Forging method of TC11 small-diameter bars for tissue blades

By employing a forging method with multi-process collaborative control, the problems of uneven microstructure and high cost of TC11 small-diameter bars have been solved, achieving high yield and excellent mechanical properties, making them suitable for key components such as aero-engine blades.

CN123102894APending Publication Date: 2026-11-17HUNAN GOLDSKY TITANIUM IND TECH CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611455763.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-18
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies for manufacturing small-diameter TC11 bars suffer from insufficient microstructure uniformity and high costs. Traditional processes cannot meet the high reliability requirements of blades and have low yields.

Method used

A forging method with multi-process coordinated control, including ingot forging, recrystallization GSCH forging, two-phase region homogenization forging, sequential forging, and structural annealing, is adopted. By repeatedly switching facets and controlling the temperature of titanium forging, the deformation dead zone and heat loss are reduced, and the uniformity of the microstructure and the yield are improved.

Benefits of technology

It achieves uniform microstructure and significant cost reduction of TC11 small-diameter bars, improves yield, and provides excellent mechanical properties, meeting the high flaw detection requirements of aero-engine blades and broadening the application range.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123102894A_ABST
    Figure CN123102894A_ABST
Patent Text Reader

Abstract

A forging method for TC11 small-diameter bars for blades is disclosed, the method including: (1) ingot forging; (2) recrystallization G-S-C-H forging; (3) two-phase homogenization forging; (4) transition forging; (5) structural annealing of transition bars; (6) radial forging.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the technical field of titanium alloy material processing, and in particular to a forging method for TC11 small-diameter bars used for forming blades. Background Technology

[0002] TC11 titanium alloy (Ti-6.5Al-3.5Mo-1.5Zr-0.3Si) is a high-temperature, high-strength titanium alloy with excellent thermal strength, fatigue performance and fracture toughness. It is widely used in key components such as compressor blades and discs of aero-engines.

[0003] TC11 small-diameter bars (Φ30~100mm) are the core blanks for manufacturing blades. They require uniform microstructure, no obvious anisotropy, fine and uniformly distributed primary α phase, and control of production costs to meet the needs of large-scale production.

[0004] In existing technologies, the manufacturing of small-diameter TC11 bars presents two major challenges: First, insufficient microstructure uniformity. Traditional casting processes easily lead to the formation of coarse β grains and elongated α phases, resulting in residual microstructural defects after forging. This results in significant differences in the transverse and longitudinal microstructure of the bars. Furthermore, the uncontrollable temperature field and deformation stress during the precision forging of small-diameter bars further exacerbate the microstructure inhomogeneity. Since the GJB494A-2008 standard has high requirements for the microstructure and ultrasonic flaw detection clutter levels of TC11 bars (for rotor blades and stator blades), traditional high-low process technology cannot meet the high reliability requirements of the blades. Second, high cost. Traditional processes require multiple high-temperature forging cycles and complex heat treatments. The forging process is prone to cracking (end-end bursting), and the high material wear during grinding leads to low yield and increased costs.

[0005] To address the aforementioned issues, existing technologies, such as the patent titled "A Method for Preparing Small-Diameter Bars of Highly Uniform TC11 Titanium Alloy" (patent number CN202311705061.3), propose a solution of recrystallization and high-temperature homogenization. Although the solution adopts a different "high-low-high-low" alternating deformation mode in a single temperature zone, it does not specifically address the forging details control of TC11 transition billets, the elimination of deformation dead zones, and the uniformity of transition structure. Furthermore, in the two-phase region, this solution still uses conventional methods to gradually elongate large square billets into Φ200 transition round bars through multiple heat treatments. During this process, the bars are not only prone to cracking, but the numerous heat treatments also increase energy and grinding costs, failing to fundamentally resolve the contradiction between poor structural uniformity, excessive costs, and low yield.

