A triangular-hole conductive tip, its manufacturing process, and a method for detecting wear on the power supply section of the conductive tip.
By improving the wear resistance and self-centering capability of the conductive tip through triangular hole structure and cold extrusion molding technology, and combining it with current characteristic monitoring to realize wear warning, the problems of rapid wear of conductive tip and poor protective gas conduction are solved, thereby improving welding stability and production efficiency.
Patent Information
- Application Number
- CN202611214096.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-11
- Publication Date
- 2026-11-17
AI Technical Summary
Existing contact tips suffer from problems such as rapid wear, unstable conductivity, uneven weld seam, increased spatter, and short lifespan under long-term high-speed wire feeding welding conditions. Furthermore, they lack effective wear warning and have poor protective gas flow guidance, leading to a decline in welding quality and production efficiency.
The conductive nozzle features a triangular hole structure, combined with cold extrusion molding and heat treatment technology to form a work-hardened wear-resistant layer. It also provides passive wear warning by observing changes in welding current characteristics and integrates an air distribution structure to optimize the protective airflow field.
It improves the self-centering accuracy and welding stability of the contact tip, reduces wire feeding friction resistance, extends service life, reduces spatter and porosity defects, and achieves accurate wear warning and efficient protective gas flow.
Smart Images

Figure CN123103130A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of welding equipment technology, and in particular to a triangular hole conductive nozzle, its manufacturing process, and a method for detecting wear on the power supply section of the conductive nozzle. Background Technology
[0002] Gas shielded arc welding (GSAW) is one of the most widely used welding processes in modern manufacturing, with applications in fields such as engineering machinery, automobile manufacturing, shipbuilding, and steel structures. The contact tip, as a core and easily worn component of the GSAW torch, has two main functions: first, to continuously conduct welding current to the welding wire through close contact with the wire via its inner hole, igniting and maintaining a stable arc between the wire and the base metal; and second, to guide and position the continuously fed welding wire, ensuring accurate alignment between the wire's exit position and the weld seam. The conductivity, wear life, and guiding accuracy of the contact tip directly determine the stability of the welding arc, the quality of the weld formation, and the continuous operating efficiency of welding production.
[0003] Currently, most conductive tips in the industry are made of copper-based alloys such as pure copper, chromium-zirconium copper, and beryllium copper, with the inner hole mostly being a circular through-hole structure. In actual production, the failure of conductive tips mainly manifests as inner hole wear: the welding wire passes through the inner hole continuously at a constant speed driven by the wire feeding mechanism. Copper shavings, oxide scale, and spatter from the welding process on the surface of the welding wire continuously rub against the inner hole wall, especially in the power supply contact area near the outlet, where the wear rate is fastest due to the coupling effect of arc heat radiation and frictional wear. As the wear of the inner hole increases, the hole diameter gradually expands, the contact area between the welding wire and the inner hole decreases, and the contact resistance increases, leading to problems such as unstable conductivity, arc drift, and increased spatter. In severe cases, it can cause welding defects such as welding wire misalignment, weld deviation, and excessive porosity, and even failures such as welding wire sticking to and burning off the conductive tip.
[0004] Currently, most mainstream conductive tips in the industry adopt a circular inner hole structure. Under long-term high-speed wire feeding welding conditions, the inherent structural defects of the circular hole gradually become apparent:
[0005] 1. To ensure smooth wire feeding, the inner diameter of the round hole must be slightly larger than the diameter of the welding wire. There is a radial movement gap in the welding wire within the hole. During the wire feeding process, the welding wire is easily affected by the resistance of the wire feeding hose, the squeezing of the wire feeding wheel, and the heat deformation of welding. This can cause the welding wire to run eccentrically against the wall of one side of the hole, resulting in the displacement of the conductive contact point, the drift of the arc root, and uneven width of the weld. In severe cases, it can lead to a surge in spatter.
[0006] 2. The round hole and the welding wire are in contact with each other on an arc surface, resulting in a large actual contact area and high frictional resistance during wire feeding. For soft or thin-walled welding wires such as aluminum welding wire and flux-cored welding wire, problems such as wire being squeezed and deformed, and the copper plating layer on the surface being scraped off are likely to occur. In high-speed automated welding scenarios, wire feeding jamming and poor retraction are likely to occur.
[0007] 3. Copper shavings that fall off the surface of the welding wire and molten metal slag that splashes during welding can easily get stuck between the welding wire and the hole wall after entering the round hole, causing hard jamming. This can result in unstable wire feeding and arc interruption, or even welding wire sticking and burning the contact tip, causing unplanned downtime.
[0008] 4. The end face of the round hole and the inner hole are continuous arc surfaces. Welding spatter is prone to adhere and solidify over a large area on the exit end face and the inner hole wall, and it is difficult to remove completely during cleaning. Repeated cleaning can easily damage the precision of the inner hole.
[0009] 5. Eccentric operation of the welding wire will cause concentrated wear on one side of the round hole, quickly wear out the axial groove, and after the hole diameter is out of round, the centering and conductivity will drop sharply, resulting in a short effective service life and severe performance degradation throughout the entire life cycle.
[0010] 6. The structure of the round hole tightly wrapping the welding wire is not conducive to heat dissipation in the inner hole. During continuous high-current welding, the temperature at the tip of the contact tip rises rapidly, and the base material is prone to oxidation and softening, which further accelerates wear and increases the risk of wire sticking.
[0011] To improve the performance of conductive nozzles, the industry has developed irregular internal hole structures such as triangular holes and plum blossom holes to solve the above problems.
[0012] However, existing technologies still have the following shortcomings:
[0013] Firstly, most conductive nozzles do not have wear warning functions. Maintenance personnel can only replace them periodically based on experience or only stop the machine to replace them after welding defects occur. The former leads to excessive waste of consumables, and the latter is prone to batch welding quality problems. There is a lack of simple and reliable passive wear identification mechanism.
[0014] Secondly, the methods for improving wear resistance are limited, and relying solely on material upgrades is costly. The work hardening effect brought about by the molding process is not synergistically designed with the material heat treatment strengthening, resulting in limited improvement in wear resistance.
