A composite device and heating method for laser induction heating of metal surfaces
By using laser-induction heating composite equipment and closed-loop temperature control, the instability and consistency problems in the preparation of superhydrophobic metal surfaces have been solved, achieving efficient and stable superhydrophobic effects, simplifying large-area processing, and reducing environmental pollution.
Patent Information
- Application Number
- CN202611482646.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-22
- Publication Date
- 2026-11-17
AI Technical Summary
Existing processes for preparing superhydrophobic metal surfaces suffer from problems such as instability after processing, poor batch consistency, instability and pollution from chemical treatment, and difficulty in large-area continuous processing.
By employing a laser induction heating composite device that combines an induction component and a laser, and through closed-loop temperature control, the heating, heat preservation, and cooling of metal workpieces are achieved, promoting the evolution of the surface chemical state towards a lower surface energy direction and forming a superhydrophobic effect.
It improves the efficiency and consistency of superhydrophobic processing of metal surfaces, reduces environmental pollution, simplifies the process flow, and avoids the instability of chemical treatment and the difficulties of large-area processing.
Smart Images

Figure CN123103222A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of laser processing technology, and in particular to a composite device and method for laser induction heating of metal surfaces. Background Technology
[0002] Existing methods for fabricating superhydrophobic metallic surfaces mainly include natural aging after laser micro / nano shaping, chemical low-surface-energy modification after laser shaping, furnace heat treatment after laser shaping, and combinations of mechanical, chemical, or coating methods with laser processing. These processes primarily suffer from the following drawbacks: 1. Laser processing typically does not immediately produce a stable superhydrophobic state. The initial surface after laser processing often exhibits hydrophilicity or even superhydrophilicity, failing to achieve the superhydrophobic effect of a metal surface.
[0003] 2. Natural aging is used to change the surface from hydrophilic to hydrophobic, which takes a long time and results in poor batch consistency.
[0004] 3. Chemical treatment methods are used, but the chemical structure is unstable and there is a possibility of generating pollutants.
[0005] 4. Existing processes are difficult to perform continuous large-area processing on metal workpieces, resulting in unstable processing quality. Summary of the Invention
[0006] To address the shortcomings of existing technologies, the present invention aims to provide a composite device and method for laser induction heating of metal surfaces, which can achieve superhydrophobic effects on metal surfaces, has high processing efficiency, high product processing consistency and good stability, and reduces environmental pollution.
[0007] The embodiments of the present invention are achieved through the following technical solutions: A composite device for laser induction heating of metal surfaces, comprising: The laser assembly includes a laser for outputting a laser beam, a beam expander assembly arranged sequentially along the laser beam transmission direction, a galvanometer scanning head, and a field lens; A control unit, which is electrically connected to the laser; Metal workpieces; The sensing component includes a dual-channel induction power supply and an upper induction coil and a lower induction coil located on the upper and lower sides of the metal workpiece, respectively; the dual-channel induction power supply is electrically connected to the upper induction coil and the lower induction coil. A thermocouple temperature measuring assembly, wherein the two ends of the thermocouple temperature measuring assembly are electrically connected to the control unit and one end of the metal workpiece, respectively.
[0008] According to a preferred embodiment, the metal workpiece material is one or two of copper, copper alloys, aluminum and aluminum alloys, titanium and titanium alloys, stainless steel, and nickel-based alloys.
[0009] According to a preferred embodiment, the metal workpiece is a copper part.
[0010] According to a preferred embodiment, the laser is a green ultrafast laser with a wavelength of 515 nm.
