Short-process preparation device and method for multi-chamber composite gradient pressure-regulating filament
The multi-chamber composite gradient pressure-regulating wire preparation device and method solves the problem of difficult forming of alloy wire in a vacuum environment, realizes efficient and stable alloy wire preparation, and improves the forming success rate and wire quality.
Patent Information
- Application Number
- CN202611531003.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-30
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies for preparing alloy wires suffer from problems such as decreased material plasticity, easy brittle fracture, high surface residual stress, long process flow, and low forming success rate. In particular, the lack of wire ejection driving force in a vacuum environment leads to solidification blockage of the molten metal.
A multi-chamber composite gradient pressure-regulating wire preparation device is adopted. The molten metal is driven into the crystallizer by the controllable pressure difference between the vacuum melting chamber and the pressure-regulating wire forming chamber. The pressure difference and the wire guide speed are adjusted in real time by temperature sensors to ensure that the molten metal solidifies in the cooling zone of the crystallizer.
Stable and continuous forming of alloy wires in a vacuum environment has been achieved, avoiding solidification blockage, improving the internal quality and forming success rate of the wires, and shortening the process flow.
Smart Images

Figure CN123102949A_ABST
Abstract
Description
Technical Field
[0001] This application relates to a short-process preparation device and method for multi-chamber composite gradient pressure-regulating wire, belonging to the field of special metal casting and forming. Background Technology
[0002] Alloy wire, as an important branch of alloy materials, is widely used in aerospace, medical and health, and industrial manufacturing. With the development of the metal additive manufacturing industry, alloy wire is increasingly being used as a raw material in metal wire feeding additive manufacturing. Currently, the main method for preparing metal additive wire raw materials is cold drawing. However, this method leads to a significant decrease in the material's plasticity during wire production, resulting in deteriorated bending performance and brittle fracture during deformation. Simultaneously, the drawing process causes high residual stress on the wire surface, reducing fatigue life and making it prone to deformation or cracking. Furthermore, for alloys with high deformation difficulty, it is difficult to produce additive wire raw materials through cold drawing. In addition, the traditional process of first preparing alloy ingots and then performing multiple extrusion drawing processes is lengthy and time-consuming, gradually failing to meet the industry's diverse needs for alloy wire types and specifications. Therefore, developing short-process, high-performance, and multi-variety additive manufacturing alloy wire raw material forming technologies and equipment is of great practical significance.
[0003] In existing technologies, to address the problem of metal wire forming, there are related solutions for alloy continuous casting using ultrasonic vibration coupled with mechanical stirring. For example, patent CN204639082U discloses an ultrasonic stirring device for the crystallization zone of alloy continuous casting, which uses an ultrasonic generator on the crystallizer to ultrasonically stir the alloy melt to refine grains and improve segregation. Patent CN114130975A discloses a device and method for composite vibration continuous casting of homogeneous fine-grained ingots, which uses a combination of a pre-stirrer and a vibrator. First, pre-stirring homogenizes the melt, and then strong and effective vibration is applied to refine the microstructure of the solidifying molten metal. However, these methods have revealed a series of problems in practical applications: mechanical stirring in a non-vacuum environment can cause oxidation and gas entrapment in the molten metal inside the crucible; the generated bubbles hinder the downward flow of molten metal droplets and easily cause metal wire breakage; if a vacuum melting furnace is used, there is a lack of wire-driving force during the casting process, and the molten metal solidifies in the crystallizer, easily causing blockage. Furthermore, while ultrasonic vibration can reduce segregation and refine grains, it cannot effectively provide feeding power for the molten metal. The molten metal is still prone to solidification and blockage in the mold, leading to wire forming failure. These problems severely restrict the success rate of alloy wire forming and the yield of formed wires. Summary of the Invention
[0004] To address the problem of molten metal solidifying and becoming blocked in the crystallizer due to lack of wire ejection force during continuous casting of alloy wires in a vacuum environment, this application provides a short-process preparation device and method for multi-chamber composite gradient pressure-regulating wires.
[0005] This application discloses a short-process preparation device for multi-chamber composite gradient pressure-regulating wire, comprising a vacuum melting chamber, a pressure-regulating wire-forming chamber, a plug, a pressure-regulating pipeline for the melting chamber, a pressure-regulating pipeline for the wire-forming chamber, an induction coil, a crucible, a crystallizer, a wire guide rod, and a wire collector.
[0006] The crucible is placed inside the vacuum melting chamber, and a drain port is provided at the bottom of the crucible. An induction coil is used to heat the alloy raw material inside the crucible.
[0007] The pressure-regulating filament forming chamber is located below the vacuum melting chamber, and the crystallizer is located inside the pressure-regulating filament forming chamber. The liquid inlet of the crystallizer corresponds to the liquid outlet of the crucible.
[0008] The plug is located at the drain port of the crucible. The plug has a sealed state and a lifted state. In the sealed state, the plug seals the drain port, so that the vacuum melting chamber and the pressure regulating filament forming chamber form two independent sealed chambers. In the lifted state, the drain port is open, and the vacuum melting chamber and the pressure regulating filament forming chamber are connected through the drain port.
[0009] The pressure regulating pipeline of the melting chamber is connected to the vacuum melting chamber and is used to evacuate the vacuum melting chamber and introduce inert gas.
[0010] The pressure regulating pipeline of the filament forming chamber is connected to the pressure regulating filament forming chamber and is used to evacuate the pressure regulating filament forming chamber and introduce inert gas;
[0011] A temperature sensor is installed above the liquid inlet of the crystallizer to monitor the temperature of the molten metal at the liquid inlet of the crystallizer in real time.