[0015] Third, the shielding gas has poor flow guidance effect. The existing contact nozzle only serves as a conductive and guiding component. The shielding gas mainly relies on the welding torch nozzle for flow guidance. Turbulence zone is easily formed in the outlet area of the contact nozzle, and air is easily drawn into the arc area, resulting in defects such as porosity in the weld.
[0016] Fourth, existing conductive tip wear detection solutions are mostly designed for special oscillating welding torches with built-in welding wire guides, which are complex in structure and cannot be adapted to general-purpose integrated conductive tips. Moreover, the detection logic mostly uses a single current threshold comparison, which is severely affected by operating conditions such as power grid voltage fluctuations, wire feed speed adjustments, and changes in process parameters, resulting in a high false alarm rate. It cannot accurately distinguish between operating condition fluctuations and actual wear, nor can it achieve graded assessment of wear degree and prediction of remaining life. Summary of the Invention
[0017] To solve the above problems, the present invention adopts the following technical solution.
[0018] A triangular-hole conductive nozzle includes a nozzle body, which has a threaded connection section, a cylindrical section, and a tapered section arranged sequentially along the axial direction. The nozzle body has an inner hole along the axial direction for the welding wire to pass through. The inner hole is divided into an outlet section and an inlet section. The outlet section is located within the tapered section and is a triangular hole with a triangular cross-section. The inlet section is a circular hole with a circular cross-section, the cross-sectional area of which is not greater than the area of the inscribed circle of the triangular hole. A tapered hole is provided at the top of the outlet section. The triangular hole constitutes the power supply contact part of the conductive nozzle. A wear warning transition section is provided between the triangular hole and the circular hole of the inlet section. The inner diameter of the wear warning transition section is greater than the circumscribed circle diameter of the triangular hole. When the power supply contact part of the triangular hole wears to its limit, the welding wire contacts the inner wall of the wear warning transition section, the power supply point moves backward towards the wire inlet side, and the welding current drops to a preset wear threshold, achieving early wear identification.
[0019] Furthermore, the outer walls of the cylindrical and conical sections are symmetrically provided with clamping planes for tightening the clamping tool.
[0020] Furthermore, the outer wall of the cylindrical section is provided with a circumferentially extending gas distribution ring groove, and multiple inclined guide gas holes are evenly distributed circumferentially in the gas distribution ring groove. The guide gas holes extend obliquely from the gas distribution ring groove toward the front end of the conical section, and are used to guide the protective gas to the welding area to form a uniform protective atmosphere.
[0021] Furthermore, the three edges of the triangular hole are all provided with transition rounded corners, and the inner wall of the triangular hole is formed by cold extrusion to form a work-hardened wear-resistant layer, the hardness of which is higher than the hardness of the conductive nozzle body substrate.
[0022] A manufacturing process for the above-mentioned triangular hole conductive tip includes the following steps in sequence:
[0023] Process 1: Material cutting. Take copper-chromium-zirconium alloy rods and feed them into the cutting equipment. Cut the rods into billets according to the design length. After completion, randomly inspect the appearance, outer diameter and length of the billets.
[0024] Step 2: Drilling. Drill axial through holes in the blank to form a circular inlet section inner hole and a wear warning transition section cavity. Use a through needle and a no-go gauge to check the hole diameter for pass and no-go, and discard blanks with out-of-tolerance hole diameters.
[0025] Step 3: Triangular and conical hole forming. Position and clamp the drilled blank, and use a cold extrusion triangular punch to extrude the triangular hole outlet section and the front conical hole at the conical end of the blank. After forming, inspect the outline, fillet and taper dimensions of the triangular hole.
[0026] Step 4: CNC machining. After cleaning the copper shavings and impurities from the surface of the blank, the blank is fed into the vibratory plate of the CNC lathe to machine the threaded connection section, cylindrical section, conical section and air distribution ring groove. At the same time, the symmetrical clamping plane and air guide hole of the cylindrical section are milled. After machining, the blank is inspected against the full dimensions of the drawing.
[0027] Step 5: Surface treatment. The workpiece is successively subjected to pickling, multi-stage cleaning with pure water, and passivation to remove machining burrs, oil stains and oxide scale from the inner hole and outer surface.
[0028] Step 6: Full inspection of finished products, checking the threads, inner holes, shape, clamping surfaces, and appearance defects of the workpiece item by item;
[0029] Step 7: Quantitative sealing and packaging, qualified products are repackaged, labeled and put into storage.
[0030] Furthermore, after drilling in step 2, a solution heat treatment is added: the billet is placed in an argon-protected furnace for heat preservation, and then water-quenched for cooling; after CNC machining in step 4, an aging heat treatment is added: after heat preservation, it is slowly cooled in the furnace, and chromium-zirconium strengthening phase is precipitated in the matrix to improve the matrix strength, electrical conductivity and wear resistance.
[0031] Furthermore, in step 5, the pickling process involves soaking in a sulfuric acid solution, followed by ultrasonic cleaning with deionized water, and then soaking in a benzotriazole passivation solution before drying.
[0032] A method for detecting wear on the power supply section of a triangular-hole conductive nozzle includes the following steps:
[0033] S1. Initial Calibration: After installing a brand-new triangular hole contact tip, the welding current time-domain signal during the stable welding stage is collected under standard welding process parameters; the ratio of the difference between the current peak and valley values within the time window to the average current value is defined as the current fluctuation rate; the frequency band more than 3 times the fundamental frequency of the welding current is defined as the high-frequency band; the ratio of the high-frequency band energy to the total energy of the entire frequency band is defined as the high-frequency energy proportion; the current spectrum is obtained by fast Fourier transform of the collected time-domain signal, and a benchmark feature vector including the benchmark current mean, benchmark current fluctuation rate, and benchmark high-frequency energy proportion is established; at the same time, based on the wear evolution law of the three-point contact of the triangular hole, a three-level wear membership function of light wear, moderate wear, and extreme wear is established through wear calibration test, and each level of membership function corresponds to the membership mapping relationship of each feature quantity;
[0034] S2. Real-time feature extraction: During the welding production process, real-time welding current data is continuously collected in fixed time windows. The average current value and current fluctuation rate are calculated for the time domain signal of each time window. At the same time, the high-frequency energy ratio is extracted by fast Fourier transform to form a real-time feature vector.
