A ceramic slurry spraying method

The ceramic slurry spraying method, which employs triple closed-loop control and independent double-sided drying, solves the problems of large size, high cost, and low utilization rate of existing equipment, achieving efficient and precise ceramic slurry coating and improving production efficiency and product quality.

CN123102553APending Publication Date: 2026-11-17GUANGDONG DONGBO AUTOMATION EQUIP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611599014.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-15
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing ceramic slurry spraying equipment is bulky, complex in structure, expensive, has low slurry utilization, and limited positioning accuracy, making it difficult to meet the needs of compact production lines and experimental equipment.

Method used

The system employs a triple closed-loop control system consisting of "encoder longitudinal length control + visual lateral correction + metering pump volumetric metering" to achieve precise and quantitative spraying of ceramic slurry. Combined with independent double-sided drying and online detection, it eliminates slurry splashing and scraper residue.

Benefits of technology

It increased slurry utilization by more than 40%, reduced equipment footprint and maintenance costs, improved coating accuracy and yield, and avoided metal shavings contamination.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123102553A_ABST
    Figure CN123102553A_ABST
Patent Text Reader

Abstract

This invention belongs to the field of battery equipment technology, specifically relating to a ceramic slurry spraying method, which includes at least the following steps: unwinding an electrode sheet with preset slots; visually positioning and precisely spraying ceramic slurry onto the slots on the A-side of the electrode sheet using an A-side coating mechanism; drying and shaping the ceramic slurry on the A-side; flipping the electrode sheet from A-side upward to B-side upward using a reversing guide mechanism; visually positioning and precisely spraying ceramic slurry onto the slots on the B-side of the electrode sheet using a B-side coating mechanism; drying and shaping the ceramic slurry on the B-side; online detection of the ceramic coatings on the A-side and B-side using a double-sided detection mechanism; and rewinding. The precisely sprayed coating process includes: obtaining the lateral offset of the slots using a CCD visual detection mechanism; obtaining the longitudinal belt length of the electrode sheet using a belt encoder; and controlling the nozzle to perform follow-up spraying and shut-off within the corresponding slot area using a motion controller based on the slot start and end pulses, with no spraying in areas without slots.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of battery equipment technology, and specifically relates to a method for spraying ceramic slurry. Background Technology

[0002] Lithium-ion batteries, as a type of rechargeable battery, primarily rely on the intercalation and deintercalation of lithium ions between the positive and negative electrodes to achieve charging and discharging. Due to their advantages such as high energy density, high average output voltage, low self-discharge rate, long cycle life, and the ability to charge and discharge at high rates, they have been widely used in consumer electronics, electric vehicles, and energy storage systems.

[0003] A typical lithium-ion battery cell structure includes a positive electrode, a negative electrode, a separator, and an electrolyte. The positive and negative electrode plates are respectively welded with positive and negative tabs to conduct current. During cell packaging and subsequent module assembly, the tabs need to pass through the packaging area of ​​the aluminum-plastic film (for pouch cells) or the top cover (for prismatic cells). To prevent short circuits between the tabs and the heat-sealing layer of the aluminum-plastic film, or between the tabs and the battery casing, specific areas on the tabs must be insulated.

[0004] The current industry practice is to create a slot (also called an "insulation clearance area" or "adhesive break area") on the tab, coat a portion of this slot with an insulating medium, and then weld the tab to the electrode. The insulating material used is often a ceramic slurry (mainly composed of inorganic ceramic particles such as alumina and magnesium oxide mixed with a binder). This utilizes the high temperature resistance, high insulation strength, and good chemical stability of ceramic materials to form a reliable insulating barrier between the tab and the encapsulation layer.

[0005] In existing electrode ceramic slurry coating processes, specialized spraying equipment is typically used to coat the electrode slots. This type of equipment generally includes a slurry supply system, atomizing nozzles, positioning fixtures, waste gas collection devices, and a drying station. The entire system is complex and occupies a large area. Furthermore, slurry atomization during spraying causes a certain amount of splashing waste, requiring supporting protective and recovery structures, further increasing the equipment's size and energy consumption.