[0006] Therefore, there is an urgent need to develop a special forging process that adapts to the multi-element alloying characteristics of TC11, so as to achieve a synergistic improvement in the uniformity of microstructure at the free end of small-diameter bars, low cost, and high yield. Summary of the Invention

[0007] To overcome the shortcomings of the prior art, the technical problem to be solved by the present invention is to provide a forging method for TC11 small-size bars for blades, which can solve the problems of uneven microstructure and high cost of traditional processes, obtain small-size bars with fine and uniform primary α phase, no obvious anisotropy, and excellent flaw detection performance, while reducing production energy consumption and material costs.

[0008] The technical solution of this invention is: a forging method for TC11 small-diameter bars used for tissue blades, comprising the following steps: (1) Ingot forging: The TC11 titanium alloy ingot with a diameter of Φ680mm is heated at 1150~1200℃ for a long time, and the heating time is not less than 1500min. Then it is upsetting and drawing into a square billet in 1~2 heats on a 45MN fast forging machine, and then air-cooled. (2) Recrystallization GSCH forging: (2.1) The billet from step (1) is upsetting and drawing in one heat at 30~60℃ below the β transformation temperature to a billet of 400~600, and then immediately returned to the furnace after forging; (2.2) The billet is held at 40~60℃ above the β transformation temperature for about 90~120 minutes, and then upsetting and drawing in one heat to a billet, and then cooled in a way that is slightly faster than air cooling after forging; (3) Two-phase region homogenization forging: The billet completed in step (2) is subjected to multiple face switching operations at 30~60℃ below the β transformation temperature. The billet is forged from octagon to square, then back to octagon, and finally forged to a 400~500 hexagonal billet through upsetting or drawing operations. (4) Forging in sequence: The forging billet completed in step (3) is forged in multiple passes using a large precision forging machine, and finally made into a Φ160~200 transfer bar with an overall deformation of not less than 50%; (5) Structural annealing of the transition bar: Place the transition round bar completed in step (4) in a box-type resistance furnace and hold it at 30~60℃ below the β transition temperature for 60~90min, then remove it from the furnace and air cool it. (6) Radial forging: The transformed bar completed in step (5) is kept at 30~60℃ below the β transformation temperature for a period of time, and then radial forging is carried out on the SKK17 precision forging machine for 1~2 fires. The deformation of the billet in a single fire is about 70~80%, and the deformation in a single pass is no more than 25%. Finally, it is forged into finished bar with a specification of 70 or above.

[0009] Compared with the prior art, the present invention has the following beneficial effects:

[0010] 1. Cost reduction and efficiency improvement: Under the premise of repeated facet switching, reducing the deformation dead zone and ensuring the uniformity of the structure, the number of cold material heats is reduced by hot material remelting through multiple heats, and the anisotropy of the structure that may be increased by drawing heats is reduced by large precision forging. While reducing the total energy consumption of production, the production cycle is shortened, and the processing cost per piece is reduced by more than 15%. The cost reduction effect is significantly better than the average reduction of 10% for general titanium alloys.

[0011] 2. Temperature-controlled titanium forging significantly improves yield: By strictly controlling the forging parameters to match the billet reduction and feed rate, the forging time is shortened while ensuring sufficient deformation, achieving temperature-controlled titanium forging. By wrapping the ends with lattice asbestos, heat loss during deformation is reduced. At the same time, the head and bottom reversal avoids repeated deformation in local areas. By controlling variables, the uncertainty caused by the temperature and stress fields is reduced, thereby reducing the occurrence of end-blowing and surface and internal micro-cracks in the billet during the forging process. Compared with traditional processes, it avoids multiple forging stops for grinding and the material loss from sawing the ends after end-blowing. Grinding loss is reduced from over 30% to below 15%, and the product yield is steadily increased from 70% to over 75%, significantly improving material utilization.

[0012] 3. Achieving highly homogenized and refined product structure, with mechanical properties superior to conventional processes, and flaw detection performance meeting the stringent requirements of blade standards: Through multi-process coordinated control of high-temperature homogenization in billet preparation + large deformation + recrystallization + two-phase region homogenization forging + sequential forging + structural annealing + radial forging, especially by utilizing multiple reversing upsetting below the phase transformation point, coarse β grains and casting defects are effectively broken and eliminated. This process transfers deformation uniformity from large-size billets to small-size finished products, obtaining a microstructure with fine and uniform primary α phase, no obvious anisotropy, and no inherited structural defects, fully meeting the high flaw detection and microstructure requirements of GJB494A-2008 standard for blade rods.