[0035] S3. Fuzzy Comprehensive Judgment: Substitute each feature quantity in the real-time feature vector into the three-level wear membership function to calculate the membership degree of each feature quantity corresponding to each wear level. Then, obtain the comprehensive membership degree value through weighted average and take the wear level corresponding to the maximum comprehensive membership degree as the current judgment result. When the wear level is judged to be the extreme wear level for a consecutive preset number of time windows, trigger the contact tip replacement warning.
[0036] Furthermore, in the fuzzy comprehensive determination of step S3, the load current of the wire feeding motor is introduced as an auxiliary correction feature, and an adaptive weight allocation algorithm is used to adjust the weight coefficients of the electrical feature and the wire feeding resistance feature:
[0037] The operating current of the wire feeding motor is collected in real time, and the characteristic value of the wire feeding resistance is calculated. The characteristic value of the wire feeding resistance is the ratio of the real-time current of the wire feeding motor to the reference current of the wire feeding motor during the calibration stage. The weights are dynamically allocated according to the ratio of the current welding current fluctuation rate to the reference current fluctuation rate: when the ratio is ≤1.2, the weight of the comprehensive welding current characteristic is set to 0.7 and the weight of the wire feeding resistance characteristic is set to 0.3; when the ratio is ≥1.5, the weight of the comprehensive welding current characteristic is reduced to 0.5 and the weight of the wire feeding resistance characteristic is increased to 0.5; when the ratio is between 1.2 and 1.5, the weights are calculated by linear interpolation. The comprehensive membership value is recalculated based on the weighted feature vector to correct the wear judgment result.
[0038] Furthermore, in step S2, the collected real-time welding current data is first normalized and corrected for operating conditions before feature extraction; simultaneously, a wear trend prediction mechanism based on the sliding window least squares method is introduced:
[0039] The normalization correction formula for operating conditions is:
[0040]
[0041] Among them I 实测 U is the measured instantaneous current value. 基准 U is the reference value for welding voltage during the calibration phase. 实测 This is the current measured welding voltage value, v 基准 To calibrate the wire feed speed, v 实测 This is the current measured wire feeding speed;
[0042] Collect the membership values of the limit wear for a preset number of N consecutive time windows. With the cumulative welding time as the abscissa and the membership value of the limit wear as the ordinate, use the sliding window least squares method to fit the wear degree evolution curve and extrapolate to predict the remaining welding time when the membership value reaches the limit wear threshold. When the predicted remaining welding time is lower than the preset safety threshold, trigger a preventive replacement warning in advance.
[0043] Compared with the prior art, the present invention has the following advantages:
[0044] The conductive tip of this invention adopts a triangular hole outlet section structure, which has high self-centering accuracy and good welding stability. The triangular hole relies on three contact edges to form a natural three-claw self-centering structure, and the welding wire is always constrained on the central axis of the hole. Even if there is slight wear on the hole wall, the centering effect can still be maintained. This avoids the problems of eccentric conduction and arc drift in the round hole from the root. The weld formation is uniform and consistent, and the amount of spatter is significantly reduced.
[0045] The present invention features a triangular hole that makes line contact with the welding wire along three axial edges. The actual contact area is much smaller than that of the arc surface contact of the circular hole, which greatly reduces the frictional resistance of wire feeding and makes wire feeding smoother and easier. It is especially suitable for soft welding wires such as aluminum welding wire and flux-cored welding wire, which can reduce the problems of wire extrusion deformation and coating scraping, and support higher-speed automated welding.
[0046] The three corners of the triangular hole of the present invention form independent chip gaps. Copper chips that fall off the welding wire and splashed slag can be pushed into the corner gaps and will not be squeezed between the welding wire and the contact wall, causing jamming. This greatly reduces wire blockage, nozzle sticking and arc interruption failures, and extends the continuous welding time.
[0047] The effective contact area between the triangular hole end face and the inner wall of this invention is small, making it difficult for welding spatter to adhere firmly to the contact edge; a small amount of spatter falling into the corner gap does not affect the normal passage of the welding wire, and spatter in the non-contact area is easier to remove during cleaning, resulting in higher maintenance efficiency.
[0048] The three edges of the triangular hole in this invention bear wear evenly, avoiding the problem of concentrated wear grooves on one side of the circular hole. As the amount of wear increases, the geometric structure can still keep the welding wire centered, and the conductivity and guiding performance decays gradually. The performance retention is better throughout the entire life cycle, and the effective service life is significantly improved.
[0049] The three-point contact pressure of the triangular hole in this invention is uniform and consistent, making it less prone to momentary disconnection or sudden resistance changes during dynamic wire feeding, and the arc combustion is more stable; at the same time, the corner gap forms a natural heat dissipation channel, which can accelerate the dissipation of heat from the inner hole, avoid overheating and oxidation of the conductive tip caused by excessive tight wrapping, and indirectly extend the service life.
[0050] This invention features a built-in wear warning transition section, eliminating the need for additional sensors. It identifies the wear limit simply by observing changes in the welding current, achieving passive wear warning. This effectively prevents welding quality problems caused by excessive wear of the conductive tip. The structure is simple and reliable, and it is compatible with all standard welding torch interfaces.
[0051] The present invention integrates a gas distribution structure into the conductive nozzle. Through the circumferential gas distribution ring groove and the inclined guide gas hole, the protective gas is precisely guided to the welding area. This can optimize the distribution of the protective gas flow field at the outlet, reduce turbulence and air entrainment, improve the weld protection effect, and reduce the incidence of porosity defects.
[0052] This invention employs cold extrusion to form triangular holes, which can create a continuous work-hardened layer on the inner wall, improving surface hardness and wear resistance. Combined with solution treatment and aging heat treatment, precipitation strengthening further enhances the matrix strength and conductivity, achieving a synergistic effect of deformation strengthening and precipitation strengthening, significantly extending wear life while ensuring high conductivity.
[0053] The preparation process of this invention is mature and controllable. The surface quality of the inner hole formed by cold extrusion is better than that of traditional drilling process. The material flow lines are complete without cutting, the product consistency is good, it is suitable for industrial mass production, and the production cost is controllable.