[0011] A heating method for a laser induction heating composite device for metal surfaces specifically includes the following steps: Step S100: Immerse the metal workpiece in anhydrous ethanol for 2-10 minutes to remove grease and organic contaminants, followed by ultrasonic cleaning. Step S200: After removing the metal workpiece, dry it with one or two of the following gases: dry nitrogen, argon, and clean compressed air that has been treated to remove oil and water. Fix the metal workpiece in a fixture or worktable, so that the area to be processed is within the effective coupling range between the upper and lower induction coils and the scanning range of the galvanometer, and calibrate the focus, adjust the gap between the upper and lower induction coils and the metal workpiece, and adjust the temperature emissivity of the thermocouple equipment. Step S300: Turn on the dual-channel induction power supply and heat the area to be processed to the first target temperature T0 through temperature closed loop; Step S400: After the metal workpiece reaches the first target temperature T0, the ultrafast laser and galvanometer scanning head are turned on. The laser beam is first used to perform parallel reciprocating scanning along the first direction D1, and then to perform parallel reciprocating scanning along the second direction D2 that intersects the first direction D1, with an intersection angle of α. Step S500: Control the area to be processed to reach the second target temperature T1 when the laser beam scanning ends; Step S600: After the laser beam scanning is completed, the laser beam output of the ultrafast laser is turned off, the sensing component remains working, and the metal workpiece is kept at the second target temperature T1 for a duration of N. Step S700: Turn off induction heating, remove the metal workpiece using a heat-resistant fixture or allow it to cool naturally on the fixture; After cooling, the static water contact angle, roll-off angle, surface morphology, and in-plane consistency of the metal workpiece are tested.
[0012] According to a preferred embodiment, in step S100, the ultrasonic medium is anhydrous ethanol.
[0013] According to a preferred embodiment, in step S300, the metal workpiece is a copper workpiece, and the first target temperature T0 range can be selected as 60 to 100°C; after reaching the set value, it can be stabilized for 0.1 min to 5 min to reduce the initial temperature fluctuation.
[0014] According to a preferred embodiment, in step S400, the α phase intersection angle is 30° to 90°, wherein the upper sensing component operates continuously during laser processing.
[0015] According to a preferred embodiment, in step 500, the range of the second target temperature T1 can be selected as 120 to 200°C. If the temperature reaches the second target temperature T1 ahead of schedule, the control unit reduces the sensing power of the dual-channel induction power supply or maintains a constant temperature. If the temperature rise is delayed, the power of the dual-channel induction power supply is increased without exceeding the safety limit.
[0016] According to a preferred embodiment, in step S600, the second target temperature T1 is in the range of 120 to 200°C, and the heat preservation duration N is in the range of 30 min to 2 h.
[0017] According to a preferred embodiment, in step S400, the α phase intersection angle is 90°, the laser beam scanning speed is 200mm / s, the laser power is 20W, and the path formed by the laser beam scanning in the first direction D1 is perpendicular to the path formed by the laser beam scanning in the second direction D2, so as to cause the surface of the metal workpiece to form a grid-like structure.
[0018] The technical solutions of the embodiments of the present invention have at least the following advantages and beneficial effects: This invention is equipped with a sensing component that can promote the heating, heat preservation and cooling of metal workpieces. By using inductive heat to regulate the state of the surface layer and adsorbents induced by laser, the chemical state of the metal workpiece surface is promoted to evolve towards a lower surface energy direction, which can achieve the effect of superhydrophobicity of the metal surface, with high processing efficiency, high product processing consistency and good stability, and reduced environmental pollution. Attached Figure Description
[0019] To more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings used in the embodiments will be briefly introduced below. It should be understood that the following drawings only show some embodiments of the present invention and should not be regarded as a limitation on the scope. For those skilled in the art, other related drawings can be obtained based on these drawings without creative effort.
[0020] Figure 1 This is a schematic diagram of the structure of a metal surface laser induction heating composite device provided in an embodiment of the present invention; Figure 2 This is a schematic diagram of the metal workpiece surface processing in step S400 provided in an embodiment of the present invention; Figure 3 A flowchart illustrating a heating method for a laser induction heating composite device for metal surfaces, provided in an embodiment of the present invention; Figure 4A schematic diagram of heating temperature and time data for a metal surface laser induction heating composite device provided in an embodiment of the present invention; Figure 5 This is a schematic diagram of the metal workpiece surface of the laser beam scanning processing path provided in an embodiment of the present invention; Figure 6 This is a schematic diagram illustrating the changes in the chemical state of a metal workpiece surface provided in an embodiment of the present invention; Figure 7 This is a schematic diagram of the surface structure and test data of the first sample plate after processing, provided in an embodiment of the present invention; Figure 8 This is a schematic diagram of the surface structure and test data of the second sample after processing, provided in an embodiment of the present invention. Figure 9 A schematic diagram of the wetting angle test of the surface structure of the first sample plate after processing, provided in an embodiment of the present invention; Figure 10 This is a schematic diagram of the wetting angle test of the surface structure of the second sample after processing, provided in an embodiment of the present invention.
