A calcium zirconate-based ceramic core, its preparation method, and its application
By leveraging the synergistic effect of calcium citrate precursor with Isobam600, Isobam104, and yttrium sol, the problems of slurry dispersion stability and core removal in calcium zirconate-based ceramic cores were solved, enabling the preparation of high-performance ceramic cores suitable for precision casting of titanium alloys.
Patent Information
- Application Number
- CN202611197337.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-07
- Publication Date
- 2026-11-17
AI Technical Summary
The existing Isobam water-based gel system has problems in preparing calcium zirconate-based ceramic cores, such as poor slurry dispersion stability, easy agglomeration and sedimentation of powder, poor water collapse of sintered cores, and difficulty in core removal after casting.
A calcium citrate precursor was used to achieve ionic-level uniform dispersion of the calcium source. A composite gel network was constructed by combining Isobam600 and Isobam104. Yttrium oxide components were introduced through yttrium sol to form a hydrated lime phase, which solved the problems of insufficient slurry dispersion stability and difficulty in core removal.
Stable preparation of high solids content slurry was achieved, resulting in gel-cured molding and high-performance sintered bodies with high integrity. These sintered bodies possess excellent mechanical properties and water-collapse core-removal performance, simplifying the production process and improving the yield.
Smart Images

Figure CN123102931A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of ceramic core preparation technology, specifically to a calcium zirconate-based ceramic core, its preparation method, and its application. Background Technology
[0002] In the precision casting of titanium alloys, ceramic cores, as the core components for forming complex internal cavities, must simultaneously meet the requirements of high temperature resistance, low titanium reactivity, high dimensional accuracy, and easy core removal. Calcium zirconate ceramics, due to their excellent high-temperature stability, low titanium reactivity, wear resistance, and thermal shock resistance, are considered ideal candidate materials for ceramic cores in the precision casting of titanium alloys and have attracted widespread attention.
[0003] Gel casting, a green and net-size ceramic molding technology, utilizes in-situ chemical reactions within the slurry to form a three-dimensional polymer network structure, achieving uniform fixation of ceramic particles and enabling the preparation of high-density ceramic green bodies with complex shapes. This technology boasts a short molding cycle, reliable green body performance, and high dimensional accuracy, facilitating industrial-scale mass production. In recent years, novel water-based gel systems, represented by isobutylene-maleic anhydride copolymer (Isobam), have attracted widespread attention in the field of ceramic gel casting. Existing technology employs a composite Isobam water-based gel system using Isobam 600 as a dispersant and Isobam 104 as a gelling agent, successfully preparing silicon nitride ceramics through gel casting. This system requires no additional initiators or catalysts, and the sintered silicon nitride ceramics prepared achieve a flexural strength of up to 454 MPa. However, this system is mainly applicable to non-oxide ceramic systems such as silicon nitride. When it is directly used to prepare calcium zirconate-based ceramic cores, the following technical problems exist: On the one hand, the surface charge characteristics of calcium zirconate powder are significantly different from those of materials such as alumina. The existing Isobam dispersion mechanism is difficult to achieve efficient and stable dispersion of calcium zirconate powder, resulting in poor slurry dispersion stability and easy agglomeration and sedimentation of powder particles, leading to uneven distribution of green body components, which in turn affects the limited mechanical properties of the ceramic core after sintering. On the other hand, the ceramic cores prepared with the existing Isobam characteristics have insufficient water collapse resistance, making core removal after casting difficult and seriously affecting the molding qualification rate. Summary of the Invention
[0004] To address the shortcomings of existing technologies, this invention provides a calcium zirconate-based ceramic core, its preparation method, and its application. The invention involves mixing and grinding citric acid monohydrate and calcium acetate to prepare a calcium citrate precursor, which is then mixed with Isobam 600, Isobam 104, and yttrium sol and ball-milled. The resulting slurry is degassed under vacuum and injected into a mold, followed by curing, demolding, drying, binder removal, and high-temperature sintering to obtain the calcium zirconate-based ceramic core. This invention achieves uniform ionic dispersion of the calcium source using the calcium citrate precursor and avoids slurry defects caused by free calcium ions. The material flocculation method utilizes a composite structure of Isobam 600 and Isobam 104 to construct a water-based network structure that combines dispersion and gel enhancement functions. Yttrium oxide components are introduced through yttrium sol and form a hydrateable lime phase after sintering. This method solves the shortcomings of existing Isobam systems, such as poor slurry dispersion stability and easy powder agglomeration and sedimentation. At the same time, it overcomes the process defects of poor water collapse properties of sintered cores and difficulty in core removal after casting. Thus, it achieves the integrated preparation of calcium zirconate-based ceramic cores with high solid content slurry stability and excellent mechanical properties and water collapse core removal performance.
