A flexible beneficiation process for hematite with fine selection capabilities
The hematite beneficiation process, which combines closed-circuit crushing and screening, wet grinding, and flexible magnetic separation, solves the problems of low flexibility and low resource utilization in traditional hematite beneficiation, and achieves efficient, low-consumption, diversified production and environmentally friendly treatment.
Patent Information
- Application Number
- CN202611086024.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-21
- Publication Date
- 2026-11-17
AI Technical Summary
Traditional hematite beneficiation processes suffer from several problems, including inflexibility in adjustment, inability to zone and schedule mixed slurry transportation, large fluctuations in feed concentration, low water resource recovery and utilization rate, high water consumption in production, severe equipment wear, limited product variety, and poor market adaptability.
A flexible separation method combining closed-circuit crushing and screening, wet closed-circuit grinding, weak magnetic separation and switchable strong magnetic separation is adopted. Combined with multi-stage thickening and dewatering and pump pool buffer, the slurry is transferred in zones and water resources are recycled. A switchable concentrate and tailings thickening system is set up to construct a flexible mineral processing technology.
It enables dynamic adjustment of the production process based on ore grade, reduces energy consumption during equipment idling, improves iron recovery rate, stabilizes sorting effect, reduces water consumption, adapts to diversified market demands, and reduces equipment wear and wastewater discharge.
Smart Images

Figure CN123102492A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of hematite processing and application technology, and in particular to a flexible beneficiation process for hematite with a fine selection function. Background Technology
[0002] Hematite is a typical weakly magnetic iron oxide mineral and one of the core raw materials for the domestic steel industry. Current hematite beneficiation processes generally employ a fixed, rigid integrated process of crushing, grinding, magnetic separation, and concentration / dewatering. In traditional processes, the strong magnetic separation section operates continuously throughout the entire process, unable to flexibly start and stop based on the real-time grade of the scavenging concentrate; the concentrate, middlings awaiting recycling, and tailings produced by magnetic separation share only one buffer tank, making it impossible to schedule the mixed transport of the slurry by zone; there is no concentration adjustment pretreatment process between the first and second stages of strong magnetic scavenging, resulting in large fluctuations in feed concentration; the concentrate concentration system has a single function, producing only a single iron concentrate product and unable to divert middlings as needed; simultaneously, the concentrate and tailings concentration and return water system is simple, resulting in low water resource recovery and high water consumption during production.
[0003] Traditional rigid mineral processing has many shortcomings: First, the beneficiation stage cannot be switched, resulting in idling and significant waste of water and electricity when the ore grade is high, and the lack of a grinding reflux and upgrading loop when the ore grade is low, leading to a significant reduction in iron recovery rate. Second, the absence of a zoned pump pool buffer structure results in mixed conveying of various slurries, making it easy for coarse impurities to enter the strong magnetic equipment, causing cylinder wear and disordered separation magnetic field. Third, the lack of a middlings thickening unit between the two scavenging stages leads to unstable feed concentration, poor capture efficiency of fine hematite in the second-stage scavenging stage, and the inability to reuse overflow water on-site. Fourth, crushing and grinding are only simple processes without closed-loop screening and grading to control the feed particle size, exacerbating grinding load and ore over-grinding. Fifth, the production mode is singular, with a single thickening system unable to switch between producing concentrate and middlings, resulting in poor market adaptability. Sixth, the lack of a cascade water return design leads to large amounts of mineral processing wastewater discharged and high environmental treatment costs. Therefore, this invention proposes a flexible hematite beneficiation process with beneficiation functions. Summary of the Invention
[0004] The technical problem to be solved by the present invention is to provide a flexible beneficiation process for hematite with a fine selection function, so as to solve the problems mentioned in the background art.
[0005] To solve the above-mentioned technical problems, one technical solution adopted by the present invention is to provide a flexible beneficiation process for hematite with a fine selection function, comprising the following steps:
[0006] S1. The hematite raw material is subjected to closed-circuit crushing and screening to obtain solid granular material that meets the particle size requirements for entering the mill.
[0007] S2. The crushed solid granular material is subjected to wet closed-circuit grinding and classification, and water is added for grinding to prepare a slurry material that meets the fineness requirements of beneficiation.
