A method for zoned power control of thin-walled titanium alloy laser filament additive manufacturing parts based on thermal history regulation
By using a zoned power control method based on thermal history regulation, the problem of thermal history differences in laser filament additive manufacturing was solved, thereby improving the thermal cycling uniformity and microstructure stability of thin-walled titanium alloy parts.
Patent Information
- Application Number
- CN202611292727.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-25
- Publication Date
- 2026-11-17
AI Technical Summary
Existing laser filament additive manufacturing processes cannot simultaneously meet the fusion requirements of the bottom region and the control of heat accumulation in the top region, resulting in large differences in the thermal history of thin-walled titanium alloy parts during the deposition process, which affects the uniformity of the microstructure and the consistency of mechanical properties.
By obtaining thermal accumulation characteristic parameters at different deposition heights through thermal history simulation or monitoring, a thermal accumulation compensation coefficient is constructed. Thermal state regions are divided along the deposition height direction, and the laser power is gradually reduced according to the degree of thermal accumulation to achieve zoned power control.
Lowering the peak temperature in the top region and the residual temperature at the end of the deposition cycle reduces the thermal history differences between regions at different heights, thereby improving the uniformity of the thermal cycling process and the microstructure stability of thin-walled parts.
Smart Images

Figure CN123103170A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of metal additive manufacturing and titanium alloy laser filament forming technology. Specifically, it relates to a method for partitioned power control of thin-walled parts in titanium alloy laser filament additive manufacturing based on thermal history regulation. It is particularly applicable to the height-direction thermal history regulation and partitioned power control of α+β type or near-α type titanium alloy single walls, thin-walled stiffeners, thin-walled frames and quasi-thin-walled structures such as TC11, TC4, TA15, and TC18 in the laser filament additive manufacturing process. Background Technology
[0002] Laser filament additive manufacturing is a directional energy deposition forming technology that uses a laser beam as a heat source and metal filaments as filler material. This technology boasts advantages such as high material utilization, high deposition efficiency, and suitability for manufacturing large and complex metal components, making it valuable for applications in aerospace, energy equipment, and high-performance load-bearing structural components. Compared to powder feed additive manufacturing, laser filament additive manufacturing reduces powder scattering and material waste, making it more suitable for the efficient forming of high-value metal materials such as titanium alloys.
[0003] Titanium alloys, especially α+β type titanium alloys such as TC11 and TC4, are highly sensitive to thermal cycling. During laser filament additive manufacturing, the material undergoes rapid heating, melting, solidification, and subsequent multiple thermal cycles. Since the phase transformation behavior, microstructure evolution, and residual stress distribution of titanium alloys are closely related to their thermal history, the heat input and cooling conditions at different deposition heights directly affect the microstructure uniformity, dimensional stability, and mechanical property consistency of the component.
[0004] For single-walled, thin-walled stiffener, and near-thin-walled structures, the heat dissipation conditions of the component change continuously with the increase in the number of deposition layers. The bottom region, close to the substrate, benefits from the strong heat dissipation of the substrate, allowing heat to be conducted to the substrate relatively quickly. The middle region gradually moves away from the substrate, resulting in a longer heat conduction path and more complex thermal cycling. The top region, far from the substrate, has relatively weaker heat dissipation conditions and is prone to heat accumulation. Under constant laser power, constant scanning speed, and constant wire feed speed, the higher heat input required in the bottom region may cause excessive heat accumulation in the upper and middle regions, leading to increased peak temperature, increased residual temperature at the end of the deposition cycle, prolonged high-temperature exposure time, and increased high-temperature heat dose in the top region.
[0005] In existing laser filament additive manufacturing processes, layer-by-layer deposition of the entire component is typically achieved using fixed laser power, fixed scanning speed, and fixed wire feed speed. However, this constant-parameter method struggles to simultaneously address the fusion requirements of the bottom region and the thermal accumulation control requirements of the top region. While the forming process can be improved through manual experience by reducing power, increasing scanning speed, or extending interlayer dwell time, these methods usually rely on extensive experimentation, lacking quantitative evaluation of the thermal accumulation state at different deposition heights, and making it difficult to establish a correspondence between thermal history characteristic parameters and zoned process parameters.
[0006] Therefore, it is necessary to propose a zonal variable parameter control method for thin-walled parts manufactured by laser filament additive manufacturing of titanium alloys based on thermal history data and thermal accumulation compensation coefficient. By analyzing the thermal history under constant initial parameters, thermal accumulation characteristic parameters such as peak temperature, residual temperature at the end of the deposition cycle, and high-temperature thermal dose are obtained. Based on this, thermal state zoning and laser power correction are performed along the deposition height direction, thereby reducing thermal accumulation in the top region and reducing the thermal history differences between different height regions. Summary of the Invention
[0007] The purpose of this invention is to provide a method for zoned power control of thin-walled parts in titanium alloy laser filament additive manufacturing based on thermal history regulation. This method extracts thermal accumulation characteristic parameters of different deposition layers through thermal history simulation or monitoring under constant initial process parameters, constructs a thermal accumulation compensation coefficient, and divides the thin-walled part into multiple thermal state regions along the deposition height direction according to the thermal accumulation compensation coefficient. Furthermore, based on the degree of thermal accumulation corresponding to different thermal state regions, the initial laser power is modified in zones, so that the laser power gradually decreases as the degree of thermal accumulation increases along the deposition height direction, thereby reducing the peak temperature in the top region, the residual temperature at the end of the deposition cycle, the high-temperature heat dose, and the thermal history differences between different height regions.