[0054] The wear detection method of this invention adopts fuzzy comprehensive judgment by multi-dimensional feature fusion, combining current amplitude, fluctuation characteristics and frequency domain energy characteristics to comprehensively reflect the wear evolution process of the triangular hole conductive tip. The judgment accuracy is much higher than that of the single threshold judgment method. The introduction of wire feeding resistance characteristics to assist in verification can further distinguish abnormal states such as contact wear and wire feeding jamming.
[0055] The detection method of this invention sets up a normalization correction and adaptive weight adjustment mechanism for working conditions, which can effectively eliminate interference from working conditions such as power grid voltage fluctuations and wire feeding speed adjustments. It can maintain stable detection accuracy and low false alarm rate even in complex industrial environments. It also has a wear trend prediction function, which can predict the remaining service life in advance, support preventive maintenance, and help optimize the welding production operation and maintenance rhythm and improve production continuity. Attached Figure Description
[0056] Figure 1 This is a perspective view of the triangular hole conductive nozzle of the present invention;
[0057] Figure 2 This is a front view of the triangular hole conductive nozzle of the present invention;
[0058] Figure 3 for Figure 2 Sectional view along line AA;
[0059] Figure 4 is a flowchart of the wear detection method of the present invention.
[0060] Explanation of reference numerals in the attached figures:
[0061] In the diagram: 1. Threaded connection section; 2. Cylindrical section; 3. Conical section; 4. Inlet section; 5. Outlet section; 6. Wear warning transition section; 7. Air distribution ring groove; 8. Air guide hole; 9. Clamping plane. Detailed Implementation
[0062] The technical solutions of the present invention will be clearly and completely described below with reference to the accompanying drawings of the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without creative effort are within the scope of protection of the present invention.
[0063] In the description of this invention, it should be noted that the terms "upper," "lower," "inner," "outer," "top / bottom," etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. They are used only for the convenience of describing the invention and for simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on the invention. Furthermore, the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance.
[0064] In the description of this invention, it should be noted that, unless otherwise explicitly specified and limited, the terms "installed," "equipped with," "sleeved / connected," "connected," etc., should be interpreted broadly. For example, "connection" can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium; it can be a connection within two components. Those skilled in the art can understand the specific meaning of the above terms in this invention based on the specific circumstances.
[0065] Example
[0066] like Figure 1-3 As shown, the triangular-hole conductive nozzle of the present invention has a conductive nozzle body with a rotating structure. The conductive nozzle body is provided with a threaded connection section 1, a cylindrical section 2, and a tapered section 3 sequentially from back to front along the axial direction. The threaded connection section 1 is used to connect with the conductive nozzle seat at the front end of the welding torch, realizing mechanical fixation and conductive path conduction; the cylindrical section 2 is the main support section of the conductive nozzle; the tapered section 3 is a front end shrinking structure, used to reduce the end size, adapt to the internal space of the welding torch nozzle, and be close to the welding area.
[0067] In this embodiment, the conductive nozzle body has a through-hole along the axial direction, allowing the welding wire to enter from the rear end and exit from the front end. The inner hole is divided into an inlet section 5, a wear warning transition section 6, and a triangular hole outlet section 4 from back to front.
[0068] In this embodiment, the inlet section 5 is a circular hole with a circular cross-section. The hole diameter is slightly larger than the diameter of the welding wire. It mainly serves as a guide for the welding wire to enter. The cross-sectional area of the circular hole is not larger than the area of the inscribed circle of the triangular hole, so as to ensure that the welding wire can reliably contact the hole wall after entering the triangular hole area.
[0069] In this embodiment, the triangular outlet section 4 is located within the conical section 3, and its cross-section is an equilateral triangle with rounded corners on all three edges to prevent the edges from scratching the welding wire. The three sides of the triangular hole form a three-point contact portion with the welding wire, which provides more contact points and more stable conductivity compared to the line contact of a traditional round hole, while also providing better centering and guiding effect for the welding wire. The front end of the triangular outlet section 4 is provided with a front conical hole 7, which is an outwardly expanding conical hole that reduces slag accumulation at the outlet and guides the welding wire to be fed out smoothly.
[0070] In this embodiment, the wear warning transition section 6 is located between the inlet section 5 and the triangular hole outlet section 4. The wear warning transition section 6 is a cylindrical cavity with an inner diameter larger than the outer diameter of the triangular hole. During normal use of the contact tip, the welding wire only contacts the inner wall of the triangular hole outlet section 4 to supply power, and the power supply point is located in the front triangular hole area. When the triangular hole continues to wear and the diameter gradually expands to its limit, the welding wire will shift backward and contact the inner wall of the wear warning transition section 6. At this time, the power supply point moves backward toward the inlet side, the effective conductive length of the welding wire increases, the loop resistance increases, and ultimately the welding current drops significantly. By identifying this change in current characteristics, it can be determined that the contact tip has reached the wear limit, realizing passive wear warning. The axial length of the wear warning transition section 6 has been optimized to ensure that the current drop after wear is sufficient to be detected and identified, while avoiding excessive backward movement of the power supply point, which would cause excessive current drop and affect welding stability.
[0071] In this embodiment, two clamping planes 9 are symmetrically arranged on the outer wall of the cylindrical section 2 to provide a force application surface for clamping tools such as wrenches, which facilitates the installation and removal of the conductive nozzle and avoids slippage during tightening.
[0072] In this embodiment, the outer wall of the cylindrical section 2 is also provided with a circumferentially extending gas distribution ring groove 7. The gas distribution ring groove 7 is an annular groove that communicates with the shielding gas cavity inside the welding torch. Multiple inclined guide gas holes 8 are evenly distributed circumferentially at the bottom of the gas distribution ring groove 7. The guide gas holes 8 extend radially inward and inclined towards the front end of the conical section 3, forming a certain angle with the axis of the contact tip. After the shielding gas enters the gas distribution ring groove 7 from the welding torch gas path, it is evenly distributed through the multiple guide gas holes 8 and blown out towards the front welding area along the inclined direction. This forms a uniform annular shielding gas curtain around the contact tip, optimizing the flow field distribution in the arc area, reducing turbulence and air entrainment, and improving the weld protection effect.
