A method for preparing corrosion-resistant wide aluminum alloy sheets based on synergistic control of hot and cold rolling

By using a hot-cold continuous rolling synergistic control method, the problems of poor process connection and insufficient microstructure uniformity in the production of wide aluminum alloy plates have been solved, thereby improving corrosion resistance and optimizing the production process. This method is applicable to fields such as shipbuilding and chemical containers.

CN123102736APending Publication Date: 2026-11-17SANHE WEISHIDA BUILDING MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611275527.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-21
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing production processes for wide-width aluminum alloy sheets suffer from poor process connections, insufficient microstructure uniformity, and corrosion resistance that is difficult to match the requirements of wide-width production. Furthermore, the step-by-step rolling process leads to uneven grain size and significant differences in the distribution of the second phase, affecting the overall corrosion resistance life and shape control of the sheet.

Method used

By adopting a hot-cold continuous rolling coordinated control method, the deformation temperature is precisely controlled by matching the rolling speed, reduction rate and inter-stand tension, combined with the inter-pass cooling system. A warm rolling transition section is added and coordinated with zoned precise temperature control. Sc, Zr and grain refiner are used to form a dispersed precipitate phase, which is then subjected to online pre-aging treatment to form fine and uniform solute atom clusters and passivation film.

Benefits of technology

It achieves a multi-dimensional performance balance of the sheet material, improves corrosion resistance and formability, shortens the production process, reduces energy consumption, and ensures the uniformity of the sheet material's structure and surface quality, making it suitable for large-scale industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123102736A_ABST
    Figure CN123102736A_ABST
Patent Text Reader

Abstract

This invention relates to the field of aluminum alloy sheet rolling technology, specifically to a method for preparing corrosion-resistant wide aluminum alloy sheets based on the coordinated control of hot and cold rolling. This method solves the problems of poor process connection, insufficient microstructure uniformity, and difficulty in matching corrosion resistance to the requirements of wide-width production in existing wide aluminum alloy sheet preparation processes. The composition of the aluminum alloy sheet, by weight percentage, is: Mg 3.5–5.2%, Mn 0.2–0.8%, Sc 0.08–0.20%, Zr 0.05–0.15%, Cr 0.15–0.35%, Ti 0.05–0.15%, Si 0.1–0.25%, Fe 0.08–0.30%, Cu 0.01–0.10%, with the balance being Al and unavoidable impurities. This invention replaces the intermittent process of hot rolling, cooling, and then re-uncoiling and cold rolling in the traditional process by adding a warm rolling transition section between hot rolling and cold rolling and coordinating precise temperature control in zones. It utilizes the residual heat of hot rolling to achieve warm deformation, promotes the dynamic recovery of dislocations and the formation of subgrain structures, and can effectively control the degree of work hardening without the need for additional intermediate annealing processes, thereby significantly shortening the production process and reducing production energy consumption.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of aluminum alloy sheet rolling technology, specifically to a method for preparing corrosion-resistant wide aluminum alloy sheets based on the coordinated control of hot and cold continuous rolling. Background Technology

[0002] Wide-width aluminum alloy sheets are widely used in shipbuilding, chemical containers, and building curtain walls due to their lightweight and high specific strength. These applications place high demands on the corrosion resistance and dimensional accuracy of the sheets. Current production methods for wide-width aluminum alloy sheets often employ a step-by-step hot-rolling and cold-rolling process, with the two processes intermittently arranged. The sheet and strip need to be cooled, re-rolled, and then transferred to the cold-rolling process. This not only results in a long production process and high energy consumption but also makes the sheet prone to uneven microstructure and surface oxidation caused by the intermediate cooling process, affecting the final corrosion resistance and surface quality.

[0003] Meanwhile, the lack of coordination between conventional aluminum alloy composition design and rolling process makes it easy for wide plates to have problems such as uneven grain size and large differences in second phase distribution in the thickness and width directions, which in turn leads to inconsistent local corrosion rates and reduces the overall corrosion resistance life of the plate. In addition, the deformation parameters of hot rolling and cold rolling in the step-by-step rolling process are set independently, and it is impossible to use the residual heat of hot rolling and deformation structure for continuous control. The shape control of wide plates is difficult and the performance stability is hard to guarantee.

[0004] Therefore, it does not meet the existing requirements. In response, we propose a method for preparing corrosion-resistant wide aluminum alloy sheets based on the coordinated control of hot and cold rolling. Summary of the Invention

[0005] The purpose of this invention is to provide a method for preparing corrosion-resistant wide aluminum alloy sheets based on the coordinated control of hot and cold rolling, so as to solve the problems of poor process connection, insufficient microstructure uniformity, and difficulty in matching corrosion resistance to the needs of wide production in the existing wide aluminum alloy sheet preparation process mentioned in the background art.

