A continuous extrusion die with non-uniform depth resistance control structure and its forming method
By setting a central flow divider block and differentiating rheological resistance in shallow and deep groove areas within the mold, the problem of uneven flow during aluminum alloy profile forming is solved, achieving efficient one-time forming and high-quality aluminum profile production.
Patent Information
- Application Number
- CN202611285159.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-24
- Publication Date
- 2026-11-17
AI Technical Summary
In traditional continuous extrusion processes, uneven metal flow during aluminum alloy profile forming can lead to problems such as localized accumulation in the center, incomplete filling at the edges, and cracking. Existing mold designs cannot effectively control rheological resistance, resulting in low production efficiency and poor product quality.
A continuous extrusion die with a non-equal depth resistance control structure is used to differentiate and control the rheological resistance by setting a central flow divider block, a central shallow groove area, and a lateral deep groove guide area within the die. This makes the flow velocity in the central region and the two side regions tend to be coordinated, achieving one-time molding.
It achieves efficient one-time forming of aluminum profiles, reduces secondary shaping processes, improves the flatness and surface quality of products, reduces production energy consumption and costs, and extends the service life of molds.
Smart Images

Figure CN123102779A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of extrusion die technology, specifically a continuous extrusion die and forming method with an integrated molding and non-equal depth resistance control structure. Background Technology
[0002] High aspect ratio aluminum alloy profiles are increasingly widely used in modern industry due to their combination of lightweight, high ductility and good mechanical properties.
[0003] However, its preparation process faces many technical bottlenecks: Traditional continuous extrusion processes use conventional dies for direct extrusion forming. When the aluminum billet enters the narrow and wide forming cavity from the wide extrusion roller groove, the metal flow lacks effective guidance. Due to the low flow resistance in the center and the high flow resistance at the edges, the metal fluid is prone to flowing too fast in the center while the edges are insufficiently supplied. This uneven velocity field distribution (with extremely large fluctuations) can lead to localized accumulation and thickening in the center of the formed aluminum sheet, while the edges are not fully filled, resulting in stretching or even cracking.
[0004] To overcome the above-mentioned deficiencies, existing technologies mainly solve the problem through the following two technical means, specifically: The first method involves a traditional U-shaped mold combined with a secondary flattening process. This involves designing the outlet in a U-shape to slow the flow speed and "roll up" the wide metal before extrusion, shortening the widening distance. Multiple rollers are then added for secondary unfolding and flattening. As can be seen, this purely physical bending / flattening process is lengthy and introduces internal stress: after extruding the U-shaped profile, a dedicated unfolding and flattening process must be added. This not only extends the production line length and increases energy consumption, but the secondary unfolding and flattening also generates residual bending stress within the profile, leading to significant thickness variations.
[0005] The second type: Modular gradient unfolding mold. This technology uses multiple modules to form a gradient unfolding cavity inside the mold that transitions from a "U" shape at the entrance to a "I" shape at the exit, attempting to achieve physical flattening within the mold. For example, Chinese patent application (CN113134521A) discloses a gradually unfolding die structure for continuous extrusion forming of copper and copper alloy strips. Specifically, it includes: a connecting module and a forming die; the front end of the connecting module is connected to the extrusion device, and the rear end is connected to the forming die; the connecting module is a plate-like structure with a certain thickness; the connecting surface of the connecting module and the extrusion device is machined with an mounting surface matching the shape of the extrusion device; a right-angle deformation zone is provided at the point opposite the extrusion port of the connecting module and the extrusion device, and a connecting cavity opposite to the cavity of the forming die is machined at the rear of the right-angle deformation zone; a connecting groove is machined on the back of the connecting module for connecting and positioning the forming die; a gradually unfolding cavity channel is machined inside the forming die, extending from a "U"-shaped structure at the inlet to a "I"-shaped structure at the outlet; a sizing band of 4-10mm length is provided at the tail end of the cavity channel. The forming die is composed of N modules of a certain thickness, bolted together, and the inner wall of the cavity channel inside the assembled forming die has a continuous gradually unfolding curved surface. It is evident that the splicing structure presents certain risks of material leakage and processing: the gradient unfolding mold needs to be divided into N pieces for bolt splicing. Under harsh working conditions of continuous extrusion at temperatures above 500℃ and high extrusion pressure, the splicing gaps are prone to causing metal overflow (material leakage) or deformation misalignment; moreover, multiple non-standard gradient curved surface modules have high requirements for processing and assembly precision, resulting in high manufacturing and assembly costs.