[0012] The wire guide rod is located at the outlet of the crystallizer and is used to pull the solidified filament out of the crystallizer;
[0013] The filament collector is located downstream of the lead rod and is used to collect the filaments.
[0014] Preferably, the preparation apparatus also includes a controller, which is connected to a temperature sensor, a pressure regulating device on the pressure regulating pipeline of the melting chamber, a pressure regulating device on the pressure regulating pipeline of the wire forming chamber, and a wire guide rod. The controller adjusts the pressure difference between the pressure in the vacuum melting chamber and the pressure in the pressure regulating wire forming chamber in real time according to the temperature data of the temperature sensor, so as to control the rate at which the molten metal enters the crystallizer and the traction speed of the wire guide rod, so that the solid-liquid phase region of the molten metal is located in the cooling region of the crystallizer.
[0015] Preferably, the plug is connected to a drive rod that passes through the wall of the vacuum melting chamber or the pressure regulating wire forming chamber, and a dynamic sealing structure is provided between the drive rod and the wall.
[0016] Preferably, the mold end pipes inside the crystallizer are inclined outwards.
[0017] Preferably, the wire collector includes a winding drum and a wire feeding and pressing device; the wire feeding and pressing device is located on the inlet side of the winding drum and is used to guide the wire to the winding drum and make the wire tightly arranged on the winding drum, which is used to rotate and wind up the wire.
[0018] Preferably, the vacuum melting chamber is equipped with an observation window for observing the state of the molten metal inside the vacuum melting chamber.
[0019] This application also provides a preparation method based on the above-mentioned multi-chamber composite gradient pressure-regulating wire short-process preparation device, including:
[0020] Step 1: Place the alloy raw material in the crucible, with the plug in a sealed state, so that the vacuum melting chamber and the pressure regulating wire forming chamber form two independent sealed chambers;
[0021] Step 2: Evacuate the vacuum melting chamber through the pressure regulating pipeline of the melting chamber, and evacuate the pressure regulating and spinning chamber through the pressure regulating pipeline of the spinning chamber.
[0022] Step 3: Activate the induction coil to perform induction melting, so that the alloy raw materials are melted into molten metal and then kept at a constant temperature;
[0023] Step 4: When the pressure in the vacuum melting chamber is less than or equal to the pressure in the pressure regulating wire forming chamber, inert gas is introduced into the vacuum melting chamber through the melting chamber pressure regulating pipe to make the pressure in the vacuum melting chamber greater than the pressure in the pressure regulating wire forming chamber. Then, the plug is switched to the raised state. When the pressure in the vacuum melting chamber is greater than the pressure in the pressure regulating wire forming chamber, the plug can be directly switched to the raised state. Then, inert gas is introduced into the vacuum melting chamber through the melting chamber pressure regulating pipe to make the pressure in the vacuum melting chamber continuously greater than the pressure in the pressure regulating wire forming chamber. Under the combined action of gravity and gas pressure difference, the molten metal enters the crystallizer through the drain port.
[0024] Step 5: Use a temperature sensor to monitor the temperature of the molten metal at the inlet of the crystallizer in real time, and adjust the pressure difference between the pressure in the vacuum melting chamber and the pressure in the wire forming chamber in real time according to the temperature data of the temperature sensor, so as to control the rate at which the molten metal enters the crystallizer and the traction speed of the wire rod, so that the solid-liquid phase region of the molten metal is located in the cooling area of the crystallizer.
[0025] Step 6: The molten metal cools and solidifies in the crystallizer to form a wire.
[0026] Step 7: The wire guide rod pulls the wire out of the crystallizer;
[0027] Step 8: The filament collector collects the filaments.
[0028] Preferably, the pressure in the pressure regulating and spinning chamber is P2, and the atmospheric pressure is P0. In step two, P1 and P2 are made to satisfy any of the following relationships:
[0029] P1=P2 <P0;
[0030] P1 <P2=P0;
[0031] P0>P1>P2.
[0032] Preferably, in step five, when the melt temperature detected by the temperature sensor is higher than the cooling temperature range of the crystallizer, the pressure difference between the pressure in the vacuum melting chamber and the pressure in the pressure regulating wire forming chamber is reduced, thereby reducing the melt flow rate and the traction speed of the wire guide rod; when the melt temperature detected by the temperature sensor is lower than the cooling temperature range of the crystallizer, the pressure difference between the pressure in the vacuum melting chamber and the pressure in the pressure regulating wire forming chamber is increased, thereby increasing the melt flow rate and the traction speed of the wire guide rod is increased.
[0033] Preferably, in step eight, the filament formed by cooling and solidification is collected into strands of metal wire by a winding bobbin and a wire pressing device, and the semi-finished metal wire is taken out.
[0034] The beneficial effects of this application are as follows: This application controls the flow channel between the crucible drain port and the crystallizer inlet by using a plug, and establishes a controllable pressure difference by adjusting the pressure in the vacuum melting chamber and the pressure-adjusting wire forming chamber through the pressure-adjusting pipelines of the melting chamber and the wire forming chamber, respectively. This allows the molten metal to enter the crystallizer under the dual drive of gas pressure and gravity, solving the problem of molten metal solidification blockage and wire forming failure caused by the lack of wire ejection driving force in continuous casting under vacuum conditions, and realizing the stable and continuous forming of fine diameter wire. This application adopts vacuum induction melting technology, which melts alloy raw materials in a vacuum environment, effectively removing gaseous impurities such as hydrogen and oxygen, avoiding oxidation of molten metal and gas entrapment, eliminating the defect of wire breakage caused by bubbles from the source, and improving the internal quality of the wire.