[0006] As lithium battery production moves towards high-speed, compact production lines, and as new processes such as laboratory R&D, small-batch trial production, and stacking / intercalation of electrodes increasingly demand miniaturized and flexible equipment, existing spraying equipment has the following significant shortcomings: 1. The equipment is bulky and difficult to integrate into space-constrained compact production lines or experimental equipment; 2. The complex structure and high cost, with the overlapping of the atomization and recovery systems, result in high overall manufacturing and maintenance costs; 3. Low slurry utilization rate, atomized spraying results in splattering and overspraying, leading to significant waste of ceramic slurry; 4. Positioning accuracy is limited. The width of the electrode slot is usually narrow, and traditional nozzles have difficulty achieving neat edges and preventing overflow outside the slot, which affects the subsequent welding yield.

[0007] Therefore, the present invention aims to provide a ceramic slurry spraying method, which achieves slurry only in the tank and zero splashing in the non-tank area through a triple closed loop of "encoder longitudinal length setting + visual lateral correction + metering pump volume measurement". The slurry utilization rate is more than 40% higher than the traditional topcoat + scraper removal process, and completely eliminates the scraper residue cleaning process, thus eliminating the pollution of metal shavings brought in by the scraper. Summary of the Invention

[0008] The purpose of this invention is to address the shortcomings of existing technologies by providing a ceramic slurry spraying method. This method achieves slurry application only within the tank area and zero splashing in the non-tank area through a triple closed loop of "encoder longitudinal length setting + visual lateral correction + metering pump volumetric metering". The slurry utilization rate is more than 40% higher than the traditional topcoat + scraper removal process, and the scraper residue cleaning process is completely eliminated, thus preventing metal shavings contamination brought in by the scraper.

[0009] To achieve the above objectives, the present invention adopts the following technical solution: A method for spraying ceramic slurry includes at least the following steps: S1, unwinding an electrode sheet with a preset slot; S2, the A-side coating mechanism performs visual positioning and precise quantitative spraying of ceramic slurry onto the A-side groove of the electrode sheet; S3, the ceramic slurry on surface A is dried and shaped by the first drying mechanism; S4, the electrode is flipped from A-side up to B-side up by the reversing guide mechanism; S5, through the B-side coating mechanism, visually locates and precisely sprays ceramic slurry onto the B-side groove of the electrode; S6, the ceramic slurry on side B is dried and shaped by the second drying mechanism; S7, the position, thickness and appearance of the ceramic coating on the A and B sides are inspected online by a double-sided inspection mechanism, and then the coil is wound up; The fixed-point quantitative spray coating described in steps S2 and S5 includes: obtaining the lateral offset of the slot through a CCD vision inspection mechanism, obtaining the longitudinal belt length of the electrode through a belt encoder, and controlling the nozzle to perform follow-up spraying and shut-off in the corresponding slot interval according to the slot start pulse and end pulse by the motion controller, and not spraying in the slot area.

[0010] As an improvement to the ceramic slurry spraying method of the present invention, the follow-up quantitative coating specifically includes: The spraying interval along the length of the slot is divided into spray start time T1 and spray stop time T2. When the electrode tape reaches the CCD field of view and identifies the starting edge of the slot, the current encoder pulse value is recorded as the starting reference. Combined with the preset slot length and the current tape linear speed, the motion controller calculates the corresponding T1 and T2 for the slot. When T1 is reached, the metering pump and the nozzle solenoid valve are turned on to inject slurry. When T2 is reached, they are turned off. The un-slotted area between adjacent slots is closed and not sprayed throughout the entire process.

[0011] As an improvement to the ceramic slurry spraying method of the present invention, the quantitative control adopts a closed-loop adjustment of "flow rate-speed-thickness": the theoretical wet thickness H = Q / (V(T2-T1)×W) is calculated based on the volumetric flow rate Q of the metering conveyor, the speed V of the main drive belt, and the known groove width W; at the same time, a wet glue detection component is set downstream of the nozzle to measure the actual wet thickness online, and the speed of the metering pump is corrected by feedback, so that the single-point wet thickness deviation is controlled within the set range.