[0021] Icons: 1. Ultrafast laser; 2. Beam expander assembly; 3. Galvanometer scanning head; 4. Field lens; 5. Upper induction coil; 6. Lower induction coil; 7. Dual-channel induction power supply; 8. Thermocouple temperature measurement device; 9. Metal workpiece; 10. Control unit; D1, First direction; D2, Second direction. Detailed Implementation
[0022] To better understand and implement this invention, the technical solutions in the embodiments of this invention will be clearly and completely described below with reference to the accompanying drawings.
[0023] In the description of this invention, it should be noted that the terms "upper", "lower", "front", "rear", "left", "right", "vertical", "horizontal", "top", "bottom", "inner", "outer", etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. They are only for the convenience of describing this invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on this invention.
[0024] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. The terminology used herein in the description of the invention is for the purpose of describing particular embodiments only and is not intended to be limiting of the invention. Example
[0025] Reference Figures 1 to 10A composite device for laser induction heating of metal surfaces includes: a laser assembly, comprising a laser for outputting a laser beam, a beam expander assembly 2, a galvanometer scanning head 3, and a field lens 4 arranged sequentially along the laser beam transmission direction; a control unit 10, which is electrically connected to the laser; a metal workpiece 9; an induction assembly including a dual-channel induction power supply 7 and an upper induction coil 5 and a lower induction coil 6 located on the upper and lower sides of the metal workpiece 9 respectively; the dual-channel induction power supply 7 is electrically connected to the upper induction coil 5 and the lower induction coil 6; and a thermocouple temperature measuring assembly, the two ends of which are electrically connected to the control unit 10 and one end of the metal workpiece 9 respectively.
[0026] Optionally, the metal workpiece 9 is made of one or two of the following materials: copper, copper alloys, aluminum and aluminum alloys, titanium and titanium alloys, stainless steel, and nickel-based alloys.
[0027] Optionally, the metal workpiece 9 is a copper part.
[0028] Optionally, the laser is a green ultrafast laser with a wavelength of 515 nm.
[0029] A heating method for a laser induction heating composite device for metal surfaces specifically includes the following steps: Step S100: Immerse the metal workpiece 9 in anhydrous ethanol for 2-10 minutes to remove grease and organic contaminants, followed by ultrasonic cleaning. Step S200: After removing the metal workpiece 9, dry it with one or two of the following gases: dry nitrogen, argon, and clean compressed air that has been treated to remove oil and water. Fix the metal workpiece 9 to the fixture or worktable so that the area to be processed is within the effective coupling range between the upper induction coil 5 and the lower induction coil 6 and within the scanning range of the galvanometer. Then, calibrate the focus, adjust the gap between the upper induction coil 5, the lower induction coil 6 and the metal workpiece 9, and adjust the temperature measurement emissivity of the thermocouple device. Step S300: Turn on the dual-channel induction power supply 7 and heat the area to be processed to the first target temperature T0 through temperature closed loop; Step S400: After the metal workpiece 9 reaches the first target temperature T0, the ultrafast laser 1 and the galvanometer scanning head 3 are turned on. The laser beam is first used to perform parallel reciprocating scanning along the first direction D1, and then to perform parallel reciprocating scanning along the second direction D2 that intersects the first direction D1, with an intersection angle of α. Step S500: Control the area to be processed to reach the second target temperature T1 when the laser beam scanning ends; Step S600: After the laser beam scanning is completed, the laser beam output of the ultrafast laser 1 is turned off, the sensing component remains working, and the metal workpiece 9 is kept at the second target temperature T1 for a duration of N. Step S700: Turn off induction heating and remove the metal workpiece 9 using a heat-resistant fixture or allow it to cool naturally on the fixture. After cooling, the static water contact angle, roll-off angle, surface morphology, and in-plane consistency of the metal workpiece 9 were tested.
[0030] Optionally, in step S100, the ultrasonic medium is anhydrous ethanol.