[0005] To achieve the above objectives, the technical solution adopted by the present invention is as follows: The first objective of this invention is to provide a method for preparing a calcium zirconate-based ceramic core, comprising the following steps: S1. Slurry preparation: Citric acid monohydrate and calcium acetate are mixed and ground to obtain calcium citrate precursor; Isobam600 powder, NH3·H2O and water are mixed to obtain premixed solution; calcium citrate precursor, premixed solution, calcium zirconate powder, Isobam104 powder and yttrium sol are mixed and ball-milled to obtain slurry.
[0006] Calcium acetate exhibits extremely high solubility in water, exceeding that of common calcium salts. This high solubility ensures uniform contact between calcium ions and citrate ions in the liquid phase, facilitating a complete chelation reaction. Acetate ions readily undergo thermal decomposition during subsequent binder removal and sintering processes, being discharged with volatile products, thus reducing the adverse effects of residual anionic impurities on the ceramic core's performance. Using calcium acetate as the calcium source improves the uniformity of the precursor composition and the stability of the slurry system, thereby enhancing the molding quality of calcium zirconate-based ceramic cores.
[0007] S2. Gel curing molding: After vacuum degassing, the slurry is injected into the mold, cured and molded, then demolded and dried to obtain a calcium zirconate-based ceramic green body.
[0008] S3. Sintering and forming: The calcium zirconate-based ceramic green body is debinded to obtain a green body; then the green body is sintered to obtain a calcium zirconate-based ceramic core.
[0009] Preferably, the solid content of calcium zirconate powder in the slurry is 30%~50%; based on the mass of calcium zirconate powder (aggregate powder), the addition amount of calcium citrate is 0.6wt%, the addition amount of Isobam 600 powder is 0.1wt%~1wt%, the addition amount of Isobam 104 powder is 0.3wt%, and the addition amount of yttrium sol is 1.0wt%~5.0wt%. Pure zirconium oxide undergoes a crystal phase transformation during heating, accompanied by volume changes, which easily leads to ceramic cracking and difficulty in core removal. This invention selects calcium zirconate as aggregate to stabilize the crystal structure, while introducing calcium citrate and yttrium sol to synergistically improve the structural stability and water collapse resistance of the calcium zirconate-based ceramic core.
[0010] Aggregate powder is the main material of ceramic core. After sintering, it forms a ceramic skeleton mainly composed of calcium zirconate, which endows the calcium zirconate-based ceramic core with high temperature resistance, dimensional stability and resistance to molten metal corrosion. Its solid content is preferably 30%~50%, which aims to balance the fluidity of the slurry and the molding strength of the green body. When the solid content is less than 30%, there is too much water in the slurry, resulting in large drying shrinkage, low green body strength, and easy cracking or deformation. When the solid content is higher than 50%, the viscosity of the slurry increases significantly, the fluidity becomes poor, and it is easy to generate bubbles, agglomerate and incomplete filling of the mold.
[0011] Introducing calcium citrate as a calcium source precursor into the system serves two purposes: firstly, it facilitates the uniform distribution of the calcium source in the slurry, avoiding the direct introduction of large amounts of free calcium ions that could cause flocculation; secondly, it decomposes during subsequent binder removal and sintering processes to generate calcium-related components, participating in the formation of the ceramic skeleton and regulating the pore structure, thus improving the post-cast core removal performance of calcium zirconate-based ceramic cores. The preferred addition amount is 0.6 wt% of the calcium zirconate powder mass. This amount provides a suitable calcium source without significantly increasing slurry viscosity or disrupting the stability of the Isobam gel system. If the addition amount is too low, the calcium source regulation effect is not significant, and the improvement on pore structure and core removal performance is limited; if the addition amount is too high, it can easily lead to decreased slurry stability, local agglomeration, and an increase in calcium-rich phases after firing, thereby affecting the strength and dimensional stability of the calcium zirconate-based ceramic core.
[0012] Isobam 600 primarily functions as a dispersant and auxiliary gelling agent. In the presence of ammonia and water, Isobam 600 forms a water-soluble polymer system containing carboxylates, which adsorbs onto the surface of aggregate powder, improving the dispersion stability of the powder in water-based slurries, reducing the risk of agglomeration and sedimentation, and ensuring good flowability of the slurry even at high solid content. Its preferred addition amount is 0.1wt%~1wt% of the aggregate mass. Below 0.1wt%, the adsorption and dispersion effect on the powder surface is insufficient, leading to easy sedimentation and flocculation of the slurry, and unstable setting time and green body uniformity. Above 1wt%, the organic content increases, the slurry viscosity rises, flowability decreases, and the subsequent binder removal burden increases, easily causing defects such as pores, cracks, or residual carbon.
