusher to crush it to below 3 mm. Then, screen it through a 3 mm drum screen. The material on the screen is returned to the crusher for recycling and crushing, while the material under the screen is sent to a classifier for air classification under a wind speed of 30 Hz to obtain light fine powder and heavy particles.

[0058] Prepare non-fired bricks according to the following proportions: 55 kg heavy granules, 25 kg light fine powder, 15 kg cement, 3 kg quicklime, 1.5 kg gypsum, and 0.5 kg sodium sulfate. After mixing evenly, add water and stir. Press into shape under a pressure of 15 MPa. After natural curing for 28 days, the compressive strength is tested to be 15.6 MPa.

[0059] Example 2 100 kg of kaolin-based coal gangue mud with a moisture content of 20% was mixed with 70 kg of fine sand and 30 kg of dust from a dust collector, and processed using the same method as in Example 1. Non-fired bricks were prepared according to the following proportions: 50 kg of heavy granules, 30 kg of lightweight fine powder, 15 kg of cement, 3 kg of quicklime, 1.5 kg of gypsum, and 0.5 kg of sodium sulfate. After curing for 28 days, the compressive strength was tested and found to be 14.8 MPa.

[0060] Comparative Example 1 100 kg of kaolin-based coal gangue mud with a moisture content of 22% was fed directly into a hammer crusher without adding any dry additives. The equipment stopped after running for 5 minutes due to material blockage and could not continue processing.

[0061] Comparative Example 2 100 kg of kaolin-based coal gangue mud with a moisture content of 22% was mixed with 50 kg of fine sand and 50 kg of dust from a dust collector. The mixture was crushed and screened according to the method in Example 1, but without air separation by a classifier. The crushed mixture was directly prepared into non-fired bricks according to the same proportion as in Example 1 (55 kg of heavy particles and 25 kg of light fine powder). After curing under the same conditions for 28 days, the compressive strength was tested to be 7.6 MPa.

[0062] Comparative Example 3 The heavy particles and light fine powder obtained from the air classifier in Example 1 were used to prepare non-fired bricks according to the following ratio: 55 kg of heavy particles, 25 kg of light fine powder, 15 kg of cement, 0 kg of quicklime, 0 kg of gypsum, and 0 kg of sodium sulfate (i.e., no composite activator was added). After curing under the same conditions for 28 days, the compressive strength was tested to be 8.9 MPa.

[0063] Performance testing The unfired brick test blocks of Examples 1-2 and Comparative Examples 2-3 were all subjected to 28-day compressive strength tests in accordance with GB / T 4111-2013 "Test Methods for Concrete Blocks and Bricks". The results are shown in Table 1.

[0064] Table 1. Comparison of 28-day compressive strength of unfired bricks in the Example and Comparative Examples

[0065] As can be seen from Table 1: Comparative Example 2, without air classification, directly used bricks from coal gangue mud, fine sand, and dust without separation. Its 28-day compressive strength was only 7.6 MPa, lower than the national standard GB / T 21144-2007's strength requirement for MU10 solid concrete bricks (≥10 MPa). Example 1, after air classification, used heavy particles and light fine powder as aggregate and filler, respectively, achieving a strength of 15.6 MPa, a 106% increase compared to Comparative Example 2. This demonstrates that air classification plays a crucial role in achieving synergistic utilization of the various components of coal gangue mud and improving the density and strength of the bricks.

[0066] Although Comparative Example 3 underwent air classification, it did not contain the composite activator (quicklime + gypsum + sodium sulfate), and its 28-day compressive strength was only 8.9 MPa. Example 1, with the same materials but with the addition of the composite activator, achieved a strength of 15.6 MPa, a 75% increase compared to Comparative Example 3. This indicates that the "quicklime + gypsum + sodium sulfate" composite activator system has a significant synergistic effect on activating the pozzolanic activity of fine-grained gangue, and is a necessary condition for obtaining high strength in non-fired bricks.

[0067] The experimental data above show that the steps of the technical solution of the present invention have a synergistic effect, producing an unexpected technical effect of "1+1>2".

[0068] The method employed in this invention does not introduce external moisture, thus preventing the kaolin-based coal gangue sludge from reabsorbing water and reverting to a clay-like state during wet processing. This reduces material adhesion during crushing and screening, and the lightweight fine powder is separated from the heavy particles through circulating screening and air classification. The resulting lightweight fine powder and heavy particles are used as filler and aggregate in non-fired bricks, respectively, achieving the separate utilization of lightweight fine powder and heavy particles in the kaolin-based coal gangue sludge.

[0069] The present invention specifically embodies the following beneficial effects: Technological Innovation: This invention employs a combined "dry crushing-screening-air separation" process to treat kaolin-based coal gangue slime. No external water is introduced throughout the process, avoiding the problem of kaolin re-agglomeration when exposed to water in wet treatment. This solves the industry problem of the difficulty in resource utilization of highly viscous coal slime.