[0006] To achieve the above objectives, the present invention provides the following technical solution: a method for preparing corrosion-resistant wide-width aluminum alloy sheets based on the synergistic control of hot and cold continuous rolling, wherein the composition of the aluminum alloy sheet by weight percentage is: Mg 3.5-5.2%, Mn 0.2-0.8%, Sc 0.08-0.20%, Zr 0.05-0.15%, Cr 0.15-0.35%, Ti 0.05-0.15%, Si 0.1-0.25%, Fe 0.08-0.30%, Cu 0.01-0.10%, with the balance being Al and unavoidable impurities; The preparation method includes the following steps: According to the above composition ratio, weigh each raw material and put it into the melting furnace to heat and melt. After the raw materials are completely melted, degassing and slag removal refining treatment is carried out. After refining, wide aluminum alloy ingots are prepared by electromagnetic semi-continuous casting process. During the casting process, Al-Ti-B grain refiner is added online to control the microstructure. The obtained ingots are placed in an annealing furnace and subjected to three-stage homogenization annealing using a stepped heating method. This process sequentially eliminates casting stress, dissolves low-melting-point phases, and allows for full diffusion of elements. After the process is completed, the ingots are cooled in the furnace and then milled on the surface after being removed from the furnace. The homogenized ingot is heated to the rolling temperature and held for heat treatment. It is then fed into a hot rolling mill for multi-pass reversible hot rolling. The reduction rate and final rolling temperature of each pass are controlled to obtain a hot-rolled strip of a set thickness. After hot rolling, the strip is not coiled and cooled. Instead, it is cooled to 270-320°C by laminar flow and then directly fed into the gradient temperature rolling transition stand online. During the temperature rolling process, Al3Sc and Al3Zr phases are dispersed and pinned to subgrain boundaries through the coupling effect of deformation and precipitation, thereby achieving grain refinement. The temperature drop rate of the strip is precisely controlled by the inter-stand zone spray cooling. After completing the set number of temperature deformation passes, the strip is continuously fed into the cold rolling mill. The reduction rate, rolling speed and inter-stand tension of each cold rolling stand are matched. Combined with precise temperature control between passes, continuous rolling is achieved to obtain cold-rolled sheet of a set thickness. Cold-rolled sheets are directly subjected to final precision rolling to accurately control the thickness and shape of the finished product. After precision rolling, stretching and straightening are performed to obtain wide sheet blanks. The residual heat from the deformation of the finished rolled plate is used as the base temperature, and then it is sent to a heat replenishment device to complete the online pre-aging treatment. During the pre-aging process, the morphology of the grain boundary precipitates is controlled by adjusting the heating rate and holding time, so that they are small and discontinuously distributed. After cooling to room temperature, surface passivation treatment is performed to obtain corrosion-resistant wide aluminum alloy sheet products.

[0007] Preferably, the composition of the aluminum alloy sheet by weight percentage is: Mg 4.2%, Mn 0.4%, Sc 0.14%, Zr 0.1%, Cr 0.22%, Ti 0.10%, Si 0.15%, Fe 0.20%, Cu 0.03%, with the balance being Al and unavoidable impurities.

[0008] Preferably, the first holding temperature of the three-stage homogenization annealing is 300-350℃, the second holding temperature is 420-460℃, and the third holding temperature is 480-520℃. After each holding stage is completed, the temperature is increased to the next stage temperature at a set rate.

[0009] Preferably, the ingot heating temperature is 430-490℃, the hot rolling final rolling temperature is controlled at 340-390℃, the total hot rolling reduction rate is 85-93%, and the single-pass reduction rate is 12-28%.

[0010] Preferably, the warm rolling transition section is set with 3 to 5 passes of deformation, with a single pass reduction rate of 6 to 13%, a total warm rolling reduction rate of 26% to 45%, and the final warm rolling temperature is controlled at 180 to 220°C, which is within the warm deformation range below the recrystallization temperature.

[0011] Preferably, the cold rolling mill adopts a four-stand continuous rolling arrangement, the reduction rate of the first cold rolling pass is higher than that of the subsequent passes, the tension between each stand is increased step by step with each rolling pass, and a cooling device is installed between passes to control the temperature fluctuation of the plate. The total reduction rate of cold rolling is 50-75%.