[0013] 4. Promising application prospects: It broadens the application range of TC11 titanium alloy, overcomes the common technical problem in the industry that traditional processes cannot achieve both high uniformity and low cost, and produces small-sized TC11 bars with excellent internal structure, high surface quality, and excellent batch consistency. It is particularly suitable for key load-bearing components such as compressor blades of aero-engines. Attached Figure Description

[0014] Figure 1The images show the microstructures of TC11 small-diameter bars of different sizes obtained in Examples 1, 2, and 3. (a) is a microstructure image of the edge portion of the head cross-section of a Φ70mm bar; (b) is a microstructure image of the core portion of the head cross-section of a Φ70mm bar; (c) is a microstructure image of the edge portion of the head cross-section of a Φ85mm bar; (d) is a microstructure image of the core portion of the head cross-section of a Φ85mm bar; (e) is a microstructure image of the edge portion of the head cross-section of a Φ100mm bar; and (f) is a microstructure image of the core portion of the head cross-section of a Φ100mm bar.

[0015] Figure 2 This is a flowchart illustrating the forging method of TC11 small-diameter bars for the tissue blades according to the present invention. Detailed Implementation

[0016] like Figure 2 As shown, a forging method for small-diameter TC11 bars used for tissue blades includes the following steps: (1) Ingot forging: The TC11 titanium alloy ingot with a diameter of Φ680mm is heated at 1150~1200℃ for a long time, and the heating time is not less than 1500min. Then it is upsetting and drawing into a square billet in 1~2 heats on a 45MN fast forging machine, and then air-cooled. (2) Recrystallization GSCH forging: (2.1) The billet from step (1) is upsetting and drawing in one heat at 30~60℃ below the β transformation temperature to a billet of 400~600, and then immediately returned to the furnace after forging; (2.2) The billet is held at 40~60℃ above the β transformation temperature for about 90~120 minutes, and then upsetting and drawing in one heat to a billet, and then cooled in a way that is slightly faster than air cooling after forging; (3) Two-phase region homogenization forging: The billet completed in step (2) is subjected to multiple face switching operations at 30~60℃ below the β transformation temperature. The billet is forged from octagon to square, then back to octagon, and finally forged to a 400~500 hexagonal billet through upsetting or drawing operations. (4) Forging in sequence: The forging billet completed in step (3) is forged in multiple passes using a large precision forging machine, and finally made into a Φ160~200 transfer bar with an overall deformation of not less than 50%; (5) Structural annealing of the transition bar: Place the transition round bar completed in step (4) in a box-type resistance furnace and hold it at 30~60℃ below the β transition temperature for 60~90min, then remove it from the furnace and air cool it. (6) Radial forging: The transformed bar completed in step (5) is kept at 30~60℃ below the β transformation temperature for a period of time, and then radial forging is carried out on the SKK17 precision forging machine for 1~2 fires. The deformation of the billet in a single fire is about 70~80%, and the deformation in a single pass is no more than 25%. Finally, it is forged into finished bar with a specification of 70 or above.

[0017] Compared with the prior art, the present invention has the following beneficial effects:

[0018] 1. Cost reduction and efficiency improvement: Under the premise of repeated facet switching, reducing the deformation dead zone and ensuring the uniformity of the structure, the number of cold material heats is reduced by hot material remelting through multiple heats, and the anisotropy of the structure that may be increased by drawing heats is reduced by large precision forging. While reducing the total energy consumption of production, the production cycle is shortened, and the processing cost per piece is reduced by more than 15%. The cost reduction effect is significantly better than the average reduction of 10% for general titanium alloys.