[0006] In summary, both U-shaped molds and gradient unfolding molds essentially guide the metal physically in terms of its "geometric shape," lacking direct intervention in the "rheological resistance" within the metal fluid. Their ability to suppress ultra-high-speed metal flow at the center is limited, thus restricting product yield. Summary of the Invention
[0007] The purpose of this invention is to overcome the shortcomings of existing technologies by providing a continuous extrusion die and forming method with a non-uniform depth resistance control structure. This invention differentiates the rheological resistance in the width direction of the billet by setting a central flow divider, a central shallow groove area, and a lateral deep groove guide area within the billet's moving flow channel. This makes the flow velocity in the central region and the two side regions more coordinated, thereby solving the problem of uneven flow velocity during continuous extrusion of profiles with large width-to-thickness ratios and achieving one-time forming without secondary shaping.
[0008] To achieve the above-mentioned objectives of this invention, the present invention provides the following technical solution: A continuous extrusion die with a non-equal depth resistance control structure includes an integral die. One end of the die is provided with a top groove, and the other end is provided with a discharge port. The bottom of the top groove is provided with a first inlet and a second inlet. The bottom surface of the top groove is provided with a central flow divider block. The first inlet and the second inlet are located on the outer periphery of the central flow divider block. A flow guide channel that gradually narrows along the billet feeding direction is formed between the first inlet and the second inlet. The second inlet and the discharge port are connected by a billet movement channel. The blank movement channel is a continuous, seamless channel formed inside the mold; The billet moving channel includes a feed diversion section, a gradually expanding transition section and a sizing extrusion section that are connected sequentially along the billet feeding direction. The flow width from the feed diversion section to the gradually expanding transition section gradually increases along the billet feeding direction. The sizing extrusion section has a sizing cross section corresponding to the discharge port.
[0009] In some embodiments, the feed diversion section is formed by a central diversion block and two side channels, and its cross-sectional profile is U-shaped. The bottom surface of the inner cavity of the gradually expanding transition section is a three-dimensional curved surface with a depth that changes continuously along the feed direction of the billet. The three-dimensional curved surface includes a central shallow groove area in the middle of the width direction and lateral deep groove guide areas on both sides of the central shallow groove area. The depth of the central shallow groove area is less than the depth of the lateral deep groove guide areas, so that a high rheological resistance area is formed in the middle of the width direction and a low rheological resistance area is formed on both sides. In the longitudinal section along the billet feeding direction and passing through the bottom of the lateral deep groove guide area, the angle between the tangents of the bottom of the deep grooves on both sides of the sizing extrusion section and the axial direction of the discharge port is 0 to 5°, and the axial direction of the discharge port is the direction of the extrusion sizing axis of the sizing extrusion section.
[0010] In some embodiments, the second inlet has an arched structure, and the top of the inner arc-shaped side of the second inlet is cut flat to form a straight chord edge, which extends along the width direction of the outlet and corresponds to the position of the central shallow groove area in the width direction.
[0011] In some embodiments, the first inlet and the second inlet are smoothly transitioned by an inclined sidewall, which causes the flow width of the guide channel to gradually decrease from the first inlet to the second inlet.
[0012] Furthermore, the die feeding axis is parallel to the extrusion sizing axis of the sizing section, and the two axes have an eccentricity e in the vertical direction, where 2mm≤e≤5mm.
[0013] Furthermore, the central diversion block is a wedge-shaped or trapezoidal diversion block, and the first and second inlets are arranged vertically and surround the outer periphery of the central diversion block.
[0014] A method for processing a billet moving flow channel includes the following steps: S1. Using annealed H13 hot work die steel as the blank, a carbide round nose end mill with AlTiN coating is used to mill the blank in layers from the feed end and the discharge end inwards, forming a basic U-shaped flow channel outline. A machining allowance of 0.3-0.5mm is reserved on the inner wall of the flow channel. The milling process parameters are: spindle speed 2400-2800r / min, feed rate 1400-1800mm / min, axial depth of cut 3-4mm, radial width of cut 5-7mm. After rough machining, the blank is subjected to quenching and high-temperature tempering heat treatment to control the hardness to HRC 48-52. S2. Prepare a copper forming electrode that is compatible with the U-shaped flow channel cavity at the feed end, clamp it in an electrical discharge machining (EDM) machine, extend it into the flow channel from the feed end for electrical discharge machining, and remove the reserved allowance by instantaneous local high temperature of 8000-12000℃. During the machining process, the electrode and the cavity wall maintain a discharge gap of 0.03-0.05mm.
[0015] S3. A copper forming electrode matching the flat profile of the discharge end is used to extend into the flow channel from the discharge end for electrical discharge finishing. The machining references at both ends are calibrated by machine tool coordinates so that the cavity machining at the feed end and discharge end can be advanced to the middle of the flow channel and smoothly merged to obtain a continuous, seamless through-type billet moving flow channel.