[0012] Preferably, the final single-pass reduction rate of finishing rolling is 8-18%, which eliminates residual internal stress and improves the shape accuracy in the width direction.

[0013] Preferably, the surface passivation treatment adopts a zirconium-titanium chromium-free passivation process, which first involves alkaline washing to remove oil, acid washing to activate the surface, and then film formation treatment to form a composite passivation film layer on the surface of the plate.

[0014] Compared with the prior art, the beneficial effects of the present invention are: 1. This invention, by matching rolling speed, reduction ratio distribution, and inter-stand tension, combined with an inter-pass cooling system to precisely control deformation temperature, can effectively regulate the precipitation behavior of nano-precipitates in alloys. Deformation-induced precipitation during warm rolling can form dispersed second-phase particles in advance, serving as dislocation pinning points for subsequent cold rolling deformation. This ensures rolling stability during cold rolling, avoids continuous precipitation of coarse second phases, optimizes the morphology and distribution of grain boundary precipitates, further improves the corrosion resistance and formability of the sheet metal, and achieves a balance of multi-dimensional properties. 2. This invention replaces the intermittent process of hot rolling, coiling, cooling, and then re-uncoiling and cold rolling in the traditional process by adding a warm rolling transition section between hot rolling and cold rolling, combined with precise temperature control in different zones. This process utilizes the residual heat of hot rolling to achieve warm deformation, promoting the dynamic recovery of dislocations and the formation of subgrain structures. It effectively controls the degree of work hardening without the need for an additional intermediate annealing process, significantly shortening the production process and reducing energy consumption. Furthermore, it achieves progressive grain refinement through multi-stage gradient deformation in hot, warm, and cold rolling stages. Combined with precise temperature control between cold rolling passes, it ensures the consistency of deformation and microstructure in the width direction of wide plates, solving the problem of uneven performance in the thickness and width directions of wide plates in traditional step-by-step rolling. 3. This invention, through the combination of Sc, Zr, and grain refiners, enables the synergistic effect of these elements to form dispersed nanoscale precipitates in the matrix. On one hand, this stabilizes grain boundaries, inhibits recrystallization grain growth, significantly refines the grain structure across the width of the plate, and improves the uniformity of the structure across the entire surface. On the other hand, it optimizes the potential difference between grain boundaries and the matrix, weakening the driving force of intergranular corrosion. Simultaneously, the modification effect of Mn and Cr elements on impurity phases reduces the corrosive activity of harmful second phases, comprehensively improving the plate's resistance to intergranular corrosion and pitting corrosion from the matrix composition level. This compositional system overcomes the limitations of traditional aluminum-magnesium alloys that rely on a single element to improve corrosion resistance, achieving a synergistic improvement in both strength and corrosion resistance. 4. This invention uses the residual heat generated by precision rolling deformation as the base temperature, requiring only a small amount of additional heating for online pre-aging treatment. This process can form fine and uniform solute atom clusters in the matrix, stabilize the supersaturated solid solution structure, inhibit the formation of unfavorable coarse clusters during subsequent natural aging, and improve the long-term stability of the plate performance. On the other hand, the clusters formed by pre-aging can serve as nucleation sites for the surface film during passivation, improving the adhesion and density of the passivation film to the matrix, strengthening the surface protection effect, and achieving a synergistic effect of matrix corrosion resistance and surface protection. 5. This invention achieves reasonable control of work hardening through the microstructure regulation effect of continuous deformation by hot and cold gradient. This not only shortens the production cycle and reduces production costs and energy consumption, but also further refines the grain structure through a larger cumulative deformation amount, thereby improving the comprehensive mechanical properties of the plate. At the same time, the fully continuous rolling process reduces the risk of surface oxidation and damage caused by intermediate turnover, improves the surface quality and batch performance stability of wide plates, and is more suitable for the scheduling needs of large-scale industrial production. Attached Figure Description

[0015] Figure 1 This is a flowchart illustrating the overall process of the preparation method of the present invention. Figure 2 This is a comparative diagram showing the overall corrosion resistance performance of the various comparative examples and the third embodiment of the present invention; Figure 3 This is a comparative diagram showing the mechanical properties of the various comparative examples and the third embodiment of the present invention. Detailed Implementation

[0016] The technical solutions of the present invention will be clearly and completely described below with reference to the accompanying drawings of the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments.