[0013] Isobam 104 primarily functions as a gel molding and wet preform reinforcement component, forming a water-based composite Isobam gel system together with Isobam 600. Its role is to form a gel network of sufficient strength after injection molding, improving the structural integrity of the wet preform and enabling smooth demolding, handling, and drying. Its addition amount is fixed at 0.3 wt% of the aggregate mass, aiming to ensure gel curing strength while controlling the total amount of organic matter. If the addition amount is too low, the wet preform strength is insufficient, making it prone to collapse, edge chipping, or cracking during demolding; if it is too high, the slurry viscosity increases, the injection molding fluidity deteriorates, and the amount of organic matter decomposition increases during the glue removal process, easily causing cracking or post-firing defects in the preform.
[0014] The addition amount of yttrium sol is 1.0 wt% to 5.0 wt% of the calcium zirconate powder. Within this range, the yttrium sol can form effective bridging and coating between particles, enhancing the particle bonding force after the slurry solidifies. The wet blank is less prone to collapse, chipping, or cracking, facilitating demolding. Simultaneously, the slurry viscosity is controllable, the dispersion is uniform, and the injection molding filling performance is good. Below this range, the bonding effect provided by the yttrium sol is insufficient, resulting in lower wet blank strength, easy deformation, edge chipping, or cracking during demolding, and poor integrity of the green blank. Above this range, the slurry viscosity increases, the fluidity deteriorates, air bubbles are easily introduced, or uneven filling occurs; the wet and green blanks become too dense and the bonding too strong, making demolding difficult; and shrinkage and internal stress increase, easily leading to warping, cracking, or excessively high residual strength.
[0015] Preferably, the molar ratio of citric acid monohydrate to calcium acetate is 1-3:1 to ensure sufficient calcium ion chelation. When the molar ratio of citric acid monohydrate to calcium acetate is less than 1:1, there is insufficient citrate, resulting in inadequate calcium ion chelation and some calcium being lost. 2+ It exists in a free state; free calcium ions readily react with other anions in the system to form precipitates, and cannot be uniformly dispersed at the ionic level, resulting in the calcium zirconate phase content not meeting the standard; at the same time, free Ca... 2+ It can compress the electric double layer on the surface of particles, causing slurry flocculation and agglomeration, and reducing the density of the green body. When the molar ratio of citric acid monohydrate to calcium acetate is higher than 3:1, excess citric acid will generate a large amount of gas during the decomposition process, which can easily lead to cracking of the green body; and the increase in organic residue will affect the chemical purity of the ceramic core.
[0016] Preferably, the drying conditions for preparing the calcium citrate precursor are: drying at 90℃~120℃ for 1.5h~3h.
[0017] Preferably, the mass ratio of Isobam600 powder to NH3·H2O is 4~5:1, and the mass percentage of Isobam600 in the premixed solution is 0.1wt%~1.0wt%.
[0018] Preferably, the vacuum degassing conditions are: degassing at 0.7MPa~1MPa for 10min~30min.
[0019] Preferably, the curing conditions are: curing at 50℃~80℃ for 30min~50min.
[0020] Preferably, the drying process in preparing calcium zirconate-based ceramic green bodies is as follows: after demolding, dry at room temperature for 10h~24h, and then dry at a humidity of 55%~85% and a temperature of 30℃~60℃ for 12h~24h.
[0021] Preferably, the conditions for the glue removal process are: heating to 600℃~800℃ at room temperature at a heating rate of 1℃ / min~5℃ / min, and holding at this temperature for 1h~2h.
[0022] Preferably, the sintering conditions are as follows: after debinding, continue to heat to 1500℃~1550℃ at a heating rate of 1℃ / min~3℃ / min, and hold at that temperature for 2h~4h.
[0023] Preferably, the milling media is zirconia balls, the ball-to-material ratio is 1:1~3, the milling speed is 70r / min~90r / min, and the milling time is 12h~24h.
[0024] A second objective of this invention is to provide a calcium zirconate-based ceramic core prepared by the above-described method, wherein the phase composition of the calcium zirconate-based ceramic core is yttrium oxide-stabilized zirconium oxide and a lime phase.
[0025] A third objective of this invention is to provide the application of the aforementioned calcium zirconate-based ceramic core in the precision casting of titanium alloys.