[0012] As an improvement to the ceramic slurry spraying method of the present invention, in the fixed-point quantitative follow-up spraying coating, the coating station is equipped with four nozzles corresponding to four slots arranged along the conveyor belt direction; during the unidirectional conveyor belt movement of the electrode sheet, the nozzles perform spraying on the corresponding slots until the target total thickness is reached.

[0013] As an improvement to the ceramic slurry spraying method of the present invention, a wet adhesive detection step for surface A is set between step S2 and step S3 to determine in real time whether there is any interruption in adhesive or missed spraying; a wet adhesive detection step for surface B is set between step S5 and step S6.

[0014] As an improvement to the ceramic slurry spraying method of the present invention, between steps S1 and S2, the following are performed in sequence: unwinding tension adjustment, A-side brush dust removal, process correction, and A-side groove guidance and positioning; between steps S3 and S4, the following are performed in sequence: second process correction, first tension control, B-side brush dust removal, and B-side groove guidance and positioning after flipping, to ensure the alignment accuracy between the B-side groove and the nozzle after flipping.

[0015] As an improvement to the ceramic slurry spraying method of the present invention, the following steps are performed sequentially between steps S6 and S7: third process correction, second tension control, A-side dry adhesive detection, B-side dry adhesive detection, laser marking and coding, A / B-side brush dust removal, A / B-side iron removal, marking re-inspection, and winding correction; wherein the A-side dry adhesive detection and B-side dry adhesive detection are arranged obliquely, and laser thickness sensors and / or CCD line scanning optical components are used to synchronously collect double-sided coating data.

[0016] As an improvement to the ceramic slurry spraying method of the present invention, in step S2 and / or step S5, a low-pressure narrow-slit air knife is set at an acute angle of 15° to 30° downstream of the nozzle along the conveyor belt direction. During the spraying process, the air knife delivers air synchronously to blow away the floating material on the electrode surface. The air knife pressure is controlled at 0.02 MPa to 0.08 MPa, and the airflow sweeps across the electrode surface without perpendicularly impacting the inside of the slot, thus preventing the slurry in the slot from being blown away.

[0017] As an improvement to the ceramic slurry spraying method of the present invention, the first drying mechanism and the second drying mechanism are independent drying sections, each with an independent temperature-controlled air supply channel, which supplies air only to the corresponding coating surface and does not cross-contaminate the air; the coating is cooled and shaped rapidly by a cooling roller or air-cooling section at the drying outlet before entering the next process.

[0018] Compared with the prior art, the present invention has at least the following advantages: First, it boasts superior spraying accuracy and material utilization: Through a triple closed loop of "encoder longitudinal length setting + visual lateral correction + metering pump volumetric metering", it achieves zero splashing in the tank area and only the tank area has slurry. The slurry utilization rate is more than 40% higher than the traditional topcoat + scraper removal process, and it completely eliminates the scraper residue cleaning process, thus preventing metal shavings pollution brought in by the scraper.

[0019] Second, closed-loop detection in both wet and dry states: detection is initiated during the wet adhesive stage (wet adhesive detection components determine presence or absence and cut-off of adhesive), and laser / CCD re-inspection is performed during the dry adhesive stage (position + thickness + appearance). Defects are identified within the "reworkable window" rather than being discovered and scrapped after rewinding, resulting in a significant improvement in overall yield.

[0020] Third, the method and equipment layout are perfectly aligned: the tension control, correction, dust removal, and iron removal nodes between each step correspond one-to-one with the various mechanisms of the equipment, so that the method can be implemented as specific hardware actions, rather than an abstract process; in particular, the link of drying A side → flipping → dust removal of B side ensures that the dried coating on A side is not damaged during the flipping process, and that there is no powder falling from A side before B side enters the coating process, so that the two coatings do not interfere with each other. Attached Figure Description

[0021] Figure 1 This is a three-dimensional structural diagram of the present invention.

