A method for multi-field control and parameter matching of composite magnetically controlled MIG welding arc
By configuring a composite magnetic field generator and an alternating composite magnetic field, precise control of the multi-physics field of the MIG welding arc was achieved, solving the problems of unrevealed multi-physics field coupling evolution law and insufficient excitation current matching in the existing technology, thus improving welding quality and stability.
Patent Information
- Application Number
- CN202610948592.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-06-29
- Publication Date
- 2026-11-17
AI Technical Summary
Existing magnetically controlled MIG welding technology suffers from insufficient systematic research on alternating composite magnetic fields, lack of revelation of the evolution law of multi-physics field coupling, lack of quantitative matching between excitation current and welding current, resulting in the attenuation of magnetic field control effect during high-current welding, and the numerical simulation ignores the influence of droplet transition, resulting in limited calculation accuracy.
By configuring a composite magnetic field generator, an alternating composite magnetic field is generated. Utilizing the coupling effect of external electromagnetic force and self-induced electromagnetic force, the MIG welding arc is driven to periodically deflect in the direction perpendicular to the weld and tilt forward in the welding advance direction. This establishes a quantitative matching relationship between the excitation current and the welding current, enabling precise control of the multi-physics field.
It effectively suppressed forming defects such as undercut and hump under high-speed welding conditions, realized stable control of MIG welding arc and reliable prediction of process parameters, and improved welding quality.
Smart Images

Figure CN123103124A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of welding technology, specifically to a method for multi-field control and parameter matching of composite magnetically controlled MIG welding arc. Background Technology
[0002] Gas metal arc welding (GMAW) offers advantages such as low cost, high efficiency, and simple operation, making it widely used in the equipment manufacturing industry. Increasing welding speed is a crucial way to improve production efficiency; however, high-speed MIG welding is prone to weld formation defects such as undercut and humped weld beads. External magnetic field-assisted welding technology can effectively suppress these defects by controlling the arc morphology and molten pool flow.
[0003] However, existing magnetically controlled MIG welding technology has the following shortcomings: (1) Most studies focus on magnetic fields in a single direction (transverse, longitudinal or sharp-angle magnetic fields), while there are few systematic studies on externally applied alternating composite magnetic fields; (2) The understanding of the thermodynamic characteristics of electric arcs under the action of magnetic fields is mostly limited to the macroscopic deflection level, and lacks a systematic revelation of the coupling evolution law of multiple physical fields such as temperature field, current density field, electromagnetic force field, velocity field, and pressure field. (3) The matching of excitation current and welding current relies heavily on experience and lacks a quantitative matching relationship, which leads to a significant decrease in the magnetic field control effect during high-current welding. (4) Existing numerical simulations often neglect the influence of droplet transition, resulting in limited computational accuracy.
[0004] This invention, through systematic numerical simulation, reveals for the first time the comprehensive control mechanism of the multi-physics field of the MIG arc by the applied alternating composite magnetic field, and establishes a quantitative matching relationship between the excitation current and the welding current, providing a theoretical basis and data support for the optimized design of the magnetically controlled MIG welding process. Summary of the Invention
[0005] The purpose of this invention is to overcome the shortcomings of existing technologies and provide a method for multi-field control and parameter matching of composite magnetically controlled MIG welding arcs. By systematically revealing the control laws of composite magnetic fields on arc temperature, current density, self-induced electromagnetic force, applied electromagnetic force, fluid velocity, and arc pressure, this invention establishes a quantitative matching relationship between excitation current and welding current, achieving precise control of the thermodynamic characteristics of the MIG arc. This provides a theoretical basis and process parameter design method for defect suppression in high-speed MIG welding. To achieve the above objectives, the present invention provides the following technical solution: The present invention provides a method for multi-field control and parameter matching of composite magnetic control MIG welding arc, including the following steps: S100, a composite magnetic field generating device is configured at the nozzle of the MIG welding gun, the composite magnetic field generating device includes multiple electromagnet cores distributed in a Y shape, and an excitation coil is wound on each of the electromagnet cores; S200, alternating excitation current is alternately supplied to the excitation coils on both sides to generate an alternating composite magnetic field in the arc space; the alternating composite magnetic field generates a periodically alternating transverse magnetic field component in the direction perpendicular to the weld seam, and generates a longitudinal magnetic field component with a constant direction in the welding advance direction. S300 utilizes the external electromagnetic force generated by the interaction between the alternating composite magnetic field and the MIG welding arc plasma to couple and control the multi-physics field of the MIG welding arc, driving the MIG welding arc to periodically deflect in the direction perpendicular to the weld seam and maintain forward tilt in the welding forward direction, so as to change the pressure distribution of the arc on the workpiece surface. S400: Based on the target arc deflection angle and the target arc tilt angle, obtain a quantitative matching combination of the alternating excitation current and the welding current; wherein, based on the characteristic that the self-induced electromagnetic force of the arc increases with the increase of the welding current and its ability to resist deflection by the external magnetic field is enhanced, when the increase of the welding current causes the actual arc deflection angle or tilt angle to show a decreasing trend, the input amplitude of the alternating excitation current is correspondingly increased to maintain the arc deflection angle and tilt angle within the set effective control threshold.
[0006] Furthermore, the composite magnetic field generating device includes three electromagnet cores arranged in a Y-shape, and the magnetic poles of the three electromagnet cores exhibit an alternating distribution of N and S poles when the excitation coil is energized. When the excitation coil on one side is energized, the magnetic pole of the corresponding electromagnet core on that side has the opposite polarity to the magnetic poles of the other two electromagnet cores, so as to form a magnetic field line loop from the N pole to the S pole in the arc space.
