A dispersion pretreatment method to improve the flotation separation effect of molybdenite and chalcopyrite
By employing a physical dispersion method combining ultrasound and mechanical stirring, along with sodium hexametaphosphate and sodium carbonate dispersants, the agglomeration problem of molybdenite was solved, achieving efficient separation of molybdenite and chalcopyrite, improving copper-molybdenum separation efficiency, and ensuring that the copper content of the molybdenum concentrate meets the standards.
Patent Information
- Application Number
- CN202611380939.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-07
- Publication Date
- 2026-11-17
AI Technical Summary
Molybdenite is prone to hydrophobic aggregation under the action of non-polar oil collectors, which encapsulates chalcopyrite particles, resulting in low copper-molybdenum separation efficiency and difficulty in meeting the copper content standard of molybdenum concentrate.
A physical dispersion method combining ultrasonic waves and mechanical stirring is employed, along with sodium hexametaphosphate and sodium carbonate dispersants. The pH of the slurry is adjusted to 12, and physical and chemical dispersion treatment is carried out to break up molybdenite agglomerates. Through chemical adsorption onto the mineral surface, electrostatic repulsion is increased, thereby achieving effective separation of molybdenite and chalcopyrite.
This improved the flotation separation efficiency of molybdenite and chalcopyrite, ensuring that the copper content in the molybdenum concentrate meets the standards, and enhancing the copper-molybdenum separation efficiency.
Smart Images

Figure CN123102486A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of metallurgical technology, specifically relating to a dispersion pretreatment method for improving the flotation separation effect of molybdenite and chalcopyrite. Background Technology
[0002] Molybdenum, as an important strategic non-ferrous metal resource, is mainly used in the steel industry to produce special steels. With the development of the steel manufacturing industry, the demand for molybdenum ore resources is becoming increasingly urgent. Molybdenite is the main source of molybdenum, with nearly 50% of the world's molybdenum coming from copper-molybdenum ores, among which porphyry copper-molybdenum ores are the most typical. According to the molybdenum concentrate standard GB3200-89, most grades of molybdenum concentrate require a copper impurity content of ≤0.5%. Excessive copper content will seriously affect the subsequent molybdenum smelting and the quality of related products.
[0003] Currently, the copper-suppressing flotation process is the most widely used and effective method for separating copper-molybdenum sulfide minerals. However, in actual flotation, molybdenite has extremely strong natural hydrophobicity and is prone to hydrophobic agglomeration under the action of non-polar oil collectors. The agglomerates formed will encapsulate chalcopyrite particles, significantly reducing the copper-molybdenum separation efficiency, making it difficult for most copper-molybdenum beneficiation plants to meet the copper content standards of molybdenum concentrate.
[0004] Therefore, it is necessary to develop an efficient, stable, and low-cost dispersion pretreatment method to solve the problem of molybdenite agglomeration encapsulating chalcopyrite and improve the separation effect of copper-molybdenum flotation. This has become an urgent technical problem to be solved in the current mineral processing field. Summary of the Invention
[0005] The purpose of this invention is to provide a dispersion pretreatment method to improve the flotation separation effect of molybdenite and chalcopyrite.
[0006] The objective of this invention is achieved as follows: the dispersion pretreatment method for improving the flotation separation effect of molybdenite and chalcopyrite includes pretreatment, physical dispersion treatment, chemical dispersion treatment, and flotation separation steps, specifically including: A. Pretreatment: The mixed minerals of molybdenite and chalcopyrite are crushed, ground and screened to obtain mixed mineral particles a with a grinding fineness of -0.074 mm or more, accounting for more than 80%; B. Material dispersion processing: 1) Prepare a mineral slurry with a concentration of 25-40% by mixing mineral particles a, adjust the pH value to 12, and stir evenly to obtain mineral slurry b; 2) The slurry b is dispersed by ultrasonication and mechanically stirred to obtain slurry c; C. Chemical dispersion treatment: A dispersant is added to slurry c for dispersion treatment to obtain slurry d; the dispersant is composed of sodium hexametaphosphate and sodium carbonate. D. Flotation separation: Molybdenum collector and frother are added to the slurry d for flotation separation to obtain molybdenum concentrate and tailings.