[0031] Optionally, in step S300, the metal workpiece 9 is a copper part, and the first target temperature T0 range can be selected as 60 to 100°C; after reaching the set value, it can be stabilized for 0.1 min to 5 min to reduce the initial temperature fluctuation.
[0032] Optionally, in step S400, the α phase angle is 30° to 90°, wherein the upper sensing component operates continuously during laser processing.
[0033] Optionally, in step 500, the range of the second target temperature T1 can be selected as 120 to 200°C. If the temperature reaches the second target temperature T1 ahead of schedule, the control unit 10 reduces the sensing power of the dual-channel induction power supply 7 or maintains a constant temperature. If the temperature rise is delayed, the power of the dual-channel induction power supply 7 is increased without exceeding the safety limit.
[0034] Optionally, in step S600, the second target temperature T1 ranges from 120 to 200°C, and the heat preservation duration N ranges from 30 min to 2 h.
[0035] Optionally, in step S400, the α phase angle is 90°, the laser beam scanning speed is 200 mm / s, the laser power is 20 W, and the path formed by the laser beam scanning in the first direction D1 is perpendicular to the path formed by the laser beam scanning in the second direction D2, so as to cause the surface of the metal workpiece to form a grid-like structure.
[0036] Working principle of the invention: The present invention is equipped with a sensing component, which can promote the heating, heat preservation and cooling of the metal workpiece 9. By using the inductive heat to regulate the state of the laser-induced surface layer and adsorbent, the chemical state of the surface of the metal workpiece 9 is promoted to evolve towards a low surface energy direction, which can achieve the superhydrophobic effect of the metal surface, with high processing efficiency, high product processing consistency and good stability, and reduced environmental pollution.
[0037] The metal workpiece 9 mentioned in this invention includes, but is not limited to, copper parts. In this embodiment, a copper part is selected. The corresponding laser parameters are as follows: the laser is an ultrafast laser 1 with a wavelength of 515nm. Alternatively, a laser with a wavelength of 343-1064nm can be selected. The pulse width is adjustable and is set to 490fs in this embodiment. The pulse width range can be selected from 200fs to 10ps. The average laser power is 20W, the spacing between adjacent scan lines is 50μm, the actual focused spot is 20μm, and the single pulse energy is 102μJ. Its scanning pattern is two sets of mutually perpendicular grid-like paths, i.e., the intersection angle is 90°, forming a pattern as shown below. Figure 2 The trajectory shown is a grid pattern. Specifically, the laser scanning speed can be selected from 50 to 2000 mm / s, the scanning spacing from 10 to 100 μm, the number of scans from 1 to 50, and the focusing of the field lens 4 from 100 to 250 mm, with an actual focusing range of 20 to 50 μm. Specific parameters should ensure that the energy per unit area and peak energy density meet the conditions for forming micro / nano hierarchical structures, while avoiding the smoothing of nano-secondary structures by large-area continuous molten pools. The frequency of the dual-path induction power supply 7 can be matched according to the material resistivity, permeability, workpiece thickness, target skin depth, and coupling gap; for local surface heating, 10 to 500 kHz is preferred. For high-conductivity, near-nonmagnetic materials such as copper, increasing the frequency helps reduce the skin depth, but a larger workpiece does not necessarily require a higher frequency; a lower frequency can be used for deep heating of thick parts, while a higher frequency can be used for shallow local heating of thin parts.