[0026] Compared with the prior art, the beneficial effects of the present invention are as follows: 1. This invention provides a method for preparing calcium zirconate-based ceramic cores. Citric acid monohydrate and calcium acetate are mixed and ground to obtain a calcium citrate precursor. Isobam 600 powder, NH3·H2O, and water are mixed to obtain a premixed solution. The calcium citrate precursor, premixed solution, calcium zirconate powder, Isobam 104 powder, and yttrium sol are mixed and ball-milled to obtain a slurry. The slurry is vacuum degassed and then injected into a mold, followed by curing, demolding, drying, debinding, and high-temperature sintering to obtain the calcium zirconate-based ceramic core. This invention, by constructing a synergistic preparation system of "calcium citrate chelation dispersion - composite Isobam gel curing - yttrium sol interface regulation," solves the shortcomings of existing Isobam systems, such as poor slurry dispersion stability and easy powder agglomeration and sedimentation. It also overcomes the process defects of poor water collapse properties and difficulty in core removal after casting in sintered cores, achieving stable preparation of high-solids-content slurries, high-integrity gel curing, and consistent acquisition of high-performance sintered bodies.
[0027] 2. Addressing the shortcomings of existing Isobam slurry systems, such as high viscosity and difficulty in increasing solid content, this invention achieves efficient powder dispersion through the synergistic effect of calcium citrate chelation dispersion and Isobam 600. Specifically, citric acid monohydrate and calcium acetate coordinate in aqueous solution to form a calcium citrate chelate, ensuring uniform dispersion of calcium ions at the ionic scale and effectively shielding free Ca2+. 2+ The charge neutralization effect of Isobam 600 avoids electrostatic flocculation of the slurry caused by multivalent ions; at the same time, Isobam 600 further enhances powder dispersibility through an electrostatic steric stabilization mechanism. The synergistic effect of these two factors increases the slurry solid content to 30%~50% while maintaining good fluidity, ensuring complete mold filling, and effectively reducing air bubbles and defects inside the green body.
[0028] 3. To address the shortcomings of existing Isobam systems, such as insufficient wet preform strength and severe adhesion between the preform and the mold, this invention achieves a synergistic solution through Isobam104 gel reinforcement and yttrium sol interface isolation. On one hand, Isobam104 forms a three-dimensional network structure under heating conditions, endowing the wet preform with the necessary structural strength, making it less prone to deformation or cracking during demolding and handling. On the other hand, yttrium sol particles form a physical isolation layer on the surface of the preform during the curing stage, significantly reducing the interfacial adhesion between the wet preform and the mold, and greatly improving the demolding success rate and preform integrity.
[0029] 4. This invention further utilizes the synergistic effect of yttrium sol and calcium citrate to optimize the performance of the sintered body and its post-cast core removal capability. During the sintering stage, yttrium oxide in the yttrium sol acts as a crystal stabilizer, doping into the zirconium oxide lattice and suppressing the tetragonal-to-monoclinic phase transformation at high temperatures. Simultaneously, it promotes grain boundary diffusion and densification, improving the sintering density and high-temperature mechanical properties of the ceramic core. Meanwhile, the calcium oxide generated from the in-situ decomposition of calcium citrate partially reacts with zirconium oxide to form the calcium zirconate main crystalline phase, while some remains as a hydrated lime phase. This ensures sintering strength while imparting excellent post-cast water-collapse core removal performance to the core. The ceramic core of this invention has a relative density of over 92.5% and a flexural strength as high as 92 MPa.
[0030] 5. Compared with the ball milling time of 15h to 24h in the prior art, the present invention shortens the ball milling time to 9h to 12h, while significantly reducing the amount of organic matter added (the total amount of Isobam added does not exceed 1.3wt%), simplifying the glue removal process, and significantly improving production efficiency and yield. Attached Figure Description
[0031] Figure 1 This is a physical image of the calcium zirconate-based ceramic core prepared according to the present invention.
[0032] Figure 2 The image shows the XRD pattern of the calcium zirconate-based ceramic core from Example 1. Detailed Implementation
[0033] The technical solution of the present invention will be clearly and completely described below with reference to the data in the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.
[0034] It should be noted that the technical terms used in this invention are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of this invention. Unless otherwise specified, all raw materials, reagents, instruments and equipment used in the following embodiments of this invention can be purchased on the market or prepared by existing methods.
[0035] In the existing technology, although the isobutylene-maleic anhydride copolymer (Isobam) water-based gel system has been used for gel casting of ceramic materials such as silicon nitride, when used for the preparation of calcium zirconate-based ceramic cores, there are still technical problems such as poor slurry dispersion stability, easy agglomeration and sedimentation of powder, poor water collapse of sintered cores, and difficulty in core removal after casting.