[0007] The specific steps are as follows: 1. Mineral pretreatment: A mixture of molybdenite and chalcopyrite was selected, and after crushing, grinding, and sieving, 80% of the mixed mineral particles a were obtained with a grinding fineness of -0.074 mm. The mixed mineral particles were ultrasonically cleaned with deionized water to remove surface impurities, and then dried in a vacuum low-temperature environment at 60℃ for 24 hours and vacuum sealed for later use. The mass ratio of molybdenite to chalcopyrite in the mixed mineral was 5:1.
[0008] 2. Pulp preparation: The pretreated mixed mineral particles were added to deionized water and stirred evenly to prepare a slurry with a concentration of 25% to 40%. The pH of the slurry was adjusted to 12 using sodium hydroxide and stirred evenly.
[0009] 3. Physical dispersion processing: After being thoroughly stirred into the slurry with the adjusted pH value, ultrasonic dispersion was first performed using an ultrasonic disperser with an ultrasonic power of 200-300W and an ultrasonic time of 35 minutes. The slurry temperature was maintained at 25℃-30℃ to avoid excessive temperature affecting the surface properties of molybdenite. Subsequently, mechanical stirring was performed using a mechanical stirring device with a stirring speed of 1300r / min and a stirring time of 25 minutes to achieve the initial dispersal of molybdenite agglomerates.
[0010] 4. Chemical dispersion treatment: In the slurry after physical dispersion treatment, a mixture of 200 mg / L sodium hexametaphosphate and 360 mg / L sodium carbonate was added as a dispersant. The mixture was stirred for 3 minutes to allow the mixed dispersant to be fully adsorbed on the mineral surface, thus completing the dispersion pretreatment.
[0011] 5. Flotation separation: The pre-treated slurry was transferred to a flotation machine, and 100 mg / L of emulsified kerosene was added as a molybdenum collector. The kerosene emulsifier was sodium dodecylbenzene sulfonate, and the dosage was 0.5-1% of the kerosene mass. Methyl isobutyl methanol was used as a frother at a dosage of 30 mg / L. After stirring for 3 minutes, flotation separation was carried out for 4 minutes to obtain molybdenum concentrate and tailings.
[0012] This invention employs a composite dispersion method that combines physical and chemical dispersion, and its mechanism of action is as follows: 1. Physical dispersion mechanism: Ultrasonic dispersion utilizes the cavitation effect to form microbubbles in the slurry. The impact force generated when the bubbles burst can break up large molybdenite agglomerates. At the same time, the molybdenite particles are subjected to periodic stretching and compression, further destroying the agglomerate structure. Mechanical stirring provides sufficient shear force through the optimal rotation speed to completely break up the small agglomerates remaining after ultrasonic dispersion. At the same time, it makes the components in the slurry uniformly mixed, creating conditions for the action of chemical dispersants.
[0013] 2. Chemical Dispersion Mechanism: Both sodium carbonate and sodium hexametaphosphate are chemically adsorbed onto the surfaces of chalcopyrite and molybdenite, significantly reducing the surface potential of both minerals. At pH 12, the dominant dispersing component of sodium carbonate in the pulp is CO3. 2- It adsorbs onto the surface of minerals, while sodium hexametaphosphate is HPO4. 2- With PO4 3- Both ions can be adsorbed onto the mineral surface. On the one hand, the ions adsorbed on the surface of molybdenite generate steric repulsion, preventing the molybdenite particles from re-aggregating; on the other hand, the adsorption of ions significantly reduces the surface potential of the mineral, increasing the electrostatic repulsion between particles and further enhancing the dispersion effect; at the same time, the dispersion combination has minimal impact on the dispersion of chalcopyrite, ensuring that chalcopyrite is in a stable dispersed state and avoiding heterogeneous agglomeration with molybdenite, thereby achieving effective separation of molybdenite and chalcopyrite.