[0038] The induction power of the dual-channel induction power supply 7 can be determined based on the mass, thickness, coil structure, and heating rate of the metal workpiece 9. Small copper parts can use a 0.5–5kW power supply; large parts can have their rated power increased to approximately 10kW or higher. Rated power is not equivalent to continuous full-power output; the control unit 10 should adjust the actual power and duty cycle based on temperature feedback. The frequency of the induction power supply can be matched to the resistivity, permeability, workpiece thickness, target skin depth, and coupling gap of the copper material. For localized surface heating, a frequency of 10–500kHz is preferred. For high-conductivity, near-nonmagnetic materials such as copper, increasing the frequency helps reduce the skin depth, but a larger workpiece does not necessarily require a higher frequency; lower frequencies are suitable for deep heating of thicker parts, while higher frequencies are suitable for shallow localized heating of thinner parts. The holding time N can be selected from 30 min to 2 h to complete the adsorption and enrichment of low surface energy carbon components. The superhydrophobic properties are determined by both the surface geometry and the surface chemical state. Ultrafast laser ablation creates intersecting micro-grooves, periodic micro-nano textures, nanopores, and redeposited nanoparticles on the metal surface, forming a multi-scale hierarchical rough structure. Simultaneously, oxidation and hydroxylation occur on the fresh surface, forming metal oxides, hydroxides, adsorbed water, and polar hydroxyl groups. At this point, the high surface energy couples with the roughness, causing the surface to initially exhibit hydrophilic or superhydrophilic behavior. The synchronous heating of the metal workpiece 9 by the laser sensing component does not rely on directly generating superhydrophobicity by adding hydrophilic groups. Instead, it enables the rapid formation, stabilization, and controlled evolution of the laser-induced oxide layer, while simultaneously promoting the removal of adsorbed water, partial dehydration of hydroxides, removal or rearrangement of polar hydroxyl groups, and accelerating the adsorption, enrichment, and orientation of low-surface-energy carbonaceous components such as C-C and C-H in the environment on the high specific surface area structure, thereby reducing the surface polarity and surface free energy of the metal workpiece 9. After controlled heating, short-term heat preservation, and natural cooling, the low surface energy chemical state and the micro / nano hierarchical structure work together to allow water droplets to form discrete contacts only on the tops of the micro-protrusions, while trapping air within the grooves, tending towards a Cassie-Baxter type solid-air composite contact state, thus reducing the actual solid-liquid contact area. This invention does not limit the mechanism to a specific oxide valence state transition. The oxide / hydroxide ratio, surface hydroxyl groups, and carbon-containing adsorbates may differ depending on the metal, atmosphere, and temperature. This invention utilizes inductive thermal modulation and laser beam induction to guide the surface layer and adsorbate state of the metal workpiece 9, promoting the evolution of the surface chemical state of the metal workpiece 9 towards a lower surface energy direction.
[0039] This application achieves integrated operation at the same workstation. The laser uses a laser beam to perform micro-nano shaping on the metal workpiece 9, and the sensing components continuously complete the heating and short-term heat preservation of the metal workpiece 9 within the same fixture and workstation, eliminating the steps of transfer, furnace loading, overall heating and cooling, and furnace unloading, thus simplifying the process flow.
[0040] This application is beneficial for shortening the wetting state transition time. The synchronous action of induced heat and laser beam scanning can promote the removal of adsorbed water, removal or rearrangement of polar hydroxyl groups, stabilization of the oxide layer, and adsorption and enrichment of low surface energy carbon components, reducing the waiting time that relies solely on natural aging at room temperature.
[0041] This application does not require external chemical low surface energy modification, does not use fluorinated silanes, fatty acids or polymer coatings, and can reduce the steps of solution preparation, soaking, cleaning, curing and waste liquid treatment, and reduce the amount of organic solvents and fluorinated substances used.
[0042] In this embodiment, the control unit 10 can realize recipe management, timing triggering, temperature PID closed loop, and data recording. The first target temperature T0, the second target temperature T1, the heat preservation duration N, and laser and scanning parameters can be input to the control unit 10 through the process recipe. The temperature sensor can be set to detect the real-time temperature of the surface of the metal workpiece 9 and provide real-time feedback to the control unit 10. In addition, it can work with the control unit 10 to determine and manage the laser power, pulse width, repetition frequency, etc., determine and manage the trajectory, speed, and spacing of the galvanometer scanning head 3, and determine and manage the power and frequency of the dual-channel induction power supply 7.
[0043] Specifically, in step S300, the metal workpiece 9 is a copper part, and the first target temperature T0 range can be selected as 100℃; after reaching the set value, it can be stabilized for 0.1 to 5 minutes to reduce initial temperature fluctuations. In step S400, the α phase angle is 90°, and the upper sensing component works continuously during laser processing. In step 500, the second target temperature T1 range can be selected as 200℃, and in step S600, the temperature of the second target temperature T1 is 200℃, and the holding time N is 30 minutes.