[0073] In this embodiment, the inner wall of the triangular hole outlet section 4 is formed by cold extrusion. During the cold extrusion process, the material undergoes plastic deformation, the grains are refined, and the dislocation density is significantly increased, thereby forming a continuous work-hardened wear-resistant layer on the surface. Its hardness is higher than that of the conductive nozzle body matrix, which can effectively improve the friction and wear resistance of the inner hole. Combined with subsequent heat treatment precipitation strengthening, wear resistance and conductivity can be improved simultaneously.
[0074] Manufacturing process of triangular hole conductive tip
[0075] In this embodiment, the conductive tip substrate is made of copper-chromium-zirconium alloy rod, and the specific manufacturing process includes the following steps in sequence:
[0076] Step 1: Blanking. Select copper-chromium-zirconium alloy rods with a diameter that meets the design requirements, feed them into an automatic cutting machine, and cut them into rod-shaped blanks according to the designed length of the conductive tip. After cutting, sample the blanks for inspection to check for cracks, dents, and other defects. At the same time, check the outer diameter and length dimensions, and discard blanks with dimensions that are out of tolerance to ensure consistency in subsequent processing.
[0077] Step 2: Drilling and Solution Heat Treatment. The billet is clamped in the drilling machine station, and a deep-hole drill is used to drill through the billet along its axial direction. First, the smaller diameter inlet section 5 (inner hole) is machined, and then a larger diameter wear warning transition section 6 (cavity) is machined using a reamer, ensuring the coaxiality of the two sections meets the requirements. After drilling, a standard through-hole needle and no-go-no-hole gauge are used to check the hole diameter for permeability, and billets with out-of-tolerance hole diameters are discarded.
[0078] After drilling, solution heat treatment is performed: the billet is neatly placed in an argon-protected furnace and held at a set temperature for a period of time to allow chromium and zirconium in the alloy to fully dissolve into the copper matrix to form a supersaturated solid solution; after holding, it is quickly taken out and water-quenched to cool it down, and the high-temperature solid solution state is retained to room temperature to prepare for subsequent aging precipitation strengthening.
[0079] Step 3: Cold Extrusion Forming of Triangular and Conical Holes. The solution-treated billet is positioned and clamped in the tooling of the cold extrusion equipment. A high-precision cemented carbide triangular punch is used to apply axial extrusion pressure from the conical end of the billet, forming the triangular hole exit section 4 and the conical hole structure at the front end in a single extrusion process. During cold extrusion, the material undergoes plastic flow along the punch contour, forming a complete inner wall of the triangular hole, while simultaneously producing a work-hardening effect on the surface. After extrusion forming, a special inspection tool is used to check the contour dimensions of the triangular hole, the size of the transition fillet, and the taper of the conical hole to ensure that the forming accuracy meets the requirements.
[0080] Step 4: CNC Machining and Aging Heat Treatment. After cleaning the copper shavings and extrusion burrs from the surface of the blank, it is fed into the vibratory feeder mechanism of the CNC lathe. CNC turning sequentially processes the external thread of the threaded connection section 1, the outer diameter of the cylindrical section 2, the outer conical surface of the tapered section 3, and the air distribution ring groove 7 on the outer wall of the cylindrical section 2. After turning, the machining station is switched to milling to machine the symmetrical clamping planes on both sides of the cylindrical section 2. Simultaneously, deep hole drilling is used to machine multiple inclined guide air holes 8 at the bottom of the air distribution ring groove 7. After all machining is completed, a full-dimensional inspection is performed against the product drawings to ensure that all dimensional tolerances meet the design requirements.
[0081] After machining, the workpiece undergoes aging heat treatment: the workpiece is placed in an aging furnace and held at a set temperature for a period of time to allow the chromium-zirconium reinforcing phase to precipitate in the supersaturated solid solution, thereby improving the strength and hardness of the matrix while maintaining excellent electrical conductivity; after the holding period, the workpiece is slowly cooled with the furnace to avoid generating internal stress.
[0082] Step 5: Surface Treatment. The workpiece undergoes pickling, multi-stage pure water cleaning, and passivation treatment in sequence: First, it is immersed in a dilute sulfuric acid solution to remove oxide scale and oil stains from the inner and outer surfaces of the workpiece; then, it is ultrasonically cleaned multiple times with deionized water to thoroughly remove residual acid and debris from the inner pores; finally, it is immersed in a benzotriazole passivation solution to form a passivation protective film on the workpiece surface, preventing oxidation and discoloration during storage and improving appearance quality and rust resistance. After treatment, the workpiece is dried.
[0083] Step 6: Finished Product Inspection. Each item on the dried finished product is inspected, including thread check, internal hole contour accuracy, external dimensions, clamping surface parallelism, and visual inspection for defects. Defective products are rejected.
[0084] Step 7: Quantitative Sealing and Packaging. The inspected and qualified finished products are packaged in the prescribed quantities, sealed, and labeled before being stored in the warehouse.
[0085] Wear detection method for power supply section of triangular hole conductive nozzle
[0086] like Figure 4 As shown, the wear detection method for the power supply section of the triangular hole conductive nozzle of the present invention specifically includes the following steps:
[0087] S1 Initial Calibration
[0088] After installing a brand-new triangular contact tip on the welding torch, a trial welding was performed under the preset standard welding process parameters, and the welding current time-domain signal during the stable welding stage was collected as reference data.
[0089] First, define the characteristic parameters: define the current fluctuation rate as the ratio of the difference between the peak and valley values of the current within the time window to the average value of the current, which is used to reflect the degree of current fluctuation; define the frequency band that is more than three times the fundamental frequency of the welding current as the high-frequency band, and define the high-frequency energy ratio as the ratio of the signal energy in the high-frequency band to the total energy of the entire frequency band, which is used to reflect the degree of high-frequency disturbance caused by poor contact.
[0090] The collected reference current signal is analyzed and processed to calculate the reference current mean, reference current fluctuation rate, and reference high-frequency energy ratio. These three factors together constitute the reference feature vector.