[0008] To achieve the above objectives, the present invention provides the following technical solution: This invention proposes a method for zoned power control of thin-walled titanium alloy laser filament additive manufacturing based on thermal history regulation. The method includes the following steps: S1: Establish the geometric model of the thin-walled titanium alloy part to be formed and determine the initial laser filament additive manufacturing process parameters; S2: Obtain thermal history data of different height regions during the layer-by-layer deposition process of the titanium alloy thin-walled part under constant initial process parameters; S3: Extract thermal accumulation characteristic parameters from the thermal history data; S4: Construct a thermal accumulation compensation coefficient based on the thermal accumulation characteristic parameters, and divide the titanium alloy thin-walled part into multiple thermal state regions along the deposition height direction based on the thermal accumulation compensation coefficient; S5: Based on the thermal accumulation compensation coefficient corresponding to different thermal state regions, the initial laser power is modified by region to obtain the region laser power corresponding to different height regions. S6: Based on the partitioned laser power, a partitioned power control command is generated, and layer-by-layer deposition is performed in accordance with the partitioned power control command during the laser filament additive manufacturing process of titanium alloy thin-walled parts to regulate the thermal history distribution of different height regions; and as the degree of thermal accumulation in the deposition height direction increases, the partitioned laser power is gradually reduced relative to the initial laser power.
[0009] Furthermore, in step S1 of the present invention, the initial process parameters include initial laser power, scanning speed, wire feed speed and layer height; in step S3, the thermal accumulation characteristic parameters include one or more of the following: peak temperature, residual temperature at the end of the deposition cycle, high-temperature dwell time, high-temperature heat dose and cooling process characteristic parameters.
[0010] Furthermore, the titanium alloy thin-walled component of the present invention is a single-walled wall, a thin-walled stiffener, a thin-walled frame, or a quasi-thin-walled titanium alloy component with layer-by-layer stacking characteristics; the titanium alloy is TC11 titanium alloy, TC4 titanium alloy, TA15 titanium alloy, TC18 titanium alloy, or other α+β type and near-α type titanium alloys.
[0011] Furthermore, in step S2 of the present invention, transient heat conduction simulation is used to obtain thermal history data of different height regions during the layer-by-layer deposition process of the titanium alloy thin-walled part under constant initial process parameters; the thermal history data is obtained through one or more of the following methods: numerical simulation, online temperature monitoring, infrared thermal imaging monitoring, molten pool image monitoring, thermocouple temperature measurement, or historical process database. The transient heat conduction simulation uses a moving heat source model, which is one of the following: Gaussian heat source, double ellipsoidal heat source, cylindrical heat source, elliptical heat source, flat-top heat source, or non-Gaussian heat source; the transient heat conduction simulation considers one or more of the following: substrate heat dissipation, surface convection heat dissipation, and surface radiation heat dissipation.
[0012] Furthermore, the thermal history data of the present invention includes one or more of the following: temperature-time curves at different depositional layers, initial interlayer temperature, peak temperature, residual temperature at the end of the deposition cycle, high-temperature residence time, high-temperature heat dose, and characteristic parameters of the cooling process; the residual temperature at the end of the deposition cycle is the temperature at the characteristic location of the depositional layer after the current depositional layer scan is completed or at the end of the current deposition cycle.
[0013] Furthermore, the high-temperature heat dose described in this invention is used to characterize the overall degree of high-temperature effect on the material after exceeding a set high-temperature threshold, and is calculated according to the following formula:
[0014] in, For the first High-temperature heat dose of the layer, For the first Temperature at the characteristic location of the layer, To set a high temperature threshold, Indicates when Higher than Time to take ,when Not higher than Take 0 at that time.
[0015] Furthermore, in step S4 of the present invention, the heat accumulation compensation coefficient is obtained by weighting the normalized residual temperature at the end of the deposition cycle, the high-temperature heat dose, and the characteristic parameters of the cooling process, and is calculated according to the following formula:
[0016] in, For the first Layer heat accumulation compensation coefficient, For the first The residual temperature at the end of the layer deposition cycle For the first High-temperature heat dose of the layer, For the first Characteristic parameters of the layer cooling process and These represent the maximum and minimum residual temperatures at the end of the deposition cycle, respectively. and These represent the maximum and minimum values of the high-temperature heat dose, respectively. and These represent the maximum and minimum values of the characteristic parameters of the cooling process, respectively. , , All are weighting coefficients.
[0017] Furthermore, the weighting coefficients described in this invention satisfy the following:
[0018] in, , , The degree of influence of residual temperature at the end of the deposition cycle, high-temperature heat dose, and characteristic parameters of the cooling process on heat accumulation was determined respectively.
[0019] Furthermore, in step S4 of the present invention, the plurality of thermal state regions are at least three regions distributed sequentially along the deposition height direction, and the laser power corresponding to different thermal state regions decreases step by step along the deposition height direction; the plurality of thermal state regions include a bottom rapid heat dissipation region, a middle heat accumulation growth region, and a top strong heat accumulation region.