[0044] This application can avoid the overall peeling off of independent modification layers. The functional surface is mainly formed by the micro-nano structure and surface chemical state of the metal substrate itself, and there is no problem of the overall peeling off of independent thick coatings. At the same time, it should be recognized that strong friction may still damage the micro-nano structure, and the specific wear resistance shall be based on actual measurement.
[0045] This application enables localized, rapid, and non-contact heating. Electromagnetic induction directly generates eddy current heat inside the conductive workpiece, resulting in a fast response and easy start-up and shutdown. It can limit the main heat effect to the current processing area and adjacent areas, reducing unnecessary heating of non-processing areas and temperature-sensitive components.
[0046] The temperature trajectory of this application is linked to the scanning progress. The target temperature is generated based on the completed scanning area, path length or partition position, and the sensor output is adjusted in a closed loop. This can reduce the thermal history differences caused by complex patterns, pauses and multi-channel scanning, and improve the consistency of large-area processing.
[0047] The heat-affected zone of this application is controllable. By combining and controlling the first target temperature T0, the second target temperature T1, the heating slope, the holding time, the power, and the frequency, excessive oxidation, structural remelting, and thermal deformation of the substrate can be avoided, and it can be adapted to different metals and thicknesses.
[0048] This application can reduce secondary pollution. After cleaning, the metal workpiece 9 does not need to be transferred to a chemical tank or heating furnace. All treatment can be completed in the same fixture, reducing the re-adhesion of dust, oil and fingerprints during the handling process.
[0049] This application is easy to automate and trace. The laser, galvanometer, sensing components, and thermocouple temperature measuring equipment 8 are managed by the collaborative control unit 10, which can record temperature curves, scanning trajectories, process formulas, and alarm information, facilitating production line integration and quality traceability.
[0050] This application provides comprehensive protection, covering processing methods, fixed equipment, and scanning progress-temperature closed-loop control strategies, forming a complete technology chain from surface configuration and thermochemical regulation to equipment integration.
[0051] This method does not include the steps of coating, impregnating, or vapor-depositing a low surface energy modification layer containing fluorinated silanes, fatty acids, silane coupling agents, silicone oils, or polymers after laser processing. The heat treatment of the sensing components and the laser configuration are integrated processes performed continuously in the same station, rather than separate furnace post-processing.
[0052] This embodiment includes Figure 7 , Figure 8 This diagram illustrates the inspection results after processing two different metal workpieces (9 templates) using this method. Figure 7 Below, Figure 8 The images below depict the periodic surface structure of nine metal workpiece templates. The laser processing method used is laser etching, and the heating method is induction heating. Figure 7 The etching depth on the surface of the nine metal workpiece samples is generally in the range of 35-36 μm. Figure 8 The etching depth on the surface of the nine metal workpiece samples is generally in the range of 61-64 μm. This embodiment... Figure 9 , Figure 10 These are schematic diagrams showing the wetting angle tests after machining nine metal workpiece templates. Both contact angles are greater than 150°. Figure 9 The contact angle of the metal tool surface is 156°. Figure 10 The contact angle of the metal tool surface is 154°; the surface of the metal workpiece 9 sample material after laser treatment is generally hydrophilic with an angle of <10°, while in this embodiment, after induction heating and a series of heat preservation and cooling treatments, the surface of the metal workpiece 9 becomes superhydrophobic with an angle of ≥150°. Figure 6 In the diagram, θ is the contact angle, and a, b, and c are the processing flow and principle diagram, respectively.
[0053] The technical means disclosed in this invention are not limited to those disclosed in the above embodiments, but also include technical solutions composed of any combination of the above technical features. It should be noted that those skilled in the art can make various improvements and modifications without departing from the principles of this invention, and these improvements and modifications are also considered within the scope of protection of this invention.
Claims
1. A composite device for laser induction heating of metal surfaces, characterized in that, include: The laser assembly includes a laser for outputting a laser beam, a beam expander assembly arranged sequentially along the laser beam transmission direction, a galvanometer scanning head, and a field lens; A control unit, which is electrically connected to the laser; Metal workpieces; The sensing component includes a dual-channel induction power supply and an upper induction coil and a lower induction coil located on the upper and lower sides of the metal workpiece, respectively; the dual-channel induction power supply is electrically connected to the upper induction coil and the lower induction coil. A thermocouple temperature measuring assembly, wherein the two ends of the thermocouple temperature measuring assembly are electrically connected to the control unit and one end of the metal workpiece, respectively.