[0070] Formula innovation: This invention adopts a six-component formula of "fine aggregate + fine powder filler + cement + quicklime + gypsum + sodium sulfate". Among them, "quicklime + gypsum + sodium sulfate" constitute an "alkali-sulfur" composite activating system. The three work synergistically to enable the compressive strength of the non-fired bricks to reach 15.6 MPa after 28 days, which is 75% higher than the control sample (8.9 MPa) without the addition of composite activator.

[0071] Full utilization: This invention utilizes all the fine sand (screened by hydrocyclone) and dust (collected by dust collector) generated during the coal gangue sludge treatment process as raw materials for non-fired bricks, achieving zero discharge and full utilization of coal gangue washing by-products.

[0072] The basic principles of this application have been described above with reference to specific embodiments. However, it should be noted that the advantages, benefits, and effects mentioned in this application are merely examples and not limitations, and should not be considered as essential features of each embodiment of this application. Furthermore, the specific details disclosed above are for illustrative and facilitative purposes only, and are not limitations. These details do not limit the application to the necessity of employing the specific details described above. The above description is provided to enable any person skilled in the art to make or use this application. Various modifications to these aspects will be readily apparent to those skilled in the art, and the general principles defined herein can be applied to other aspects without departing from the scope of this application. Therefore, this application is not intended to be limited to the aspects shown herein, but rather to be accorded the widest scope consistent with the principles and novel features of this application.

[0073] The above are merely preferred embodiments of this application and are not intended to limit the scope of this application. Any modifications or equivalent substitutions made within the spirit and principles of this application shall be included within the protection scope of this application.

[0074] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.

Claims

1. A dry treatment method for kaolin-based coal gangue sludge, characterized in that, Including the following steps: S1. Mix the kaolin-based coal gangue mud in a hydrated state with dry granular additives at a mass ratio of 1:0.5-2 to obtain a mixture; S2. The mixture is mechanically crushed without introducing external moisture to obtain crushed material; S3. Screen the crushed material to obtain oversize and undersize material, and return the oversize material to be mechanically crushed. S4. The undersize material is classified by air separation to obtain light fine powder and heavy particles.

2. The dry treatment method for kaolin-based coal gangue slime according to claim 1, characterized in that, The dry granular additive includes at least one of fine sand and dust from a dust collector.

3. The dry treatment method for kaolin-based coal gangue slime according to claim 2, characterized in that, The water content of the kaolin-based coal gangue mud is 15-25%, the particle size of the fine sand is 0.1-5mm, the water content of the fine sand is ≤20%, and the water content of the dust from the dust collector is ≤8%.

4. The dry treatment method for kaolin-based coal gangue slime according to claim 1, characterized in that, The mechanical crushing specifically involves crushing the mixture to a particle size of less than 3 mm to obtain the crushed material.

5. The dry treatment method for kaolin-based coal gangue slime according to claim 1, characterized in that, The specific process of screening the crushed material is as follows: the crushed material is screened through a 3mm screen to obtain the oversize material and the undersize material.

6. The dry treatment method for kaolin-based coal gangue slime according to claim 1, characterized in that, The specific method of air-classifying the undersize material is as follows: the undersize material is fed into a classifier, and the classifier performs air-classification on the undersize material at a frequency of 28-35Hz.

7. The dry treatment method for kaolin-based coal gangue slime according to claim 1, characterized in that, The light fine powder has a particle size of 0.01-0.5 mm and a bulk density of 0.6-0.9 g / cm³. 3 The heavy particles have a particle size of 0.5-3 mm and a bulk density of 1.2-1.6 g / cm³. 3 .

8. A coal gangue-based non-fired brick, characterized in that, include: The mixture comprises 45-55 parts fine aggregate, 25-35 parts fine powder filler, 10-18 parts cement, 2-5 parts quicklime, 1-2 parts gypsum, and 0.3-0.8 parts sodium sulfate; wherein the fine aggregate and the fine powder filler are heavy particles and light fine powder obtained by the dry processing method of kaolin-based coal gangue mud as described in any one of claims 1-7.

9. A coal gangue-based non-fired brick according to claim 8, characterized in that, The mass ratio of the fine aggregate, the fine powder filler, the cement, the quicklime, the gypsum, and the sodium sulfate is 55:25:15:3:1.5:0.

5.

10. A coal gangue-based non-fired brick according to claim 8, characterized in that, The fine aggregate is fine sand obtained by grading kaolin-based coal gangue mud through a hydrocyclone screen, and the fine powder filler is dust obtained by grading kaolin-based coal gangue mud through a dust collector.