[0007] Furthermore, the material of the electromagnet core is electrical pure iron DT4C, and the number of turns of the excitation coil uniformly wound on each electromagnet core is set to 300~360 turns.
[0008] Furthermore, the output frequency of the alternating excitation current is set to 15~20Hz, and the magnetic induction intensity of the generated alternating composite magnetic field is limited to 5~10mT in the MIG welding arc region and 30~35mT in the workpiece region.
[0009] Furthermore, when the excitation coils on both sides are alternately energized, the direction of the magnetic field lines in space of the alternating composite magnetic field is controlled as follows: In the direction perpendicular to the weld seam, the magnetic field lines in the arc column area periodically change their direction of entry and exit; in the direction of welding advance, the magnetic field lines always enter from the rear side of the MIG welding arc and exit from the front side, so as to form a longitudinal magnetic field component with a constant direction.
[0010] Furthermore, in S300, the mechanical coupling mechanism by which the external electromagnetic force drives the MIG welding arc deflection and forward tilt is specifically as follows: In the direction perpendicular to the weld seam, the self-induced electromagnetic force generated by the MIG welding arc and the external electromagnetic force are in the same direction and superimposed on one side of the welding wire axis, and in opposite directions and cancel each other out on the other side, thereby causing a difference in radial force on the arc, driving the MIG welding arc to periodically deflect from the side with greater force to the side with less force. In the welding forward direction, the force on the arc behind the welding wire is always greater than that on the front side, driving the MIG welding arc to remain tilted forward.
[0011] Furthermore, in S300, the specific manifestations of coupling and controlling the multiphysics field of the MIG welding arc include: Under the coupling effect of the velocity field and the pressure field, the external electromagnetic force causes the motion of the arc plasma to change from being mainly vertical longitudinal flow to being mainly horizontal radial flow, so as to reduce the impact of the plasma on the surface of the workpiece; the pressure distribution of the MIG welding arc on the surface of the workpiece changes from a dumbbell-shaped distribution with a surface peak to a fan-shaped distribution that gradually decreases from top to bottom in the longitudinal direction.
[0012] Furthermore, the effective control threshold is set as follows: the actual arc deflection angle is not less than 10° and the actual arc forward tilt angle is not less than 20°. When obtaining the quantitative matching combination of the alternating excitation current and the welding current, the following control strategy is adopted: When the welding current is in the range of 200A to 250A, the input amplitude of the alternating excitation current is configured to be no less than 6A; When the welding current is greater than or equal to 250A, the input amplitude of the alternating excitation current is increased to more than 8A to compensate for the increased arc stiffness caused by the large current and ensure that the attitude of the MIG welding arc meets the effective control threshold.
[0013] Furthermore, in S400, the specific process of obtaining the quantitative matching combination of the alternating excitation current and the welding current includes a step of pre-calculation using numerical simulation based on the magnetohydrodynamic control equations before actual welding: In the numerical simulation, the self-induced electromagnetic force of the MIG welding arc and the external electromagnetic force generated by the external composite magnetic field are simultaneously introduced into the source term of the momentum conservation equation. The arc deflection angle and forward tilt angle under a given welding current condition are predicted by transient solution, and then the corresponding recommended alternating excitation current is matched.
[0014] Beneficial effects
[0015] This invention utilizes a Y-shaped composite magnetic field generator and an alternating composite magnetic field to drive the MIG welding arc to produce regular lateral periodic deflection and continuous longitudinal forward tilting. This transforms the traditional bimodal distribution of arc pressure into a fan-shaped distribution that decreases from top to bottom, effectively alleviating the local impact pressure of plasma on the molten pool and suppressing forming defects such as undercut and hump under high-speed welding conditions. Simultaneously, this invention establishes a quantitative matching strategy between the alternating excitation current and the welding current based on an effectively adjustable threshold. By dynamically compensating for the excitation amplitude, it overcomes the problem of attenuation of magnetic control effect caused by the enhancement of self-induced electromagnetic force under high current conditions, achieving stable control of the multi-physics field of the MIG welding arc and reliable prediction of process parameters under multiple welding specifications. Attached Figure Description
[0016] Figure 1 This is a flowchart illustrating the overall execution process of the method of the present invention; Figure 2 This is a block diagram of the parameter quantitative matching control logic of the present invention. Detailed Implementation
[0017] To enable those skilled in the art to better understand the present invention, the technical solutions of the present invention will be clearly and completely described below with reference to the accompanying drawings of the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort should fall within the scope of protection of the present invention.
[0018] It should be noted that the terms "first," "second," etc., in the specification, claims, and accompanying drawings of this invention are used to distinguish similar objects and are not necessarily used to describe a specific order or sequence. It should be understood that such data can be interchanged where appropriate so that the embodiments of the invention described herein can be implemented in orders other than those illustrated or described herein. Furthermore, the terms "comprising" and "having," and any variations thereof, are intended to cover a non-exclusive inclusion; for example, a process, method, system, product, or apparatus that comprises a series of steps or units is not necessarily limited to those steps or units explicitly listed, but includes other steps or units not explicitly listed or inherent to such processes, methods, products, or apparatus.