[0091] Meanwhile, the distribution law of characteristic values under different wear degrees was obtained through wear calibration test. Based on the wear evolution mechanism of three-point contact of triangular hole, wear membership functions of three levels of light wear, moderate wear and extreme wear were established. Each level of membership function corresponds to the membership mapping relationship of each characteristic quantity, which is used for subsequent fuzzy comprehensive judgment.
[0092] S2 Real-time Feature Extraction
[0093] During the actual welding production process, real-time data of the welding current is continuously collected in fixed-duration time windows. For the time-domain signal within each time window, the average current value and current fluctuation rate are first calculated; then, a fast Fourier transform is performed on the time-domain signal to obtain the current spectrum, and the energy proportion of the high-frequency band is extracted; the above three features are combined to form the real-time feature vector of the current time window.
[0094] Before feature extraction, the collected real-time welding current data is first normalized and corrected using the following formula:
[0095]
[0096] Among them I 实测 U is the measured instantaneous current value. 基准 U is the reference value for welding voltage during the calibration phase. 实测 This is the current measured welding voltage value, v 基准 To calibrate the wire feed speed, v 实测 This is the current measured wire feeding speed;
[0097] The voltage correction term eliminates the impact of grid voltage fluctuations on current amplitude, and the wire feeding speed correction term eliminates current changes caused by process parameter adjustments, so that the corrected current value only reflects the conduction state of the contact tip itself, eliminating external operating condition interference.
[0098] S3 Fuzzy Comprehensive Judgment
[0099] Substitute each feature quantity in the real-time feature vector into the three-level wear membership function to calculate the membership degree of each feature quantity corresponding to the three wear levels of light, moderate and extreme. Perform a weighted average of the membership degrees of each feature to obtain the comprehensive membership degree value of the current time window, and take the wear level corresponding to the maximum comprehensive membership degree as the judgment result of the current time window.
[0100] To improve the reliability of the judgment, a continuous multi-window judgment rule is adopted: only when a preset number of time windows are all judged to be at the extreme wear level will the contact nozzle replacement warning be finally triggered, thus avoiding false triggering caused by momentary interference.
[0101] Further, in the fuzzy comprehensive judgment process, the load current of the wire feeding motor is introduced as an auxiliary correction feature, and an adaptive weight distribution algorithm is used to dynamically adjust the weight coefficients of the electrical feature and the wire feeding resistance feature.
[0102] Specifically, the working current of the wire feeding motor is collected in real time, and the ratio of the real-time current of the wire feeding motor to the reference current of the wire feeding motor in the calibration stage is taken as the wire feeding resistance characteristic value. After the edge of the triangular hole is worn, burrs, pits or out-of-roundness are easily formed on the inner wall, which will increase the wire feeding resistance and raise the load current of the wire feeding motor. This feature can assist in verifying the wear state from the mechanical dimension.
[0103] Weights are dynamically allocated according to the ratio of the current welding current volatility to the reference current volatility: when this ratio is small, it indicates that the welding process is stable and the electrical feature has high credibility, so a higher weight is assigned to the comprehensive welding current feature; when this ratio is large, it indicates that the current fluctuation is significant and the credibility of the electrical feature decreases, so the weight of the wire feeding resistance feature is increased accordingly; when the ratio is in the transition interval between the two thresholds, the weights are smoothly transitioned by the linear interpolation method. The feature vector is re-weighted based on the adjusted weights to calculate the corrected comprehensive membership value, which further improves the judgment accuracy.
[0104] Specifically,
[0105] In the initial calibration stage, the feature data of the triangular-hole contact tip in the full cycle from brand new to limit wear is obtained through wear calibration tests. Based on the statistical law of the tests, a triangular membership function corresponding to three levels of mild wear, moderate wear and limit wear is constructed for each feature respectively. The triangular membership function has a simple form and clear physical meaning, which adapts to the continuous and gradual wear law of the welding process. The function is defined as follows:
[0106] For any feature value x, its membership degree μ(x) corresponding to a certain wear level is determined by three parameters of this level: the feature lower limit a, the feature peak b, and the feature upper limit c:
[0107] When x≤a or x≥c, μ(x)=0, that is, this feature value does not belong to this wear level at all;
[0108] When a<x≤b, μ(x)=(x-a) / (b-a), and the membership degree rises linearly with the feature value;
[0109] When b<x<c, μ(x)=(c-x) / (c-b), and the membership degree decreases linearly with the feature value.
[0110] The corresponding physical laws between each feature and the wear level are as follows:
[0111] Average welding current: The more severe the wear, the further back the power supply point, the greater the circuit resistance, and the lower the average current. Therefore, mild wear corresponds to the high current range, extreme wear corresponds to the low current range, and moderate wear is in between.
[0112] Current fluctuation rate: The more severe the wear, the more unstable the edge contact state, and the greater the current fluctuation amplitude. Therefore, mild wear corresponds to the low fluctuation rate range, and extreme wear corresponds to the high fluctuation rate range.
[0113] High-frequency energy percentage: The more severe the wear, the more frequent the instantaneous jumps at the contact points, and the more high-frequency components the current signal has. Therefore, mild wear corresponds to a low percentage range, while extreme wear corresponds to a high percentage range.
[0114] Wire feeding resistance characteristic value: The more severe the wear, the higher the degree of burrs and out-of-roundness on the inner wall, and the greater the wire feeding resistance. Therefore, mild wear corresponds to the low resistance range, and extreme wear corresponds to the high resistance range.
[0115] Substitute each feature value in the real-time feature vector into the triangular fuzzy membership function corresponding to the three wear levels to calculate the membership degree of a single feature to each level.
[0116] Taking the average current characteristic as an example: Let the membership parameters of mild wear be (a1, b1, c1), the parameters of moderate wear be (a2, b2, c2), and the parameters of extreme wear be (a3, b3, c3); Substitute the real-time average current I into the three functions to obtain the three membership values of μmild (I), μmedium (I), and μextreme (I), with a value range of 0 to 1. The larger the value, the higher the degree to which the feature matches the corresponding wear level.
[0117] In the same manner, the membership degree of each of the three levels corresponding to the current fluctuation rate, high-frequency energy ratio, and wire feeding resistance characteristic value is calculated sequentially.