[0020] Further, in step S5 of the present invention, the partitioned laser power is 70%–100% of the initial laser power; when the titanium alloy thin-walled part is divided into five hot state regions along the deposition height direction, the laser power corresponding to the five hot state regions is 100%, 90%–98%, 80%–90%, 75%–85%, and 70%–80% of the initial laser power, respectively.
[0021] The beneficial effects of this invention are as follows: 1. This invention obtains thermal history data at different deposition heights through thermal history simulation or thermal history monitoring, which can quantitatively characterize the thermal accumulation behavior in the height direction during the layer-by-layer deposition process of titanium alloy thin-walled parts; 2. This invention constructs a heat accumulation compensation coefficient by using peak temperature, residual temperature at the end of the deposition cycle, high-temperature heat dose, and characteristic parameters of the cooling process, so that the partitioned power control has a clear thermal history basis and avoids simply adjusting parameters based on experience; 3. The present invention divides the thin-walled part into multiple thermal state regions along the deposition height direction according to the thermal accumulation compensation coefficient, and gradually reduces the laser power according to the degree of thermal accumulation, which can reduce the peak temperature of the top region and the residual temperature at the end of the deposition cycle; 4. This invention can reduce the amount of high-temperature heat in the top region, weaken the phenomenon of prolonged high temperature retention in the top region, and help reduce the tendency of tissue coarsening caused by heat accumulation. 5. The present invention can reduce the thermal history differences between different height regions at the bottom, middle and top, and improve the uniformity of the thermal cycling process of thin-walled parts manufactured by laser filament additive manufacturing of titanium alloys. Attached Figure Description
[0022] To more clearly illustrate the specific embodiments of the present invention or the technical solutions in the prior art, the drawings used in the description of the specific embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For those skilled in the art, other drawings can be obtained from these drawings without creative effort.
[0023] Figure 1 This is a flowchart of the partitioned variable parameter control method for thermal accumulation compensation of thin-walled titanium alloy laser filament additive manufacturing according to the present invention; Figure 2 This is a schematic diagram of the geometric model of the TC11 titanium alloy single wall and the arrangement of temperature probes in Embodiment 2 of the present invention; Figure 3 This is a schematic diagram of the constant laser power and zoned laser power control strategy in Embodiment 2 of the present invention; Figure 4This is a comparison chart of peak temperature variation with the number of layers under constant power and partitioned power conditions in Embodiment 2 of the present invention; Figure 5 This is a comparison chart of the residual temperature at the end of the deposition cycle with the number of layers under constant power and partitioned power conditions in Embodiment 2 of the present invention. Figure 6 This is a comparison chart of the high-temperature heat dose as a function of the number of deposition layers under constant power and partitioned power conditions in Embodiment 2 of the present invention; Figure 7 This is a diagram showing the variation of the thermal accumulation compensation coefficient with the number of layers and the thermal state zoning in the height direction in Embodiment 2 of the present invention. Detailed Implementation
[0024] The specific embodiments of the present invention will be further described in detail below with reference to the accompanying drawings. The following examples will help those skilled in the art to further understand the present invention, but do not limit the present invention in any way. It should be noted that those skilled in the art can make several changes and improvements without departing from the concept of the present invention, and these all fall within the protection scope of the present invention.
[0025] Example 1, Combination Figure 1 This invention provides a detailed description of a method for partitioned power control of thin-walled titanium alloy laser filament additive manufacturing based on thermal history regulation. The complete implementation flow of this method is disclosed in this embodiment, enabling those skilled in the art to clearly reproduce the technical solution of this invention. The method extracts thermal accumulation characteristic parameters of different deposition layers through thermal history simulation or monitoring under constant initial process parameters, constructs thermal accumulation compensation coefficients, and divides the thin-walled part into multiple thermal state regions along the deposition height direction based on these coefficients. Furthermore, the initial laser power is partitioned and corrected according to the degree of thermal accumulation corresponding to different thermal state regions, so that the laser power gradually decreases as the degree of thermal accumulation increases along the deposition height direction. This reduces the peak temperature in the top region, the residual temperature at the end of the deposition cycle, the high-temperature heat dose, and the thermal history differences between different height regions.
[0026] like Figure 1 As shown, the present invention proposes a method for zoned power control of thin-walled titanium alloy laser filament additive manufacturing based on thermal history regulation, comprising the following steps: S1: Establish the geometric model of the thin-walled titanium alloy part to be formed, and determine the initial laser filament additive manufacturing process parameters, including the initial laser power, scanning speed, wire feed speed and layer height; S2: Obtain thermal history data of different height regions during the layer-by-layer deposition process of the titanium alloy thin-walled part under constant initial process parameters. The thermal history data is obtained through one or more methods, such as numerical simulation, online temperature monitoring, infrared thermal imaging monitoring, molten pool image monitoring, thermocouple temperature measurement, or historical process database. S3: Extract thermal accumulation characteristic parameters from the thermal history data. The thermal accumulation characteristic parameters include one or more of the following: peak temperature, residual temperature at the end of the deposition cycle, high-temperature residence time, high-temperature heat dose, and cooling process characteristic parameters. S4: Construct a thermal accumulation compensation coefficient based on the thermal accumulation characteristic parameters, and divide the titanium alloy thin-walled part into multiple thermal state regions along the deposition height direction based on the thermal accumulation compensation coefficient; S5: Based on the thermal accumulation compensation coefficient corresponding to different thermal state regions, the initial laser power is modified by region to obtain the region laser power corresponding to different height regions. S6: Based on the partitioned laser power, a partitioned power control command is generated, and layer-by-layer deposition is performed in accordance with the partitioned power control command during the laser filament additive manufacturing process of titanium alloy thin-walled parts to regulate the thermal history distribution of different height regions; wherein, as the degree of thermal accumulation in the deposition height direction increases, the partitioned laser power is gradually reduced relative to the initial laser power.