[0022] Figure 2 This is a front view structural diagram of the present invention.

[0023] Figure 3 This is a top view of the structure of the present invention.

[0024] Figure 4 This is a side view of the structure of the present invention.

[0025] Figure 5This is a process flow diagram of the present invention. Detailed Implementation

[0026] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only a part of the embodiments of the present invention, and not all of them. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.

[0027] It should be noted that all directional indications (such as up, down, left, right, front, back, etc.) in the embodiments of the present invention are only used to explain the relative positional relationship and movement of the components in a specific posture (as shown in the figure). If the specific posture changes, the directional indication will also change accordingly.

[0028] Furthermore, the use of terms such as "first" and "second" in this invention is for descriptive purposes only and should not be construed as indicating or implying their relative importance or implicitly specifying the number of technical features indicated. Therefore, a feature defined as "first" or "second" may explicitly or implicitly include at least one of that feature. Additionally, the technical solutions of the various embodiments can be combined with each other, but only on the basis of being achievable by those skilled in the art. If the combination of technical solutions is contradictory or impossible to implement, such a combination of technical solutions should be considered non-existent and not within the scope of protection claimed by this invention.

[0029] like Figures 1 to 4 As shown, the present invention provides a ceramic slurry spraying device, comprising: The unwinding mechanism 10 is used to unwind the electrode sheet with a preset slot. A-side coating mechanism 20 is used to quantitatively coat ceramic slurry onto the grooves on the A-side of the electrode sheet; The first drying unit 30 is used to dry and shape the ceramic slurry coated on surface A. The reversing guide mechanism 40 is used to guide the electrode sheet that has been dried by the first drying mechanism and has A side facing up to B side facing up. B-side coating mechanism 50 is used to quantitatively coat ceramic slurry onto the grooves on the B-side of the electrode. The second drying unit 60 is used to dry the ceramic slurry coated on side B. The double-sided inspection mechanism 70 is used to inspect the position, thickness, and appearance of the ceramic coating on side A and side B. The winding mechanism 80 is used to wind up the electrode sheets that have been coated and dried on both sides. The second drying mechanism 60 is located above the first drying mechanism 30, and the winding mechanism 80 and the unwinding mechanism 10 are both on the same side of the first drying mechanism 30. This invention features a compact layout and saves space. By placing the second drying mechanism 60 above the first drying mechanism 30, and arranging the winding mechanism 80 and the unwinding mechanism 10 on the same side of the first drying mechanism 30, the entire machine adopts a compact conveyor belt layout of "U-shape + stacked layers." While maintaining the independent drying lengths of surfaces A and B, the overall length of the equipment is significantly shortened, reducing the area occupied by the cleanroom and lowering the infrastructure costs of the production line. Both the unwinding mechanism 10 and the winding mechanism 80 include a winding roller and a drive mechanism.

[0030] Both the A-side coating mechanism 20 and the B-side coating mechanism 50 include: The slot visual inspection component 21 (51) is used to identify the lateral position of the electrode slot; The first main drive roller 22 (52) is used to clamp the electrode sheet and move it forward. A belt encoder is mounted on the first main drive roller 22 (52) to provide feedback on the belt length of the electrode sheet; The servo spraying component 24 (54) performs follow-up quantitative coating on the slot based on the signals from the slot visual inspection component 21 (51) and the belt encoder. The feeding assembly 25 includes a ceramic slurry storage tank 251, a metering conveyor 252 and a coating nozzle 253 (553), the coating nozzle 253 being connected to the ceramic slurry storage tank 251 (551) via the metering conveyor 252; Wet adhesive detection component 26 (56) is used to detect the state of wet adhesive after coating.