[0118] This method categorizes features into two main types: comprehensive welding current features and wire feed resistance features. The comprehensive welding current features include three sub-features: mean current, current fluctuation rate, and high-frequency energy percentage. The weights of these two types of features are not fixed values but are dynamically adjusted based on the stability of the current welding process, as follows:
[0119] Calculate the volatility ratio k: k = real-time current volatility / reference current volatility
[0120] Two threshold values are set: a low threshold k1 and a high threshold k2. In this embodiment, k1 is set to 1.2 and k2 is set to 1.5.
[0121] Weighting rules:
[0122] When k≤k1, the welding process is stable, and the electrical feature has high reliability, the weight of the current comprehensive feature w_electric is set to 0.7, and the weight of the wire feeding resistance feature w_resistance is set to 0.3;
[0123] When k≥k2, the current fluctuates drastically, the reliability of the electrical feature decreases, and the reference value of the mechanical resistance feature increases, set w_electric=0.5, w_resistance=0.5;
[0124] When k1<k<k2, the linear interpolation method is used for smooth weight transition, and the calculation formula is:
[0125] w_electric=0.7-(0.7-0.5)×(k-k1) / (k2-k1)
[0126] w_resistance=1-w_electric
[0127] For the three sub-features within the welding current comprehensive feature, fixed base weights are adopted: the weight of the current mean value is 0.4, the weight of the current fluctuation rate is 0.3, and the weight of the high-frequency energy proportion is 0.3, and the membership degrees of the current comprehensive feature to the three grades are obtained by weighted summation.
[0128] Comprehensive membership degree calculation and grade determination
[0129] First, calculate the membership degrees of the current comprehensive feature:
[0130] μ_electric_light=0.4×μ_current_mean_light+0.3×μ_fluctuation_rate_light+0.3×μ_high_frequency_proportion_light
[0131] Similarly, μ_electric_medium and μ_electric_extreme are calculated.
[0132] Then, combined with the membership degrees of the wire feeding resistance feature μ_resistance_light, μ_resistance_medium, and μ_resistance_extreme, the final comprehensive membership degrees are calculated:
[0133] μ_comprehensive_light=w_electric×μ_electric_light+w_resistance×μ_resistance_light
[0134] Similarly, μ_comprehensive_medium and μ_comprehensive_extreme are calculated.
[0135] Compare the numerical values of the three comprehensive membership degrees, and take the wear grade corresponding to the maximum value as the wear determination result of the current time window.
[0136] To avoid misjudgment caused by interferences such as welding spatter and instantaneous grid fluctuation, this method introduces a continuous window verification mechanism: set the continuous window number threshold N, which can be 3-5. Only when the determination results of N consecutive time windows are all the extreme wear grade, the warning signal for replacing the contact tip is officially triggered. This rule can effectively filter out single-point misjudgment caused by instantaneous interference, and greatly improve the detection reliability.
[0137] S4 Wear trend prediction
[0138] During real-time monitoring, a wear trend prediction mechanism based on the sliding window least squares method is introduced. The membership values of the limit wear threshold are collected for multiple consecutive time windows. With the cumulative welding time as the x-axis and the membership value of the limit wear threshold as the y-axis, the evolution curve of the wear degree is fitted using the sliding window least squares method. The remaining welding time corresponding to the membership value reaching the limit wear threshold is extrapolated and predicted. When the predicted remaining welding time is lower than a preset safety threshold, a preventative replacement warning is triggered in advance, reminding maintenance personnel to arrange a replacement plan and avoid sudden failures during production.
[0139] The above are merely preferred embodiments of the present invention; however, the scope of protection of the present invention is not limited thereto. Any equivalent substitutions or modifications made by those skilled in the art within the scope of the technology disclosed in the present invention, based on the technical solution and its improved concept, should be covered within the scope of protection of the present invention.
Claims
1. A triangular orifice conductive tip characterized by, The device includes a conductive nozzle body, which comprises a threaded connection section (1), a cylindrical section (2), and a tapered section (3) arranged sequentially along the axial direction. The conductive nozzle body has an inner hole along the axial direction for the welding wire to pass through. The inner hole is divided into an outlet section (4) and an inlet section (5). The outlet section (4) is located within the tapered section (3). The outlet section (4) is a triangular hole with a triangular cross-section. The inlet section (5) is a circular hole with a circular cross-section. The cross-sectional area of the circular hole is not greater than the area of the inscribed circle of the triangular hole. 4) has a conical hole at the top, and the triangular hole forms the power supply contact part of the conductive nozzle. A wear warning transition section (6) is provided between the triangular hole and the circular hole of the inlet section (5). The inner diameter of the wear warning transition section (6) is larger than the outer circle diameter of the triangular hole. The axial length of the wear warning transition section (6) is 4-6mm. When the power supply contact part of the triangular hole is worn to the limit, the welding wire contacts the inner wall of the wear warning transition section (6), the power supply point moves backward to the inlet side, and the welding current drops to the preset wear threshold, so as to realize early wear identification.
2. The orifice conducting tip according to claim 1, wherein The outer walls of the cylindrical section (2) and the conical section (3) are symmetrically provided with clamping planes (9) for clamping tools to tighten.
3. The orifice conducting tip according to claim 1, wherein The outer wall of the cylindrical section (2) is provided with a circumferentially extending gas distribution ring groove (7). Multiple inclined guide gas holes (8) are evenly distributed in the circumferential direction in the gas distribution ring groove (7). The guide gas holes (8) extend obliquely from the gas distribution ring groove (7) towards the front end of the conical section (3) to guide the protective gas to the welding area and form a uniform protective atmosphere.
4. The orifice conducting tip of claim 1 wherein, The three edges of the triangular hole are all provided with transition rounded corners. The inner wall of the triangular hole is formed by cold extrusion to form a work-hardened wear-resistant layer. The hardness of the work-hardened wear-resistant layer is more than 15% higher than the hardness of the conductive nozzle body substrate.