[0019] 2. Temperature-controlled titanium forging significantly improves yield: By strictly controlling the forging parameters to match the billet reduction and feed rate, the forging time is shortened while ensuring sufficient deformation, achieving temperature-controlled titanium forging. By wrapping the ends with lattice asbestos, heat loss during deformation is reduced. At the same time, the head and bottom reversal avoids repeated deformation in local areas. By controlling variables, the uncertainty caused by the temperature and stress fields is reduced, thereby reducing the occurrence of end-blowing and surface and internal micro-cracks in the billet during the forging process. Compared with traditional processes, it avoids multiple forging stops for grinding and the material loss from sawing the ends after end-blowing. Grinding loss is reduced from over 30% to below 15%, and the product yield is steadily increased from 70% to over 75%, significantly improving material utilization.

[0020] 3. Achieving highly homogenized and refined product structure, with mechanical properties superior to conventional processes, and flaw detection performance meeting the stringent requirements of blade standards: Through multi-process coordinated control of high-temperature homogenization in billet preparation + large deformation + recrystallization + two-phase region homogenization forging + sequential forging + structural annealing + radial forging, especially by utilizing multiple reversing upsetting below the phase transformation point, coarse β grains and casting defects are effectively broken and eliminated. This process transfers deformation uniformity from large-size billets to small-size finished products, obtaining a microstructure with fine and uniform primary α phase, no obvious anisotropy, and no inherited structural defects, fully meeting the high flaw detection and microstructure requirements of GJB494A-2008 standard for blade rods.

[0021] 4. Promising application prospects: It broadens the application range of TC11 titanium alloy, overcomes the common technical problem in the industry that traditional processes cannot achieve both high uniformity and low cost, and produces small-sized TC11 bars with excellent internal structure, high surface quality, and excellent batch consistency. It is particularly suitable for key load-bearing components such as compressor blades of aero-engines.

[0022] Preferably, in step (1), the ingot blanking adopts two upsetting and two drawing, the upsetting and drawing method is straight upsetting and straight drawing, the final square billet shape is octagonal, the single-fire upsetting deformation is about 40~45%, and it is air-cooled after forging.

[0023] Preferably, in step (2.1), the upsetting and drawing process is carried out one upsetting and one drawing at a time, with an upsetting deformation of about 10-20%, and the final shape is octagonal, and the material is returned to the furnace after forging; in step (2.2), the upsetting and drawing process is carried out one upsetting and one drawing at a time, with an upsetting deformation of about 35-40%, and the cooling method after forging is faster than air cooling, with a cooling rate of 3.5℃ / min.

[0024] Preferably, in step (3), the material is subjected to upsetting-drawing-reversing operation in the two-phase zone, and the cycle is repeated 2 to 3 times. The upsetting deformation in a single fire is about 35%. The material facet switching operation is ◇→□→◇. Each time the material is upsetting and drawing, dot matrix asbestos is wrapped around both ends of the billet. When the material is drawn, the first two passes are full anvil feeding, and the pressing amount is controlled at about 80 to 120 mm. The material is drawn from operation A to operation B. After one pass, the head and bottom of the billet are interchanged, and the next upsetting-drawing-reversing operation is performed. Finally, the billet is forged into a sixteen-square billet.

[0025] Preferably, in steps (2), (3), and (4), the heating and heat preservation time of the material is the minimum cross-sectional size of the billet × (0.5~0.8) min.

[0026] Preferably, in step (4), the deformation amount of each pass of the precision forging is controlled at 10-15%, and the total deformation amount is controlled at 75-85%.

[0027] Preferably, in step (5), the transition bar adopts a three-stage heating curve, preheating in the furnace in the range of 800~850℃, then heating to 30~60℃ below the β transformation temperature and holding for 120~150min, with the heating rate controlled at 5℃ / min, then slowly cooling out of the furnace, with the cooling rate controlled at 3℃ / min, until cooled to room temperature.

[0028] Preferably, in step (6), the forging frequency during radial forging is controlled at 450~600 min, and the forging speed is controlled at 3.5 m / min.

[0029] The specific embodiments of the present invention are described in more detail below.