[0016] A method for integral forming of a continuous extrusion die with a non-uniform depth resistance control structure includes the following steps: (1) Material preparation and cleaning: Select aluminum alloy to be cast into cylindrical blanks, use a rotating steel wire brush to clean the surface oxide layer, and use a dust collection device to increase the surface friction coefficient to prevent slipping; (2) Continuous extrusion molding: The extrusion wheel speed is 6-8 r / min, the die temperature is 500-550℃, the billet enters the die, and after being diverted by the central diverting block, it enters the feeding diversion section and the gradual expansion transition section in sequence. The central shallow groove area in the gradual expansion transition section generates a high rheological resistance to the middle billet in the width direction, and the lateral deep groove guiding area generates a low rheological resistance to the billets on both sides in the width direction, so that the billets on both sides are quickly replenished and enter the sizing extrusion section synchronously with the middle billet, and a flat aluminum billet with a width-to-thickness ratio greater than 20 is directly extruded in the sizing extrusion section in one straight step; (3) Online cooling: After extrusion, water spray is used for rapid cooling to shape and refine the grains, resulting in finished aluminum profiles.
[0017] In some alternative embodiments, the rotation speed of the wire brush in step (1) is 300-400 r / min; in step (3), it is cooled to 20-30°C.
[0018] In some alternative embodiments, the finished aluminum profile has a thickness deviation of ≤ ±0.02 mm and a surface roughness Ra of ≤ 0.4 μm.
[0019] Compared with the prior art, the beneficial effects of the present invention are: 1. This invention is based on a special three-dimensional flow channel inside an integrated continuous extrusion die with rheological resistance control, consisting of an integrated continuous extrusion die body and an internal non-equal depth flow channel; the die is an indivisible integral molding part, including a feed diversion section, a gradual expansion transition section and a sizing extrusion section.
[0020] 2. Both the first and second inlets of the present invention have a ∩-shaped structure. A central diversion block with a wedge-shaped / trapezoidal cross-section is provided at the center of the ∩-shaped inlet, and the central diversion block forcibly divides the main feed stream.
[0021] 3. The bottom surface of the inner cavity of the gradually expanding transition section of the present invention is a three-dimensional curved surface with a depth that continuously changes along the feed direction of the billet. The central region in the width direction (corresponding to the profile center) is extremely shallow, forming a shallow central groove area, which constitutes a high rheological resistance area and suppresses the central metal flow velocity; the two side edge regions in the width direction (corresponding to the profile edge) are provided with lateral deep groove guiding areas, which are deep and extend directly to the edge of the sizing zone, forming a low rheological resistance area and accelerating the edge fluid supply.
[0022] 4. The sizing extrusion section and eccentric design of the present invention: the angle between the tangent of the bottom of the deep groove on both sides and the edge discharge direction is set to 0 to 5°, and the two axes have an eccentricity e in the vertical direction to achieve straight and seamless guidance of the billet; in addition, the die feeding axis and the sizing axis of the sizing extrusion section are parallel to each other, and the two axes have an eccentricity e in the vertical direction, 2mm≤e≤5mm, and the eccentricity e is preferably 3mm, so that the physical length of the center streamline is longer than the length of the edge streamline, further reducing the speed difference.
[0023] 5. This invention abandons the existing "multi-module splicing and gradual flattening" scheme. It adopts an integrated three-dimensional flow channel structure, which effectively reduces the problems of mold misalignment and material leakage in gaps under high temperature and high pressure, extends the service life of the mold, and reduces the dead zone of metal flow through smooth internal transition, avoiding defects such as blank folding and flow line disorder caused by dead zones, thus improving the forming quality.
[0024] 6. This invention eliminates the entire secondary flattening process in the traditional process, shortens the production line length by more than 30%, and significantly reduces equipment energy consumption and investment.
[0025] 7. Compared to physically forced flattening, this invention uses a combination of a central flow divider block, a central shallow groove area, a lateral deep groove guiding area, and an eccentricity parameter to differentially control the rheological resistance in the width direction of the billet. This makes the flow velocity in the central and edge regions more consistent, and simulation results show that the velocity field distribution at the outlet is more uniform (as shown in the Deform simulation data). The extruded billet has better flatness, reducing incomplete filling, wavy edges, and cracking.
[0026] 8. This invention reduces the damage and internal stress caused by traditional physical bending, and the thickness deviation of the finished aluminum profile is controlled within ≤±0.02mm, and the surface roughness Ra≤0.4 micrometers. Attached Figure Description
[0027] To more clearly illustrate the specific embodiments of the present invention or the technical solutions in the prior art, the accompanying drawings used in the description of the specific embodiments or the prior art will be briefly introduced below. In all the drawings, similar elements or parts are generally identified by similar reference numerals. In the drawings, the elements or parts are not necessarily drawn to scale.
[0028] Figure 1 This is a schematic diagram of the structure of a continuous extrusion die with a non-equal depth resistance control structure according to the present invention.