[0031] The first drying mechanism 30 and the second drying mechanism 60 are independent drying sections, each with its own temperature-controlled air supply channel, and each supplies air only to the corresponding coated surface. This avoids the problem of secondary softening, displacement, or adhesion of the single-sided dried coating caused by hot air crosstalk in traditional through-type ovens. Cooling rollers or air-cooling sections are provided on the outlet side of the first drying mechanism 30 and the outlet side of the second drying mechanism 60, so that the coating can be quickly set before entering the next process, ensuring the shape and position accuracy of double-sided coating.

[0032] The unwinding mechanism 10 includes, in sequence along the belt travel direction: unwinding roller assembly 11, tension adjustment assembly 12, A / B surface dust removal assembly 13, and first process correction assembly 14.

[0033] The reversing guide mechanism 40 includes, in sequence along the conveyor belt direction: a second process correction component 41, a first tension control component 42, a B-side dust removal component 43, and a flipping component 44. The slot visual detection component of the B-side coating mechanism is obliquely positioned and located on one side of the flipping component 44. The reversing guide mechanism 40 is configured with the flipping component 44, the obliquely positioned B-side slot visual detection component, and the second process correction component 41. During the process of switching from A-side up to B-side up, correction and dust removal are completed simultaneously, ensuring accurate alignment between the B-side slot and the nozzle when entering the coating station. This prevents coating misalignment caused by accumulated tension fluctuations after flipping, ensuring stable reversal and preventing deviation during forward and reverse flipping. In this invention, conventional correction and tension control components are sufficient. The B-side dust removal component 43 uses a brush dust removal mechanism, and the flipping component 44 is implemented using a flipping roller structure.

[0034] The double-sided inspection mechanism 70 includes, in sequence along the belt conveyor direction: a second tension control component 72, a third process correction component 71, a second main drive roller 73, an A-side dry adhesive inspection component 74, a B-side dry adhesive inspection component 75, an NG laser marking component 76 (marking on the NG slot for identification), an A / B side dust and iron removal component 77 (brush and magnet assembly), and a marking re-inspection component 78. Both the A-side dry adhesive inspection component 74 and the B-side dry adhesive inspection component 75 are arranged obliquely.

[0035] The A-side dry adhesive detection component 74 and the B-side dry adhesive detection component 75 are any one or a combination of laser thickness sensors, CCD area array detection cameras, or line scan optical detection components.

[0036] The winding mechanism 80 includes a third tension control component 81, a winding correction component 82, and a winding roller component 83.

[0037] The A-side coating mechanism 20 and / or the B-side coating mechanism 50 are equipped with a low-pressure narrow-slit air knife. The low-pressure narrow-slit air knife is located downstream of the coating nozzle and is set at an acute angle to the conveyor belt direction. It is used to blow away the floating material on the surface rather than to blow away the slurry in the tank. This effectively solves the problem of slurry loss and jagged edges caused by traditional brushes or high-pressure air blowing. After the adhesive dries, the coating edge is neat and the thickness is uniform.

[0038] The slot visual inspection component 21 includes a CCD camera, a stroboscopic light source, and an image processing module. Combined with an encoder to drive the servo-guided spraying component, it achieves a lateral coating width control accuracy of ≤±0.3 mm. Through the slot visual inspection component 21 (CCD + stroboscopic light source + image processing) and the real-time position feedback from the conveyor encoder, the servo-guided spraying component is driven to perform follow-up quantitative spraying. The lateral coating width control accuracy can reach ≤±0.3 mm, precisely injecting the ceramic slurry into the preset slot of the electrode sheet, avoiding slurry overflow that could cause edge thickening, foil contamination, and material waste.

[0039] Closed-loop control of coating quality: After coating on A and B sides, wet adhesive detection components are set up respectively. The double-sided detection mechanism is equipped with independent dry adhesive detection components (laser thickness measurement / CCD line scanning) on ​​A and B sides to perform double-sided synchronous online detection of coating position, thickness and appearance. With the help of laser marking and re-inspection, the coating data of each section of electrode can be traced, and defects such as missed coating, adhesive breakage and thickness deviation can be detected in time, which significantly improves the yield rate.