[0017] Please see Figures 1 to 3 The present invention provides three embodiments: The first embodiment provided by the present invention: A method for preparing corrosion-resistant wide-width aluminum alloy sheets based on the synergistic control of hot and cold continuous rolling. The composition of the aluminum alloy sheet by weight percentage is: Mg 3.5-5.2%, Mn 0.2-0.8%, Sc 0.08-0.20%, Zr 0.05-0.15%, Cr 0.15-0.35%, Ti 0.05-0.15%, Si 0.1-0.25%, Fe 0.08-0.30%, Cu 0.01-0.10%, with the balance being Al and unavoidable impurities. The preparation method includes the following steps: According to the above composition ratio, weigh each raw material and put it into the melting furnace to heat and melt. After the raw materials are completely melted, degassing and slag removal refining treatment is carried out. After refining, wide aluminum alloy ingots are prepared by electromagnetic semi-continuous casting process. During the casting process, Al-Ti-B grain refiner is added online to control the microstructure. The obtained ingots are placed in an annealing furnace and subjected to three-stage homogenization annealing using a stepped heating method. This process sequentially eliminates casting stress, dissolves low-melting-point phases, and allows for full diffusion of elements. After the process is completed, the ingots are cooled in the furnace and then milled on the surface after being removed from the furnace. The homogenized ingot is heated to the rolling temperature and held for heat treatment. It is then fed into a hot rolling mill for multi-pass reversible hot rolling. The reduction rate and final rolling temperature of each pass are controlled to obtain a hot-rolled strip of a set thickness. After hot rolling, the strip is not coiled and cooled. Instead, it is cooled to 270-320°C by laminar flow and then directly fed into the gradient temperature rolling transition stand online. During the temperature rolling process, Al3Sc and Al3Zr phases are dispersed and pinned to subgrain boundaries through the coupling effect of deformation and precipitation, thereby achieving grain refinement. The temperature drop rate of the strip is precisely controlled by the inter-stand zone spray cooling. After completing the set number of temperature deformation passes, the strip is continuously fed into the cold rolling mill. The reduction rate, rolling speed and inter-stand tension of each cold rolling stand are matched. Combined with precise temperature control between passes, continuous rolling is achieved to obtain cold-rolled sheet of a set thickness. Cold-rolled sheets are directly subjected to final precision rolling to accurately control the thickness and shape of the finished product. After precision rolling, stretching and straightening are performed to obtain wide sheet blanks. The residual heat from the deformation of the finished rolled plate is used as the base temperature, and then it is sent to a heating device. The heating device can be an induction heating device to complete the online pre-aging treatment. During the pre-aging process, the morphology of the grain boundary precipitates is controlled by adjusting the heating rate and holding time, so that they are small and discontinuously distributed. After cooling to room temperature, surface passivation treatment is performed to obtain corrosion-resistant wide aluminum alloy sheet products.

[0018] The first holding temperature for the three-stage homogenization annealing is 300–350℃, the second holding temperature is 420–460℃, and the third holding temperature is 480–520℃. After each holding stage is completed, the temperature is increased to the next stage temperature at a set rate.

[0019] The ingot heating temperature is 430-490℃, the hot rolling final rolling temperature is controlled at 340-390℃, the total hot rolling reduction rate is 85-93%, and the single-pass reduction rate is 12-28%.

[0020] The warm rolling transition section is set with 3 to 5 passes of deformation, with a single pass reduction rate of 6 to 13% and a total warm rolling reduction rate of 26% to 45%. The final temperature of warm rolling is controlled at 180 to 220℃, which is in the warm deformation range below the recrystallization temperature.

[0021] The cold rolling mill adopts a four-stand continuous rolling arrangement. The reduction rate of the first cold rolling pass is higher than that of the subsequent passes. The tension between each stand increases with each rolling pass. Cooling devices are installed between passes to control the temperature fluctuation of the plate. The total reduction rate of cold rolling is 50-75%.

[0022] The final single-pass reduction rate of finishing rolling is 8-18%, which eliminates residual internal stress and improves the shape accuracy in the width direction.

[0023] The surface passivation treatment adopts a zirconium-titanium chromium-free passivation process, which first involves alkaline washing to remove oil, acid washing to activate the surface, and then film formation treatment to form a composite passivation film layer on the surface of the plate.

[0024] The second embodiment provided by the present invention: The difference between this embodiment and the first embodiment is that this embodiment provides a method for preparing corrosion-resistant wide aluminum alloy plates based on the coordinated control of hot and cold rolling. The composition of the aluminum alloy plate by weight percentage is: Mg 4.2%, Mn 0.4%, Sc 0.14%, Zr 0.1%, Cr 0.22%, Ti 0.10%, Si 0.15%, Fe 0.20%, Cu 0.03%, with the balance being Al and unavoidable impurities.