[0030] Material: Φ680mm TC11 titanium alloy ingot, measured β phase transformation temperature Tβ=1000℃. Example 1: Preparation of Φ70mm TC11 small-diameter bars

[0031] Ingot forging: After uniformly coating the Φ680mm TC11 titanium alloy ingot with a high-temperature anti-oxidation coating, it is placed in a chamber electric heating furnace and heated to 1200℃. It is held for 25 hours to eliminate compositional segregation. Then, it is subjected to one heat, two upsetting and two drawing operations on a 45MN high-speed forging machine. After forging, it is air-cooled. The upsetting deformation is 40%. The Φ680mm ingot is forged into an octagonal billet with a side distance of 540mm to break up the as-cast grains.

[0032] Recrystallization (GSCH) forging: First, the blank material is loaded into the furnace and heated to 950℃ (Tβ-50℃), held for 360 minutes, and then subjected to a one-upset-one-drawing operation to forge the octagonal blank with a side length of 540mm into an octagonal blank with a side length of 540mm. The upsetting deformation is 20%. Then, the hot material is returned to the furnace and held at 1050℃ (Tβ+50℃) for 90 minutes. After being taken out of the furnace, a one-upset-one-drawing operation is performed to refine the grains and improve the uniformity of the structure, forging the octagonal blank with a side length of 540mm into an octagonal blank with a side length of 450mm. The upsetting deformation is 40%. After forging, the blank is rapidly cooled. When it is taken out of the furnace, a fan can be used to blow on the upper and lower surfaces of the blank, and the cooling rate is controlled at 3.5℃ / min until it is cooled to room temperature.

[0033] Two-phase homogenization forging: The crystallized billet is heated at 950℃ (Tβ-50℃). After exiting the furnace, a one-upset-one-drawing reversal operation (shaft upset and side draw) is performed. Before upsetting and drawing, the end is covered with lattice asbestos. After upsetting, at the beginning of drawing, a large reduction (100mm) and a large feed (300~450mm) are matched. After one pass, the head and bottom are turned around for drawing. The billet after one upset and drawing is a square billet with a side-to-side distance of 500mm. After forging, it is returned to the furnace for 90 minutes. After exiting the furnace, a one-upset-one-drawing reversal operation (side upset and shaft draw) is performed. The billet after the second upset and drawing is an octagonal billet with a side-to-side distance of 540mm. After forging, it is air-cooled. During this period, the upsetting deformation is 35%. Then, the above steps are repeated 1~2 times. Finally, it is drawn to a sixteen-square billet with a side-to-side distance of 400mm.

[0034] Transition forging: The cold material after rapid forging is loaded into the furnace, heated to 950℃ (Tβ-50℃), held for 270 minutes, and then removed from the furnace to begin deformation processing; 5 passes of continuous forging are used, with a deformation amount of 25% per pass and a total deformation amount of 79%, to forge a transition billet bar with a diameter of Φ200mm.

[0035] Structural annealing of trans-order bar stock: The trans-order round bar stock is placed in a box-type resistance furnace and preheated in the range of 800~850℃ using a three-stage heating curve. Then, it is heated to 950℃ (Tβ-50℃) and held for 120~150 min, with the heating rate controlled at 5℃ / min. After that, it is taken out of the furnace and slowly cooled at a rate controlled at 3℃ / min until it reaches room temperature.

[0036] Radial forging: The annealed transfer bar is held at 950℃ (Tβ-50℃) for 120~150min, and then subjected to two radial forgings on an SKK17 precision forging machine. The total deformation of each forging is controlled at about 55% and 70% respectively. The first forging produces a round bar with a diameter of 135, and the second forging produces a finished round bar. The deformation per pass in each forging is no more than 25%. The forging frequency during radial forging is controlled at 450~600min, and the forging speed is controlled at 3.5m / min. Example 2: Preparation of Φ85mm TC11 small-diameter bars

[0037] Ingot forging: After uniformly coating the Φ680mm TC11 titanium alloy ingot with a high-temperature anti-oxidation coating, it is placed in a chamber electric heating furnace and heated to 1200℃. It is held for 25 hours to eliminate compositional segregation. Then, it is subjected to one heat, two upsetting and two drawing operations on a 45MN high-speed forging machine. After forging, it is air-cooled. The upsetting deformation is 40%. The Φ680mm ingot is forged into an octagonal billet with a side distance of 540mm to break up the as-cast grains.