[0008] S3. A flexible separation method combining weak magnetic separation and switchable strong magnetic separation is used to separate slurry materials. The separation operation can be dynamically switched according to the material grade to obtain concentrate slurry and tailings slurry respectively.
[0009] S4. The concentrate slurry and tailings slurry are concentrated and dewatered in multiple stages in series to achieve solid product recovery and production water recycling, while also having the flexible production function of switching the output of intermediate minerals as needed.
[0010] The present invention is further configured such that: the closed-circuit crushing and screening process in step 1 is a single-stage closed-circuit crushing process, the specific steps of which are:
[0011] S1-1. The raw materials are first screened and classified by roller screen. Large pieces of material on the screen are collected and processed, while qualified material under the screen is sent to high-pressure roller mill for extrusion and crushing.
[0012] S1-2. The material crushed by the high-pressure roller mill is conveyed to the banana screen for further screening. The material on the banana screen is returned to the high-pressure roller mill for re-circulation and crushing via a belt conveyor. The material under the banana screen is a qualified particle size of -5mm, which is transferred to the grinding bin via a steep-angle belt conveyor to complete the standardized crushing and preparation of the material entering the mill.
[0013] Through the above technical solution, this process utilizes a roller screen, a high-pressure roller mill, and a banana screen to build a closed-loop extrusion crushing system. Large pieces of ore are pre-separated to avoid impact damage to the roller mill equipment. The crushed material is then screened and graded twice. Oversized coarse particles are automatically returned for recycling and crushing, and uniform -5mm particle size material is stably produced and fed into the grinding chamber. This unifies the feed particle size of the grinding mill, effectively reduces the grinding load on the ball mill, reduces the problem of over-grinding of ore, and provides stable particle size raw materials for downstream magnetic separation.
[0014] The present invention is further configured such that: the closed-circuit grinding and classification process in step 2 is a single-stage closed-circuit grinding process, specifically:
[0015] S2-1. Qualified particle size material in the grinding bin is fed into the ball mill for grinding. The ground material produced by the ball mill is transported to the hydrocyclone for particle size classification.
[0016] S2-2. The qualified fine-grained overflow material obtained from hydrocyclone classification is directly fed into the subsequent magnetic separation process, while the coarse-grained underflow material obtained from hydrocyclone classification is returned to the ball mill for further grinding, realizing a closed-loop cycle of grinding operation and stabilizing the particle size of the separation feed.
[0017] Through the above technical solution, the ball mill and hydrocyclone form a hydraulic closed-loop classification structure. The coarse slurry is continuously returned to the ball mill for secondary grinding, and only the fine particles that meet the particle size standard overflow into the magnetic separation section. This avoids the interference of coarse and fine slurry with the magnetic separation magnetic field, unifies the magnetic feed particle size range, stabilizes the strong and weak magnetic separation effect, and improves the overall hematite recovery efficiency.
[0018] The present invention is further configured such that: in the weak magnetic separation process described in step 3, the qualified slurry after grinding and classification is pretreated and separated, and high-grade strong magnetic iron minerals such as magnetite associated in the slurry are preferentially recovered to obtain qualified weak magnetic concentrate and be incorporated into the concentrate system;
[0019] The tailings generated by weak magnetic separation are screened by a drum screen to remove coarse impurities. The purified fine tailings are then fed into a subsequent switchable strong magnetic separation process.
[0020] Through the above technical solution, the weak magnetic separator prioritizes the separation of associated strong magnetic magnetite in the ore, gathers high-grade iron minerals in advance and integrates them into the concentrate system, reducing the processing load of the downstream strong magnetic equipment. The weak magnetic tailings are separated from the rock coarse impurities by the drum screen, preventing the wear and blockage of the strong magnetic equipment by coarse particles, realizing the step-by-step separation of strong magnetic minerals and weak magnetic hematite, and simplifying the separation pressure of the subsequent strong magnetic section.
[0021] The present invention is further configured such that: the switchable strong magnetic separator adopts a variable process flow of one coarse, two sweeps, and one fine separation, and is equipped with a dedicated pump tank to realize material transfer and buffering, the specific process being as follows:
[0022] The material after weak magnetic separation is first subjected to strong magnetic roughing. The roughing concentrate is sent to the concentrate pump pool for buffering and collection, and the roughing tailings enter a strong magnetic scavenging stage.