[0036] To address the problems of existing technologies, the preparation method of calcium zirconate-based ceramic cores constructs a synergistic preparation system of "calcium citrate chelation dispersion - composite Isobam gel solidification - yttrium sol phase composition regulation". This system utilizes a calcium citrate precursor to achieve ionic-level uniform dispersion of the calcium source and avoid slurry flocculation caused by free calcium ions. A water-based network structure combining dispersion and gel enhancement functions is constructed using Isobam 600 and Isobam 104. Simultaneously, yttrium oxide components are introduced through yttrium sol, forming a hydrateable lime phase after sintering. This method solves the shortcomings of existing Isobam systems, such as poor slurry dispersion stability and easy powder agglomeration and sedimentation. It also overcomes the process defects of poor water collapse properties in sintered cores and difficulty in core removal after casting.
[0037] In this study, a water-based composite Isobam gel system was constructed using Isobam 104 and Isobam 600, replacing traditional acrylamide or aldehyde gel systems. The Isobam system eliminates the need for acrylamide monomers, crosslinking agents, and initiators, and also avoids the use of aldehyde curing agents, thus reducing the toxicity and environmental risks during the gel casting process from the outset. Simultaneously, Isobam 600 helps improve the dispersion stability of calcium zirconate powder in the aqueous phase, while Isobam 104 participates in the formation of the gel network, ensuring that the slurry maintains good flowability and casting properties even at high solid content. This allows for casting at high solid content and the production of ceramic green bodies with sufficient wet strength, thereby achieving green, safe, and stable preparation of calcium zirconate-based ceramic cores.
[0038] To enable those skilled in the art to more clearly understand the technical solution of the present invention, the following will provide a detailed description in conjunction with specific embodiments: Example 1 A method for preparing a calcium zirconate-based ceramic core, using composite Isobam green gel injection molding, includes the following steps: S1. Slurry Preparation: Citric acid monohydrate and calcium acetate were weighed and mixed at a molar ratio of 1:1, ground, and dried to obtain a calcium citrate precursor. Isobam 600 powder and NH3·H2O were dissolved in deionized water at a mass ratio of 4:1 to obtain a premixed solution. The calcium citrate precursor and the premixed solution were mixed, followed by the addition of calcium zirconate powder, Isobam 104 powder, and yttrium sol. The mixture was then ball-milled for 12 hours. After ball milling and mixing, a slurry was obtained. In the premixed solution, the mass percentages of Isobam 600 were 3.0 wt%, NH3·H2O were 0.75 wt%, and deionized water were 96.25 wt%.
[0039] The slurry contains 30% calcium zirconate powder by weight, and the amounts of calcium citrate, Isobam 600 powder, Isobam 104 powder, and yttrium sol added are 0.6wt%, 0.2wt%, 0.3wt%, and 1.0wt% of the calcium zirconate powder by weight, respectively. The ball milling media are zirconia balls, the ball-to-material ratio is 1:1, and the ball mill speed is 90 r / min.
[0040] S2. Gel curing molding: The slurry is placed in a vacuum degassing device and degassed for 60 minutes under a vacuum degree of -0.5MPa. Then, the degassed slurry is injected into a mold. The mold is placed in a water bath heating device and heated at a constant temperature of 50℃ for 50 minutes. After curing, the mold is demolded to obtain a wet blank. The wet blank is first dried naturally at room temperature for 24 hours, and then dried in a constant temperature and humidity chamber at 85% humidity and 30℃ for another 24 hours to obtain a calcium zirconate-based ceramic blank.
[0041] S3. Sintering and forming: The calcium zirconate-based ceramic blank is placed in a sintering furnace and heated to 600°C at a heating rate of 1°C / min, and held at that temperature for 1 hour to remove the binder, thus obtaining a green blank; in an air atmosphere, the green blank is further heated to 1500°C at a heating rate of 1°C / min, and sintered at 1500°C for 2 hours to obtain a calcium zirconate-based ceramic core.
[0042] Example 2 A method for preparing a calcium zirconate-based ceramic core, using composite Isobam green gel injection molding, includes the following steps: S1. Slurry preparation: Citric acid monohydrate and calcium acetate were weighed and mixed at a molar ratio of 2:1, ground and dried to obtain calcium citrate precursor; Isobam600 powder and NH3·H2O were dissolved in deionized water at a mass ratio of 5:1 to obtain a premixed solution; the calcium citrate precursor and the premixed solution were mixed, and then calcium zirconate powder, Isobam104 powder and yttrium sol were added, and the mixture was transferred to a ball mill jar and ball-milled for 10 hours. After ball milling and mixing, a slurry was obtained.