[0019] The present invention will now be described in further detail with reference to the accompanying drawings:
[0020] Example 1:
[0021] like Figure 1-2 As shown, a method for multi-field control and parameter matching of a composite magnetically controlled MIG welding arc includes the following steps: S100, a composite magnetic field generating device is configured at the nozzle of the MIG welding torch. The composite magnetic field generating device includes multiple electromagnet cores distributed in a Y shape, and an excitation coil is wound on each electromagnet core. S200, alternating excitation current is alternately supplied to the excitation coils on both sides to generate an alternating composite magnetic field in the arc space; the alternating composite magnetic field generates a periodically alternating transverse magnetic field component in the direction perpendicular to the weld seam, and a longitudinal magnetic field component with a constant direction in the direction of welding advance. S300 utilizes the external electromagnetic force generated by the interaction of an alternating composite magnetic field and the plasma of the MIG welding arc to couple and control the multi-physics field of the MIG welding arc, driving the MIG welding arc to deflect periodically in the direction perpendicular to the weld seam and to maintain forward tilt in the welding advance direction, thereby changing the pressure distribution of the arc on the workpiece surface. S400 obtains a quantitative matching combination of alternating excitation current and welding current based on the target arc deflection angle and the target arc tilt angle. Among them, based on the characteristic that the self-induced electromagnetic force of the arc increases with the increase of welding current and its ability to resist the deflection of the external magnetic field is enhanced, when the increase of welding current causes the actual arc deflection angle or tilt angle to decrease, the input amplitude of alternating excitation current is increased accordingly to maintain the arc deflection angle and tilt angle within the set effective control threshold.
[0022] Furthermore, the specific implementation process of step S100 is as follows: In a specific implementation, the core physical basis of step S100 of the method for multi-physics field coupling control and parameter matching of MIG welding arc under the action of an external composite magnetic field lies in the precise configuration of the spatial electromagnetic topology at the welding end of the MIG welding torch.
[0023] Specifically, a composite magnetic field generator is coaxially mounted outside the MIG welding torch nozzle. The main supporting frame of this generator is an irregularly shaped electromagnet core, made of DT4C electrical pure iron material with low coercivity and high permeability to reduce hysteresis losses under high-frequency alternating magnetic fields. Spatially, the irregularly shaped electromagnet core exhibits a three-dimensional Y-shaped topological distribution, including a common yoke and three independent magnetic pole arms extending radially from this common yoke towards the central axis of the MIG welding torch (i.e., the direction of wire extension). These are the first, second, and third magnetic pole arms. The end faces of the three magnetic pole arms all face the arc initiation space of the MIG welding arc and are distributed at a predetermined angle in the circumferential direction surrounding the wire axis, thus constructing an asymmetric magnetic flux conduction path in physical structure.
[0024] To ensure the stability of plasma control by the alternating composite magnetic field, the basic physical boundary conditions of the MIG welding torch were calibrated while configuring the composite magnetic field generator. Specifically, the welding wire diameter was limited to 1.2 mm, and the wire extension was controlled at 12 mm to provide a stable arc ignition distance and self-induced electric field space. Simultaneously, argon gas of the required purity was introduced into the nozzle of the MIG welding torch as a shielding gas, with a constant flow rate of 20 L / min. This provided a pure argon plasma fluid medium environment with stable ionization potential for the subsequent high-frequency deflection of the arc.
[0025] An excitation coil made of pure copper wire is wound along the extension path of the irregularly shaped electromagnet core. To satisfy the alternating magnetic field's lateral alternation in the direction perpendicular to the weld seam and the longitudinal constancy in the welding advance direction, the excitation coil is physically divided into independently controlled left and right coil windings. The left coil winding is wound on the outer entity of the second pole arm, and the right coil winding is wound on the outer entity of the third pole arm. The number of turns in each independent coil winding is precisely calibrated within the range of 300 to 360 turns to ensure that a magnetomotive force meeting the control threshold is generated under low input current conditions. The first pole arm, as a common magnetic guide arm for non-independent excitation, together with the second and third pole arms, spatially defines the spatial loop of the magnetic field lines.
[0026] When the excitation power supply connects the excitation signal to the composite magnetic field generator, the coordination logic of the above physical structure manifests as a specific magnetic pole evolution: within a specific energizing half-cycle, only one side of the excitation coil is in a conducting state. For example, when an excitation current is injected into the left coil winding, electromagnetic induction causes the end of the second magnetic pole arm to be energized and polarized to a specific polarity (set as the N pole). Since the first and third magnetic pole arms form a closed permeability channel through a common yoke, the ends of the first and third magnetic pole arms are synchronously induced to be polarized to the opposite polarity (i.e., the S pole) to the second magnetic pole arm. At this time, magnetic field lines emerge from the end of the second magnetic pole arm, which is the N pole, cross the open space where the arc plasma is located, and penetrate into the ends of the first and third magnetic pole arms, which are the S poles, respectively, thereby forming a solidified spatial magnetic flux loop in the MIG welding arc region. In the subsequent half-cycle, excitation current is injected into the right coil winding, and the magnetic pole distribution is reversed accordingly. The polarity state of the first magnetic pole arm is consistent with the associated logic of the conducting side magnetic pole arm. Thus, by using the fixed three-pole arm hardware topology, the periodic forced alternation of the direction of magnetic field line shuttle is realized in the arc region.
[0027] Furthermore, the specific implementation process of step S200 is as follows: After completing the spatial configuration of the composite magnetic field generator, step S200 is executed to inject an alternating composite magnetic field into the arc space. Specifically, an external alternating excitation power supply outputs alternating excitation current to the left and right coil windings. To ensure dynamic matching between the magnetic field alternation frequency and the MIG welding droplet transition cycle, the output frequency of the alternating excitation current is precisely limited to the range of 15Hz to 20Hz. In terms of time-domain control, the alternating excitation power supply is configured in a time-sequential alternating conduction mode, that is, within a complete excitation cycle, current is injected only into the left coil winding in the first half-cycle and only into the right coil winding in the second half-cycle, with no overlap in energization between the two.