[0035] This application uses a temperature sensor to monitor the temperature of the molten metal at the inlet of the crystallizer in real time, and dynamically adjusts the pressure difference between the vacuum melting chamber and the pressure regulating wire forming chamber, as well as the traction speed of the wire guide rod, based on the temperature data. This controls the rate at which the molten metal enters the crystallizer and the wire drawing speed, ensuring that the solid-liquid phase region is always within the cooling area of the crystallizer. This avoids blockage or wire breakage caused by the mismatch between the flow rate and the cooling rate, and ensures the uniformity and density of the wire structure. Attached Figure Description
[0036] Figure 1 This is a schematic diagram of the principle of the short-process preparation device for multi-chamber composite gradient pressure-regulating wire of this application;
[0037] Figure 2 for Figure 1 Side view;
[0038] Figure 3 for Figure 1 Top view;
[0039] Figure 4 This is a three-dimensional perspective view of the short-process preparation device for multi-chamber composite gradient pressure-regulating wires in this application;
[0040] Figure 5 This is a diagram showing the solid fraction distribution before the pressure regulation action;
[0041] Figure 6 This is a solid fraction distribution diagram after pressure regulation.
[0042] Figure 7 This is a temperature distribution diagram before the voltage regulation action;
[0043] Figure 8 This is a temperature distribution diagram after the voltage regulation. Detailed Implementation
[0044] The technical solutions of the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of this application, and not all embodiments. Based on the embodiments of this application, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of this application.
[0045] It should be noted that, unless otherwise specified, the embodiments and features described in this application can be combined with each other.
[0046] The present application will be further described below with reference to the accompanying drawings and specific embodiments, but this is not intended to limit the scope of the application.
[0047] This embodiment provides a short-process preparation device and method for multi-chamber composite gradient pressure-regulated wire, which solves the problems of long process flow, excessive residual stress on the surface of alloy wire, difficulty in wire formation of difficult-to-deform alloys, uneven microstructure and composition after wire formation, and oxidation, gas entrapment, and solidification blockage caused by ultrasonic vibration coupled with mechanical stirring. This application obtains high-purity molten metal through vacuum induction melting. A plug at the crucible drain port controls the flow between the vacuum melting chamber and the pressure-regulated wire forming chamber. By setting pressure-regulating pipelines in the vacuum melting chamber and the pressure-regulated wire forming chamber respectively and establishing a controllable pressure difference, the molten metal is driven into the crystallizer for cooling and solidification under the combined action of gas pressure and gravity. The solidified wire is then pulled out by a wire guide rod, achieving continuous casting. Simultaneously, a temperature sensor monitors the temperature in real time and dynamically adjusts the pressure difference to control the wire forming rate and the wire guide rod traction speed to ensure stable and continuous forming of fine-diameter wires.
[0048] Specifically, the multi-chamber composite gradient pressure-regulating wire short-process preparation device of this embodiment includes a vacuum melting chamber 1, a plug 6, a pressure-regulating wire forming chamber 5 and a wire guide rod 7 arranged sequentially from top to bottom.
[0049] The vacuum melting chamber 1 is a sealed pressure vessel, which contains an induction coil 3 and a crucible 4. The crucible 4 is located inside the induction coil 3 or coupled to the induction coil 3. The crucible 4 is used to hold the alloy raw material. The induction coil 3 is used to generate an alternating electromagnetic field after being energized, so that the alloy raw material in the crucible 4 is induced to heat up and melt.
[0050] The top or side wall of the vacuum melting chamber 1 is connected to a melting chamber pressure regulating pipeline 2. The melting chamber pressure regulating pipeline 2 can be selectively connected to a vacuum pump group and an inert gas cylinder and pressure regulating equipment for vacuuming the vacuum melting chamber 1 and introducing inert gas into the vacuum melting chamber 1.
[0051] The bottom of the crucible 4 has a drain port for the molten metal to flow out, and the position of the drain port corresponds to the position of the inlet of the crystallizer 8 inside the pressure-regulating wire-forming chamber 5 below. In this embodiment, the crucible is made of any one of the following materials: high-purity graphite, tungsten alloy, clay, or ceramic. The specific material of the crucible is determined according to the type of alloy being melted and the melting temperature. The pressure-regulating wire-forming chamber 5 is located below the vacuum melting chamber 1. The pressure-regulating wire-forming chamber 5 is a sealed pressure-bearing container, and the crystallizer 8 is installed inside it. The pressure-regulating wire-forming chamber 5 is connected to a wire-forming chamber pressure-regulating pipeline 11, which can be selectively connected to a vacuum pump group and an inert gas cylinder and pressure regulating equipment for evacuating the pressure-regulating wire-forming chamber 5 and introducing inert gas into the pressure-regulating wire-forming chamber 5.
[0052] A plug 6 is positioned at the drain port of the crucible 4, and has a sealed state and a raised state. In the sealed state, the plug 6 seals the drain port, forming two independent sealed chambers between the vacuum melting chamber 1 and the pressure-regulating wire forming chamber 5. In the raised state, the drain port is open, and the vacuum melting chamber 1 and the pressure-regulating wire forming chamber 5 are connected through the drain port. Specifically, the plug 6 is connected to a drive rod that passes through the wall of the vacuum melting chamber 1 or the pressure-regulating wire forming chamber 5. A dynamic sealing structure is provided between the drive rod and the wall, which can be any one of an O-ring dynamic seal, a lip seal, or a bellows seal. The dynamic sealing structure is used to maintain the airtightness of the vacuum melting chamber 1 or the pressure-regulating wire forming chamber 5 when the drive rod moves, and also facilitates the replacement of the crucible 4.