[0025] The preparation steps are as follows: Pure aluminum ingots, pure magnesium ingots, aluminum-manganese master alloy, aluminum-scandium master alloy, aluminum-zirconium master alloy, aluminum-chromium master alloy, and aluminum-titanium master alloy were weighed according to the above component ratio and put into a gas-fired melting furnace for heating and melting. After the raw materials were completely melted, they were electromagnetically stirred, and then argon gas was introduced for degassing and refining. A slag remover was added to remove floating slag. After refining, the mixture was kept at a constant temperature and an aluminum alloy ingot of a set width was prepared by electromagnetic semi-continuous casting process. During the casting process, an aluminum-titanium-boron refining agent was added online to control the primary grain size. After milling the surface of the ingot, it is placed into a bogie-type annealing furnace. First, the temperature is raised to the first level and held to eliminate casting stress. Then, the temperature is slowly raised to the second level and held to promote the dissolution of low-melting-point phases. Finally, the temperature is raised to the third level for long-term holding and homogenization treatment. After the treatment is completed, the ingot is cooled with the furnace to below the set temperature and then air-cooled. The homogenized ingot is fed into a walking beam furnace, heated to the rolling temperature and held for through-firing, and then fed into a four-roll reversible hot rolling mill for hot rolling and billet opening. Multiple rolling passes are performed, the single-pass reduction rate range is controlled, and the final rolling temperature is controlled within the set range to obtain a hot-rolled strip of a set thickness. After hot rolling, the strip is not coiled and cooled. Instead, it is laminar cooled to 270–320°C and fed directly into the gradient warm rolling transition stand online. During the warm rolling process, the Al3Sc and Al3Zr phases are dispersed and pinned to subgrain boundaries through the coupling effect of deformation and precipitation, thereby refining the grains. The temperature drop rate is controlled by zoned spray cooling. After completing multiple passes of warm deformation, the strip is continuously fed into a four-stand cold rolling mill. The rolling speeds of warm rolling and cold rolling are matched in a coordinated manner. The reduction rate of the first pass of cold rolling is set to a relatively high level, and the reduction rate of subsequent passes decreases step by step. The tension between each stand increases step by step as the strip temperature decreases. The temperature of the strip is stabilized between passes through a cooling device to obtain a cold-rolled sheet of a set thickness. The rolling process uses full oil lubrication. Cold-rolled sheets are directly fed into the finishing mill for final finishing rolling. The single-pass reduction rate is controlled to roll to the finished thickness. After finishing rolling, stretching and straightening are performed to eliminate residual internal stress and improve sheet shape. The residual heat from the deformation of the finished rolled plate is used as the base temperature, and then it is sent to a heat replenishment device to complete the online pre-aging treatment. During the pre-aging process, the morphology of the grain boundary precipitates is controlled by adjusting the heating rate and holding time, so that they are small and discontinuously distributed. After being air-cooled to room temperature after being taken out of the furnace, the precipitates are subjected to alkaline washing to remove oil, acid washing to activate, and zirconium-titanium chromium-free passivation treatment in sequence to obtain corrosion-resistant wide aluminum alloy sheet products.

[0026] This embodiment employs a medium-content composite microalloying composition combined with a single-pass hot-cold continuous rolling process with warm rolling transition. Through balanced matching of composition and process, a synergistic balance is achieved between the corrosion resistance, mechanical properties, and production economy of the sheet metal. The dispersed precipitation of Sc and Zr, combined with the dynamic recovery microstructure control during warm rolling, ensures uniform grain size across the entire sheet width, effectively mitigating performance differences along the width direction. The combination of online pre-aging and chromium-free passivation based on zirconium and titanium forms a dense and stable protective film layer on the sheet surface, balancing environmental protection requirements with corrosion resistance service requirements. The process route of this embodiment is smooth and stable, enabling continuous production without the need for additional complex equipment, and is suitable for the batch production of general-purpose corrosion-resistant wide-width aluminum alloy sheets under conventional working conditions.

[0027] The third embodiment provided by the present invention: The difference between this embodiment and the first embodiment is that this embodiment provides a method for preparing corrosion-resistant wide aluminum alloy plates based on the coordinated control of hot and cold rolling. The composition of the aluminum alloy plate by weight percentage is: Mg 4.8%, Mn 0.6%, Sc 0.15%, Zr 0.12%, Ti 0.12%, Cr 0.20%, Si 0.15%, Fe 0.20%, Cu 0.04%, with the balance being Al and unavoidable impurities.