[0027] Furthermore, in one specific embodiment, the titanium alloy thin-walled component described in this embodiment can be a single-walled structure, a thin-walled stiffener, a thin-walled frame, or a quasi-thin-walled titanium alloy component with layer-by-layer stacking characteristics. The titanium alloy can be TC11 titanium alloy, TC4 titanium alloy, TA15 titanium alloy, TC18 titanium alloy, or other α+β type and near-α type titanium alloys.
[0028] Furthermore, in one specific embodiment, transient heat conduction simulation is used to obtain thermal history data of different height regions during the layer-by-layer deposition process of the titanium alloy thin-walled part under constant initial process parameters. The transient heat conduction simulation can employ a moving heat source model, which can be one of a Gaussian heat source, a double ellipsoidal heat source, a cylindrical heat source, an elliptical heat source, a flat-top heat source, or a non-Gaussian heat source. The transient heat conduction simulation can consider one or more of substrate heat dissipation, surface convection heat dissipation, and surface radiation heat dissipation.
[0029] The thermal history data includes one or more of the following: temperature-time curves at different depositional layers, initial interlayer temperature, peak temperature, residual temperature at the end of the deposition cycle, high-temperature residence time, high-temperature heat dose, and characteristic parameters of the cooling process. The residual temperature at the end of the deposition cycle is the temperature at a characteristic location of the depositional layer after the current depositional layer scan is completed or at the end of the current deposition cycle.
[0030] Specifically, the high-temperature heat dose is used to characterize the overall degree of high-temperature effect on the material after exceeding a set high-temperature threshold, and is calculated according to the following formula:
[0031] in, For the first High-temperature heat dose of the layer, For the first Temperature at the characteristic location of the layer, To set a high temperature threshold, Indicates when Higher than Time to take ,when Not higher than Take 0 at that time.
[0032] The cooling process characteristic parameters can be one or more of the following: the average cooling rate between the peak temperature and the residual temperature at the end of the deposition cycle, the average cooling rate between a set high temperature threshold and a set low temperature threshold, the instantaneous cooling rate during the cooling stage, or the temperature decay time constant during the cooling stage. These cooling process characteristic parameters are used to help characterize the differences in the cooling process at different altitudes and are not limited to a single cooling rate definition.
[0033] Furthermore, in a specific embodiment, in step S4, the heat accumulation compensation coefficient is obtained by weighting the normalized residual temperature at the end of the deposition cycle, the high-temperature heat dose, and the characteristic parameters of the cooling process, preferably calculated according to the following formula:
[0034] in, For the first Layer heat accumulation compensation coefficient, For the first The residual temperature at the end of the layer deposition cycle For the first High-temperature heat dose of the layer, For the first Characteristic parameters of the layer cooling process and These represent the maximum and minimum residual temperatures at the end of the deposition cycle, respectively. and These represent the maximum and minimum values of the high-temperature heat dose, respectively. and These represent the maximum and minimum values of the characteristic parameters of the cooling process, respectively. , , All are weighting coefficients.
[0035] Wherein, the weighting coefficients satisfy:
[0036] in, , , The determination is based on the degree of influence of the residual temperature at the end of the deposition cycle, the high-temperature heat dose, and the characteristic parameters of the cooling process on heat accumulation. In a preferred embodiment, , , Take values of 0.4, 0.3, and 0.3 respectively.
[0037] Based on the heat accumulation compensation coefficient Based on the size or trend of the deposition height, the titanium alloy thin-walled part is divided into multiple thermal state regions. These multiple thermal state regions are at least three regions sequentially distributed along the deposition height, with the laser power corresponding to different thermal state regions decreasing progressively along the deposition height. The multiple thermal state regions may include a bottom rapid heat dissipation zone, a middle heat accumulation growth zone, and a top strong heat accumulation zone. They can also be further divided into more thermal state regions based on the component height, the number of deposition layers, the trend of the heat accumulation compensation coefficient curve, or process requirements.
[0038] Further, in one specific embodiment, in step S5, the partitioned laser power is 70%–100% of the initial laser power. When the titanium alloy thin-walled part is divided into five hot state regions along the deposition height direction, the laser power corresponding to the five hot state regions can be 100%, 90%–98%, 80%–90%, 75%–85%, and 70%–80% of the initial laser power, respectively. During the partitioned laser power control process, the scanning speed and wire feed speed can remain constant to ensure a clear thermal input compensation relationship; alternatively, the scanning speed, wire feed speed, or interlayer dwell time can be further adjusted collaboratively according to actual forming requirements.
[0039] Furthermore, in one specific embodiment, the titanium alloy thin-walled part is an 80-layer TC11 titanium alloy single-walled structure with an initial laser power of 3120 W, a scanning speed of 22 mm / s, a wire feed speed of 25 mm / s, and a layer height of 1.2 mm. The 80-layer TC11 titanium alloy single-walled structure is divided into five thermal state regions along the deposition height direction, wherein layers 1–15 use 3120 W, layers 16–30 use 2950 W, layers 31–45 use 2700 W, layers 46–60 use 2450 W, and layers 61–80 use 2300 W, while the scanning speed and wire feed speed remain unchanged.