[0043] The slurry contains 40% calcium zirconate powder by weight, and the amounts of calcium citrate, Isobam 600 powder, Isobam 104 powder, and yttrium sol added are 0.6wt%, 0.3wt%, 0.3wt%, and 2.0wt% of the calcium zirconate powder by weight, respectively. The ball milling media are zirconia balls, the ball-to-material ratio is 2:1, and the ball mill speed is 80 r / min.
[0044] S2. Gel curing molding: The slurry is placed in a vacuum degassing device and degassed for 40 minutes under a vacuum of -0.08MPa. Then, the degassed slurry is injected into a mold. The mold is placed in a water bath heating device and heated at 60℃ for 40 minutes. After curing, the mold is demolded to obtain a wet blank. The wet blank is first dried naturally at room temperature for 18 hours, and then dried in a constant temperature and humidity chamber at 75% humidity and 40℃ for another 20 hours to obtain a calcium zirconate-based ceramic blank.
[0045] S3. Sintering and forming: The calcium zirconate-based ceramic blank is placed in a sintering furnace and heated to 600°C at a heating rate of 3°C / min, and held at that temperature for 1.5 hours to remove the binder, thus obtaining a green blank; in an air atmosphere, the green blank is further heated to 1525°C at a heating rate of 2°C / min, and sintered at 1525°C for 3 hours to obtain a calcium zirconate-based ceramic core.
[0046] Example 3 A method for preparing a calcium zirconate-based ceramic core, using composite Isobam green gel injection molding, includes the following steps: S1. Slurry preparation: Citric acid monohydrate and calcium acetate were weighed and mixed in a molar ratio of 3:1, ground and dried to obtain calcium citrate precursor; Isobam600 powder and NH3·H2O were dissolved in deionized water in a mass ratio of 4:1 to obtain a premixed solution; the calcium citrate precursor and the premixed solution were mixed, and then calcium zirconate powder, Isobam104 powder and yttrium sol were added, and the mixture was transferred to a ball mill jar and ball-milled for 9 hours. After ball milling and mixing, a slurry was obtained.
[0047] The slurry contains 45% calcium zirconate powder by weight, and the amounts of calcium citrate, Isobam 600 powder, Isobam 104 powder, and yttrium sol added are 0.6wt%, 0.5wt%, 0.3wt%, and 3.0wt% of the calcium zirconate powder by weight, respectively. The ball milling media are zirconia balls, the ball-to-material ratio is 3:1, and the ball mill speed is 75 r / min.
[0048] S2. Gel curing molding: The slurry is placed in a vacuum degassing device and degassed for 60 minutes under a vacuum of -0.75MPa. Then, the degassed slurry is injected into a mold. The mold is placed in a water bath heating device and heated at 60℃ for 50 minutes. After curing, the mold is demolded to obtain a wet blank. The wet blank is first dried naturally at room temperature for 24 hours, and then dried for another 16 hours in a constant temperature and humidity chamber with 65% humidity and 50℃ to obtain a calcium zirconate-based ceramic blank.
[0049] S3. Sintering and forming: The calcium zirconate-based ceramic blank is placed in a sintering furnace and heated to 600°C at a heating rate of 4°C / min, and held at that temperature for 2 hours to remove the binder, thus obtaining a green blank; in an air atmosphere, the green blank is further heated to 1500°C at a heating rate of 3°C / min, and sintered at 1500°C for 4 hours to obtain a calcium zirconate-based ceramic core.
[0050] Example 4 A method for preparing a calcium zirconate-based ceramic core, using composite Isobam green gel injection molding, includes the following steps: S1. Slurry preparation: Citric acid monohydrate and calcium acetate were weighed and mixed at a molar ratio of 2:1, ground and dried to obtain calcium citrate precursor; Isobam600 powder and NH3·H2O were dissolved in deionized water at a mass ratio of 5:1 to obtain a premixed solution; the calcium citrate precursor and the premixed solution were mixed, and then calcium zirconate powder, Isobam104 powder and yttrium sol were added, and the mixture was transferred to a ball mill jar and ball-milled for 12 hours. After ball milling and mixing, a slurry was obtained.
[0051] The slurry contains 50% calcium zirconate powder by weight, and the amounts of calcium citrate, Isobam 600 powder, Isobam 104 powder, and yttrium sol added are 0.6wt%, 0.7wt%, 0.3wt%, and 5.0wt% of the calcium zirconate powder by weight, respectively. The ball milling media are zirconia balls, the ball-to-material ratio is 3:1, and the ball mill speed is 70 r / min.