2. The metal surface laser induction heating composite device according to claim 1, characterized in that, The metal workpiece material is one or two of the following: copper, copper alloys, aluminum and aluminum alloys, titanium and titanium alloys, stainless steel, and nickel-based alloys.
3. The metal surface laser induction heating composite device according to claim 1, characterized in that, The metal workpiece is a copper part.
4. The metal surface laser induction heating composite device according to claim 3, characterized in that, The laser is a green ultrafast laser with a wavelength of 515nm.
5. A heating method for a metal surface laser induction heating composite device, comprising using the metal surface laser induction heating composite device as described in any one of claims 1 to 4, characterized in that, Specifically, the following steps are included: Step S100: Immerse the metal workpiece in anhydrous ethanol for 2-10 minutes to remove grease and organic contaminants, followed by ultrasonic cleaning. Step S200: After removing the metal workpiece, dry it with one or two of the following gases: dry nitrogen, argon, and clean compressed air that has been treated to remove oil and water. Fix the metal workpiece in a fixture or worktable, so that the area to be processed is within the effective coupling range between the upper and lower induction coils and the scanning range of the galvanometer, and calibrate the focus, adjust the gap between the upper and lower induction coils and the metal workpiece, and adjust the temperature emissivity of the thermocouple equipment. Step S300: Turn on the dual-channel induction power supply and heat the area to be processed to the first target temperature T0 through temperature closed loop; Step S400: After the metal workpiece reaches the first target temperature T0, the ultrafast laser and galvanometer scanning head are turned on. The laser beam is first used to perform parallel reciprocating scanning along the first direction D1, and then to perform parallel reciprocating scanning along the second direction D2 that intersects the first direction D1, with an intersection angle of α. Step S500: Control the area to be processed to reach the second target temperature T1 when the laser beam scanning ends; Step S600: After the laser beam scanning is completed, the laser beam output of the ultrafast laser is turned off, the sensing component remains working, and the metal workpiece is kept at the second target temperature T1 for a duration of N. Step S700: Turn off induction heating, remove the metal workpiece using a heat-resistant fixture or allow it to cool naturally on the fixture; After cooling, the static water contact angle, roll-off angle, surface morphology, and in-plane consistency of the metal workpiece are tested.
6. The heating method of a metal surface laser induction heating composite device according to claim 5, characterized in that, In step S100, the ultrasonic medium is anhydrous ethanol.
7. The heating method of a metal surface laser induction heating composite device according to claim 5, characterized in that, In step S300, the metal workpiece is a copper part, and the first target temperature T0 range can be selected as 60 to 100℃; after reaching the set value, it can be stabilized for 0.1 min to 5 min to reduce the initial temperature fluctuation.
8. The heating method of a metal surface laser induction heating composite device according to claim 5, characterized in that, In step S400, the α phase intersection angle is 30° to 90°, during which the upper sensing component works continuously.
9. The heating method of a metal surface laser induction heating composite device according to claim 8, characterized in that, In step 500, the range of the second target temperature T1 can be selected as 120 to 200°C. If the temperature reaches the second target temperature T1 ahead of schedule, the control unit reduces the sensing power of the dual-channel induction power supply or maintains a constant temperature. If the temperature rise is delayed, the power of the dual-channel induction power supply is increased without exceeding the safety limit.
10. The heating method of a metal surface laser induction heating composite device according to claim 9, characterized in that, In step S600, the second target temperature T1 is in the range of 120 to 200°C, and the heat preservation duration N is in the range of 30 min to 2 h.
11. The heating method of a metal surface laser induction heating composite device according to claim 8, characterized in that, In step S400, the α phase angle is 90°, the laser beam scanning speed is 200 mm / s, the laser power is 20 W, and the path formed by the laser beam scanning in the first direction D1 is perpendicular to the path formed by the laser beam scanning in the second direction D2, so as to cause the surface of the metal workpiece to form a grid-like structure.