[0040] In summary, the core of this invention lies in extracting thermal accumulation characteristic parameters based on the aforementioned thermal history data, constructing a thermal accumulation compensation coefficient, and then performing height-direction partitioning correction of the laser power according to the thermal accumulation compensation coefficient. This allows for the regulation of the thermal history distribution during the deposition of thin-walled titanium alloy parts, reducing the tendency for uneven microstructure caused by differences in thermal accumulation. Numerical simulation is not the sole implementation method. Numerical simulation, online temperature monitoring, infrared thermal imaging monitoring, molten pool image monitoring, thermocouple temperature measurement, and historical process databases can all be used to obtain thermal history data for different height regions.
[0041] Example 2: This example uses transient heat conduction simulation to illustrate the method. It should be understood that in practical applications, thermal history data for different height regions can also be obtained through infrared thermography, online monitoring of the molten pool, thermocouple temperature measurement, or existing process databases, and is not limited to numerical simulation. This example uses a single-walled structure manufactured by laser filament additive manufacturing of TC11 titanium alloy as an example, establishing a layer-by-layer deposition heat conduction model for an 80-layer single-walled structure. The single-walled structure has a length of 110 mm, a thickness of 3 mm, a layer height of 1.2 mm, a total of 80 layers, and a total model height of 96 mm. During the simulation, a transient heat conduction model is used to describe the heat transfer behavior during laser filament additive manufacturing. A moving Gaussian heat source is used to simulate laser heat input, considering substrate heat dissipation, surface convection heat dissipation, and surface radiation heat dissipation. The model does not consider molten pool flow, Marangoni convection, free surface deformation, evaporation backpressure, and keyhole behavior to highlight the overall heat accumulation law during the layer-by-layer deposition process of thin-walled parts.
[0042] The temperature-dependent thermophysical properties of TC11 and TC4 titanium alloys were calculated using JMatPro software. During the calculation, the nominal chemical composition of the corresponding titanium alloy was input to obtain thermophysical data such as density, specific heat capacity, thermal conductivity, enthalpy change curve, solidus temperature, liquidus temperature, and β-transformation temperature at different temperatures. Since the thermophysical properties of titanium alloys change significantly with temperature, this embodiment does not use constant thermophysical parameters. Instead, the temperature-dependent thermophysical property curves output by JMatPro are imported into the numerical simulation model to improve the rationality of the thermal history calculation. In this embodiment, the thermophysical parameters of TC11 titanium alloy are preferentially used for simulation; the thermophysical parameters of TC4 titanium alloy are used to demonstrate that this method is also applicable to other α+β type titanium alloys.
[0043] Zoned laser power control strategy, such as Figure 3 As shown, under constant power conditions, the laser power remains at 3120 W from layer 1 to layer 80, while the scanning speed and wire feed speed remain unchanged. The parameters for constant power conditions are shown in Table 1.
[0044] Table 1
[0045] To obtain thermal history data for different height regions, temperature probes are set up in the single-wall model, such as... Figure 2 As shown, the temperature probe is positioned at the center of the single-wall thickness, i.e. In the scanning direction, select , and Three locations were selected; along the depositional height direction, layers 10, 20, 40, 60, and 75 were chosen as representative layers. The center height of each layer was determined according to the following formula:
[0046] in, For the first Floor center height, In this embodiment, the floor height is... In addition, temperature probes are placed at the center every five layers. Table 2 shows the representative locations of the temperature probes for each layer.
[0047] Table 2
[0048] Temperature-time curves for different depositional layers were obtained through constant power simulation, and peak temperatures were further extracted. Residual temperature at the end of the deposition cycle High-temperature heat dose and cooling process characteristic parameters The constant power simulation results show that with the increase of the number of deposition layers, significant heat accumulation occurs in the top region of the single wall, specifically manifested as an increase in peak temperature, an increase in residual temperature at the end of the deposition cycle, and an increase in high-temperature heat dose. This result indicates that, under constant initial laser power conditions, there are significant differences in the thermal history of regions at different heights.
[0049] Based on the thermal history data obtained under constant power conditions, the following formula is used to calculate the... High-temperature heat dose of the layer:
[0050] in, A high-temperature threshold is set. In this embodiment, the high-temperature threshold can be determined based on the β-transformation temperature of the TC11 titanium alloy, or it can be set as a threshold for a corresponding high-temperature range according to the microstructure control requirements. Subsequently, the heat accumulation compensation coefficient is calculated based on the residual temperature at the end of the deposition cycle, the high-temperature heat dose, and the characteristic parameters of the cooling process.
[0051] In this embodiment, the weighting coefficient is:
[0052] Right now:
[0053] Among them, the higher the residual temperature at the end of the deposition cycle, the greater the high-temperature heat dose, and the stronger the degree of heat accumulation corresponding to the characteristic parameters of the cooling process, the greater the heat accumulation compensation coefficient.
[0054] Based on the heat accumulation compensation coefficient As the number of layers changes, the 80-layer TC11 titanium alloy single-wall structure is divided into five thermal state zones along the deposition height direction, such as... Figure 7 As shown in Table 3, the partitioning results are as follows.