[0029] Figure 2 for Figure 1 Schematic diagram of the cross-sectional structure of AA; Figure 3 for Figure 1 Schematic diagram of the cross-sectional structure of BB; Figure 4 This is a schematic diagram of the blank movement channel inside the mold in this invention; Figure 5 This is a three-dimensional structural diagram of the mold in this invention; Figure 6 This is a schematic diagram of the bottom structure of the mold in this invention; Figure 7 This is a schematic diagram of the physical structure of the mold in this invention; Figure 8 This is a cross-sectional view of the mold in this invention; Figure 9 This is a schematic diagram showing the billet movement channel in the mold of the present invention. The area covered by dark yellow in the figure is the billet movement channel. Figure 10 This is a schematic diagram illustrating the shape change trend of the extruded material as it flows through the billet movement channel within the die in this invention. Figure 11 This is a schematic diagram of the Deform extruded profile of the present invention; Figure 12 for Figure 11 A schematic diagram of the velocity field distribution of extruded profiles; Figure 13 This is a schematic diagram of an existing mold for deforming extruded profiles; Figure 14 for Figure 13 Schematic diagram of the velocity field of extruded profiles; The reference numerals and their corresponding component names in the figure are as follows: 1-Mold, 101-Top recess, 102-Bottom recess 2-First feed inlet, 3-Second feed inlet, 4-Central splitter block, 41-Chord edge, 401-Feed splitter section, 402-Gradual transition section, 403-Sizing extrusion section; 5-Discharge port. Detailed Implementation
[0030] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0031] Example 1: like Figures 1 to 12 As shown, this disclosure discloses a continuous extrusion die with a non-equal depth resistance control structure, including a die 1. One end of the die 1 is provided with a top groove 101, and the other end is provided with a discharge port 5. The bottom of the top groove 101 has a first inlet 2 and a second inlet 3. A guide channel that gradually narrows along the material feeding direction is formed between the first inlet 2 and the second inlet 3. The second inlet and the discharge port 5 are connected by a billet moving flow channel. The billet moving flow channel includes a feed diversion section, a gradually expanding transition section and a sizing extrusion section connected in sequence, with the flow width increasing sequentially along the billet feeding direction. The cross-sectional profile of the feed diversion section is ∩-shaped. The bottom surface of the inner cavity of the gradually expanding transition section is a three-dimensional curved surface with a continuously changing depth along the billet feeding direction. The central area in the width direction constitutes a high rheological resistance zone, and the two edge areas on both sides in the width direction constitute a low rheological resistance zone. The angle between the tangent of the bottom of the deep groove on both sides of the sizing extrusion section and the edge discharge direction is 0 to 5°.
[0032] The angle between the tangent of the bottom of the deep groove on both sides of the sizing extrusion section and the edge discharge direction can be selected as 0°, 1°, 2°, 3°, 4°, or 5°. When the angle is 0°, the bottom of the deep groove is parallel to the discharge direction, the material flows in a straight line, the streamline is straight, there is no lateral diversion thrust, and the lateral disturbance of the material flow is minimal. As the angle gradually increases, the bottom of the groove forms an inclined guiding structure, which can guide the material at the edge, adjust the material speed in the edge area, reduce the difference in flow velocity between the center and the edge of the profile cross-section, and improve the unevenness of the finished product wall thickness. By selecting different angles, various extrusion conditions can be matched; a larger angle enhances the edge guiding capacity, while a smaller angle weakens the additional shear effect and reduces the phenomenon of material stagnation in the area. At the same time, the gradient angle selection can standardize the trial mold adjustment plan, reduce multiple machining modifications of the mold, and reduce debugging costs; it also balances the lateral shear distribution inside the flow channel, reduces appearance defects such as wrinkles and ripples, and improves the surface forming quality of the extruded profile.
[0033] The second inlet has an arched structure, and the top of the inner arc-shaped side of the second inlet is cut flat to form a straight chord edge 41. The chord edge 41 is used to balance the flow rate in the width direction of the billet and achieve synchronous discharge.
[0034] The chord edge 41 can guide the billet to disperse to both sides, increase the flow resistance in the middle of the flow channel, slow down the billet flow rate in the central area, and make the billet flow rate along the entire width direction tend to be consistent, so as to realize the synchronous discharge of the billet and improve the uniformity of extruded product molding.
[0035] Understandably, the billet is squeezed and flows sequentially through the feed diversion section, the gradual expansion transition section and the sizing extrusion section, and the billet width gradually increases; in conjunction with the chord edge structure to balance the flow velocity in the width direction, synchronous and uniform discharge is achieved.
[0036] The first and second inlets are smoothly transitioned by an inclined sidewall. That is, the two are smoothly transitioned along the material feeding direction by an inclined sidewall, forming a guide channel with a gradually narrowing cross-section.