[0038] Recrystallization (GSCH) forging: First, the blank material is loaded into the furnace and heated to 950℃ (Tβ-50℃), held for 360 minutes, and then subjected to a one-upset-one-drawing operation to forge the octagonal blank with a side length of 540mm into an octagonal blank with a side length of 540mm. The upsetting deformation is 20%. Then, the hot material is returned to the furnace and held at 1050℃ (Tβ+50℃) for 90 minutes. After being taken out of the furnace, a one-upset-one-drawing operation is performed to refine the grains and improve the uniformity of the structure, forging the octagonal blank with a side length of 540mm into an octagonal blank with a side length of 450mm. The upsetting deformation is 40%. After forging, the blank is rapidly cooled. When it is taken out of the furnace, a fan can be used to blow on the upper and lower surfaces of the blank, and the cooling rate is controlled at 3.5℃ / min until it is cooled to room temperature.

[0039] Two-phase homogenization forging: The crystallized billet is heated at 950℃ (Tβ-50℃). After exiting the furnace, a one-upset-one-drawing reversal operation (shaft upset and side draw) is performed. Before upsetting and drawing, the end is covered with lattice asbestos. After upsetting, at the beginning of drawing, a large reduction (100mm) and a large feed (300~450mm) are matched. After one pass, the head and bottom are turned around for drawing. The billet after one upset and drawing is a square billet with a side-to-side distance of 500mm. After forging, it is returned to the furnace for 90 minutes. After exiting the furnace, a one-upset-one-drawing reversal operation (side upset and shaft draw) is performed. The billet after the second upset and drawing is an octagonal billet with a side-to-side distance of 540mm. After forging, it is air-cooled. During this period, the upsetting deformation is 35%. Then, the above steps are repeated 1~2 times. Finally, it is drawn to a sixteen-square billet with a side-to-side distance of 400mm.

[0040] Transition forging: The cold material after rapid forging is loaded into the furnace, heated to 950℃ (Tβ-50℃), held for 270 minutes, and then removed from the furnace to begin deformation processing; 5 passes of continuous forging are used, with a deformation amount of 25% per pass and a total deformation amount of 79%, to forge a transition billet bar with a diameter of Φ200mm.

[0041] Structural annealing of trans-order bar stock: The trans-order round bar stock is placed in a box-type resistance furnace and preheated in the range of 800~850℃ using a three-stage heating curve. Then, it is heated to 950℃ (Tβ-50℃) and held for 120~150 min, with the heating rate controlled at 5℃ / min. After that, it is taken out of the furnace and slowly cooled at a rate controlled at 3℃ / min until it reaches room temperature.

[0042] Radial forging: The annealed transfer bar is held at 950℃ (Tβ-50℃) for 120~150min, and then subjected to two radial forgings on an SKK17 precision forging machine. The total deformation of each forging is controlled at about 35% and 70% respectively. The first forging produces a round bar with a diameter of 160mm, and the second forging produces a finished round bar. The deformation per pass in each forging is no more than 25%. The forging frequency during radial forging is controlled at 450~600min, and the forging speed is controlled at 3.5m / min. Example 3: Preparation of Φ100mm TC11 small-diameter rods

[0043] Ingot forging: After uniformly coating the Φ680mm TC11 titanium alloy ingot with a high-temperature anti-oxidation coating, it is placed in a chamber electric heating furnace and heated to 1200℃. It is held for 25 hours to eliminate compositional segregation. Then, it is subjected to one heat, two upsetting and two drawing operations on a 45MN high-speed forging machine. After forging, it is air-cooled. The upsetting deformation is 40%. The Φ680mm ingot is forged into an octagonal billet with a side distance of 540mm to break up the as-cast grains.