[0023] The first-stage high-intensity magnetic scavenging concentrate is fed into the concentrate pump pool, and the first-stage high-intensity magnetic scavenging tailings are fed into the second-stage high-intensity magnetic scavenging.
[0024] The concentrate from the second-stage strong magnetic scavenging is sent to the concentrate pump pool, and the tailings from the second-stage strong magnetic scavenging are sent to the tailings pump pool for buffering and collection.
[0025] When the grades of the first-stage and second-stage strong magnetic scavenging concentrates are lower than the preset standards, the two types of scavenging concentrates are combined and sent to the strong magnetic cleaning operation. The cleaned concentrate is fed into the concentrate pump pool, and the cleaned tailings are returned to the grinding tail pump pool and then returned to the grinding process for recycling.
[0026] Through the above technical solution, this process is equipped with three independent buffer devices: concentrate pump pool, tailings pump pool, and grinding tail pump pool, to realize the zoned and directional transfer of slurry. Under high-grade conditions, strong magnetic separation can be shut down to shorten the separation process and reduce the energy consumption of equipment idling. Under low-grade conditions, strong magnetic separation can be started to improve the quality. Unqualified tailings are returned to the grinding mill for re-grinding. The process can dynamically switch between long and short separation processes according to the grade of the concentrate, realizing flexible and adaptive production in mineral processing, taking into account both concentrate grade and metal recovery rate.
[0027] The present invention is further configured to: set up a middlings thickening process between the first-stage strong magnetic scavenging and the second-stage strong magnetic scavenging, and use an inclined plate thickener to perform solid-liquid thickening pretreatment on the tailings of the first-stage strong magnetic scavenging to achieve precise control of slurry concentration;
[0028] The inclined plate thickener concentrates and separates high-concentration slurry from low-concentration water. The high-concentration slurry is sent to a second-stage strong magnetic scavenging operation for further separation, while the separated low-concentration water is incorporated into the production circulating water system for reuse.
[0029] Through the above technical solution, the inclined plate thickener completes solid-liquid separation and concentration of the tailings from the first-stage strong magnetic scavenging, adjusts the low-concentration slurry to a concentration range suitable for strong magnetic separation, enhances the capture capacity of the second-stage strong magnetic scavenging for fine-grained hematite, and the clarified water separated by the thickener is directly recycled into the circulating water system on-site, reducing the amount of fresh water replenishment in the plant area and alleviating the processing pressure on the downstream tailings thickening equipment.
[0030] The present invention is further configured to employ a four-stage thickener series cascade thickening and water return process on the concentrate side, with the specific material flow direction as follows:
[0031] The concentrate produced by the magnetic separation operation is collected in the concentrate pump pool and then transported to the No. 1 concentrate concentration tank for staged concentration.
[0032] The overflow from concentration tank No. 1 flows into concentration tank No. 2, the overflow from concentration tank No. 2 flows into concentration tank No. 3, the overflow from concentration tank No. 3 flows into concentration tank No. 4, and the final overflow from concentration tank No. 4 is sent to the production turbid water tank for reuse as production circulating water.
[0033] The underflow from concentrate tanks No. 1, 2, and 3 is uniformly sent to the filter pump pool. After dewatering by the filter, the iron concentrate product is obtained. The overflow and filtrate generated by the filter are returned to concentrate tank No. 2 for recycling.
[0034] Through the above technical solution, the four-stage series concentrate concentrator achieves step-by-step solid-liquid separation. The overflow water from each stage is collected, recycled, and reused. The concentrated underflow is sent to the filtration equipment to produce iron concentrate. The filtrate generated by filtration is returned to the first-stage concentrate tank for secondary separation, thus constructing a closed-loop water circulation system on the concentrate side. The solid-liquid separation is sufficient, the water recovery and utilization rate is high, and there is no disorderly wastewater discharge.
[0035] The present invention is further configured such that: the No. 3 concentrate concentration tank also has the function of middlings concentration. Under the condition of middlings production, the underflow of the No. 3 concentrate concentration tank is diverted to the No. 6 filter press, and the middlings product is obtained by filter pressing. The filtrate produced by filter pressing flows into the No. 3 tailings concentration tank to participate in the tailings water circulation.