[0037] To better separate the materials, a central diversion block is added. The bottom surface of the settling tank is equipped with a central diversion block, and the first and second inlets are arranged vertically and located on the outer periphery of the central diversion block.
[0038] It should be noted that after the billet arrives at the settling tank, it undergoes preliminary flow distribution through the central diversion block, and enters the first and second feed ports located on the outer periphery of the central diversion block respectively, thereby achieving initial diversion of the billet and alleviating the problem of flow deviation caused by concentrated feeding.
[0039] It should also be noted that the die feeding axis of this invention is parallel to the extrusion sizing axis of the sizing section, and the two axes have an eccentricity e in the vertical direction, where 2mm ≤ e ≤ 5mm. The eccentricity e can be 2mm, 3mm, 4mm, or 5mm, etc. In this embodiment, the eccentricity e is preferably 3mm. The eccentricity e can be selected according to the forming conditions to flexibly adjust the material flow compensation amplitude in the upper and lower regions. The eccentric misalignment of the axes can change the travel path of the billet before entering the sizing extrusion section, balance the material travel resistance and internal pressure distribution in the upper and lower regions of the flow channel, improve the problem of inconsistent flow velocity in the upper and lower parts of the billet, alleviate the upper and lower wall thickness deviation of the extruded profile, reduce the local stagnant material area in the flow channel, and enable the billet to smoothly transition into the sizing extrusion section, effectively improving the cross-sectional forming accuracy of the extruded profile.
[0040] like Figure 6 As shown, the bottom of the mold is provided with a bottom groove 102, and the bottom surface of the bottom groove 102 is provided with a discharge port 5. If the discharge port is directly opened on the bottom surface of the mold, the billet will directly hit the bottom plate of the mold after flowing out, and the flow direction will turn sharply. It is easy to form vortices at the corners and retain aluminum material, causing surface defects of the profile. At the same time, the newly extruded profile is easily deformed due to the constraint of the rigid bottom plate.
[0041] This invention adds a bottom sink 102 to the bottom of the mold, with the discharge port located on the top surface of the bottom sink 102. After the billet is extruded through the discharge port, it enters the cavity of the bottom sink 102, resulting in a smooth flow transition and eliminating dead zones where materials stagnate. The buffer space formed by the sink 102 facilitates the release of residual extrusion stress in the profile, improving the straightness of the aluminum profile with a large width-to-thickness ratio. Furthermore, the sink 102 is an empty cavity, allowing operators to easily observe the discharge status. It also provides operating space for polishing the discharge port edge and repairing the mold, and can disperse the concentrated load on the edge of the discharge port, reducing wear and deformation of the discharge port.
[0042] In an optional embodiment of this disclosure, a processing method for a billet moving channel is provided, specifically as follows: A method for processing a billet moving flow channel includes the following steps: S1. Using annealed H13 hot work die steel as the blank, a carbide round nose end mill with AlTiN coating is used to mill the blank in layers from the feed end and the discharge end inwards, forming a basic U-shaped flow channel outline. A machining allowance of 0.3-0.5mm is reserved on the inner wall of the flow channel. The milling process parameters are: spindle speed 2400-2800r / min, feed rate 1400-1800mm / min, axial depth of cut 3-4mm, radial width of cut 5-7mm. After rough machining, the blank is subjected to quenching and high-temperature tempering heat treatment to control the hardness to HRC 48-52. S2. Prepare a copper forming electrode that is compatible with the U-shaped flow channel cavity at the feed end, clamp it in an electrical discharge machining tool, extend it into the flow channel from the feed end for electrical discharge machining, and remove the reserved material by instantaneous local high temperature of 8000~12000℃. During the machining process, the electrode and the cavity wall maintain a discharge gap of 0.03~0.05mm. S3. A copper forming electrode matching the flat profile of the discharge end is used to extend into the flow channel from the discharge end for electrical discharge finishing. The machining references at both ends are calibrated by machine tool coordinates so that the cavity machining at the feed end and discharge end can be advanced to the middle of the flow channel and smoothly merged to obtain a continuous, seamless through-type billet moving flow channel.