[0044] Recrystallization (GSCH) forging: First, the blank material is loaded into the furnace and heated to 950℃ (Tβ-50℃), held for 360 minutes, and then subjected to a one-upset-one-drawing operation to forge the octagonal blank with a side length of 540mm into an octagonal blank with a side length of 540mm. The upsetting deformation is 20%. Then, the hot material is returned to the furnace and held at 1050℃ (Tβ+50℃) for 90 minutes. After being taken out of the furnace, a one-upset-one-drawing operation is performed to refine the grains and improve the uniformity of the structure, forging the octagonal blank with a side length of 540mm into an octagonal blank with a side length of 450mm. The upsetting deformation is 40%. After forging, the blank is rapidly cooled. When it is taken out of the furnace, a fan can be used to blow on the upper and lower surfaces of the blank, and the cooling rate is controlled at 3.5℃ / min until it is cooled to room temperature.

[0045] Two-phase homogenization forging: The crystallized billet is heated at 950℃ (Tβ-50℃). After exiting the furnace, a one-upset-one-drawing reversal operation (shaft upset and side draw) is performed. Before upsetting and drawing, the end is covered with lattice asbestos. After upsetting, at the beginning of drawing, a large reduction (100mm) and a large feed (300~450mm) are matched. After one pass, the head and bottom are turned around for drawing. The billet after one upset and drawing is a square billet with a side-to-side distance of 500mm. After forging, it is returned to the furnace for 90 minutes. After exiting the furnace, a one-upset-one-drawing reversal operation (side upset and shaft draw) is performed. The billet after the second upset and drawing is an octagonal billet with a side-to-side distance of 540mm. After forging, it is air-cooled. During this period, the upsetting deformation is 35%. Then, the above steps are repeated 1~2 times. Finally, it is drawn to a sixteen-square billet with a side-to-side distance of 400mm.

[0046] Transition forging: The cold material after rapid forging is loaded into the furnace, heated to 950℃ (Tβ-50℃), held for 270 minutes, and then removed from the furnace to begin deformation processing; 5 passes of continuous forging are used, with a deformation amount of 25% per pass and a total deformation amount of 79%, to forge a transition billet bar with a diameter of Φ200mm.

[0047] Structural annealing of trans-order bar stock: The trans-order round bar stock is placed in a box-type resistance furnace and preheated in the range of 800~850℃ using a three-stage heating curve. Then, it is heated to 950℃ (Tβ-50℃) and held for 120~150 min, with the heating rate controlled at 5℃ / min. After that, it is taken out of the furnace and slowly cooled at a rate controlled at 3℃ / min until it reaches room temperature.

[0048] Radial forging: The annealed transfer bar is held at 950℃ (Tβ-50℃) for 120~150min, and then radial forging is performed on an SKK17 precision forging machine with a total deformation of 70%. The deformation per pass per forging is no more than 25%. The forging frequency during radial forging is controlled at 450~600min, and the forging speed is controlled at 3.5m / min.

[0049] The mechanical properties of the TC11 small-diameter bars with diameters of Φ70mm, Φ85mm, and Φ100mm prepared by this invention are shown in Table 1. They fully meet the requirements of the GJB494A-2008 standard and have sufficient margin.

[0050] Table 1

[0051] The microstructure is fine and uniform with minimal edge-to-center differences, and there are no coarse or elongated α phases. It has excellent flaw detection performance, and the clutter can reach Φ0.8-9~12dB, which fully meets the stringent requirements for use in aero-engine components.

[0052] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention in any way. Any simple modifications, equivalent changes, and alterations made to the above embodiments based on the technical essence of the present invention shall still fall within the protection scope of the present invention.