[0014] 3. Synergistic effect mechanism: Physical dispersion provides the basis for chemical dispersion. Large agglomerates are broken up by ultrasonic waves and mechanical stirring, increasing the contact area between molybdenite surface and dispersing agent. Chemical dispersion, on the other hand, consolidates the effect of physical dispersion. Spatial hindrance and electrostatic repulsion prevent particles from re-agglomerating. The two work synergistically to achieve efficient and stable dispersion of molybdenite, preventing it from encapsulating chalcopyrite, thereby improving the flotation separation effect. Attached Figure Description
[0015] Figure 1 This is a schematic diagram of the process flow of the present invention; Figure 2 This is a schematic diagram illustrating the mechanism of action of the present invention. Detailed Implementation
[0016] The present invention will be further described below with reference to embodiments, but this is not intended to limit the present invention in any way. Any modifications or substitutions made based on the teachings of the present invention shall fall within the protection scope of the present invention.
[0017] The dispersion pretreatment method for improving the flotation separation effect of molybdenite and chalcopyrite according to the present invention includes pretreatment, physical dispersion treatment, chemical dispersion treatment, and flotation separation steps, specifically including: A. Pretreatment: The mixed minerals of molybdenite and chalcopyrite are crushed, ground and screened to obtain mixed mineral particles a with a grinding fineness of -0.074 mm or more, accounting for more than 80%; B. Material dispersion processing: 1) Prepare a mineral slurry with a concentration of 25-40% by mixing mineral particles a, adjust the pH value to 12, and stir evenly to obtain mineral slurry b; 2) The slurry b is dispersed by ultrasonication and mechanically stirred to obtain slurry c; C. Chemical dispersion treatment: A dispersant is added to slurry c for dispersion treatment to obtain slurry d; the dispersant is composed of sodium hexametaphosphate and sodium carbonate. D. Flotation separation: Molybdenum collector and frother are added to the slurry d for flotation separation to obtain molybdenum concentrate and tailings.
[0018] In step 2), the ultrasonic dispersion power is 200-300W, the ultrasonic time is 30-40min, and the temperature of the slurry is maintained at 25-30℃.
[0019] The mechanical stirring speed described in step 2) is 1000~1500 r / min, and the stirring time is 20~30 min.
[0020] The molybdenum collector mentioned in step D is emulsified kerosene.
[0021] The kerosene emulsifier in the emulsified kerosene is sodium dodecylbenzene sulfonate, and the amount used is 0.5~1% of the kerosene mass.
[0022] The foaming agent mentioned in step D is methyl isobutyl alcohol.
[0023] The present invention will be further described below with reference to specific embodiments: Example 1
[0024] (1) Take molybdenum concentrate A from a certain mine. The molybdenum concentrate contains 42.93% molybdenum and 1.45% copper. The molybdenum concentrate does not meet the requirement of Cu≤0.5%. Calcium oxide is used to adjust the pH of the slurry to 12 and stir evenly.
[0025] (2) After stirring the slurry with the pH value adjusted, use an ultrasonic disperser to disperse it ultrasonically. The ultrasonic power is 200-300W and the ultrasonic time is 35min. The slurry temperature is kept at 25℃-30℃. Then transfer it to the flotation machine and set the flotation machine stirring speed to 1300r / min and the stirring time to 25min.
[0026] (3) Add a mixture of 750 g / t sodium hexametaphosphate and 1500 g / t sodium carbonate as a dispersant to the slurry after physical dispersion treatment, and continue stirring for 3 min to allow the mixed dispersant to be fully adsorbed on the mineral surface, thus completing the dispersion pretreatment.
[0027] (4) The slurry that has undergone dispersion pretreatment is transferred into the flotation machine, and 20 g / t of kerosene is added as a molybdenum collector; methyl isobutyl methanol is used as a frother, and the amount of frother is 10 g / t. After stirring for 3 min, flotation separation is carried out for 4 min to obtain molybdenum concentrate and tailings.