[0036] With the above technical solution, using the No. 3 concentrate concentrator as the material diversion node, the same concentrate concentrator system can switch between two production modes. During normal production, all the bottom flow is used to prepare high-grade iron concentrate. When the market needs low-grade raw materials, the bottom flow is diverted to produce middlings products. There is no need to add a complete set of concentration and filter press equipment, which reduces equipment investment and plant area, and realizes flexible product switching output.
[0037] The present invention is further configured to employ a three-stage thickener series thickening and water recovery process on the tailings side, with the specific material flow direction as follows:
[0038] The tailings produced by magnetic separation are collected in a tailings pump pool and then transported to tailings thickening tanks at various stages for progressive thickening.
[0039] The overflow from tailings thickener No. 1 flows into tailings thickener No. 2, the overflow from tailings thickener No. 2 flows into tailings thickener No. 3, and the final overflow from tailings thickener No. 3 is sent to the production turbid water tank for reuse as production circulating water.
[0040] The bottom flow from each tailings thickening tank is uniformly sent to the tailings filter press pool, where it is filtered by a filter press to obtain the finished tailings product. The filter filtrate is then returned to the No. 3 tailings thickening tank for closed-loop recycling.
[0041] Through the above technical solution, all tailings are collected and fed into a three-stage series thickening system, where solid tailings and clean water are separated in stages. Overflow clean water is recycled and reused, and the filtrate from the filter press is returned to the final thickening tank for secondary solid-liquid separation. The entire tailings treatment process achieves dry tailings stacking and zero discharge of production wastewater, significantly reducing the consumption of fresh water in mineral processing and meeting environmental protection control requirements.
[0042] The beneficial effects of this invention are as follows:
[0043] 1. The present invention proposes a flexible beneficiation process for hematite with a fine selection function. By setting up a switchable strong magnetic fine selection process, and with the addition of a concentrate pump pool, a tailings pump pool, and a grinding tail pump pool for zonal buffering of various slurries, the fine selection section can be dynamically started and stopped according to the grade of the scavenged concentrate. When the ore grade is high, the fine selection is turned off to shorten the separation process and reduce the water and electricity consumption caused by the equipment running idle. When the ore grade is low, the fine selection is turned on to improve the quality. Unqualified tailings are returned to the grinding mill for re-grinding. This solves the defects of traditional rigid processes that cannot adapt to fluctuations in ore grade, have high energy consumption, and unstable metal recovery rate.
[0044] 2. The flexible beneficiation process for hematite with a fine selection function proposed in this invention completes the middlings concentration pretreatment by adding an inclined plate thickener between the first-stage and second-stage strong magnetic scavenging. This can adjust the low-concentration scavenging tailings to the optimal separation concentration, improve the capture efficiency of fine-grained hematite in the second-stage scavenging, and the clarified water separated by the thickener is directly fed into the circulating water system for on-site reuse, reducing the supply of fresh water in the plant area and reducing the processing load of the downstream tailings concentration equipment.
[0045] 3. The flexible beneficiation process for hematite with a fine selection function proposed in this invention prioritizes the recovery of associated magnetite in the ore by setting up a weak magnetic separation pretreatment step at the front end, thus pre-aggregating high-grade iron minerals. The weak magnetic tailings are screened by a drum screen to remove coarse rock impurities before entering the strong magnetic section, avoiding wear and blockage of the strong magnetic equipment by large particles, and reducing the processing load of the entire strong magnetic unit.
[0046] 4. The flexible beneficiation process for hematite with a fine selection function proposed in this invention configures a four-stage series cascade thickening system on the concentrate side, with the No. 3 concentrate thickening tank as the diversion node. The same set of equipment can flexibly switch to produce two types of products: high-grade iron concentrate and low-grade middlings. No additional thickening and filter press units are required, which reduces equipment investment and site occupation and adapts to diversified market product demands. Attached Figure Description
[0047] Figure 1 This is a flowchart of a flexible beneficiation process for hematite with a fine selection function according to the present invention. Detailed Implementation
[0048] The preferred embodiments of the present invention will now be described in detail with reference to the accompanying drawings, so that the advantages and features of the present invention can be more easily understood by those skilled in the art, thereby providing a clearer and more explicit definition of the scope of protection of the present invention.