[0052] S2. Gel curing molding: The slurry is placed in a vacuum degassing device and degassed for 20 minutes under a vacuum of -1.0 MPa. Then, the degassed slurry is injected into a mold. The mold is placed in a water bath heating device and heated at 70°C for 30 minutes. After curing, the mold is demolded to obtain a wet blank. The wet blank is first dried naturally at room temperature for 12 hours, and then dried in a constant temperature and humidity chamber at 85% humidity and 60°C for another 12 hours to obtain a calcium zirconate-based ceramic blank.
[0053] S3. Sintering and forming: The calcium zirconate-based ceramic blank is placed in a sintering furnace and heated to 800°C at a heating rate of 5°C / min, and held at that temperature for 2 hours to remove the binder, thus obtaining a green blank; in an air atmosphere, the green blank is further heated to 1550°C at a heating rate of 3°C / min, and sintered at 1550°C for 2 hours to obtain a calcium zirconate-based ceramic core.
[0054] Comparative Example 1 A method for preparing a calcium zirconate-based ceramic core, using composite Isobam green gel injection molding, includes the following steps: S1. Slurry Preparation: Isobam 600 powder and NH3·H2O were dissolved in deionized water at a mass ratio of 5:1 to obtain a premixed solution. Calcium zirconate powder and Isobam 104 powder were added, and the mixture was ball-milled for 10 hours. After ball milling and mixing, a slurry was obtained. The solid content of calcium zirconate powder in the slurry was 45%, and the addition amounts of Isobam 600 powder and Isobam 104 powder were 0.3wt% and 0.3wt% of the mass of calcium zirconate powder, respectively. The ball milling media were zirconia balls, the ball-to-powder ratio was 2:1, and the ball speed was 75 r / min.
[0055] S2. Gel curing molding: The slurry is placed in a vacuum degassing device and degassed for 30 minutes under a vacuum of -0.9MPa. Then, the degassed slurry is injected into a mold. The mold is placed in a water bath heating device and heated at 60℃ for 40 minutes. After curing, the mold is demolded to obtain a wet blank. The wet blank is first dried naturally at room temperature for 18 hours, and then dried in a constant temperature and humidity chamber at 75% humidity and 50℃ for another 16 hours to obtain a calcium zirconate-based ceramic blank.
[0056] S3. Sintering and forming: The calcium zirconate-based ceramic blank is placed in a sintering furnace and heated to 600°C at a heating rate of 3°C / min, and held at that temperature for 2 hours to remove the binder, thus obtaining a green blank; in an air atmosphere, the green blank is further heated to 1525°C at a heating rate of 2°C / min, and sintered at 1525°C for 3 hours to obtain a calcium zirconate-based ceramic core.
[0057] like Figure 1As shown, the calcium zirconate-based ceramic core blank prepared by this invention has no cracks or defects on its surface.
[0058] Depend on Figure 2 The phase composition of the calcium zirconate-based ceramic core of this invention is calcium zirconate and lime phase (free calcium oxide). Calcium zirconate has a high melting point (approximately 2340℃), excellent high-temperature stability, good thermal shock resistance, and excellent resistance to alkaline slag and various molten metals, which is beneficial for improving the service life of the calcium zirconate-based ceramic core during titanium alloy casting. The free calcium oxide phase imparts excellent water-collapsible properties to the calcium zirconate-based ceramic core, facilitating core removal after casting. Simultaneously, calcium oxide acts as a grain growth inhibitor, effectively suppressing abnormal grain growth of calcium zirconate and refining grain size, thereby improving the mechanical properties and dimensional accuracy of the calcium zirconate-based ceramic core.
[0059] To evaluate the water collapse and core removal performance of the calcium zirconate-based ceramic core of the present invention, the sintered samples obtained in Examples 1 to 4 and Comparative Example 1 were immersed in deionized water at 80°C for 30 min and 60 min respectively, then dried to constant weight and the mass loss rate was calculated. The results are shown in Table 1.