[0028] Under this alternating excitation mechanism, the distribution of magnetic field lines in the arc space undergoes periodic spatial reconstruction. During the half-cycle when the left coil winding is conducting, the magnetic field lines originate from the second pole arm and converge towards the first and third pole arms in three-dimensional space. Projecting this spatial magnetic flux density vector onto an orthogonal coordinate system, in the direction perpendicular to the weld (defined as the xoz plane), the magnetic field vector manifests as a transverse magnetic field component traversing the arc column region from left to right; in the welding advance direction (defined as the yoz plane), the magnetic field vector manifests as a longitudinal magnetic field component entering from the rear side of the MIG welding arc and dissipating from the front side.
[0029] When switching to the half-cycle of the right coil winding conduction, the source of the magnetic field lines shifts to the third magnetic pole arm. At this time, the distribution pattern of the spatial magnetic flux density vector undergoes a mirror reversal: in the direction perpendicular to the weld (xoz plane), the magnetic field vector changes to traversing the arc column region from right to left, causing the transverse magnetic field component to complete a 180-degree periodic directional alternation; while in the welding advance direction (yoz plane), since the spatial geometric position of the first magnetic pole arm relative to the conducting arm does not undergo a longitudinal reversal, the magnetic field lines still maintain the physical state of entering from the rear side of the MIG welding arc and scattering from the front side. Through the alternating conduction of the left and right coils, without introducing mechanical moving parts, a dynamic composite magnetic field with transverse periodic direction changes, constant longitudinal direction, and continuous superposition is synthesized within the arc action area.
[0030] Furthermore, by calibrating the amplitude of the alternating excitation current input, the magnetic induction intensity of the alternating composite magnetic field at different spatial gradients was strictly controlled. After attenuation and distribution by the spatial magnetic circuit medium, the magnetic induction intensity of this composite magnetic field in the core region where the MIG welding arc plasma accumulates is maintained between 5 mT and 10 mT, ensuring that the magnetic field can effectively penetrate into the plasma without causing arc interruption. In the molten pool and heat-affected zone near the workpiece surface, the magnetic field lines are highly enriched due to the accretion effect of the ferromagnetic workpiece, and its magnetic induction intensity is limited to between 30 mT and 35 mT. This gradient magnetic induction distribution from top to bottom provides a prerequisite physical field constraint for subsequent asymmetric coupling control of the arc's multiphysics field.
[0031] Furthermore, the specific implementation process of step S300 is as follows: After continuously injecting an alternating composite magnetic field into the arc space, step S300 is executed to achieve deep coupling control of the multiphysics field of the MIG welding arc. The physical origin of this control process lies in the spatial cross-product interaction between the magnetic flux density vector of the alternating composite magnetic field and the current density vector inside the MIG welding arc plasma, thereby exciting a high-frequency dynamic external electromagnetic force field inside the plasma.
[0032] First, at the underlying mechanical coupling mechanism, the applied electromagnetic field completely disrupts the axisymmetric contraction equilibrium dominated solely by self-induced electromagnetic force within the conventional MIG welding arc. In the transverse section perpendicular to the weld direction, the applied electromagnetic force exhibits a vector distribution with completely opposite directions on both sides of the welding wire's central axis; this applied electromagnetic force vector is linearly superimposed on the self-induced electromagnetic force vector, which consistently contracts radially inward. On one side of the welding wire axis, the two mechanical vectors converge, resulting in a mechanical enhancement effect; while on the opposite side, the two mechanical vectors are opposite in direction, resulting in a mechanical cancellation effect. This localized asymmetric mechanical interference constructs an extremely steep transverse fluid pressure gradient within the plasma, forcing the plasma stream to undergo macroscopic displacement from the force-enriched side to the force-attenuated side, thereby driving the arc to produce periodic transverse oscillations. Simultaneously, in the longitudinal section along the welding advance direction, the plasma behind the welding wire is continuously compressed by the downward component of the applied electromagnetic force, while the front side is lifted by the upward component of the applied electromagnetic force. This constant longitudinal pressure difference rigidly constrains the arc's main axis to a forward-leaning posture. During this process, the maximum value of the self-induced electromagnetic force (the order of magnitude is maintained at) It remains dynamically anchored to the deflected core region of the electric arc, thus constraining the accumulation of the electric arc plasma.
[0033] Based on the aforementioned asymmetric dynamic reconstruction, the velocity field (kinematic response) of the arc plasma undergoes a fundamental transformation. Driven by the coupling of self-induced electromagnetic force and applied electromagnetic force, the trajectory of the plasma fluid micro-particles is partially stripped away from the traditional single vertical axial high-speed jet and transformed into a horizontal radial diffusion flow. This mechanism directly suppresses the maximum longitudinal velocity of the plasma within the range of 200 m / s to 480 m / s; simultaneously, due to the alternating transverse pressure gradient, periodically reversing local fluid vortices are excited on both sides of the welding wire axis. This conversion from longitudinal kinetic energy to radial kinetic energy weakens the rigid impact of the plasma on the molten pool in the vertical direction.
[0034] The reconstruction of the velocity field directly dominates the evolution of the topological morphology of the macroscopic pressure field. The pressure distribution of a conventional static MIG welding arc exhibits an axisymmetric bimodal distribution structure with dual extreme peaks at the wire tip and the workpiece surface. However, under the multi-field coupling effect of this invention, due to the hysteresis of the longitudinal high-speed jet and the dissipation of the radial flow, the hydrodynamic impact of the plasma on the workpiece surface is significantly softened. The macroscopic arc pressure field is reshaped from a bimodal distribution into a gradient decay distribution structure that monotonically decreases from top to bottom along the longitudinal direction. The destructive pressure peaks on the workpiece surface are completely eliminated, and the maximum absolute pressure within the arc system (reduced from approximately 800 Pa in the conventional state to the range of 620 Pa to 710 Pa) is retained only in the wire tip region, where the electromagnetic contraction effect is most intense. This suppresses the initiation of physical forming defects such as weld pool collapse, undercut, and hump weld beads under high-speed welding conditions from a hydrodynamic perspective.