[0049] like Figure 1 As shown, a flexible beneficiation process for hematite with a finer selection function includes the following steps:
[0050] S1. The hematite raw material is subjected to closed-circuit crushing and screening to obtain solid granular material that meets the particle size requirements for entering the mill. The closed-circuit crushing and screening process is a single-stage closed-circuit crushing process, and the specific steps are as follows:
[0051] S1-1. The raw materials are first screened and classified by roller screen. Large pieces of material on the screen are collected and processed, while qualified material under the screen is sent to high-pressure roller mill for extrusion and crushing.
[0052] S1-2. The material crushed by the high-pressure roller mill is conveyed to the banana screen for further screening. The material on the banana screen is returned to the high-pressure roller mill for re-circulation and crushing via a belt conveyor. The material under the banana screen is a qualified particle size of -5mm, which is transferred to the grinding bin via a steep-angle belt conveyor to complete the standardized crushing and preparation of the material entering the mill. This process uses a roller screen, a high-pressure roller mill, and a banana screen to build a closed-loop extrusion crushing system to pre-separate large pieces of ore to avoid impact damage to the roller mill equipment. The crushed material is screened and graded twice. Oversized coarse particles are automatically returned for recirculation crushing, and a stable output of uniform -5mm particle size material is sent to the grinding bin to unify the grinding feed particle size, effectively reduce the grinding load of the ball mill, reduce the problem of over-grinding of ore, and provide stable particle size raw materials for downstream magnetic separation.
[0053] S2. The crushed solid particulate material is subjected to wet closed-circuit grinding and classification, and water is added for grinding to prepare a slurry material that meets the fineness requirements for beneficiation. The closed-circuit grinding and classification process is a single-stage closed-circuit grinding process, specifically as follows:
[0054] S2-1. Qualified particle size material in the grinding bin is fed into the ball mill for grinding. The ground material produced by the ball mill is transported to the hydrocyclone for particle size classification.
[0055] S2-2. The qualified fine-particle overflow material obtained from hydrocyclone classification is directly fed into the subsequent magnetic separation process, while the coarse-particle underflow material obtained from hydrocyclone classification is returned to the ball mill for further grinding, realizing a closed-loop cycle of grinding operation, stabilizing the particle size of the separation feed, and forming a hydraulic closed-loop classification structure with the ball mill and hydrocyclone. The coarse-particle slurry is continuously returned to the ball mill for secondary grinding, and only the fine-particle overflow that meets the particle size standard enters the magnetic separation section, avoiding interference of the magnetic separation magnetic field with the mixed coarse and fine slurry, unifying the magnetic separation feed particle size range, stabilizing the strong and weak magnetic separation effect, and improving the overall hematite recovery efficiency.
[0056] S3. A flexible separation method combining weak magnetic separation and switchable strong magnetic separation is used to separate slurry materials. The separation operation can be dynamically switched according to the material grade to obtain concentrate slurry and tailings slurry respectively.
[0057] The weak magnetic separation process pre-treats and separates the qualified slurry after grinding and classification, prioritizing the recovery of high-grade strongly magnetic iron minerals such as magnetite associated with the slurry, obtaining qualified weak magnetic concentrate and flowing into the concentrate system. The tailings generated by the weak magnetic separation are coarsely separated and impurities are removed by a drum screen. The purified fine tailings are sent to the subsequent switchable strong magnetic separation process. The weak magnetic separator prioritizes the separation of strongly magnetic magnetite associated with the ore, pre-aggregating high-grade iron minerals and flowing into the concentrate system, reducing the processing load of the downstream strong magnetic equipment. The weak magnetic tailings are separated from the rock coarse impurities by a drum screen to prevent coarse particles from wearing and clogging the strong magnetic equipment, realizing the step-by-step separation of strongly magnetic minerals and weakly magnetic hematite, simplifying the separation pressure of the subsequent strong magnetic section.