[0043] This method first uses CNC milling to roughly shape the basic contour of the U-shaped flow channel from both the feed and discharge ends of the mold, reserving allowance for electrical discharge machining (EDM). Then, using forming electrodes adapted to the contours of the feed and discharge ends respectively, pulse discharge machining is performed from both ends into the flow channel until they smoothly converge in the middle, constructing a continuous and interconnected billet moving flow channel. This method overcomes the technical difficulties of insufficient tool rigidity, poor accessibility in narrow areas, and easy generation of tool steps and surface tool marks during single CNC finishing of narrow, gradually deformed U-shaped flow channels, as well as the insufficient forming accuracy in the middle section and uneven transition of the beginning and end sections in unidirectional EDM. By combining rough milling pre-forming with bidirectional opposing electrical discharge machining, the processing difficulty of narrow and deep cavity molds is effectively reduced and the processing efficiency is improved. Bidirectional opposing electrical discharge machining can make the entire flow channel obtain uniform forming accuracy, ensuring a smooth and gradual transition of the contour from the feed end to the discharge end and high dimensional consistency. At the same time, it can completely eliminate residual tool marks and micro-concave and convex defects from milling, significantly improve the smoothness of the inner wall of the flow channel, reduce the frictional resistance of billet conveying, reduce material retention, sticking and scratches on the product, ensure stable and uniform billet conveying, effectively suppress turbulence and material accumulation, and improve the finished product qualification rate of the mold and the dimensional stability of the extruded product.
[0044] like Figure 2-4 As shown in Figure 9, the gradually expanding transition section has a three-dimensional non-uniform depth curved surface at the bottom of the inner cavity. The central region in the width direction (corresponding to the profile center) is extremely shallow, forming a shallow central groove area, which constitutes a high rheological resistance zone and suppresses the central metal flow velocity; the two edge regions in the width direction (corresponding to the profile edges) are provided with lateral deep groove guiding areas, which are deep and extend directly to the edge of the sizing zone, forming a low rheological resistance zone and accelerating the edge fluid supply.
[0045] Understandably, the "shallow and deep trenches" synergistic resistance control structure of the gradually expanding transition section has a contracting "shallow trench zone" in the central area to increase resistance, and a deepening "deep trench zone" on both sides to reduce resistance.
[0046] like Figure 2-4As shown in Figure 9, a structure of a billet moving flow channel is given. The billet moving flow channel includes a feed diversion section 401, a gradually expanding transition section 402, and a sizing extrusion section 403 connected in sequence. The feed diversion section 401 is connected to the second inlet 3, which has an arched structure, and the sizing extrusion section 403 is connected to the outlet 5. The feed diversion section 401, the gradually expanding transition section 402, and the sizing extrusion section 403 are smoothly connected to each other in sequence.
[0047] Understandably, mold 1 has a gradually changing U-shaped through cavity inside, which serves as a flow channel for billet movement. The cavity is arranged through the billet conveying direction, with an arc-shaped arched wall at one end to form the feeding end and a straight open end to form the discharging end. Along the billet conveying direction, the cross-sectional width of the cavity continuously and smoothly widens from the feeding end to the discharging end. The feeding end and discharging end of the cavity are connected to the mold feeding port and discharging port, respectively, forming a continuous through space for billet passage.
[0048] Please refer to Figure 10 , 11 As shown, after the billet enters the gradually changing U-shaped through-cavity from the feed inlet, as the billet moves along the cavity, the cross-section of the extruded profile gradually expands from an arc shape towards both ends, until reaching the sizing extrusion section 403, where the profile cross-section takes on a flat plate-like structure. Compared to extruded products produced by existing technologies, such as... Figure 13 As shown, the extruded product obtained by the present invention has a smooth, flat plate-like structure, while the extruded product obtained by prior art (such as...) Figure 13 As shown, it is uneven, wrinkled, and has surface defects.
[0049] In an optional embodiment of this disclosure, a method for integrated molding using the continuous extrusion die of the present invention is provided, as follows: A method for integral forming of a continuous extrusion die with a non-uniform depth resistance control structure includes the following steps: (1) Material preparation and cleaning: Select aluminum alloy to be cast into cylindrical blanks, use a rotating wire brush to clean the surface oxide layer, and use a dust collection device to increase the surface friction coefficient to prevent slippage; the rotation speed of the rotating wire brush is 300-400 r / min.
[0050] (2) Continuous extrusion molding: The extrusion wheel speed is 6-8 r / min, the die temperature is 500-550℃, the billet enters the die, is split by the central flow divider, and enters the feeding flow divider section and the gradual expansion transition section in sequence. The gradual expansion transition section is provided with a central shallow groove area and a lateral deep groove guide area on both sides of the width direction. This realizes the deceleration of the central shallow groove area and the rapid replenishment of the lateral deep groove guide area, and directly extrudes a flat aluminum billet with a width-to-thickness ratio greater than 20 in one straight extrusion at the sizing extrusion section.
[0051] (3) Online cooling: After extrusion, water spray is used for rapid cooling (cooling to 20-30℃) to shape and refine the grains, and obtain the finished aluminum profile.
[0052] The above forming method reduces the damage and internal stress caused by traditional physical bending. The thickness deviation of the finished aluminum profile is ≤ ±0.02mm, and the surface roughness Ra is ≤ 0.4μm.