[0053] The lead screw 7 is located at the outlet of the crystallizer 8, which is situated upstream of the lead screw 7 within the pressure-regulating wire-forming chamber 5. The lead screw 7 is connected to a lifting drive mechanism, which drives the lead screw 7 to move vertically upwards or downwards. The lifting drive mechanism can be any of a hydraulic cylinder, pneumatic cylinder, or screw-nut mechanism, with its fixed end located at the bottom or side wall of the pressure-regulating wire-forming chamber 5, and its movable end connected to the lead screw 7. After the wire solidifies in the crystallizer 8, it is pulled out of the outlet of the pressure-regulating wire-forming chamber 5 by the lead screw 7. Initially, the lead screw 7 is in a low position, and its tip is disconnected from the outlet of the crystallizer 8. When the lead screw 7 is driven upwards to a high position by the lifting drive mechanism, its tip engages with the outlet of the crystallizer 8, sealing the outlet. After induction melting is completed, the alloy raw material is completely melted to form molten metal and then kept at a constant temperature. At this point, the lifting drive mechanism is activated, driving the lead wire 7 upward to a high position, so that the top end of the lead wire 7 aligns with the outlet of the crystallizer 8, sealing the outlet of the crystallizer 8. After the molten metal cools and solidifies in the crystallizer 8 to form a wire, the lifting drive mechanism is activated, driving the lead wire 7 downward, and the lead wire 7 pulls the wire out of the crystallizer 8. The lead wire 7 is used to provide continuous traction force, pulling the solidified wire drawn from the end of the crystallizer 8 out at a uniform speed through the outlet of the pressure-regulating wire forming chamber 5.
[0054] The wire collector 12 is located downstream of the wire guide rod 7 and is used to collect the wire. After the wire is pulled out from the pressure regulating and spinning chamber 5 by the wire guide rod 7, it enters the wire collector 12.
[0055] This embodiment controls the flow path between the crucible drain and the crystallizer inlet by using a plug, and independently adjusts the pressure in the vacuum melting chamber and the pressure-adjusting wire forming chamber via pressure-adjusting pipes 11 in the melting chamber and wire forming chamber respectively to establish a controllable pressure difference. This allows the molten metal to enter the crystallizer under the dual drive of air pressure and gravity, solving the problem of molten metal solidification blockage and wire forming failure caused by the lack of wire-extrusion driving force in continuous casting under vacuum conditions, and achieving stable and continuous forming of fine-diameter wire. This embodiment replaces the traditional mechanical drawing force with air pressure drive, so the molten metal is not subjected to mechanical extrusion during filling and solidification, avoiding the generation of high residual stress on the wire surface, and significantly improving the bending performance and fatigue life of the wire. This embodiment integrates vacuum induction melting and continuous casting into a short-process technology, completing the process from alloy melting to wire forming continuously in the same device, eliminating the need to prepare alloy ingots first and then undergo multiple extrusion and drawing processes, significantly shortening the process flow and production cycle.
[0056] Temperature sensor 9 is positioned above the inlet of crystallizer 8 to monitor the temperature of the molten metal at the inlet of crystallizer 8 in real time. Temperature sensor 9 can be either a thermocouple or an infrared temperature probe, with its sensing end extending into the pressure-regulating wire-forming chamber 5 and near the inlet of crystallizer 8, to monitor the temperature of the molten metal flowing into crystallizer 8 in real time. Temperature sensor 9 uses a type K thermocouple with a measurement range of 0℃ to 1600℃ and a measurement accuracy of ±1℃. In a preferred embodiment, the preparation apparatus also includes a controller. The controller is connected to temperature sensor 9, pressure regulating equipment on the pressure regulating pipeline 2 of the melting chamber, pressure regulating equipment on the pressure regulating pipeline 11 of the wire-forming chamber, and wire guide rod 7. The controller adjusts the pressure difference between the vacuum melting chamber 1 and the pressure regulating wire-forming chamber 5 in real time based on the temperature data from temperature sensor 9 to control the rate at which the molten metal enters crystallizer 8 and the traction speed of wire guide rod 7, ensuring that the solid-liquid phase region of the molten metal is located within the cooling region of crystallizer 8. The controller uses a programmable logic controller or an industrial computer. It receives the analog signal from the temperature sensor 9, performs PID calculations after analog-to-digital conversion, and outputs control signals to the pressure regulating device on the pressure regulating pipeline 2 of the melting chamber, the pressure regulating device on the pressure regulating pipeline 11 of the wire forming chamber, and the drive motor of the wire drawing rod 7.
[0057] In a preferred embodiment, the mold end pipe within the crystallizer 8 is configured with an outwardly inclined structure. Specifically, a mold is disposed inside the crystallizer 8, the cross-sectional shape of the mold's internal cavity matching the cross-sectional shape of the desired filament, and the mold extends from the cooling area of the crystallizer 8 to the bottom outlet of the pressure-regulating filament forming chamber 5. The mold end pipe is inclined outward relative to the vertical direction at an angle of 5° to 30°. When the solidified filament is pulled out from the mold end pipe, this inclined structure reduces the contact area between the filament surface and the inner wall of the mold end pipe, thereby reducing the frictional resistance during filament removal.
[0058] In a preferred embodiment, the wire collector 12 includes a winding drum and a wire feeding and pressing device. The winding drum is a cylindrical rotating drum driven by a drive motor to rotate around its own axis, used for rotating and winding the wire. The wire feeding and pressing device is located on the inlet side of the winding drum and includes a wire feeding guide wheel and a pressing wheel. The wire feeding guide wheel reciprocates along the axial direction of the winding drum, evenly distributing the wire in the axial direction of the winding drum. The pressing wheel presses against the surface of the winding drum, applying a compressive force to the wire wound on the winding drum, making the wire tightly wound and neatly arranged.