Claims

1. A forging method for small-diameter TC11 bars used for tissue blades, characterized in that: It includes the following steps: (1) Ingot forging: The TC11 titanium alloy ingot with a diameter of Φ680mm is heated at 1150~1200℃ for a long time, and the heating time is not less than 1500min. Then it is upsetting and drawing into a square billet in 1~2 heats on a 45MN fast forging machine, and then air-cooled. (2) Recrystallization GSCH forging: (2.1) The billet from step (1) is upsetting and drawing in one heat at 30~60℃ below the β transformation temperature to a billet of 400~600, and then immediately returned to the furnace after forging; (2.2) The billet is held at 40~60℃ above the β transformation temperature for about 90~120 minutes, and then upsetting and drawing in one heat to a billet, and then cooled in a way that is slightly faster than air cooling after forging; (3) Two-phase region homogenization forging: The billet completed in step (2) is subjected to multiple facet switching operations at 30~60℃ below the β transformation temperature. The billet is forged from octagon to square, then back to octagon, and finally forged to a 400~500 hexagonal billet through upsetting or drawing operations. (4) Forging in sequence: The forging billet completed in step (3) is forged in multiple passes using a large precision forging machine, and finally a Φ160~200 transfer bar is produced, with an overall deformation of not less than 50%; (5) Structural annealing of the transition bar: Place the transition round bar completed in step (4) in a box-type resistance furnace and hold it at 30~60℃ below the β transition temperature for 60~90min, then remove it from the furnace and air cool it. (6) Radial forging: The transformed bar completed in step (5) is kept at 30~60℃ below the β transformation temperature for a period of time, and then radial forging is carried out on the SKK17 precision forging machine for 1~2 fires. The deformation of the billet in a single fire is about 70~80%, and the deformation in a single pass is no more than 25%. Finally, it is forged into finished bar with a specification of 70 or above.

2. The forging method for TC11 small-diameter bars for tissue blades according to claim 1, characterized in that: In step (1), the ingot blanking adopts two upsetting and two drawing, the upsetting and drawing method is straight upsetting and straight drawing, the final square billet shape is octagonal, the single-fire upsetting deformation is about 40~45%, and it is air-cooled after forging.

3. The forging method for TC11 small-diameter bars for tissue blades according to claim 2, characterized in that: In step (2.1), upsetting and drawing are performed one upsetting and one drawing at a time, with upsetting deformation of about 10-20%, and the final shape is octagonal. The material is then returned to the furnace after forging. In step (2.2), upsetting and drawing are performed one upsetting and one drawing at a time, with upsetting deformation of about 35-40%. The material is cooled after forging at a rate faster than air cooling, with a cooling rate of 3.5℃ / min.

4. The forging method for TC11 small-diameter bars for tissue blades according to claim 3, characterized in that: In step (3), the material is subjected to upsetting-drawing-reversing operation in the two-phase zone, and the cycle is repeated 2 to 3 times. The upsetting deformation in a single fire is about 35%. The material facet switching operation is ◇→□→◇. Each time the material is upsetting and drawing, dot matrix asbestos is wrapped around both ends of the billet. When the material is drawn, the first two passes are full anvil feeding, and the pressing amount is controlled at about 80 to 120 mm. The material is drawn from operation A to operation B. After one pass, the head and bottom of the billet are interchanged, and the next upsetting-drawing-reversing operation is carried out. Finally, it is forged into a sixteen-square billet.

5. The forging method for TC11 small-diameter bars for tissue blades according to claim 4, characterized in that: In steps (2), (3), and (4), the heating and heat preservation time of the material is the minimum cross-sectional size of the billet × (0.5~0.8) min.

6. The forging method for TC11 small-diameter bars for tissue blades according to claim 5, characterized in that: In step (4), the deformation amount of each pass of the precision forging is controlled at 10-15%, and the total deformation amount is controlled at 75-85%.

7. The forging method for TC11 small-diameter bars for tissue blades according to claim 6, characterized in that: In step (5), the transition bar adopts a three-stage heating curve, preheating in the furnace in the range of 800~850℃, then heating to 30~60℃ below the β transformation temperature and holding for 120~150min, with the heating rate controlled at 5℃ / min, then slowly cooling out of the furnace, with the cooling rate controlled at 3℃ / min, until cooled to room temperature.

8. The forging method for TC11 small-diameter bars for tissue blades according to claim 7, characterized in that: In step (6), the forging frequency during radial forging is controlled at 450~600 min, and the forging speed is controlled at 3.5 m / min.

Citation Information

Patent Citations

  • A method for preparing high-uniform TC11 titanium alloy small-size bars

    CN117444117B