[0058] The switchable high-intensity magnetic separation adopts a variable process flow of one roughing, two scavenging, and one finishing stage, equipped with a dedicated pump pool for material transfer and buffering. The specific process is as follows: the material after weak magnetic separation undergoes high-intensity magnetic roughing; the roughing concentrate is sent to the concentrate pump pool for buffering and collection, while the roughing tailings enter the first stage of high-intensity magnetic scavenging; the first stage high-intensity magnetic scavenging concentrate is sent to the concentrate pump pool, and the first stage high-intensity magnetic scavenging tailings are sent to the second stage high-intensity magnetic scavenging; the second stage high-intensity magnetic scavenging concentrate is sent to the concentrate pump pool, and the second stage high-intensity magnetic scavenging tailings are sent to the tailings pump pool for buffering and collection; when the grades of the first stage and second stage high-intensity magnetic scavenging concentrates are lower than a preset standard, the two scavenging stages will be switched off. The concentrate is combined and sent to the high-intensity magnetic separation operation. The selected concentrate is fed into the concentrate pump pool, and the selected tailings are returned to the grinding tail pump pool. From there, they are returned to the grinding process for reprocessing. This process is equipped with three independent buffer devices: concentrate pump pool, tailings pump pool, and grinding tail pump pool, to achieve zonal and directional transfer of slurry. Under high-grade conditions, the high-intensity magnetic separation can be shut down to shorten the separation process and reduce the energy consumption of equipment idling. Under low-grade conditions, the high-intensity magnetic separation can be started to improve the quality. Unqualified tailings are returned to the grinding process for re-grinding. The process can dynamically switch between long and short separation processes according to the grade of the concentrate, achieving flexible and adaptive production in mineral processing, taking into account both concentrate grade and metal recovery rate.
[0059] A middlings thickening process is set up between the first-stage and second-stage high-intensity magnetic scavenging. An inclined plate thickener is used to perform solid-liquid thickening pretreatment on the tailings from the first-stage high-intensity magnetic scavenging to achieve precise control of the slurry concentration. The inclined plate thickener thickens and separates high-concentration slurry and low-concentration water. The high-concentration slurry is sent to the second-stage high-intensity magnetic scavenging operation for further separation, while the separated low-concentration water is incorporated into the production circulating water system for reuse. The inclined plate thickener completes solid-liquid separation and thickening of the tailings from the first-stage high-intensity magnetic scavenging, adjusting the low-concentration slurry to a concentration range suitable for high-intensity magnetic separation, thereby improving the second-stage high-intensity magnetic scavenging's ability to capture fine-grained hematite. The clarified water separated by the thickener is directly incorporated into the circulating water system for on-site reuse, reducing the amount of fresh water supplied to the plant and alleviating the processing pressure on the downstream tailings thickening equipment.
[0060] S4. Multi-stage series concentration and dewatering of concentrate slurry and tailings slurry are carried out to realize the recovery of solid finished products and the recycling of production water, while also having the flexible production function of switching the output of intermediate minerals as needed.
[0061] A four-stage thickener series cascade thickening and water return process is adopted on the concentrate side, with the specific material flow direction as follows:
[0062] The concentrate produced by magnetic separation is collected in the concentrate pump pool and then transported to the No. 1 concentrate concentrator for staged concentration. The overflow from the No. 1 concentrator flows into the No. 2 concentrator, the overflow from the No. 2 concentrator flows into the No. 3 concentrator, the overflow from the No. 3 concentrator flows into the No. 4 concentrator, and the final overflow from the No. 4 concentrator is sent to the production turbid water tank for reuse as production circulating water.
[0063] The underflow from concentrate concentrators No. 1, 2, and 3 is uniformly fed into the filter pump pool. After dewatering by the filter, the iron concentrate product is obtained. The overflow and filtrate generated by the filter are returned to concentrate concentrator No. 2 for recycling. The four-stage series concentrate concentrators achieve step-by-step solid-liquid separation. The overflow water from each stage is collected, recycled, and reused. The concentrated underflow is centrally fed into the filtration equipment to produce iron concentrate. The filtrate generated by filtration is returned to the first-stage concentrate tank for secondary separation, thus constructing a closed-loop water circulation system on the concentrate side. Solid-liquid separation is sufficient, the clean water recovery and utilization rate is high, and there is no disorderly wastewater discharge.