[0059] In a preferred embodiment, an observation window 10 is provided on the side wall or top cover of the vacuum melting chamber 1. The observation window 10 is made of high-transmittance, heat-resistant glass, and its position corresponds to the surface of the molten metal in the crucible 4. The operator can directly observe the state of the molten metal, the temperature distribution, and the melting process inside the vacuum melting chamber 1 through the observation window 10.
[0060] When using the above-mentioned multi-chamber composite gradient pressure-regulating filament short-process preparation device to prepare filaments, the preparation method shall be carried out according to the following steps.
[0061] Step 1: Sealing and loading.
[0062] The alloy raw material is placed in the crucible 4, and the plug 6 is in a sealed state, so that the vacuum melting chamber 1 and the pressure regulating wire forming chamber 5 form two independent sealed chambers.
[0063] Step 2: Simultaneous vacuuming.
[0064] Before using the equipment, the airtightness of the vacuum melting chamber 1 and the pressure regulating spinning chamber 5 is first tested. After confirming that the airtightness is good, the vacuum melting chamber 1 is evacuated through the pressure regulating pipeline 2 of the melting chamber, and the pressure regulating spinning chamber 5 is evacuated through the pressure regulating pipeline 11 of the spinning chamber. The pressure inside the vacuum melting chamber 1 is set as P1, the pressure inside the pressure regulating spinning chamber 5 is set as P2, and the atmospheric pressure is set as P0, such that P1 and P2 satisfy any of the following relationships: P1 = P2 <P0;P1<P2=P0;P0> P1>P2. Specifically, the pressure inside the vacuum melting chamber 1 and the pressure regulating wire forming chamber 5 is evacuated to a predetermined vacuum level to remove air, water vapor, and gases adsorbed on the surface of the alloy raw materials. Step 3: Induction melting and heat preservation.
[0065] Induction coil 3 is activated for induction melting, causing the alloy raw material to melt into molten metal and then held at that temperature. An alternating current is passed through induction coil 3 to generate an alternating electromagnetic field, inducing a current within the alloy raw material in crucible 4, causing it to heat and melt. The current magnitude and frequency are determined based on the type of alloy being melted; for special alloys, the current frequency is controlled at 1500Hz. After induction heating to the target temperature, the alloy raw material is completely melted into molten metal, and this temperature is held at the target temperature to homogenize the composition and temperature of the molten metal.
[0066] Step 4: Lift the plug and pressurize to fill the mold.
[0067] Based on the initial relationship between P1 and P2 in step two, inert gas is first introduced into the vacuum melting chamber 1 through the melting chamber pressure regulating pipe 2, so that the pressure P1 in the vacuum melting chamber 1 increases to be greater than or equal to the pressure P2 in the pressure regulating wire forming chamber 5; then the plug 6 is switched to the raised state, so that the drain port at the bottom of the crucible 4 is opened; then inert gas is introduced into the vacuum melting chamber 1 through the melting chamber pressure regulating pipe 2, so that the pressure P1 in the vacuum melting chamber 1 is greater than the pressure P2 in the pressure regulating wire forming chamber 5, and the molten metal in the crucible 4 flows downward into the crystallizer 8 under the combined action of gravity and gas pressure difference.
[0068] Specifically, when P1=P2<P0 in step 2, inert gas is first introduced to raise P1 to be greater than or equal to P2, then the plug 6 is lifted, and inert gas is continuously introduced to make P1 greater than P2; when P1<P2=P0 in step 2, inert gas is first introduced to raise P1 to be greater than or equal to P2, then the plug 6 is lifted, and inert gas is continuously introduced to make P1 greater than P2; when P0>P1>P2 in step 2, P1 is already greater than P2, the plug 6 can be directly lifted, and inert gas is continuously introduced to increase the pressure difference to a required value.
[0069] In the above operations, before lifting the plug 6, the pressure P1 in the vacuum melting chamber 1 is adjusted to be greater than or equal to the pressure P2 in the pressure-regulating wire forming chamber 5, which prevents the gas in the pressure-regulating wire forming chamber 5 from being squeezed into the vacuum melting chamber 1 through the liquid discharge port caused by the pressure in the pressure-regulating wire forming chamber 5 being greater than the pressure in the vacuum melting chamber 1. During this process, the flow channel is continuously filled with molten metal, and the gas space of the vacuum melting chamber 1 is not directly communicated with the gas space of the pressure-regulating wire forming chamber 5.
[0070] Step 5: Temperature feedback closed-loop control.
[0071] A temperature sensor 9 is used to monitor in real time the temperature of the molten metal at the liquid inlet of the crystallizer 8, and the pressure difference between the pressure in the vacuum melting chamber 1 and the pressure in the pressure-regulating wire forming chamber 5 is adjusted in real time according to the temperature data from the temperature sensor 9, so as to control the rate at which the molten metal enters the crystallizer 8 and the traction speed of the wire leading rod 7, so that the solid-liquid phase region of the molten metal is located in the cooling zone of the crystallizer 8.