[0028] According to the test results, the copper grade in the molybdenum concentrate obtained in this embodiment is 0.48%, and the molybdenum grade is 48.56%, indicating that the molybdenum concentrate product is qualified.
[0029] Example 2
[0030] (1) Take molybdenum concentrate B from a certain mine. The molybdenum concentrate contains 48.96% molybdenum and 0.97% copper. The molybdenum concentrate does not meet the requirement of Cu≤0.5%. Calcium oxide is used to adjust the pH of the slurry to 12 and stir evenly.
[0031] (2) After stirring the slurry with the pH value adjusted, use an ultrasonic disperser to disperse it ultrasonically. The ultrasonic power is 300W-400W and the ultrasonic time is 20min. The slurry temperature is maintained at 25℃-30℃. Then transfer it to the flotation machine and set the flotation machine stirring speed to 15000r / min and the stirring time to 20min.
[0032] (3) Add a mixture of 1500 g / t sodium hexametaphosphate and 750 g / t sodium carbonate as a dispersant to the slurry after physical dispersion treatment, and continue stirring for 3 min to allow the mixed dispersant to be fully adsorbed on the mineral surface, thus completing the dispersion pretreatment.
[0033] (4) The slurry that has undergone dispersion pretreatment is transferred into the flotation machine, and kerosene 30g / t is added as a molybdenum collector; methyl isobutyl methanol is used as a frother, and the amount of frother is 20g / t. After stirring for 3min, flotation separation is carried out for 4min to obtain molybdenum concentrate and tailings.
[0034] According to the test results, the copper grade in the molybdenum concentrate obtained in this embodiment is 0.50%, and the molybdenum grade is 50.14%, indicating that the molybdenum concentrate product is qualified.
Claims
1. A dispersion pretreatment method for improving the effect of molybdenite and chalcopyrite floatation separation, characterized in that, The dispersion pretreatment method for improving the flotation separation effect of molybdenite and chalcopyrite comprises pretreatment, physical dispersion treatment, chemical dispersion treatment and flotation separation steps, and specifically comprises the following steps: A. Pretreatment: the mixed mineral of molybdenite and chalcopyrite is crushed, ground and screened to obtain mixed mineral particles a with a grinding fineness of more than 80% of-0.074 mm; B. Material dispersion treatment: 1) the mixed mineral particles a are prepared into a slurry with a concentration of 25-40%, the pH value is adjusted to 12, and the slurry b is obtained after uniform stirring; 2) the slurry b is dispersed by ultrasonic waves and mechanically stirred to obtain the slurry c; C. Chemical dispersion treatment: the dispersant is added to the slurry c for dispersion treatment to obtain the slurry d; the dispersant is composed of sodium hexametaphosphate and sodium carbonate; D. Flotation separation: the molybdenum collector and the foaming agent are added to the slurry d for flotation separation to obtain molybdenum concentrate and tailings.
2. The dispersion pretreatment method for improving the separation effect of molybdenite from chalcopyrite according to claim 1, characterized by, The power of the ultrasonic dispersion in B step 2) is 200-300 W, the ultrasonic time is 30-40 min, and the temperature of the slurry is maintained at 25-30℃.
3. The dispersion pretreatment method for improving the separation effect of molybdenite and chalcopyrite according to claim 1, characterized by, The stirring speed of the mechanical stirring in B step 2) is 1000-1500 r / min, and the stirring time is 20-30 min.
4. The dispersion pretreatment method for improving the separation effect of molybdenite from chalcopyrite according to claim 1, characterized by, The molybdenum collector in D step is emulsified kerosene.
5. The dispersion pretreatment method for improving the separation effect of molybdenite and chalcopyrite according to claim 5, characterized by, The kerosene emulsifier of the emulsified kerosene is sodium dodecyl benzene sulfonate, and the amount is 0.5-1% of the mass of kerosene.
6. The dispersion pretreatment method for improving the separation effect of molybdenite from chalcopyrite according to claim 1, characterized by, The foaming agent in D step is methyl isobutyl carbinol.