[0064] The No. 3 concentrate thickener also functions as a middlings concentrate thickener. During middlings production, the underflow from the No. 3 concentrate thickener is diverted to the No. 6 filter press. After filtration, the middlings product is obtained. The filtrate produced by filtration flows into the No. 3 tailings thickener to participate in the tailings water circulation. Using the No. 3 concentrate thickener as a material diversion node, the same concentrate thickening system can switch between two production modes. During normal production, all underflow is used to prepare high-grade iron concentrate. When the market needs low-grade raw materials, the underflow is diverted to produce middlings products. There is no need to add a complete set of thickening and filtration equipment, which reduces equipment investment and plant area, and realizes flexible product switching output.
[0065] A three-stage thickener series thickening and water recovery process is adopted on the tailings side, with the specific material flow direction as follows:
[0066] Tailings from magnetic separation are collected in a tailings pump pool and then transported to tailings thickeners at each stage for concentration. The overflow from tailings thickener No. 1 flows into tailings thickener No. 2, the overflow from tailings thickener No. 2 flows into tailings thickener No. 3, and the final overflow from tailings thickener No. 3 is sent to the production turbid water tank for reuse as production circulating water. The underflow from each tailings thickener is sent to a tailings filter press pump pool, where it is filtered to obtain the finished tailings. The filter filtrate is returned to tailings thickener No. 3 for closed-loop recycling. All tailings are collected and enter a three-stage series thickening system to separate solid tailings from clean water at each stage. The overflow clean water is recycled and reused, and the filter filtrate is returned to the final thickener for secondary solid-liquid separation. The entire tailings treatment process achieves dry tailings stacking and zero discharge of production wastewater, significantly reducing the consumption of fresh water in mineral processing and meeting environmental protection requirements.
[0067] The above description is merely an embodiment of the present invention and does not limit the patent scope of the present invention. Any equivalent structural or procedural transformations made based on the content of the present invention's specification and drawings, or direct or indirect applications in other related technical fields, are similarly included within the patent protection scope of the present invention.
Claims
1. A flexible beneficiation process for hematite with a fine-refining function, characterized in that: Includes the following steps: S1. The hematite raw material is subjected to closed-circuit crushing and screening to obtain solid granular material that meets the particle size requirements for entering the mill. S2. The crushed solid granular material is subjected to wet closed-circuit grinding and classification, and water is added for grinding to prepare slurry material that meets the fineness requirements of beneficiation. S3. A flexible separation method combining weak magnetic separation and switchable strong magnetic separation is used to separate slurry materials. The separation operation can be dynamically switched according to the material grade to obtain concentrate slurry and tailings slurry respectively. S4. The concentrate slurry and tailings slurry are concentrated and dewatered in multiple stages in series to achieve solid product recovery and production water recycling, while also having the flexible production function of switching the output of intermediate minerals as needed.
2. The flexible beneficiation process for hematite with a finer selection function according to claim 1, characterized in that: The closed-circuit crushing and screening process described in step 1 is a single-stage closed-circuit crushing process, and the specific steps are as follows: S1-1. The raw materials are first screened and classified by roller screen. Large pieces of material on the screen are collected and processed, while qualified material under the screen is sent to high-pressure roller mill for extrusion and crushing. S1-2. The material crushed by the high-pressure roller mill is conveyed to the banana screen for further screening. The material on the banana screen is returned to the high-pressure roller mill for re-circulation and crushing via a belt conveyor. The material under the banana screen is a qualified particle size of -5mm, which is transferred to the grinding bin via a steep-angle belt conveyor to complete the standardized crushing and preparation of the material entering the mill.
3. The flexible beneficiation process for hematite with a finer selection function according to claim 1, characterized in that: The closed-circuit grinding and classification process described in step 2 is a single-stage closed-circuit grinding process, specifically as follows: S2-1. Qualified particle size material in the grinding bin is fed into the ball mill for grinding. The ground material produced by the ball mill is transported to the hydrocyclone for particle size classification. S2-2. The qualified fine-grained overflow material obtained from hydrocyclone classification is directly fed into the subsequent magnetic separation process, while the coarse-grained underflow material obtained from hydrocyclone classification is returned to the ball mill for further grinding, realizing a closed-loop cycle of grinding operation and stabilizing the particle size of the separation feed.