[0035] Furthermore, multi-physics coupling control not only acts on the steady-state arc space but also dynamically intervenes in the transient droplet transition cycle of MIG welding. During the process of the liquid metal at the end of the welding wire necking and forming a droplet, the external electromagnetic force field excited by the alternating composite magnetic field directly cuts into the force balance system of the droplet. Under the drag of the external electromagnetic force with lateral periodic changes in direction, the droplet suspended at the end of the welding wire is not only subjected to conventional gravity and surface tension but also gains lateral oscillation kinetic energy at the same frequency as the alternating frequency. This lateral high-frequency oscillation effectively promotes the instability and fracture of the necking liquid bridge and accelerates the droplet's detachment frequency. At the same time, in the flight trajectory of the droplet falling from the arc column to the molten pool, the enthalpy and kinetic energy it carries are forcibly and uniformly dispersed within the aforementioned expanded 120-degree wide sector, completely changing the deep penetration behavior of the droplet's vertical coarse transition in the absence of a magnetic field, and further homogenizing the weld formation at the transient microscopic level of heat and mass transfer.
[0036] In terms of thermodynamic and electrical macroscopic performance, the temperature field evolves from an initial axisymmetric concentrated distribution to an asymmetric broadening distribution accompanied by high-frequency transverse oscillations of the magnetic field frequency and a continuous forward tilt in the longitudinal direction. The effective thermal coupling area between the high-temperature region of the arc core and the workpiece interface expands from a confined circular stagnation point to a wide sector with an angle of approximately 120 degrees, significantly improving the wetting and heating efficiency of the bevel sidewalls. Moreover, the highest thermodynamic temperature of the arc core region remains stably anchored in the ultra-high enthalpy range of 25000K to 36000K. At the same time, the current density field maintains a strictly vertical downward vector within a short-range core radius of 10mm from the welding wire axis to maintain the stability of electron emission at the arc root; while in the long-range region greater than 10mm, the current density vector generates a radial conduction component that follows the alternating rhythm of the excitation current to match the plasma conduction channel after macroscopic deflection.
[0037] Furthermore, the specific implementation process of step S400 is as follows: After completing the dynamic reconstruction of the arc multiphysics field, step S400 is executed to establish a quantitative matching control mechanism between the alternating excitation current and the welding current. To establish this matching relationship, a numerical simulation calculation step based on the magnetohydrodynamic (MHD) control equations is introduced before inputting the actual execution command to the external control equipment to output a recommended combination of process parameters.
[0038] The objective execution process of numerical simulation calculation is as follows: A three-dimensional computational domain for MIG welding arc was constructed, encompassing the wire end face, nozzle wall, and workpiece surface. This domain was spatially discretized using a hexahedral unstructured mesh, with the minimum mesh size for the arc core region set to 0.025 mm. A pressure-based separation solver and the SIMPLE algorithm were used within the computer system for transient solution. In the momentum conservation equation upon which the solution process depends, both self-induced electromagnetic force and applied electromagnetic force components were simultaneously introduced into the momentum source term. The source term expression was defined as the current density vector. The cross product with the total magnetic flux density vector in space, i.e. .
[0039] During the computational domain initialization phase, the argon plasma physical model of the MIG welding arc is set as a continuous fluid medium satisfying the Local Thermodynamic Equilibrium (LTE) assumption. Simultaneously, the key thermophysical parameters of the argon plasma, along with transport coefficients (specifically including electrical conductivity, thermal conductivity, dynamic viscosity, and specific heat capacity) and radiation coefficient, are defined as coupled functions that dynamically change nonlinearly with the local grid node temperature, breaking through the limitations of constant settings. This strong temperature coupling setting of the physical parameters ensures that the Joule heating term in the energy conservation equation and the electromagnetic force source term in the momentum conservation equation can map the actual thermophysical evolution inside the arc in real time.
[0040] The external magnetic field data under the given spatial coordinates is loaded into the solution domain by interpolation algorithm. Iterative calculations are then performed by combining the mass conservation equation, energy conservation equation and Maxwell's equations to output the topological data of the arc under the given welding current input. The actual deflection angle and actual forward tilt angle of the arc center axis are then extracted.
[0041] When extracting and calculating the actual deflection angle and actual forward tilt angle of the arc's central axis, a rigorous mathematical definition is established for its spatial geometric measurement benchmark: a three-dimensional orthogonal coordinate system is constructed with the undeformed welding wire central axis as the z-axis. The actual arc deflection angle θ is rigorously defined as the angle between the extracted arc three-dimensional core temperature field isosurface central axis projected onto the xoz plane perpendicular to the weld direction and the z-axis; the actual arc forward tilt angle φ is rigorously defined as the angle between the arc three-dimensional core central axis projected onto the yoz plane in the welding forward direction and the z-axis. This geometric measurement standard based on orthogonal plane projection effectively eliminates measurement interference and errors caused by the composite bending of the arc space, and establishes a unified process judgment benchmark.
[0042] Based on the above calculation model and actual physical calibration, the system presets the effective control thresholds as follows: the actual arc deflection angle is not less than 10° and the actual arc forward tilt angle is not less than 20°. Subsequently, parameter control is executed according to the following factual quantitative matching logic: First type of control condition (constant welding current, variable excitation current input): When the welding current is set to a constant 200A, the control system adjusts the input amplitude of the alternating excitation current according to the following mapping relationship: When an alternating excitation current of 2A is input to the excitation coil, the measured value of the arc deflection angle is 8.5°~9.0° and the forward tilt angle is 19.0°~19.5°. This state does not trigger the effective control threshold. When the amplitude of the alternating excitation current is increased to 4A, the arc deflection angle is increased to 11.3°~11.7° and the forward tilt angle is increased to 20.5°~21.0°, which meets the effective control threshold. When the amplitude of the alternating excitation current is further increased to 6A, the arc deflection angle reaches 13.0°~13.5° and the forward tilt angle reaches 22.5°~23.0°.