[0040] Multi-stage dust removal, iron removal, tension adjustment, and web guiding components (A / B surface dust removal, process web guiding, and multi-stage tension control) are configured along the unwinding to rewinding route to ensure that the thin electrode sheet does not wrinkle, stretch, or scratch under high-speed belt movement. The ceramic slurry is a brittle inorganic coating, and tension fluctuations can easily lead to cracking. This solution significantly reduces the risk of belt breakage and coating cracking by segmented independent tension control. The entire process of this invention is clean and the tension is controllable.

[0041] The A-side / B-side coating mechanism is symmetrical and can be started and stopped independently. It supports both full-sided coating and single-sided coating (with the other side's mechanism bypassing), adapting to the process switching needs of different battery systems (such as separator ceramic coating, electrode edge insulation coating, etc.). The feeding assembly adopts metering conveying + closed-loop feeding of storage tanks, with wide adaptability to slurry viscosity and convenient changeover and cleaning. This invention has excellent compatibility and scalability.

[0042] In summary, the ceramic slurry spraying equipment provided by this invention solves the technical problems of poor coating accuracy, crosstalk between the two sides, large footprint, and low yield of existing equipment through the coordinated operation of intensive spatial layout, independent double-sided drying, vision servo spraying, online double-sided detection, and full-process clean tension control. It achieves high-precision, high-efficiency, and low-loss continuous production of double-sided ceramic slurry for electrodes.

[0043] In this invention, the main drive roller includes a drive steel roller and a rubber-coated pressure roller. The motor drives the steel roller to rotate, and the rubber-coated pressure roller presses the electrode sheet onto it. The electrode sheet is clamped and moves along, serving as the reference source for the overall conveyor belt speed.

[0044] like Figure 5 As shown, coating using the apparatus of the present invention includes the following steps: S1, unwinding an electrode sheet with a preset slot; S2, the A-side coating mechanism performs visual positioning and precise quantitative spraying of ceramic slurry onto the A-side groove of the electrode sheet; S3, the ceramic slurry on surface A is dried and shaped by the first drying mechanism; S4, the electrode is flipped from A-side up to B-side up by the reversing guide mechanism; S5, through the B-side coating mechanism, visually locates and precisely sprays ceramic slurry onto the B-side groove of the electrode; S6, the ceramic slurry on side B is dried and shaped by the second drying mechanism; S7, the position, thickness and appearance of the ceramic coating on the A and B sides are inspected online by a double-sided inspection mechanism, and then the coil is wound up; The fixed-point quantitative spray coating described in steps S2 and S5 includes: obtaining the lateral offset of the slot through a CCD vision inspection mechanism, obtaining the longitudinal belt length of the electrode through a belt encoder, and controlling the nozzle to perform follow-up spraying and shut-off in the corresponding slot interval according to the slot start pulse and end pulse by the motion controller, and not spraying in the slot area.

[0045] Specifically, follow-up quantitative coating includes: The spraying interval along the length of the slot is divided into spray start time T1 and spray stop time T2. When the electrode tape reaches the CCD field of view and identifies the starting edge of the slot, the current encoder pulse value is recorded as the starting reference. Combined with the preset slot length and the current tape linear speed, the motion controller calculates the corresponding T1 and T2 for the slot. When T1 is reached, the metering pump and the nozzle solenoid valve are turned on to inject slurry. When T2 is reached, they are turned off. The un-slotted area between adjacent slots is closed and not sprayed throughout the entire process.

[0046] More specifically, follow-up quantitative coating includes: (1) Lateral positioning (width direction): The CCD camera captures images of the electrode surface on the conveyor belt at a fixed frame rate. The stroboscopic light source is synchronized with the camera exposure to eliminate motion blur. The image processing module extracts the edge contour of the electrode slot, calculates the lateral offset ΔX of the slot relative to the mechanical zero position of the equipment, and sends this offset to the servo-guided spraying component in real time. This ensures that the nozzle spray centerline is aligned with the slot centerline in the width direction, compensating for the serpentine deviation of the incoming electrode material. The lateral coating width control accuracy is ≤ ±0.3 mm.