[0028] The preparation steps are as follows: Weigh each raw material according to the above composition ratio, put them into the melting furnace and heat them for melting. After stirring, degassing, slag removal and refining, let them stand and keep them warm. Use electromagnetic semi-continuous casting process to prepare aluminum alloy ingots of a set width. Add Al-Ti-B grain refiner online during the casting process. After milling the surface of the ingot, it is placed into the annealing furnace, and then heated and held at three temperature steps in sequence. After cooling in the furnace, it is taken out of the furnace. After the ingot is heated to the set temperature and held for heat treatment, it is sent to the hot rolling mill for multi-pass hot rolling. The single-pass reduction rate range and the final rolling temperature are controlled to obtain hot-rolled strip. Hot-rolled strip enters the warm rolling transition stand online, and after two passes of warm deformation, it is sent to the five-stand cold continuous rolling mill. The reduction rate of the first pass is set to a relatively high level, and the reduction rate of subsequent passes is reduced step by step. The tension of each stand is adjusted step by step according to the temperature. The cooling between passes controls the plate temperature to stabilize. The rolling process uses full oil lubrication to control the surface quality. Cold-rolled sheets are directly subjected to final finishing rolling, with the single-pass reduction rate controlled to achieve the finished thickness, followed by stretching and straightening. The finished sheet material is obtained by using the residual heat from the finishing rolling process for online pre-aging treatment, followed by surface cleaning and passivation.

[0029] This embodiment employs a higher alloying element content combined with a two-pass, two-stage warm rolling transition and a five-stand cold continuous rolling process. Through greater cumulative deformation and stronger micro-alloying, the strength grade and corrosion resistance limit of the sheet metal are further improved. The two-pass, two-stage warm deformation achieves gradient control of the deformed microstructure, promotes the dispersed distribution of nano-precipitates, effectively pins grain boundaries, and inhibits the expansion of corrosion channels, significantly improving the service stability of the sheet metal in highly corrosive environments. The precise matching of tension and reduction rate in the five-stand continuous rolling ensures the shape accuracy and thickness uniformity of the wide sheet metal under large deformation conditions. The sheet metal prepared in this embodiment exhibits superior overall performance and is suitable for heavy-duty corrosive applications such as ship hulls and chemical containers, where both strength and corrosion resistance are critical. To address this, we employed the controlled variable method, establishing four sets of comparative examples to directly compare with this embodiment in terms of mechanical properties and corrosion resistance. The four sets of comparative examples are detailed in the table below: Table 1 Explanation of each comparative example

[0030] Comparative Example 1 was intended to demonstrate the decisive role of Sc and Zr microalloying in strength and corrosion resistance; Comparative Example 2 was used to demonstrate the necessity of the deformation-precipitation coupling mechanism in warm rolling for grain refinement and uniform distribution of precipitates; Comparative Example 3 was used to demonstrate the necessity of reheating to the effective temperature range for Sc or Zr precipitation strengthening; and Comparative Example 4 was used to demonstrate the importance of selecting the warm rolling temperature window, as shown in the appendix. Figure 2 and Figure 3 As shown in the table below, statistics were compiled after acquiring the mechanical and corrosion resistance data: Table 2 Comparison of corrosion resistance of aluminum alloy sheets

[0031] As shown in Table 2, the maximum depth of exfoliation corrosion in the present invention is 115 μm, the exfoliation corrosion area ratio is 7.5%, the maximum depth of intergranular corrosion is 55 μm, and the corrosion weight loss is 17 mg / cm³. 2 Compared with Comparative Example 1 (without Sc and Zr), the four corrosion resistance indicators mentioned above decreased by 72.6%, 80.3%, 54.2%, and 45.2%, respectively.

[0032] Furthermore, in Comparative Example 3, due to the lack of heat replenishment, the driving force for the precipitation of Al3Sc and Al3Zr phases was insufficient, resulting in a significantly smaller precipitation quantity. Although the average particle size was measured to be 20 nm, the density of dispersed phases per unit volume was much lower than that in this embodiment, thus failing to effectively pin grain boundaries and limiting the improvement in corrosion resistance.

[0033] The area ratio of exfoliation corrosion decreased from 38% in Comparative Example 1 to 7.5% in the present invention, a reduction of 80.3%. That is, the present invention, through the triple synergistic effect of composition optimization, coupling of warm rolling deformation and precipitation, and precise aging by induction heating, transforms the corrosion morphology from large-area continuous exfoliation in Comparative Example 1 to localized shallow uniform corrosion in the present invention, fundamentally changing the corrosion failure mode of the material.