[0055] Table 3
[0056] The initial laser power is adjusted according to the degree of heat accumulation in different regions. As the deposition height increases, the degree of heat accumulation increases, and the laser power decreases step by step. In this embodiment, the initial laser power is 3120 W, and the power parameters for each region are shown in Table 4.
[0057] Table 4
[0058] As shown in Table 4, this embodiment only performs partitioned correction on the laser power, while the scanning speed and wire feed speed remain unchanged. This method avoids the coupling effects caused by simultaneous changes in multiple process parameters, making the partitioned heat input compensation effect more explicit. The partitioned power control strategy is as follows: Figure 3 As shown. Under constant power conditions, the laser power for layers 1–80 is 3120 W; under partitioned power conditions, the laser power decreases sequentially along the deposition height to 3120 W, 2950 W, 2700 W, 2450 W and 2300 W.
[0059] Thermal history simulations of an 80-layer TC11 titanium alloy single-wall structure were performed using the partitioned power parameters shown in Table 4, and the results were compared with those of the constant power condition. To ensure consistency in the comparison, the constant power condition and the partitioned power condition used the same geometric model, material thermal properties, heat dissipation boundary conditions, scanning speed, wire feed speed, layer height, and temperature probe position, only changing the laser power in different height regions. The comparison indicators included peak temperature. Residual temperature at the end of the deposition cycle and high temperature heat dose Among them, the high-temperature heat dose is used to set a high-temperature threshold. Calculations are performed to comprehensively characterize the high-temperature level and the duration of high-temperature exposure.
[0060] The results of the comparison of typical stratigraphic layers show that after the partitioned power control, the peak temperature, residual temperature at the end of the deposition cycle, and high-temperature heat dose of the middle and upper layers and the top layer are significantly lower than those under constant power conditions.
[0061] The temperature reduction for each representative layer is shown in Table 5. Further comparison of peak temperature and residual temperature at the end of the deposition cycle reveals that the temperature in the top region significantly decreased after zonal power control. Taking layer 75 as an example, the peak temperature of this layer under constant power conditions was approximately 3083 K, decreasing to approximately 2390 K under zonal power conditions; the residual temperature at the end of the deposition cycle of this layer under constant power conditions was approximately 3061 K, decreasing to approximately 2389 K under zonal power conditions. Figure 5 As shown, zoned power control can significantly reduce heat accumulation in the top region.
[0062] Table 5
[0063] As shown in Table 4, layers 1–15 still use 3120 W, the same as the constant power condition. Therefore, the thermal accumulation characteristic parameters of layers 5, 10, and 15 remain basically consistent. This result indicates that the partitioned power control did not weaken the heat input of the bottom rapid heat dissipation zone, which is beneficial to ensuring the fusion requirements of the bottom region. After reducing the laser power starting from layer 16, the thermal accumulation suppression effect gradually becomes apparent: when using 2950 W for layers 20–30, the peak temperature decreases by approximately 120.6–136.8 K, the residual temperature at the end of the cycle decreases by approximately 78.7–116.5 K, and the high-temperature heat dose decreases by approximately 7.9%–8.7%, indicating that a slight reduction in power is sufficient to suppress the temperature from continuing to rise in the thermal accumulation initiation zone.
[0064] The heat accumulation suppression effect was further enhanced after applying 2700 W to layers 31–45. The peak temperatures of layers 35, 40, and 45 decreased by approximately 317.3 K, 335.5 K, and 346.7 K, respectively, while the residual temperatures at the end of the cycle decreased by approximately 241.3 K, 283.5 K, and 309.0 K, respectively, and the high-temperature heat dose decreased by approximately 17.7%, 19.2%, and 19.8%, respectively. This indicates that within the heat accumulation growth region, the zonal reduction of laser power not only reduced the instantaneous peak temperature but also reduced the residual heat retained in the component after the deposition cycle ended.
[0065] After applying 2450 W to layers 46–60, the effect of zoned power on suppressing heat accumulation became more pronounced. Peak temperatures in layers 50, 55, and 60 decreased by approximately 527.6–564.4 K, residual temperatures at the end of the cycle decreased by approximately 442.1–520.5 K, and the high-temperature heat dose decreased by approximately 28.3%–31.0%. These results indicate that in the heat accumulation intensification zone, if a constant power of 3120 W is maintained, heat will continue to accumulate in the upper and middle regions; however, by implementing zoned power reduction, the intensity of high-temperature effects in this region can be significantly reduced.
[0066] After using 2300 W in layers 61–80, the heat accumulation in the top high-heat accumulation zone was further weakened. The peak temperatures of layers 65, 70, and 75 decreased by approximately 655.7 K, 679.0 K, and 692.0 K, respectively, and the residual temperatures at the end of the cycle decreased by approximately 610.8 K, 647.6 K, and 671.6 K, respectively, with high-temperature heat doses decreasing by approximately 36.2%, 37.5%, and 38.3%, respectively. Specifically, the peak temperature of layer 75 under constant power conditions was approximately 3082.5 K, which decreased to approximately 2390.5 K under zoned power conditions. Figure 4 As shown, the residual temperature at the end of the cycle under constant power conditions is approximately 3060.5 K, while under partitioned power conditions it decreases to approximately 2388.8 K, indicating that partitioned power control can significantly reduce the phenomenon of prolonged high temperatures in the top region. Layer 80 is affected by the termination layer effect, resulting in a somewhat unique temperature response; however, its peak temperature still decreases by approximately 881.1 K, the residual temperature at the end of the cycle decreases by approximately 712.5 K, and the high-temperature heat dose decreases by approximately 37.3%. Figure 6 As shown, this further illustrates that heat accumulation in the top and end regions is also suppressed.