4. The flexible beneficiation process for hematite with a finer selection function according to claim 1, characterized in that: The weak magnetic separation process described in step 3 pre-treats and separates the qualified slurry after grinding and classification, giving priority to the recovery of high-grade strong magnetic iron minerals such as magnetite associated in the slurry, and obtaining qualified weak magnetic concentrate which is then incorporated into the concentrate system. The tailings generated by weak magnetic separation are screened by a drum screen to remove coarse impurities. The purified fine tailings are then sent to the subsequent switchable strong magnetic separation process.
5. The flexible beneficiation process for hematite with a finer selection function according to claim 4, characterized in that: The switchable high-intensity magnetic separator adopts a variable process flow of one coarse, two sweeps, and one fine separation, and is equipped with a dedicated pump tank to realize material transfer and buffering. The specific process is as follows: The material after weak magnetic separation is first subjected to strong magnetic roughing. The roughing concentrate is sent to the concentrate pump pool for buffering and collection, and the roughing tailings enter a strong magnetic scavenging stage. The first-stage high-intensity magnetic scavenging concentrate is sent into the concentrate pump pool, and the first-stage high-intensity magnetic scavenging tailings are sent into the second-stage high-intensity magnetic scavenging. The concentrate from the second-stage strong magnetic scavenging is sent to the concentrate pump pool, and the tailings from the second-stage strong magnetic scavenging are sent to the tailings pump pool for buffering and collection. When the grades of the first-stage and second-stage strong magnetic scavenging concentrates are lower than the preset standards, the two types of scavenging concentrates are combined and sent to the strong magnetic beneficiation operation. The beneficiated concentrate is fed into the concentrate pump pool, and the beneficiated tailings are returned to the grinding tail pump pool and then returned to the grinding process for recycling.
6. The flexible beneficiation process for hematite with a finer selection function according to claim 5, characterized in that: A middlings thickening process is set up between the first-stage and second-stage strong magnetic scavenging. An inclined plate thickener is used to perform solid-liquid thickening pretreatment on the tailings of the first-stage strong magnetic scavenging to achieve precise control of slurry concentration. The inclined plate thickener concentrates and separates high-concentration slurry from low-concentration water. The high-concentration slurry is sent to a second-stage strong magnetic scavenging operation for further separation, while the separated low-concentration water is incorporated into the production circulating water system for reuse.
7. The flexible beneficiation process for hematite with a finer selection function according to claim 1, characterized in that: A four-stage thickener series cascade thickening and water return process is adopted on the concentrate side, with the specific material flow direction as follows: The concentrate produced by the magnetic separation operation is collected in the concentrate pump pool and then transported to the No. 1 concentrate concentration tank for staged concentration. The overflow from concentration tank No. 1 flows into concentration tank No. 2, the overflow from concentration tank No. 2 flows into concentration tank No. 3, the overflow from concentration tank No. 3 flows into concentration tank No. 4, and the final overflow from concentration tank No. 4 is sent to the production turbid water tank for reuse as production circulating water. The underflow from concentrate tanks No. 1, 2, and 3 is uniformly sent to the filter pump pool. After dewatering by the filter, the iron concentrate product is obtained. The overflow and filtrate generated by the filter are returned to concentrate tank No. 2 for recycling.
8. The flexible beneficiation process for hematite with a finer selection function according to claim 7, characterized in that: The No. 3 concentrate thickener also functions as a middlings thickener. Under middlings production conditions, the underflow from the No. 3 concentrate thickener is diverted to the No. 6 filter press. After filtration, the middlings product is obtained. The filtrate produced by filtration flows into the No. 3 tailings thickener to participate in the tailings water circulation.
9. The flexible beneficiation process for hematite with a finer selection function according to claim 1, characterized in that: A three-stage thickener series thickening and water recovery process is adopted on the tailings side, with the specific material flow direction as follows: The tailings produced by magnetic separation are collected in a tailings pump pool and then transported to tailings thickening tanks at various stages for progressive thickening. The overflow from tailings thickener No. 1 flows into tailings thickener No. 2, the overflow from tailings thickener No. 2 flows into tailings thickener No. 3, and the final overflow from tailings thickener No. 3 is sent to the production turbid water tank for reuse as production circulating water. The bottom flow from each tailings thickening tank is uniformly sent to the tailings filter press pool, where it is filtered by a filter press to obtain the finished tailings product. The filter filtrate is then returned to the No. 3 tailings thickening tank for closed-loop recycling.