[0053] Comparative example: Control group 1: Traditional U-shaped continuous extrusion process.
[0054] Control group 2: Existing splicing gradient unfolding process.
[0055] This invention: Rheological resistance control mold process.
[0056] The performance parameters of this invention and control groups 1 and 2 were compared. The performance parameters included mold structure, extrusion morphology, equipment leakage risk, velocity field distribution, finished product thickness deviation, residual stress / microcracks, and the comparison information was recorded in Table 1.
[0057] Table 1 Comparison of performance index parameters
[0058] As shown in Table 1 above, this invention uses an integrated single-solid mold, overcoming the problems of existing U-shaped outlet single-module and multi-module bolt splicing. The extruded profile is a flat and wide sheet material, requiring no secondary flattening. However, the traditional U-shaped continuous extrusion process produces a U-shaped bend, and the extrusion form of the existing spliced gradual unfolding process is a flat and wide sheet material (e.g. Figure 13 (As shown), and has wrinkles.
[0059] This invention features a one-piece molded structure, which can prevent the risk of material leakage from the equipment. However, both control groups 1 and 2 have the risk of material leakage, and control group 2 has a higher risk of material leakage because it uses a spliced structure, which cannot ensure that the splice gaps are sealed.
[0060] Please refer to Figure 12 As shown, this is the velocity field distribution of the present invention. It can be seen that the present invention exhibits highly parallel color bands and is uniform across the entire cross-section. However, the velocity field distributions of control groups 1 and 2 are uneven. The velocity field distribution of control group 2 is as follows... Figure 14 As shown in the figure, the velocity field distribution of control group 2 exhibits certain velocity oscillations.
[0061] Control group 1 had a finished product thickness deviation ≥ ±0.05 mm, and control group 2 had a finished product thickness deviation of approximately ±0.04 mm. In contrast, the finished profile obtained by this invention has a finished product thickness deviation ≤ ±0.02 mm, significantly lower than control groups 1 and 2. Simultaneously, the profile surface roughness is lower, effectively solving the dimensional fluctuation problem caused by uneven flow velocity in the width direction during the extrusion process of flat aluminum billets with a large width-to-thickness ratio. This significantly improves the profile forming accuracy and surface quality.
[0062] Regarding residual stress and microcracks, control group 1 had higher residual stress, which made it easier for microcracks to be generated in the subsequent flattening process; control group 2 profiles still had a small amount of residual stress and microcracks; the present invention adopts a one-time molding method, the material flow is stable and straight during the extrusion process, the residual stress level inside the profile is low, and the risk of microcracks is low.
[0063] Using the production energy consumption and input of control group 1 as a baseline of 100%, the production energy consumption and input of control group 2 are approximately 90%. By adopting the solution of this invention, the production energy consumption and input are reduced by approximately 20% to 30% compared to control group 1, resulting in lower production costs.
[0064] The above-described embodiments are preferred embodiments of the present invention and are only used to facilitate the illustration of the present invention. They are not intended to limit the present invention in any way. Any person skilled in the art who makes local modifications or alterations to the technical content disclosed in the present invention without departing from the scope of the technical features of the present invention shall still fall within the scope of the technical features of the present invention.
Claims
1. A continuous extrusion die with a non-uniform depth resistance control structure, characterized in that: The mold includes an integrated mold (1), one end of which is provided with a top sink (101) and the other end is provided with a discharge port (5). The bottom of the top sink (101) is provided with a first inlet (2) and a second inlet (3). The bottom surface of the top sink (101) is provided with a central diversion block (4). The first inlet (2) and the second inlet (3) are located on the outer periphery of the central diversion block (4). A guide channel that gradually narrows along the billet feeding direction is formed between the first inlet (2) and the second inlet (3). The second inlet (3) and the discharge port (5) are connected by a billet moving flow channel. The blank moving channel is a through-type unsplit channel formed inside the mold (1); The billet moving channel includes a feed diversion section (401), a gradually expanding transition section (402), and a sizing extrusion section (403) connected sequentially along the billet feeding direction. The flow width of the feed diversion section (401) to the gradually expanding transition section (402) gradually increases along the billet feeding direction. The sizing extrusion section (403) has a sizing cross section corresponding to the discharge port (5).
2. The continuous extrusion die with a non-equal depth resistance control structure according to claim 1, characterized in that: The feed diversion section (401) is formed by a central diversion block and two side channels, and its cross-sectional profile is U-shaped. The bottom surface of the inner cavity of the gradually expanding transition section (402) is a three-dimensional curved surface with a continuously varying depth along the feed direction of the billet. The three-dimensional curved surface includes a central shallow groove area in the middle of the width direction and lateral deep groove guide areas on both sides of the central shallow groove area. The depth of the central shallow groove area is less than the depth of the lateral deep groove guide areas, so that a high rheological resistance area is formed in the middle of the width direction and a low rheological resistance area is formed on both sides. In the longitudinal section along the billet feeding direction and passing through the bottom of the lateral deep groove guide area, the angle between the tangent of the bottom of the deep groove on both sides of the sizing extrusion section (403) and the axial direction of the discharge port (5) is 0 to 5°, and the axial direction of the discharge port (5) is the extrusion sizing axis direction of the sizing extrusion section (403).