[0072] Specifically, when the melt temperature detected by the temperature sensor 9 is higher than the cooling temperature range of the crystallizer 8, the pressure difference between the pressure in the vacuum melting chamber 1 and the pressure in the pressure-regulating wire forming chamber 5 is reduced to decrease the melt flow rate and lower the traction speed of the wire leading rod 7; when the melt temperature detected by the temperature sensor 9 is lower than the cooling temperature range of the crystallizer 8, the pressure difference between the pressure in the vacuum melting chamber 1 and the pressure in the pressure-regulating wire forming chamber 5 is increased to raise the melt flow rate and increase the traction speed of the wire leading rod 7. Through the above closed-loop feedback control, the solid-liquid phase region of the molten metal is always located in the cooling zone of the crystallizer 8, which ensures that the wire is solidified with compactness and uniform structure, and simultaneously prevents blockage caused by premature solidification of the molten metal at the liquid inlet of the crystallizer 8 or wire breakage caused by incomplete solidification at the outlet.
[0073] Step 6: Solidification and cooling.
[0074] The molten metal cools and solidifies in the crystallizer 8 to form a wire. The molten metal flowing into the crystallizer 8 gradually solidifies under the forced cooling action of the crystallizer 8, forming a blank with a specific cross-sectional shape and size. A mold is installed inside the crystallizer 8; the molten metal flows inside the mold, and heat is transferred to the crystallizer 8 through the mold wall and carried away by the circulating cooling water within the crystallizer 8. As solidification proceeds, the wire continuously moves downwards within the mold and exits from the end pipe of the mold.
[0075] Step 7: Remove by traction.
[0076] The wire guide rod 7 pulls the wire out of the crystallizer 8. When the wire guide rod 7 is activated, it continuously pulls the solidified wire out from the outlet of the pressure-regulating wire forming chamber 5, and the pulling speed is matched with the filling rate of the molten metal.
[0077] Step 8: Collect shares.
[0078] The wire collector 12 collects the wire material. The cooled and solidified wire material is collected into strands of metal wire by the winding drum and the wire pressing device, and the semi-finished metal wire is removed. Specifically, the wire material pulled out from the pressure forming chamber 5 by the wire guide rod 7 enters the wire collector 12 under the continuous conveying of the wire guide rod 7. After entering the wire collector 12, the wire material first passes through the wire pressing device. The wire guide wheel of the wire pressing device reciprocates along the axial direction of the winding drum, evenly distributing the wire material along the axial direction of the winding drum. At the same time, the pressing wheel of the wire pressing device presses the wire material tightly against the surface of the winding drum, so that the wire material is tightly arranged on the winding drum. The winding drum rotates at a constant speed under the drive of the drive motor, continuously winding the wire material onto the surface of the winding drum to form strands of metal wire. After the metal wire on the winding drum has been collected to a predetermined weight or predetermined length, the semi-finished metal wire is removed and subjected to subsequent simple surface treatment to obtain the finished metal wire.
[0079] After step eight is completed, release the pressure in vacuum melting chamber 1 and pressure regulating wire forming chamber 5, open vacuum melting chamber 1, replace the alloy raw material, and repeat steps one to eight to achieve continuous batch production of metal wire.
[0080] This embodiment utilizes vacuum induction melting technology to melt alloy raw materials. It is a special metallurgical process that uses electromagnetic induction to heat and refine metals in a vacuum or inert gas environment. The vacuum environment can effectively remove gaseous impurities such as hydrogen and oxygen, significantly reducing the risk of material brittleness. At the same time, it can remove harmful elements with high vapor pressure (such as Pb and Sn) and avoid impurity segregation. Induction melting has high heating efficiency and also reduces dust emissions during the melting process.
[0081] This embodiment utilizes a composite gradient pressure regulation technology. Before the alloy melting process, the vacuum melting chamber and the pressure-regulating wire-forming chamber below it are evacuated to effectively remove gaseous impurities such as hydrogen and oxygen, reducing gas inclusions and melt oxidation during the melting process. During melting, the vacuum melting chamber and the pressure-regulating wire-forming chamber are isolated in advance, forming two independent cavities. After the alloy melt reaches the rated temperature and is held at that temperature, the plug is lifted, and the vacuum melting chamber is vented, making the pressure inside the vacuum melting chamber greater than the pressure inside the pressure-regulating wire-forming chamber. Under the combined action of gas pressure and gravity, the molten metal is forced into the crystallizer to solidify, achieving composite pressure regulation in the continuous casting process. Simultaneously, a temperature sensor is installed above the crystallizer to adjust the pressure difference between the vacuum melting chamber and the pressure-regulating wire-forming chamber, as well as the traction speed of the wire guide rod, by real-time sensing of the melt temperature. This further regulates the wire forming rate during continuous casting, ensuring that the solid-liquid phase region of the solidified wire is located precisely in the cooling zone of the crystallizer, optimizing the wire microstructure and achieving smooth wire forming.
[0082] This embodiment utilizes continuous casting technology to cool and crystallize the molten metal. As the metal is rapidly cooled, it crystallizes densely, has a uniform structure, and its mechanical properties are enhanced.
[0083] To verify the effect of composite gradient pressure regulation on the solid-liquid phase region, a numerical simulation was performed on the solidification process of the molten metal in the mold. Based on... Figure 5 and Figure 6 Compare the solid fraction distribution before and after the pressure regulation; based on Figure 7 and Figure 8 The temperature distribution before and after the pressure regulation was compared. The simulation results show that the composite gradient pressure regulation effectively acts on the solid-liquid phase region, placing the solid-liquid phase region within the cooling area of the crystallizer.