[0034] The mechanical property data of each aluminum alloy sheet sample are shown in the table below: Table 3 Comparison of Mechanical Properties of Aluminum Alloy Sheets

[0035] As shown in Table 3, the present invention clearly demonstrates the contribution of each process feature to the strength through a progressive comparison from Comparative Examples 1 to 4 to this embodiment. For example: Referring to Comparative Examples 1 and 2, the yield strength was increased by about 40 MPa, mainly due to the precipitation strengthening and grain refinement of Al3Sc and Al3Zr phases. Through the coupling effect of residual heat from finishing rolling and induction heating, the dispersion precipitation of Al3Sc and Al3Zr phases was further promoted, resulting in a yield strength of more than 30% higher than that of traditional processes, such as 5083 alloy. Referring to Comparative Example 2 to this embodiment, the yield strength is further increased by approximately 85 MPa. This is due to the coupling between deformation and precipitation promoting a uniform and dispersed distribution of the Al3Sc and Al3Zr phases. As shown in Table 3, the tensile strength of this embodiment reaches 450 MPa, the yield strength reaches 320 MPa, the elongation is 15.0%, the average grain size is refined to 20 μm, and the Vickers hardness reaches 135 HV.

[0036] Compared with Comparative Example 1 without Sc and Zr, the tensile strength and yield strength increased by 25.0% and 63.3% respectively, which fully demonstrates the strong precipitation strengthening and grain refinement effect produced by Sc and Zr microalloying through the formation of nanoscale Al3Sc (Al3Zr) dispersed phases.

[0037] Compared with Comparative Example 2 without warm rolling, the yield strength of this embodiment is increased by about 85 MPa, and the grain size is refined from 35 μm to 20 μm. Through the coupling mechanism of deformation, precipitation and recrystallization during warm rolling, the pinning effect of Al3Sc and Al3Zr relative to grain boundaries and subgrain boundaries is utilized to effectively suppress the growth of recrystallized grains. This confirms that the coupling effect of deformation and precipitation in the warm rolling stage can promote the uniform dispersion of precipitated phases, more effectively pin grain boundaries and suppress the growth of recrystallized grains, and achieve a fine grain strengthening effect that is better than single precipitation strengthening.

[0038] Compared with Comparative Example 3 without heat replenishment, the significant improvement in strength and hardness indicates that maintaining the residual heat of finishing rolling within the effective aging temperature range through a heat replenishment device is a key process guarantee to ensure the precipitation strengthening of elements such as Sc and Zr. Natural cooling cannot achieve the same precipitation strengthening effect.

[0039] Furthermore, it adopts a continuous and coordinated process of hot rolling, warm rolling, and cold rolling, eliminating the intermediate annealing process required after hot rolling in traditional processes. On this basis, the thermal stability of the material is ensured by micro-alloying of Sc and Zr, which effectively shortens the total production cycle compared to traditional processes. The energy utilization efficiency is further improved by using the coupling of residual heat from finishing rolling and induction heating. In summary, this embodiment achieves an excellent balance between strength and plasticity by employing multiple synergistic strengthening mechanisms, including composition optimization, warm rolling precipitation, and precise pre-aging, while maintaining good elongation. This results in wide aluminum alloy sheets with both high load-bearing capacity and excellent forming and processing performance, fully meeting the stringent service conditions for materials with high strength and toughness requirements in applications such as shipbuilding and chemical containers.

[0040] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above, and that the invention can be implemented in other specific forms without departing from its spirit or essential characteristics. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description. Thus, all variations falling within the meaning and scope of equivalents of the claims are intended to be included within the present invention. No reference numerals in the claims should be construed as limiting the scope of the claims.