[0047] (2) Longitudinal positioning (length direction): The belt encoder is installed at the end of the main drive roller shaft to provide real-time feedback of the belt length pulse of the electrode sheet. When the image processing module identifies the starting edge of a slot entering the CCD field of view, it records the current encoder count value as the "slot start reference pulse". Combined with the slot length (known process parameters) and the current belt speed, the motion controller calculates the spray start time T1 and spray stop time T2 of the slot in the longitudinal direction.

[0048] The quantitative control adopts a closed-loop adjustment of "flow rate-speed-thickness": the theoretical wet thickness H = Q / (V(T2-T1)×W) is calculated based on the volumetric flow rate Q of the metering conveyor, the speed V of the main drive belt, and the known groove width W; at the same time, a wet glue detection component is set downstream of the nozzle to measure the actual wet thickness online, and the speed of the metering pump is corrected by feedback, so that the single-point wet thickness deviation is controlled within the set range.

[0049] In the fixed-point quantitative spray coating, the coating station is equipped with four nozzles corresponding to four slots arranged along the conveyor belt direction; during the unidirectional conveyor belt movement of the electrode sheet, the nozzles perform spraying on the corresponding slots until the target total thickness is achieved.

[0050] In practice, the wet thickness is measured online using a wet adhesive detection component (laser triangulation or line scan optics), and the pump speed is corrected based on the feedback, forming a closed-loop regulation of "flow rate-speed-thickness", with the thickness deviation at a single point controlled within ±2 μm.

[0051] Between steps S2 and S3, there is an A-side wet adhesive detection step to determine in real time whether there is any glue breakage or missed spraying; between steps S5 and S6, there is a B-side wet adhesive detection step.

[0052] Between steps S1 and S2, the following are performed sequentially: unwinding tension adjustment, A-side brush dust removal, process correction, and A-side slot guidance and positioning; between steps S3 and S4, the following are performed sequentially: second process correction, first tension control, B-side brush dust removal, and B-side slot guidance and positioning after flipping, to ensure the alignment accuracy of the B-side slot and the nozzle after flipping.

[0053] Between steps S6 and S7, the following processes are executed sequentially: third process correction, second tension control, A-side dry adhesive detection, B-side dry adhesive detection, laser marking and coding, A / B-side brush dust removal, A / B-side iron removal, marking re-inspection, and winding correction; wherein the A-side dry adhesive detection and B-side dry adhesive detection are arranged obliquely, and laser thickness sensors and / or CCD line scanning optical components are used to synchronously collect double-sided coating data.

[0054] In step S2 and / or step S5, a low-pressure narrow-slit air knife is set at an acute angle of 15° to 30° downstream of the nozzle along the conveyor belt direction. During the spraying process when the nozzle is turned on, the air knife delivers air synchronously to blow away the floating material on the electrode surface. The air knife pressure is controlled at 0.02 MPa to 0.08 MPa, and the airflow sweeps across the electrode surface without perpendicularly impacting the inside of the slot, so as to avoid the slurry in the slot being blown away.

[0055] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and structure of the invention, the scope of which is defined by the appended claims and their equivalents.

Claims

1. A method for spraying ceramic slurry, characterized in that, At least the following steps are included: S1, unwinding an electrode sheet with a preset slot; S2, the A-side coating mechanism performs visual positioning and precise quantitative spraying of ceramic slurry onto the A-side groove of the electrode sheet; S3, the ceramic slurry on surface A is dried and shaped by the first drying mechanism; S4, the electrode is flipped from A-side up to B-side up by the reversing guide mechanism; S5, through the B-side coating mechanism, visually locates and precisely sprays ceramic slurry onto the B-side groove of the electrode; S6, the ceramic slurry on side B is dried and shaped by the second drying mechanism; S7, the position, thickness and appearance of the ceramic coating on the A and B sides are inspected online by a double-sided inspection mechanism, and then the coil is wound up; The fixed-point quantitative spray coating described in steps S2 and S5 includes: obtaining the lateral offset of the slot through a CCD vision inspection mechanism, obtaining the longitudinal belt length of the electrode through a belt encoder, and controlling the nozzle to perform follow-up spraying and shut-off in the corresponding slot interval according to the slot start pulse and end pulse by the motion controller, and not spraying in the slot area.