5. A process for producing the triangular orifice conductive nozzle as claimed in claim 1, characterized by, The process includes the following steps in sequence: Process 1: Material cutting. Take copper-chromium-zirconium alloy rods and feed them into the cutting equipment. Cut the rods into billets according to the design length. After completion, randomly inspect the appearance, outer diameter and length of the billets. Process 2: Drilling. Drill the blank axially to form a circular inlet section (5) inner hole and wear warning transition section (6) cavity. Use a through needle and a no-go gauge to check the hole diameter and remove blanks with out-of-tolerance hole diameter. Process 3: Triangular hole and conical hole forming. Position and clamp the drilled blank, and use a cold extrusion triangular punch to extrude the triangular hole outlet section (4) and the front conical hole at the conical end of the blank. After forming, inspect the outline, fillet and taper dimensions of the triangular hole. Process 4: CNC machining. After cleaning the copper shavings and impurities on the surface of the blank, the blank is fed into the vibratory plate of the CNC lathe. The threaded connection section (1), cylindrical section (2), conical section (3) and air distribution ring groove (7) are machined. At the same time, the symmetrical clamping plane and air guide hole (8) of the cylindrical section (2) are milled. After the machining is completed, the full dimensions are inspected against the drawings. Step 5: Surface treatment. The workpiece is successively subjected to pickling, multi-stage cleaning with pure water, and passivation to remove burrs, oil stains and oxide scale from the inner hole and outer surface. Step 6: Full inspection of finished products, checking the threads, inner holes, shape, clamping surfaces, and appearance defects of the workpiece item by item; Step 7: Quantitative sealing and packaging, qualified products are repackaged, labeled and put into storage.
6. The manufacturing process of a triangular orifice conductive nozzle according to claim 5, characterized in that, After drilling in step 2, a solution heat treatment is added: the billet is placed in an argon-protected furnace and held at 900-950℃ for 1-2 hours, followed by water quenching and cooling; after CNC machining in step 4, an aging heat treatment is added: the billet is held at 450-500℃ for 2-3 hours and then slowly cooled in the furnace, precipitating chromium-zirconium reinforcing phases in the matrix to improve the matrix strength, electrical conductivity and wear resistance.
7. The manufacturing process of a triangle orifice conductive nozzle according to claim 5, wherein, In step 5, the pickling process involves soaking in a 10%-15% sulfuric acid solution for 30-60 seconds, followed by ultrasonic cleaning with deionized water 2-3 times, with each cleaning session lasting 5-10 minutes. After that, the solution is soaked in a 0.5-1 g / L benzotriazole passivation solution for 1-2 minutes and then dried.
8. A method of detecting wear of the power supply portion of the triangular-hole conductive nozzle according to claim 1, characterized by, Includes the following steps: S1. Initial Calibration: After installing a brand-new triangular hole contact tip, the welding current time-domain signal during the stable welding stage is collected under standard welding process parameters; the ratio of the difference between the current peak and valley values within the time window to the average current value is defined as the current fluctuation rate; the frequency band more than 3 times the fundamental frequency of the welding current is defined as the high-frequency band; the ratio of the high-frequency band energy to the total energy of the entire frequency band is defined as the high-frequency energy proportion; the current spectrum is obtained by fast Fourier transform of the collected time-domain signal, and a benchmark feature vector including the benchmark current mean, benchmark current fluctuation rate, and benchmark high-frequency energy proportion is established; at the same time, based on the wear evolution law of the three-point contact of the triangular hole, a three-level wear membership function of light wear, moderate wear, and extreme wear is established through wear calibration test, and each level of membership function corresponds to the membership mapping relationship of each feature quantity; S2. Real-time feature extraction: During the welding production process, real-time welding current data is continuously collected in fixed time windows. The average current value and current fluctuation rate are calculated for the time domain signal of each time window. At the same time, the high-frequency energy ratio is extracted by fast Fourier transform to form a real-time feature vector. S3. Fuzzy comprehensive determination: Substitute each feature quantity in the real-time feature vector into the three-level wear membership function to calculate the membership degree of each feature quantity corresponding to each wear level. Then, obtain the comprehensive membership degree value through weighted average and take the wear level corresponding to the maximum comprehensive membership degree as the current determination result. When a preset number of time windows are all determined to be at the extreme wear level, a contact nozzle replacement warning is triggered.
9. The method according to claim 8, wherein In step S3, the fuzzy comprehensive determination introduces the load current of the wire feeding motor as an auxiliary correction feature, and an adaptive weight allocation algorithm is used to adjust the weight coefficients of the electrical feature and the wire feeding resistance feature. The operating current of the wire feeding motor is collected in real time, and the characteristic value of the wire feeding resistance is calculated. The characteristic value of the wire feeding resistance is the ratio of the real-time current of the wire feeding motor to the reference current of the wire feeding motor during the calibration stage. The weights are dynamically allocated based on the ratio of the current welding current fluctuation rate to the reference current fluctuation rate: when the ratio is ≤1.2, the weight of the comprehensive welding current characteristic is set to 0.7, and the weight of the wire feeding resistance characteristic is set to 0.3; when the ratio is ≥1.5, the weight of the comprehensive welding current characteristic is reduced to 0.5, and the weight of the wire feeding resistance characteristic is increased to 0.5; when the ratio is between 1.2 and 1.5, the weights are calculated using linear interpolation; the comprehensive membership value is recalculated based on the weighted feature vector to correct the wear determination result.
10. The method according to claim 8, wherein In step S2, the collected real-time welding current data is first normalized and corrected for operating conditions, and then feature extraction is performed; at the same time, a wear trend prediction mechanism based on the sliding window least squares method is introduced: The normalization correction formula for operating conditions is: where I 实测 is the measured current instantaneous value, U 基准 is the welding voltage reference value in the calibration phase, U 实测 is the current measured welding voltage value, V 基准 is the calibration wire feed speed, V 实测 is the current measured wire feed speed; Collect the membership values of the limit wear for a preset number of N consecutive time windows. With the cumulative welding time as the abscissa and the membership value of the limit wear as the ordinate, use the sliding window least squares method to fit the wear degree evolution curve and extrapolate to predict the remaining welding time when the membership value reaches the limit wear threshold. When the predicted remaining welding time is lower than the preset safety threshold, trigger a preventive replacement warning in advance.