[0043] Within this operating range, for every 2A increase in the amplitude of the alternating excitation current, the system controller will correspondingly increase the target value of the arc deflection angle by approximately 2° and the target value of the forward tilt angle by approximately 1.5°.
[0044] The second type of control condition (the physical evolution process of state decay caused by variable welding current and constant excitation current input): When the alternating excitation current amplitude is fixed at 6A, and the operating command causes the welding current to gradually increase from 200A to 350A, a specific evolution occurs in the internal physical state of the arc: the longitudinal component of the self-induced electromagnetic force changes from... The positive correlation increased to This leads to increased rigidity of the arc plasma stream, and a corresponding increase in the mechanical threshold resisting deflection by the applied magnetic field. Consequently, the measured arc deflection angle monotonically drops from 13.0°~13.5° to 6.5°~7.0°, and the forward tilt angle monotonically drops from 22.5°~23.0° to 18.5°~19.0°.
[0045] Third type of control condition (compensation and matching logic for high-current processes): Based on the state decay pattern detected in the second type of operating condition, the control system embeds the following forced compensation matching strategy: When the current welding current command is within the closed range of 200A to 250A, the lower limit of the amplitude of the alternating excitation current output by the control system is forcibly set to 6A. When the current welding current command exceeds the 250A threshold, the control system triggers a compensation mechanism as the actual arc deflection angle approaches the 10° critical line. This mechanism increases the input amplitude of the alternating excitation current from 6A to 8A or higher, thereby enhancing the welding current. The external electromagnetic force component in the process overcomes the self-induced electromagnetic force constraint caused by the surge under high welding current, ensuring that the reconstructed arc deflection angle and forward tilt angle are forcibly pulled back and stabilized within the effective control threshold range (≥10° and ≥20°).
[0046] Example 2: This embodiment provides a method for multi-field control and parameter matching of composite magnetic control MIG welding arc. The welding material is Q235 low carbon steel, the welding wire is ER50-6, and the workpiece size is 200mm×50mm×5mm.
[0047] 1. Install a magnetic field generating device: A Y-shaped three-dimensional iron core composite magnetic field generator is installed at the nozzle of the MIG welding torch. The three iron cores are arranged in a Y-shape and are made of electrical pure iron DT4C. A copper excitation coil is evenly wound on each iron core, with 300 turns.
[0048] 2. Set excitation parameters: The excitation power supply outputs an alternating excitation current with a frequency of 15Hz. The amplitude of the excitation current is set to 6A, and the two coils are alternately energized. When the left coil is energized, magnetic pole A is the N pole, and magnetic poles B and C are the S poles; when the right coil is energized, magnetic pole B is the S pole, and magnetic poles A and C are the N poles.
[0049] 3. Set welding parameters: Welding current I_w=200A, arc voltage U=28V, shielding gas (pure Ar) flow rate Q=20L / min, welding wire extension 12mm, welding wire diameter 1.2mm.
[0050] 4. Implement welding and multiphysics field control: Start the excitation power supply and MIG welding machine to ignite the electric arc. Under the influence of the alternating composite magnetic field: Temperature field: The electric arc periodically deflects left and right in the direction perpendicular to the weld (deflection angle approximately 13.2°), and tilts forward in the welding advance direction (tilt angle approximately 22.7°). The heating area of the workpiece in the high-temperature zone of the arc expands from a circle to a fan shape, increasing the heating area. The maximum arc temperature is approximately 25300K.
[0051] Current density field: The maximum current density is approximately 10. 8 A / m² appears at the tip of the welding wire. Within a radius of 10mm, it is basically vertically downward; beyond 10mm, a radial component is generated, and its direction changes periodically with the alternation of the magnetic field.
[0052] Self-induced electromagnetic field: The maximum value of the self-induced electromagnetic force is approximately 3.3 × 10⁻⁶. 6 N / m³ appears on both sides of the welding wire tip, pointing from all directions toward the deflected center of the arc, maintaining the arc shape.
[0053] External electromagnetic field: The maximum value of the external electromagnetic force is approximately 5.8 × 10⁻⁶. 5 N / m³. In the direction perpendicular to the weld, when the left coil is energized, the force on the left side is greater than that on the right side, driving the arc to deflect to the right; when the right coil is energized, the arc deflects to the left. In the welding forward direction, the force on the rear side is greater than that on the front side, driving the arc to tilt forward.
[0054] Velocity field: The maximum longitudinal velocity of the arc plasma is about 220 m / s, and periodic reverse eddies are generated on both sides of the welding wire.
[0055] Pressure field: The arc pressure is distributed in a "fan shape", with the maximum value appearing at the end of the welding wire (about 620 Pa). The pressure peak on the workpiece surface disappears, and the arc pressure distribution is more uniform than when there is no magnetic field.
[0056] 5. Verification: In this embodiment, the numerical simulation results of the arc deflection angle (approximately 13.2°) and the forward tilt angle (approximately 22.7°) are basically consistent with the experimental measurement results (the experimental values are 13.21° and 22.73°, respectively), with an error within 5%, which verifies the reliability of this method.
[0057] Example 3: This embodiment investigates the effect of different welding currents on the thermal characteristics of the electric arc. The welding currents were set to 200A, 250A, 300A, and 350A, respectively, and other parameters were the same as in Embodiment 2. =6A).