2. The ceramic slurry spraying method according to claim 1, characterized in that: The follow-up quantitative coating specifically includes: The spraying interval along the length of the slot is divided into spray start time T1 and spray stop time T2. When the electrode tape reaches the CCD field of view and identifies the starting edge of the slot, the current encoder pulse value is recorded as the starting reference. Combined with the preset slot length and the current tape linear speed, the motion controller calculates the corresponding T1 and T2 for the slot. When T1 is reached, the metering pump and the nozzle solenoid valve are turned on to inject slurry. When T2 is reached, they are turned off. The un-slotted area between adjacent slots is closed and not sprayed throughout the entire process.

3. The ceramic slurry spraying method according to claim 2, characterized in that: The quantitative control adopts a closed-loop adjustment of "flow rate-speed-thickness": the theoretical wet thickness H = Q / (V(T2-T1)×W) is calculated based on the volumetric flow rate Q of the metering conveyor, the speed V of the main drive belt, and the known groove width W; at the same time, a wet glue detection component is set downstream of the nozzle to measure the actual wet thickness online, and the speed of the metering pump is corrected by feedback, so that the single-point wet thickness deviation is controlled within the set range.

4. The ceramic slurry spraying method according to claim 1, characterized in that: In the fixed-point quantitative spray coating, the coating station is equipped with four nozzles corresponding to four slots arranged along the conveyor belt direction; during the unidirectional conveyor belt movement of the electrode sheet, the nozzles perform spraying on the corresponding slots until the target total thickness is achieved.

5. The ceramic slurry spraying method according to claim 1, characterized in that: Between steps S2 and S3, there is an A-side wet adhesive detection step to determine in real time whether there is any glue breakage or missed spraying; between steps S5 and S6, there is a B-side wet adhesive detection step.

6. The ceramic slurry spraying method according to claim 1, characterized in that: Between steps S1 and S2, the following are performed sequentially: unwinding tension adjustment, A-side brush dust removal, process correction, and A-side slot guidance and positioning; between steps S3 and S4, the following are performed sequentially: second process correction, first tension control, B-side brush dust removal, and B-side slot guidance and positioning after flipping, to ensure the alignment accuracy of the B-side slot and the nozzle after flipping.

7. The ceramic slurry spraying method according to claim 1, characterized in that: Between steps S6 and S7, the following processes are executed sequentially: third process correction, second tension control, A-side dry adhesive detection, B-side dry adhesive detection, laser marking and coding, A / B-side brush dust removal, A / B-side iron removal, marking re-inspection, and winding correction; wherein the A-side dry adhesive detection and B-side dry adhesive detection are arranged obliquely, and laser thickness sensors and / or CCD line scanning optical components are used to synchronously collect double-sided coating data.

8. The ceramic slurry spraying method according to claim 1, characterized in that: In step S2 and / or step S5, a low-pressure narrow-slit air knife is set at an acute angle of 15° to 30° downstream of the nozzle along the conveyor belt direction. During the spraying process when the nozzle is turned on, the air knife delivers air synchronously to blow away the floating material on the electrode surface. The air knife pressure is controlled at 0.02 MPa to 0.08 MPa, and the airflow sweeps across the electrode surface without perpendicularly impacting the inside of the slot, so as to avoid the slurry in the slot being blown away.

9. The ceramic slurry spraying method according to claim 1, characterized in that: The first drying mechanism and the second drying mechanism are independent drying sections, each with its own temperature-controlled air supply channel, which supplies air only to the corresponding coated surface and does not cross-contaminate the air; the coating is cooled and shaped quickly by a cooling roller or air-cooling section at the drying outlet before entering the next process.