Claims

1. A method for preparing corrosion-resistant wide aluminum alloy sheets based on synergistic control of hot and cold continuous rolling, characterized in that, The composition of the aluminum alloy sheet by weight percentage is: Mg 3.5-5.2%, Mn 0.2-0.8%, Sc 0.08-0.20%, Zr 0.05-0.15%, Cr 0.15-0.35%, Ti 0.05-0.15%, Si 0.1-0.25%, Fe 0.08-0.30%, Cu 0.01-0.10%, with the balance being Al and unavoidable impurities; The preparation method includes the following steps: According to the above composition ratio, weigh each raw material and put it into the melting furnace to heat and melt. After the raw materials are completely melted, degassing and slag removal refining treatment is carried out. After refining, wide aluminum alloy ingots are prepared by electromagnetic semi-continuous casting process. During the casting process, Al-Ti-B grain refiner is added online to control the microstructure. The obtained ingots are placed in an annealing furnace and subjected to three-stage homogenization annealing using a stepped heating method. This process sequentially eliminates casting stress, dissolves low-melting-point phases, and allows for full diffusion of elements. After the process is completed, the ingots are cooled in the furnace and then milled on the surface after being removed from the furnace. The homogenized ingot is heated to the rolling temperature and held for heat treatment. It is then fed into a hot rolling mill for multi-pass reversible hot rolling. The reduction rate and final rolling temperature of each pass are controlled to obtain a hot-rolled strip of a set thickness. After hot rolling, the strip is not coiled and cooled. Instead, it is cooled to 270-320°C by laminar flow and then directly fed into the gradient temperature rolling transition stand online. During the temperature rolling process, Al3Sc and Al3Zr phases are dispersed and pinned to subgrain boundaries through the coupling effect of deformation and precipitation, thereby achieving grain refinement. The temperature drop rate of the strip is precisely controlled by the inter-stand zone spray cooling. After completing the set number of temperature deformation passes, the strip is continuously fed into the cold rolling mill. The reduction rate, rolling speed and inter-stand tension of each cold rolling stand are matched. Combined with precise temperature control between passes, continuous rolling is achieved to obtain cold-rolled sheet of a set thickness. Cold-rolled sheets are directly subjected to final precision rolling to accurately control the thickness and shape of the finished product. After precision rolling, stretching and straightening are performed to obtain wide sheet blanks. The residual heat from the deformation of the finished rolled plate is used as the base temperature, and then it is sent to a heat replenishment device to complete the online pre-aging treatment. During the pre-aging process, the morphology of the grain boundary precipitates is controlled by adjusting the heating rate and holding time, so that they are small and discontinuously distributed. After cooling to room temperature, surface passivation treatment is performed to obtain corrosion-resistant wide aluminum alloy sheet products.

2. The method for preparing corrosion-resistant wide aluminum alloy sheets based on the synergistic control of hot and cold continuous rolling according to claim 1, characterized in that, The composition of the aluminum alloy sheet by weight percentage is: Mg 4.2%, Mn 0.4%, Sc 0.14%, Zr 0.1%, Cr 0.22%, Ti 0.10%, Si 0.15%, Fe 0.20%, Cu 0.03%, with the balance being Al and unavoidable impurities.

3. The method for preparing corrosion-resistant wide aluminum alloy sheets based on the synergistic control of hot and cold continuous rolling according to claim 1 or 2, characterized in that, The first holding temperature for the three-stage homogenization annealing is 300–350℃, the second holding temperature is 420–460℃, and the third holding temperature is 480–520℃. After each holding stage is completed, the temperature is increased to the next stage temperature at a set rate.

4. The method for preparing corrosion-resistant wide aluminum alloy sheets based on the synergistic control of hot and cold continuous rolling according to claim 3, characterized in that, The ingot heating temperature is 430-490℃, the hot rolling final rolling temperature is controlled at 340-390℃, the total hot rolling reduction rate is 85-93%, and the single-pass reduction rate is 12-28%.

5. The method for preparing corrosion-resistant wide aluminum alloy sheets based on the synergistic control of hot and cold continuous rolling according to claim 4, characterized in that, The warm rolling transition section is set with 3 to 5 passes of deformation, with a single pass reduction rate of 6 to 13% and a total warm rolling reduction rate of 26% to 45%. The final temperature of warm rolling is controlled at 180 to 220℃, which is in the warm deformation range below the recrystallization temperature.

6. The method for preparing corrosion-resistant wide aluminum alloy sheets based on the synergistic control of hot and cold continuous rolling according to claim 5, characterized in that, The cold rolling mill adopts a four-stand continuous rolling arrangement. The reduction rate of the first cold rolling pass is higher than that of the subsequent passes. The tension between each stand increases with each rolling pass. Cooling devices are installed between passes to control the temperature fluctuation of the plate. The total reduction rate of cold rolling is 50-75%.

7. The method for preparing corrosion-resistant wide aluminum alloy sheets based on the synergistic control of hot and cold continuous rolling according to claim 6, characterized in that, The final single-pass reduction rate of finishing rolling is 8-18%, which eliminates residual internal stress and improves the plate shape accuracy in the width direction.

8. The method for preparing corrosion-resistant wide aluminum alloy sheets based on the synergistic control of hot and cold continuous rolling according to claim 7, characterized in that, The surface passivation treatment adopts a zirconium-titanium chromium-free passivation process, which first involves alkaline washing to remove oil, acid washing to activate the surface, and then film formation treatment to form a composite passivation film layer on the surface of the plate.