[0058] The results are shown in the table below:
[0059] Analysis: As the welding current increases, the self-induced electromagnetic force increases significantly, the arc stiffness strengthens, and the ability to resist deflection by the external magnetic field is enhanced, resulting in a significant decrease in both the deflection angle and the forward tilt angle. When At 300A, the deflection angle has decreased to 8.6°, and the pitch angle has decreased to 19.8°, approaching the lower limit of effective control (θ=10°, φ=20°). When At 350A, the deflection angle and forward tilt angle further decreased, and the control effect of the external composite magnetic field was clearly insufficient.
[0060] Matching strategy: For the operating condition of I_w=250A, effective control can still be achieved using I_e=6A; for the operating condition of I_w=300A, the appropriate adjustment should be made... Increase to 8A or higher to restore θ≥10°, φ≥20°; for For a welding condition of 350A, it is recommended to reduce the welding speed or use other welding processes.
[0061] Example 4: (Excitation Current Influence Example - Comparison of 2A, 4A, and 6A) This embodiment investigates the effect of different excitation currents on the thermal characteristics of the electric arc. The excitation currents are set to 2A, 4A, and 6A, respectively, and other parameters are the same as in Embodiment 2. =200A).
[0062]
[0063] Analysis: Increased excitation current leads to increased external electromagnetic force, resulting in a greater pressure difference between the two sides / front and back of the welding wire axis. This increases the force driving arc deflection and forward tilt, thus increasing both the deflection and tilt angles. Simultaneously, the maximum arc pressure decreases with increasing excitation current, which helps reduce the arc's pressure on the molten pool. The arc temperature field remains essentially constant, but the temperature gradient decreases and the arc profile increases.
[0064] Preferred operating point: For =200A, =6A achieves the maximum deflection angle (13.2°) and forward tilt angle (22.7°), while minimizing arc pressure (620Pa), making it the preferred operating point. At I_e=2A, the deflection angle is insufficient (8.7° < 10°), limiting the control effect.
[0065] Example 5 (Numerical Simulation Pre-calculation Example): This embodiment demonstrates how to use numerical simulation to pre-calculate the recommended excitation current and expected arc angle for a given welding current.
[0066] 1. Establish the model: A geometric model of the MIG arc was established. The computational domain was a 20mm × 20mm × 17mm cuboid, containing the welding wire (1.2mm in diameter, simplified as a hemispherical end face), the nozzle (a ring with an inner diameter of 1.2mm and an outer diameter of 15mm), and the workpiece (simplified as a metal wall). A hexahedral unstructured mesh was used, with a minimum mesh size of 0.025mm.
[0067] 2. Set the governing equations: Load the following equations in FLUENT via a UDF: Conservation of mass: ; Conservation of momentum: ; Energy conservation: ; Electromagnetic field: Solved using UDS ;
[0068] 3. Load external magnetic field data The calculated three-dimensional distribution data of the external composite magnetic field are loaded into the electric arc model using an interpolation algorithm.
[0069] 4. Set boundary conditions: Protective gas inlet temperature 400K, velocity The welding wire tip temperature is 2600K, and the current density is calculated according to the effective current formula; the workpiece surface temperature is 1700K, and the potential is 0; the pressure outlet temperature is 1000K, and the relative pressure is 0.
[0070] 5. Solving and Post-processing: Transient solutions are obtained using a pressure-based separation solver and the SIMPLE algorithm, with a time step of 1×10⁻. 5 After the calculation reaches a stable state, the results such as arc temperature field, current density, deflection angle, and forward tilt angle are extracted.
[0071] 6. Preliminary calculation results: for =200A、 =6A, the pre-calculated values are θ≈13.2° and φ≈22.7°, which are consistent with the experimental results of Example 2. For the new operating condition... =280A, pre-calculation can quickly provide recommendations. The value and expected arc angle should be set to avoid a large number of trial welding experiments.
[0072] Example 6: (High Current Matching Example - Welding Current 300A, Excitation Current 8A) This embodiment verifies the effectiveness of increasing the excitation current to 8A when the welding current increases to 300A.
[0073] 1. Operating Condition Settings: Welding current =300A, excitation current =8A, other parameters are the same as in Example 2.
[0074] 2. Expected Results: Based on the results of Example 2, if the following is maintained =6A, in At 300A, the deflection angle is only about 8.6° and the forward tilt angle is about 19.8°, which is below the effective control threshold (θ≥10°, φ≥20°). Increasing I_e to 8A increases the applied electromagnetic force (from 5.8×10⁻⁶). 5 N / m³ increased to approximately 8.3 × 10⁻⁶ 5 The pressure difference between the two sides / front and back of the welding wire axis will recover (N / m³), and the deflection angle is expected to rise to 10°~12° and the forward tilt angle to 20°~22°.
[0075] 3. Verification: Calculations were performed using numerical simulation (according to the method in Example 5). =300A、 Under the 8A operating condition, the deflection angle was approximately 11.2° and the pitch angle was approximately 21.5°, returning to the effective control range. This indicates that the matching strategy of the present invention is effective.
[0076] 4. Maximum protection: when When it is necessary to improve to 10A or above (i.e.) When the current exceeds 330A, the system issues an alarm, indicating that the welding current exceeds the recommended process window and suggesting that the welding speed be reduced or other welding processes be used.