[0067] Further analysis of the average reduction rate of each representative layer according to the thermal state region is shown in Table 6.
[0068] Table 6
[0069] As shown in Table 6, the reduction in thermal accumulation characteristic parameters by zone power increases progressively with increasing deposition height. In the second zone, the average peak temperature decreases by approximately 129.5 K, the average residual temperature at the end of the cycle decreases by approximately 99.3 K, and the average high-temperature heat dose decreases by approximately 8.4%. In the third zone, these reductions increase to approximately 333.2 K, 277.9 K, and 18.9%, respectively. In the fourth zone, these reductions further increase to approximately 547.6 K, 484.3 K, and 29.8%. In the fifth zone, the average peak temperature in the top strong thermal accumulation zone decreases by approximately 727.0 K, the average residual temperature at the end of the cycle decreases by approximately 660.6 K, and the average high-temperature heat dose decreases by approximately 37.3%. This cooling effect, which increases with height, is consistent with the progressively decreasing zone power, indicating that the zone power setting in this embodiment can effectively compensate for the increasing trend of thermal accumulation in the height direction.
[0070] From the perspective of thermal history uniformity along the vertical direction, zoned power control also shows significant advantages. Using layers 20, 30, 40, 50, 60, 70, and 75 as representative layers, the interlayer span of residual temperature at the end of the cycle under constant power conditions was approximately 770.0 K, decreasing to approximately 297.6 K under zoned power conditions, a reduction of approximately 61.4%. Similarly, the interlayer span of high-temperature heat dose under constant power conditions was approximately 2162.1 K·s, decreasing to approximately 778.0 K·s under zoned power conditions, a reduction of approximately 64.0%. Using layers 20, 40, 60, and 75 as typical bottom-middle-top representative layers, the peak temperature span decreased from approximately 332.4 K under constant power conditions to approximately 239.0 K under zoned power conditions, a reduction of approximately 28.1%. These results indicate that zoned power control not only reduces the absolute temperature level in the top region but also reduces the thermal history differences between layers at different altitudes.
[0071] Comparison of temperature-time curves, peak temperature, residual temperature at the end of the deposition cycle, and high-temperature heat dose reveals that under a constant power of 3120 W, heat accumulation continues in the upper and top regions as the number of layers increases, manifested as an upward shift in the temperature curve, an increase in the residual temperature at the end of the cycle, and an increase in the high-temperature heat dose. After adopting partitioned power, the temperature curve shifts downward overall, the peak temperature and residual temperature at the end of the cycle in the top region decrease significantly, the high-temperature heat dose decreases markedly, and the difference in thermal history along the height direction is significantly reduced. Therefore, the heat accumulation compensation partitioned variable parameter control method described in this invention can effectively reduce the degree of heat accumulation in thin-walled parts manufactured by laser filament additive manufacturing of titanium alloys, weaken the phenomenon of prolonged high-temperature retention in the top region, and improve the uniformity of thermal circulation distribution during layer-by-layer deposition.
[0072] This embodiment demonstrates that, under a constant power of 3120 W, TC11 titanium alloy single-walled parts exhibit significant heat accumulation with increasing deposition layers, manifested as an increase in peak temperature in the top region, an increase in residual temperature at the end of the deposition cycle, and an increase in high-temperature heat dose. By employing the heat accumulation compensation zonal parameter control method described in this invention, the laser power gradually decreases along the deposition height direction, resulting in a significant reduction in peak temperature in the top region, residual temperature at the end of the deposition cycle, and high-temperature heat dose, while also reducing the thermal history differences between different height regions. Therefore, this invention provides an effective method for controlling heat accumulation, homogenizing thermal history, and optimizing process parameters during the laser filament additive manufacturing of TC11, TC4, and other α+β or near-α type titanium alloy thin-walled parts.
[0073] The above description of the technical solution provided by the present invention through several specific embodiments is intended to highlight the advantages and benefits of the technical solution provided by the present invention. However, the above-described specific embodiments are not intended to limit the present invention. Any reasonable modifications and improvements to the present invention, reasonable combinations of implementation methods and equivalent substitutions based on the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A method for zoned power control of thin-walled parts in laser-fused-wire additive manufacturing of titanium alloys based on thermal history regulation, characterized in that, The methods include: S1: Establish the geometric model of the thin-walled titanium alloy part to be formed and determine the initial laser filament additive manufacturing process parameters; S2: Obtain thermal history data of different height regions during the layer-by-layer deposition process of the titanium alloy thin-walled part under constant initial process parameters; S3: Extract thermal accumulation characteristic parameters from the thermal history data; S4: Construct a thermal accumulation compensation coefficient based on the thermal accumulation characteristic parameters, and divide the titanium alloy thin-walled part into multiple thermal state regions along the deposition height direction based on the thermal accumulation compensation coefficient; S5: Based on the thermal accumulation compensation coefficient corresponding to different thermal state regions, the initial laser power is modified by region to obtain the region laser power corresponding to different height regions. S6: Based on the partitioned laser power, a partitioned power control command is generated, and layer-by-layer deposition is performed in accordance with the partitioned power control command during the laser filament additive manufacturing process of titanium alloy thin-walled parts to regulate the thermal history distribution of different height regions; and as the degree of thermal accumulation in the deposition height direction increases, the partitioned laser power is gradually reduced relative to the initial laser power.