[0084] Example:
[0085] Equipment and raw material parameters: This embodiment uses a multi-chamber composite gradient pressure-regulating wire short-process preparation device. Vacuum melting chamber 1 is a closed pressure vessel with external dimensions of [missing information]. 500mm × 700mm; The vacuum melting chamber 1 is equipped with an induction coil 3 and a high-purity graphite crucible 4, the inner diameter of which is... The crucible has a diameter of 80mm and a height of 150mm, and the diameter of the drain outlet at the bottom of crucible 4 is... 6mm. The external dimensions of the pressure regulating filament forming chamber 5 are: The inner diameter of the mold in crystallizer 8 is 300mm × 500mm. 2.0mm. The raw material is blocky Al-4.5Cu alloy (its composition is Cu4.0). 5.0 Si≤0.2 , Fe≤0. (The balance is Al and unavoidable impurities), the diameter of the prepared filament is 2.0mm.
[0086] Implementation: Air tightness tests were conducted on the vacuum melting chamber 1 and the pressure-regulating wire forming chamber 5. After confirming good air tightness, a vacuum was evacuated from the vacuum melting chamber 1 through the pressure regulating pipe 2, and a vacuum was evacuated from the pressure-regulating wire forming chamber 5 through the pressure regulating pipe. The vacuum melting chamber 1 was evacuated to ≤5×10⁻²Pa, and the pressure-regulating wire forming chamber 5 was evacuated to ≤10Pa. The plug 6 was then sealed, creating two independent sealed chambers for the vacuum melting chamber 1 and the pressure-regulating wire forming chamber 5. Blocky Al-4.5Cu alloy raw material was added to the high-purity graphite crucible 4. The induction coil 3 was activated, with the current frequency set to 1500Hz, and the power gradually increased to 60 Hz. 80kW, controlling the molten metal temperature to 720℃ 760 Insulation 10 After 15 minutes, the alloy raw materials are completely melted to obtain a molten metal with uniform composition and temperature. The plug 6 is then switched to the raised position to open the drain port; high-purity argon gas (≥99.999%) is introduced into the vacuum melting chamber 1 through the pressure regulating pipe 2. The pressure regulating device was adjusted to raise the absolute pressure inside the vacuum melting chamber 1 to 0.04. 0.08MPa, the pressure regulating spinning chamber 5 maintains an absolute pressure of 5. 15 kPa, thus forming a 0.025 kPa zone between the vacuum melting chamber 1 and the pressure-regulating filament forming chamber 5. A controllable pressure difference of 0.075 MPa; the molten metal in crucible 4 enters the flow channel through the drain port, and then enters the crystallizer 8.
[0087] Temperature sensor 9 monitors the temperature of the molten metal at the inlet of crystallizer 8 in real time, with the target temperature controlled at 660°C. 690 When the temperature is above 690°C At this time, increase the pressure difference between the vacuum melting chamber 1 and the pressure regulating wire forming chamber 5 to reduce the melt flow rate and decrease the traction speed of the wire guide 7; when the temperature is below 660°C At the same time, the pressure difference between the vacuum melting chamber 1 and the pressure regulating wire forming chamber 5 is increased to increase the melt flow rate and the traction speed of the wire guide rod 7 is increased to ensure that the solid-liquid phase region is always within the cooling area of the crystallizer 8. The molten metal flowing into the crystallizer 8 gradually solidifies under the forced cooling action of circulating cooling water at a temperature of 20°C. 25 Cooling intensity is 120 200 The water pressure is 0.2. 0.4MPa, forming 2.0mm filament; start the lead screw 7 to continuously pull the solidified filament out from the outlet of the pressure-regulating filament forming chamber 5, with an initial pulling speed of 0.5. 0.8 Once the filament material stabilizes, gradually increase the speed to 1.0. 1.5 The traction speed is matched with the molten metal filling rate. The wire enters the wire collector 12, is guided and pressed against the surface of the winding drum by the wire feeder and pressure device. The winding drum rotates at a uniform speed under the drive motor, winding the wire into strands to obtain Al-4.5Cu wire semi-finished product. The wire semi-finished product undergoes alkali washing, acid washing, water washing, drying, and fine winding to obtain… Finished product of 2.0mm aluminum alloy additive manufacturing wire.
[0088] While this application has been described herein with reference to specific embodiments, it should be understood that these embodiments are merely examples of the principles and applications of this application. Therefore, it should be understood that many modifications can be made to the exemplary embodiments, and other arrangements can be designed without departing from the spirit and scope of this application as defined by the appended claims. It should be understood that different dependent claims and features herein can be combined in ways different from those described in the original claims. It is also understood that features described in conjunction with individual embodiments can be used in other embodiments.
Claims
1. A multi-chamber composite gradient pressure regulating wire short process manufacturing device, characterized in that, It includes a vacuum melting chamber, a pressure regulating and wire forming chamber, a plug, a pressure regulating pipeline for the melting chamber, a pressure regulating pipeline for the wire forming chamber, an induction coil, a crucible, a crystallizer, a wire guide rod, and a wire collector; The crucible is disposed inside the vacuum melting chamber, and a drain port is provided at the bottom of the crucible. The induction coil is used to heat the alloy raw material inside the crucible. The pressure-regulating filament forming chamber is located below the vacuum melting chamber, and the crystallizer is located inside the pressure-regulating filament forming chamber. The liquid inlet of the crystallizer corresponds to the liquid outlet of the crucible. The plug is located at the drain port of the crucible. The plug has a blocked state and a raised state. In the blocked state, the plug blocks the drain port, so that the vacuum melting chamber and the pressure regulating filament forming chamber form two independent sealed chambers. In the raised state, the drain port is open, and the vacuum melting chamber and the pressure regulating filament forming chamber are connected through the drain port. The pressure regulating pipeline of the melting chamber is connected to the vacuum melting chamber and is used to evacuate the vacuum melting chamber and introduce inert gas. The pressure regulating pipeline of the filament forming chamber is connected to the pressure regulating filament forming chamber and is used to evacuate the pressure regulating filament forming chamber and introduce inert gas. The temperature sensor is located above the liquid inlet of the crystallizer and is used to monitor the temperature of the molten metal at the liquid inlet of the crystallizer in real time. The wire guide rod is located at the outlet of the crystallizer and is used to pull the solidified filament out of the crystallizer; The filament collector is located downstream of the lead wire and is used to collect the filament.