[0077] The above embodiments are only used to illustrate the technical solutions of the present invention, and are not intended to limit it. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some of the technical features. Such modifications or substitutions will not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for multi-field control and parameter matching of a composite magnetically controlled MIG welding arc, characterized in that, Includes the following steps: S100, a composite magnetic field generating device is configured at the nozzle of the MIG welding torch. The composite magnetic field generating device includes multiple electromagnet cores distributed in a Y shape, and each electromagnet core is wound with an excitation coil. S200, alternating excitation current is alternately supplied to the excitation coils on both sides to generate an alternating composite magnetic field in the arc space; the alternating composite magnetic field generates a periodically alternating transverse magnetic field component in the direction perpendicular to the weld seam, and a longitudinal magnetic field component with a constant direction in the direction of welding advance. S300 utilizes the external electromagnetic force generated by the interaction between the alternating composite magnetic field and the MIG welding arc plasma to couple and control the multi-physics field of the MIG welding arc, driving the MIG welding arc to periodically deflect in the direction perpendicular to the weld seam and maintain forward tilt in the welding forward direction, so as to change the pressure distribution of the arc on the workpiece surface. S400: Based on the target arc deflection angle and the target arc tilt angle, a quantitative matching combination of alternating excitation current and welding current is obtained; wherein, based on the characteristic that the self-induced electromagnetic force of the arc increases with the increase of the welding current and its ability to resist deflection by an external magnetic field is enhanced, when the increase of the welding current causes the actual arc deflection angle or tilt angle to decrease, the input amplitude of the alternating excitation current is increased accordingly to maintain the arc deflection angle and tilt angle within the set effective control threshold.
2. The method for multi-field control and parameter matching of a composite magnetically controlled MIG welding arc according to claim 1, characterized in that, The composite magnetic field generating device includes three electromagnet cores arranged in a Y-shape, and the magnetic poles of the three electromagnet cores alternate between N and S poles when the excitation coil is energized. When the excitation coil on one side is energized, the magnetic pole of the corresponding electromagnet core on that side has the opposite polarity to the magnetic poles of the other two electromagnet cores, so as to form a magnetic field line loop from the N pole to the S pole in the arc space.
3. The method for multi-field control and parameter matching of a composite magnetically controlled MIG welding arc according to claim 2, characterized in that, The material of the electromagnet core is electrical pure iron DT4C, and the number of turns of the excitation coil uniformly wound on each electromagnet core is set to 300~360 turns.
4. The method for multi-field control and parameter matching of composite magnetically controlled MIG welding arc according to claim 3, characterized in that, The output frequency of the alternating excitation current is set to 15~20Hz, and the magnetic induction intensity of the generated alternating composite magnetic field is limited to 5~10mT in the MIG welding arc region and 30~35mT in the workpiece region.
5. The method for multi-field control and parameter matching of a composite magnetically controlled MIG welding arc according to claim 4, characterized in that, When the excitation coils on both sides are alternately energized, the direction of the magnetic field lines in space of the alternating composite magnetic field is controlled as follows: In the direction perpendicular to the weld seam, the magnetic field lines in the arc column area periodically change their direction of entry and exit; in the direction of welding advance, the magnetic field lines always enter from the rear side of the MIG welding arc and exit from the front side, so as to form a longitudinal magnetic field component with a constant direction.
6. The method for multi-field control and parameter matching of a composite magnetically controlled MIG welding arc according to claim 5, characterized in that, In S300, the mechanical coupling mechanism by which the external electromagnetic force drives the deflection and forward tilt of the MIG welding arc is specifically as follows: In the direction perpendicular to the weld seam, the self-induced electromagnetic force generated by the MIG welding arc and the external electromagnetic force are in the same direction and superimposed on one side of the welding wire axis, and in opposite directions and cancel each other out on the other side, thereby causing a difference in radial force on the arc, driving the MIG welding arc to periodically deflect from the side with greater force to the side with less force. In the welding forward direction, the force on the arc behind the welding wire is always greater than that on the front side, driving the MIG welding arc to remain tilted forward.
7. The method for multi-field control and parameter matching of a composite magnetically controlled MIG welding arc according to claim 6, characterized in that, In S300, the specific manifestations of coupling and controlling the multiphysics field of the MIG welding arc include: Under the coupling effect of the velocity field and the pressure field, the external electromagnetic force causes the motion of the arc plasma to change from being mainly vertical longitudinal flow to being mainly horizontal radial flow, so as to reduce the impact of the plasma on the surface of the workpiece; the pressure distribution of the MIG welding arc on the surface of the workpiece changes from a dumbbell-shaped distribution with a surface peak to a fan-shaped distribution that gradually decreases from top to bottom in the longitudinal direction.
8. The method for multi-field control and parameter matching of a composite magnetically controlled MIG welding arc according to claim 7, characterized in that, The effective control threshold is set as follows: the actual arc deflection angle is not less than 10° and the actual arc forward tilt angle is not less than 20°. When obtaining the quantitative matching combination of the alternating excitation current and the welding current, the following control strategy is adopted: When the welding current is in the range of 200A to 250A, the input amplitude of the alternating excitation current is configured to be no less than 6A; When the welding current is greater than or equal to 250A, the input amplitude of the alternating excitation current is increased to more than 8A to compensate for the increased arc stiffness caused by the large current and ensure that the attitude of the MIG welding arc meets the effective control threshold.
9. The method for multi-field control and parameter matching of a composite magnetically controlled MIG welding arc according to claim 8, characterized in that, In S400, the specific process of obtaining the quantitative matching combination of the alternating excitation current and the welding current includes a step of pre-calculation using numerical simulation based on the magnetohydrodynamic control equations before actual welding: In the numerical simulation, the self-induced electromagnetic force of the MIG welding arc and the external electromagnetic force generated by the external composite magnetic field are simultaneously introduced into the source term of the momentum conservation equation. The arc deflection angle and forward tilt angle under a given welding current condition are predicted by transient solution, and then the corresponding recommended alternating excitation current is matched.