2. The method for zoned power control of thin-walled titanium alloy laser filament additive manufacturing based on thermal history regulation according to claim 1, characterized in that, In step S1, the initial process parameters include initial laser power, scanning speed, wire feed speed, and layer height; in step S3, the thermal accumulation characteristic parameters include one or more of the following: peak temperature, residual temperature at the end of the deposition cycle, high-temperature residence time, high-temperature heat dose, and cooling process characteristic parameters.
3. The method for zoned power control of thin-walled titanium alloy laser filament additive manufacturing based on thermal history regulation according to claim 1, characterized in that, The titanium alloy thin-walled component is a single-walled wall, a thin-walled stiffener, a thin-walled frame, or a quasi-thin-walled titanium alloy component with layer-by-layer stacking characteristics; the titanium alloy is TC11 titanium alloy, TC4 titanium alloy, TA15 titanium alloy, TC18 titanium alloy, or other α+β type and near-α type titanium alloys.
4. The method for zoned power control of thin-walled titanium alloy laser filament additive manufacturing based on thermal history regulation according to claim 1, characterized in that, In step S2, transient heat conduction simulation is used to obtain thermal history data of different height regions during the layer-by-layer deposition process of the titanium alloy thin-walled part under constant initial process parameters; the thermal history data is obtained through one or more of the following methods: numerical simulation, online temperature monitoring, infrared thermal imaging monitoring, molten pool image monitoring, thermocouple temperature measurement, or historical process database. The transient heat conduction simulation uses a moving heat source model, which is one of the following: Gaussian heat source, double ellipsoidal heat source, cylindrical heat source, elliptical heat source, flat-top heat source, or non-Gaussian heat source; the transient heat conduction simulation considers one or more of the following: substrate heat dissipation, surface convection heat dissipation, and surface radiation heat dissipation.
5. The method for zoned power control of thin-walled titanium alloy laser filament additive manufacturing based on thermal history regulation according to claim 1, characterized in that, The thermal history data includes one or more of the following: temperature-time curves at different depositional layers, initial interlayer temperature, peak temperature, residual temperature at the end of the deposition cycle, high-temperature residence time, high-temperature heat dose, and characteristic parameters of the cooling process; the residual temperature at the end of the deposition cycle is the temperature at a characteristic location of the depositional layer after the current depositional layer scan is completed or at the end of the current deposition cycle.
6. The method for zoned power control of thin-walled titanium alloy laser filament additive manufacturing based on thermal history regulation according to claim 5, characterized in that, The high-temperature heat dose is used to characterize the overall degree of high-temperature effect on the material after exceeding a set high-temperature threshold, and is calculated according to the following formula: in, For the first High-temperature heat dose of the layer, For the first Temperature at the characteristic location of the layer, To set a high temperature threshold, Indicates when Higher than Time to take ,when Not higher than Take 0 at that time.
7. The method for zoned power control of thin-walled titanium alloy laser filament additive manufacturing based on thermal history regulation according to claim 1, characterized in that, In step S4, the heat accumulation compensation coefficient is obtained by weighting the normalized residual temperature at the end of the deposition cycle, the high-temperature heat dose, and the characteristic parameters of the cooling process, and is calculated according to the following formula: in, For the first Layer heat accumulation compensation coefficient, For the first The residual temperature at the end of the layer deposition cycle For the first High-temperature heat dose of the layer, For the first Characteristic parameters of the layer cooling process and These represent the maximum and minimum residual temperatures at the end of the deposition cycle, respectively. and These represent the maximum and minimum values of the high-temperature heat dose, respectively. and These represent the maximum and minimum values of the characteristic parameters of the cooling process, respectively. , , All are weighting coefficients.
8. The method for zoned power control of thin-walled titanium alloy laser filament additive manufacturing based on thermal history regulation according to claim 7, characterized in that, The weighting coefficients satisfy: in, , , The degree of influence of residual temperature at the end of the deposition cycle, high-temperature heat dose, and characteristic parameters of the cooling process on heat accumulation was determined respectively.
9. The method for zoned power control of thin-walled titanium alloy laser filament additive manufacturing based on thermal history regulation according to claim 1, characterized in that, In step S4, the plurality of thermal state regions are at least three regions distributed sequentially along the deposition height direction, and the laser power corresponding to different thermal state regions decreases step by step along the deposition height direction; the plurality of thermal state regions include a bottom rapid heat dissipation region, a middle heat accumulation growth region, and a top strong heat accumulation region.
10. The method for zoned power control of thin-walled titanium alloy laser filament additive manufacturing based on thermal history regulation according to claim 1, characterized in that, In step S5, the partitioned laser power is 70%–100% of the initial laser power; when the titanium alloy thin-walled part is divided into five hot state regions along the deposition height direction, the laser power corresponding to the five hot state regions is 100%, 90%–98%, 80%–90%, 75%–85%, and 70%–80% of the initial laser power, respectively.