[0060] Table 1 shows the performance test results of the calcium zirconate-based ceramic cores in Examples 1-4 and Comparative Example 1. sample Bending strength (MPa) relative density 30-minute mass loss rate 60min mass loss rate Example 1 58 92.7% 1.5% 3.1% Example 2 92 93.5% 1.0% 2.4% Example 3 38 92.8% 2.2% 4.8% Example 4 77 92.5% 1.3% 2.9% Comparative Example 1 76 92.6% 0.7% 1.5% Table 1 shows that the relative density of the calcium zirconate-based ceramic cores obtained in Examples 1 to 4 remained above 92.5%, indicating that the preparation method of the present invention can obtain sintered bodies with relatively complete structures. Among them, the flexural strength of Example 2 reached 92 MPa, significantly higher than the 76 MPa of Comparative Example 1, indicating that the composite Isobam gel system, under the preferred ratio, can improve slurry dispersion and green body uniformity, thereby improving the mechanical properties after sintering. Although the flexural strength of Examples 1 and 3 was lower than that of Comparative Example 1, they still possessed a certain flexural strength, and their relative density was close to that of Comparative Example 1, indicating that they could still form a complete ceramic skeleton, falling within the scope of the present invention's feasible implementation scheme. The decrease in strength was mainly related to the reduced slurry dispersion stability, local agglomeration, and increased glue removal defects or microcracks after the Isobam 600 addition amount deviated from the preferred value.
[0061] The mass loss rates of Examples 1-4 after soaking for 30 min were 1.5%, 1.0%, 2.2%, and 1.3%, respectively, and after soaking for 60 min, they were 3.1%, 2.4%, 4.8%, and 2.9%, respectively. In contrast, the mass loss rates of Comparative Example 1 after soaking for 30 min and 60 min were only 0.7% and 1.5%, respectively. Therefore, the embodiments of the present invention all exhibited higher mass loss rates after hot water soaking than Comparative Example 1, indicating that the present invention, through the regulation of calcium source components and sintering structure, improves the penetration and destructive effect of water on the internal structure of the ceramic core, thereby improving the water-collapse and core-removal performance of the calcium zirconate-based ceramic core.
[0062] It should be noted that when numerical ranges are involved in this invention, it should be understood that both endpoints of each numerical range, as well as any value between the two endpoints, can be selected. Since the steps and methods used are the same as in the embodiments, preferred embodiments are described here to avoid redundancy. Although preferred embodiments of the invention have been described, those skilled in the art, upon learning the basic inventive concept, can make other changes and modifications to these embodiments. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments as well as all changes and modifications falling within the scope of this invention.
Claims
1. A method for preparing a calcium zirconate-based ceramic core, characterized in that, Includes the following steps: Slurry preparation: Citric acid monohydrate and calcium acetate were mixed and ground to obtain calcium citrate precursor; Isobam 600 powder, NH3·H2O and water were mixed to obtain premixed solution; calcium citrate precursor, premixed solution, calcium zirconate powder, Isobam 104 powder and yttrium sol were mixed and ball-milled to obtain slurry; Gel curing molding: After vacuum degassing, the slurry is injected into a mold, cured and molded, then demolded and dried to obtain a calcium zirconate-based ceramic green body; Sintering and molding: The calcium zirconate-based ceramic green body is debinded to obtain a green body; then the green body is sintered to obtain a calcium zirconate-based ceramic core.
2. The preparation method according to claim 1, characterized in that, In the slurry, the solid content of calcium zirconate powder is 30%~50%; Based on the mass of calcium zirconate powder, the amount of calcium citrate added is 0.6 wt%, the amount of Isobam 600 powder added is 0.1 wt%~1 wt%, the amount of Isobam 104 powder added is 0.3 wt%, and the amount of yttrium sol added is 1.0 wt%~5.0 wt%.
3. The preparation method according to claim 1, characterized in that, The molar ratio of citric acid monohydrate to calcium acetate is 1~3:
1.
4. The preparation method according to claim 1, characterized in that, The mass ratio of Isobam600 powder to NH3·H2O is 5:1, and the mass percentage of Isobam600 in the premixed solution is 0.1wt%~1.0wt%.
5. The preparation method according to claim 1, characterized in that, The curing conditions are: curing at 50℃~80℃ for 30min~50min.
6. The preparation method according to claim 1, characterized in that, The specific drying process is as follows: after demolding, dry at room temperature for 10h~24h, and then dry at humidity of 55%~85% and temperature of 30℃~60℃ for 12h~24h.
7. The preparation method according to claim 1, characterized in that, The conditions for the glue removal process are: heating to 600℃~800℃ at a heating rate of 1℃ / min~5℃ / min at room temperature, and holding at that temperature for 1h~2h.
8. The preparation method according to claim 1, characterized in that, The sintering conditions are as follows: after debinding, continue to hold at 1500℃~1550℃ for 2h~4h.
9. A calcium zirconate-based ceramic core prepared by the preparation method according to any one of claims 1 to 8, characterized in that, The phase composition of the calcium zirconate-based ceramic core is yttrium oxide-stabilized zirconium oxide and lime phase.
10. The application of the calcium zirconate-based ceramic core as described in claim 9 in the precision casting of titanium alloys.