2. The multi-chamber composite gradient pressure zoned wire short process manufacturing apparatus of claim 1, wherein, The preparation apparatus further includes a controller, which is connected to the temperature sensor, the pressure regulating device on the pressure regulating pipeline of the melting chamber, the pressure regulating device on the pressure regulating pipeline of the wire forming chamber, and the wire guide rod. The controller adjusts the pressure difference between the pressure in the vacuum melting chamber and the pressure in the pressure regulating wire forming chamber in real time according to the temperature data of the temperature sensor, so as to control the rate at which the molten metal enters the crystallizer and the traction speed of the wire guide rod, so that the solid-liquid phase region of the molten metal is located in the cooling region of the crystallizer.
3. The multi-chamber composite gradient pressure zoned wire short process manufacturing apparatus of claim 1, wherein, The plug is connected to a drive rod, which passes through the wall of the vacuum melting chamber or the pressure regulating wire forming chamber, and a dynamic sealing structure is provided between the drive rod and the wall.
4. The multi-chamber composite gradient pressure zoned wire short- process manufacturing apparatus of claim 1, wherein, The mold end pipes inside the crystallizer are inclined outwards.
5. The multi-chamber composite gradient pressure zoned wire short- process manufacturing apparatus of claim 1, wherein, The wire collector includes a winding spool and a wire feeding and pressing device; the wire feeding and pressing device is disposed on the inlet side of the winding spool and is used to guide the wire to the winding spool and make the wire tightly arranged on the winding spool, and the winding spool is used to rotate and wind the wire.
6. The multi-chamber composite gradient pressure zoned wire short- process manufacturing apparatus of claim 1, wherein, The vacuum melting chamber is equipped with an observation window for observing the state of the molten metal inside the chamber.
7. The preparation method of the multi-chamber composite gradient pressure-regulating filament short-process preparation device according to claim 1, characterized in that, include: Step 1: Place the alloy raw material in the crucible, with the plug in a sealed state, so that the vacuum melting chamber and the pressure-adjusting wire forming chamber form two independent sealed chambers; Step 2: Evacuate the vacuum melting chamber through the pressure regulating pipeline of the melting chamber, and evacuate the pressure regulating spinning chamber through the pressure regulating pipeline of the spinning chamber; Step 3: Activate the induction coil to perform induction melting, so that the alloy raw material melts into molten metal and is kept at a constant temperature; Step 4: When the pressure in the vacuum melting chamber is less than or equal to the pressure in the pressure regulating wire forming chamber, inert gas is introduced into the vacuum melting chamber through the melting chamber pressure regulating pipe to make the pressure in the vacuum melting chamber greater than the pressure in the pressure regulating wire forming chamber. Then, the plug is switched to the raised state. When the pressure in the vacuum melting chamber is greater than the pressure in the pressure regulating wire forming chamber, the plug can be directly switched to the raised state. Then, inert gas is introduced into the vacuum melting chamber through the melting chamber pressure regulating pipe to make the pressure in the vacuum melting chamber continuously greater than the pressure in the pressure regulating wire forming chamber. Under the combined action of gravity and gas pressure difference, the molten metal enters the crystallizer through the drain port. Step 5: Use the temperature sensor to monitor the temperature of the molten metal at the inlet of the crystallizer in real time, and adjust the pressure difference between the pressure in the vacuum melting chamber and the pressure in the pressure regulating wire forming chamber in real time according to the temperature data of the temperature sensor, so as to control the rate at which the molten metal enters the crystallizer and the traction speed of the wire guide rod, so that the solid-liquid phase region of the molten metal is located in the cooling region of the crystallizer. Step 6: The molten metal is cooled and solidified in the crystallizer to form a wire. Step 7: The wire guide rod pulls the wire out of the crystallizer; Step 8: The filament collector collects the filaments.
8. The preparation method according to claim 7, characterized in that, Let the pressure in the vacuum melting chamber be P1, the pressure in the pressure regulating wire forming chamber be P2, and the atmospheric pressure be P0. In step two, P1 and P2 should satisfy any one of the following relationships: P1=P2 <P0; P1 <P2=P0; P0>P1>P2.
9. The preparation method according to claim 7, characterized in that, In step five, when the melt temperature detected by the temperature sensor is higher than the cooling temperature range of the crystallizer, the pressure difference between the pressure in the vacuum melting chamber and the pressure in the pressure regulating wire forming chamber is reduced, thereby reducing the melt flow rate and decreasing the traction speed of the wire guide rod; when the melt temperature detected by the temperature sensor is lower than the cooling temperature range of the crystallizer, the pressure difference between the pressure in the vacuum melting chamber and the pressure in the pressure regulating wire forming chamber is increased, thereby increasing the melt flow rate and increasing the traction speed of the wire guide rod.
10. The preparation method according to claim 7, characterized in that, In step eight, the cooled and solidified filament is collected into strands of metal wire by a winding bobbin and a wire pressing device, and the semi-finished metal wire is taken out.
Citation Information
Patent Citations
Device for composite vibration continuous casting of homogeneous fine grain cast ingot and continuous casting method
CN114130975A
Alloy continuous casting crystal region ultrasonic wave agitating unit
CN204639082U