3. The continuous extrusion die with a non-equal depth resistance control structure according to claim 1, characterized in that: The second inlet (3) has an arched structure, and the top of the inner arc-shaped side of the second inlet (3) is cut flat to form a straight chord edge (41). The chord edge (41) extends along the width direction of the outlet (5) and corresponds to the position of the central shallow groove area in the width direction.
4. The continuous extrusion die with a non-equal depth resistance control structure according to claim 1, characterized in that: The first inlet (2) and the second inlet (3) are smoothly transitioned by an inclined sidewall, which causes the flow width of the guide channel to gradually decrease from the first inlet (2) to the second inlet (3).
5. The continuous extrusion die with a non-equal depth resistance control structure according to claim 1, characterized in that: The feed axis of the mold (1) is parallel to the extrusion sizing axis of the sizing section (403), and the two axes have an eccentricity e in the vertical direction, 2mm≤e≤5mm.
6. The continuous extrusion die with a non-equal depth resistance control structure according to claim 1, characterized in that: The central diversion block (4) is a wedge-shaped or trapezoidal diversion block. The first inlet (2) and the second inlet (3) are arranged vertically and surround the outer periphery of the central diversion block (4).
7. A method for processing a billet moving flow channel as described in claim 1, characterized in that, Includes the following steps: S1. Using annealed H13 hot work die steel as the blank, a carbide round nose end mill with AlTiN coating is used to mill the blank in layers from the feed end and the discharge end inwards, forming a basic U-shaped flow channel outline. A machining allowance of 0.3-0.5mm is reserved on the inner wall of the flow channel. The milling process parameters are: spindle speed 2400-2800r / min, feed rate 1400-1800mm / min, axial depth of cut 3-4mm, radial width of cut 5-7mm. After rough machining, the blank is subjected to quenching and high-temperature tempering heat treatment to control the hardness to HRC 48-52. S2. Prepare a copper forming electrode that is compatible with the U-shaped flow channel cavity at the feed end, clamp it in an electrical discharge machining tool, extend it into the flow channel from the feed end for electrical discharge machining, and remove the reserved material by instantaneous local high temperature of 8000~12000℃. During the machining process, the electrode and the cavity wall maintain a discharge gap of 0.03~0.05mm. S3. A copper forming electrode matching the flat profile of the discharge end is used to extend into the flow channel from the discharge end for electrical discharge finishing. The machining references at both ends are calibrated by machine tool coordinates so that the cavity machining at the feed end and discharge end can be advanced to the middle of the flow channel and smoothly merged to obtain a smooth and continuous through-type billet moving flow channel.
8. A method for forming a continuous extrusion die for a non-equal depth resistance control structure as described in any one of claims 1-6, characterized in that, Includes the following steps: (1) Material preparation and cleaning: Select aluminum alloy to be cast into cylindrical blanks, use a rotating steel wire brush to clean the surface oxide layer, and use a dust collection device to increase the surface friction coefficient to prevent slipping; (2) Continuous extrusion molding: The extrusion wheel speed is 6-8 r / min, the die temperature is 500-550℃, the billet enters the die, and after being diverted by the central diverting block, it enters the feeding diversion section and the gradual expansion transition section in sequence. The central shallow groove area in the gradual expansion transition section generates a high rheological resistance to the middle billet in the width direction, and the lateral deep groove guiding area generates a low rheological resistance to the billets on both sides in the width direction, so that the billets on both sides are quickly replenished and enter the sizing extrusion section synchronously with the middle billet, and a flat aluminum billet with a width-to-thickness ratio greater than 20 is directly extruded in the sizing extrusion section in one straight step; (3) Online cooling: After extrusion, water spray is used for rapid cooling to shape and refine the grains, resulting in finished aluminum profiles.
9. The continuous extrusion die forming method for a non-equal depth resistance control structure according to claim 8, characterized in that: In step (1), the rotation speed of the wire brush is 300-400 r / min; In step (3), the temperature is cooled to 20-30°C.
10. The continuous extrusion die forming method for a non-equal depth resistance control structure according to claim 8, characterized in that: The thickness deviation of the finished aluminum profile is ≤ ±0.02mm, and the surface roughness Ra is ≤ 0.4μm.
Citation Information
Patent Citations
Gradually expanded die structure for continuous extrusion forming of copper and copper alloy plate strips
CN113134521A