A high-temperature solder film that can be soldered in air and its preparation method

By leveraging the synergistic effect of a benzimidazole compound thermally decomposable anti-oxidation protective layer and an activation layer formed on the surface of metal powder, the problem of solder oxidation in air atmosphere is solved, achieving high-temperature soldering stability and interface reaction capability, making it suitable for high-reliability electronic packaging connections.

CN123103244APending Publication Date: 2026-11-17CHONGQING UNIV OF TECH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202611312024.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-27
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing solders are prone to oxidation when soldering in an air atmosphere, resulting in poor interfacial wettability, low solder shear strength, and difficulty in achieving precise control of the paste morphology and large-scale application.

Method used

The self-supporting high-temperature solder film is composed of metal powder and organic carrier. A benzimidazole compound thermal decomposition type anti-oxidation protective layer is formed on the surface of the metal powder. Combined with the activation layer, reducing components are released during the soldering process to remove oxides, forming a self-supporting flexible film structure.

Benefits of technology

It enables high-temperature welding in an air environment, reduces metal powder oxidation, improves interfacial diffusion reaction capability, ensures welding quality and stability, and is suitable for high-reliability electronic packaging connections.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure FT_3
    Figure FT_3
Patent Text Reader

Abstract

This invention belongs to the field of electronic packaging and welding materials technology, specifically disclosing a high-temperature solder film that can be soldered in air and its preparation method. The solder film body comprises, by mass percentage: 60.0%~72.0% metal powder and 28.0%~40.0% organic carrier. The metal powder is at least one of copper powder and zinc powder, or a mixture of copper powder and zinc powder, coated with a benzimidazole thermally decomposable antioxidant protective layer. The organic carrier is composed of polyvinyl butyral, dibutyl phthalate, functional additives, and organic solvents. This invention significantly improves the oxidation resistance and soldering activity of easily oxidized metal powders by forming a thermally decomposable antioxidant protective layer on the surface of the metal powder and by providing or not providing a reducing activation layer on the film surface. The solder film of this invention has self-supporting properties and good flexibility, enabling high-strength, high-thermal-conductivity interfacial metallurgical connections under air atmosphere and low-pressure hot-pressing conditions, making it suitable for high-temperature packaging of power semiconductor devices.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of electronic packaging and welding materials technology, specifically relating to a high-temperature solder film that can be welded in air and its preparation method. Background Technology

[0002] With the rapid development of electronic information technology, semiconductor devices are gradually becoming smaller and more powerful. Third-generation wide-bandgap semiconductor materials, represented by silicon carbide and gallium nitride, possess advantages such as high power density, high breakdown voltage, high electron mobility, and low dielectric constant, enabling them to operate stably for extended periods in harsh and complex environments. However, compared to traditional silicon-based chips, they generate more heat. To ensure the long-term stable operation of power devices under high-temperature conditions, higher requirements are placed on interconnect materials. High-temperature solders need to have suitable melting temperatures to meet the needs of component production and assembly; their melting temperature range has been defined by the industry as 270℃~350℃. However, the service temperature of commonly used tin-based solder-packaged devices does not exceed 175℃, and the solder remelting temperature does not exceed 300℃, which cannot meet the new requirements for high-temperature solders.

[0003] Chinese patent CN119426848B (A Low-Temperature Sintering Metal Solder Paste and Its Preparation Method and Application) discloses a metal paste welding material. Although it can achieve low-temperature sintering to a certain extent, this type of paste material has the following problems in application: the high concentration of organic solvents and volatile fluxes cause rapid evaporation of the solvents when heated in an air atmosphere, which can easily lead to large-area pores and poor soldering defects inside the joint. Furthermore, it requires strict reducing atmosphere (such as formic acid or hydrogen) or high vacuum protection to prevent oxidation of metal particles. In addition, the paste morphology has problems such as poor dispensing consistency and difficulty in accurately controlling the thickness of the adhesive layer in automated assembly.

[0004] Patent CN121363026A (A High-Performance Copper-Based Metal Composite Welding Sheet and Its Preparation Method) discloses a copper-based metal composite welding sheet, but it relies on a complex electroplating process, making it difficult to achieve large-scale thin-film application of low-cost micron-sized base metal powder. During hot pressing in an air atmosphere, this type of traditional welding sheet often suffers from poor interfacial wettability and low weld shear strength due to secondary oxidation of the surface.

[0005] Furthermore, existing studies (such as Zhang Yu et al., "Preparation and Bonding Performance Study of Super Antioxidant Copper Paste", published in the Journal of Guangdong University of Technology) have attempted to use benzimidazole compounds to surface-treat micro-nano copper powder to improve its antioxidant properties, but the product form is still a paste. During the welding heating process, this type of paste is prone to inducing porosity and localized incomplete soldering inside the joint due to the rapid evaporation of organic solvents, and it is difficult to achieve precise and uniform control of the assembly layer thickness.

[0006] Therefore, how to organically combine surface anti-oxidation treatment technology with self-supporting flexible film morphology, so as to both use the protective layer to inhibit the oxidation of copper powder during storage and the initial stage of heating, and avoid the rheological defects of the paste through the film morphology, while taking into account long-term storage stability and welding activity in the air environment, has become a technical problem that urgently needs to be solved in this field. Summary of the Invention

[0007] To address the aforementioned shortcomings of existing technologies, this invention provides a high-temperature solder film that can be welded in air and a method for preparing the same.

[0008] To achieve the above objectives, the present invention adopts the following technical solution:

[0009] In a first aspect, the present invention provides a high-temperature solder film that can be welded in air, comprising a self-supporting solder film body, the solder film body being composed of metal powder and an organic carrier;

[0010] The metal powder comprises 60.0% to 72.0% by mass percentage, and the organic carrier comprises 28.0% to 40.0% by mass percentage.

[0011] The metal powder is at least one of copper powder and zinc powder, or a mixture of copper powder and zinc powder;

[0012] The surface of the metal powder is formed with a thermally decomposable anti-oxidation protective layer composed of benzimidazole compounds.

[0013] The organic carrier includes adhesives, plasticizers, and organic solvents;

[0014] The protective layer decomposes, volatilizes, or desorbs during hot-press welding at 150–300°C to expose fresh metal surfaces and promote interfacial diffusion reactions.

[0015] As a preferred embodiment, an activation layer is further provided on one or both sides of the solder film body. The activation layer releases reducing components during hot-press welding at 150–300°C to remove oxides from the interface to be soldered and the surface of the metal powder. More preferably, the activation layer is provided on both sides of the solder film body, forming an activation layer / solder film / activation layer sandwich structure.

[0016] In the above technical solution, the average particle size of the copper powder is 0.5 to 10 μm, and the average particle size of the zinc powder is 0.5 to 45 μm.

[0017] The thermally decomposable anti-oxidation protective layer is formed by adsorption, coordination or chemical reaction between a surface treatment agent and the surface of metal powder; the surface treatment agent is a benzimidazole compound, and its addition amount is 0.1% to 5.0% of the mass of the metal powder, preferably 0.3% to 2.0%; the thickness of the thermally decomposable anti-oxidation protective layer is 1 to 100 nanometers, preferably 5 to 50 nanometers.

[0018] Furthermore, the main reason why this invention can achieve welding in an air environment is the synergistic effect of the thermally decomposable anti-oxidation protective layer and the activation layer on the surface of the metal powder. To reduce the oxidation of the metal powder during storage and the initial stage of welding heating, this invention utilizes benzimidazole-based surface treatment agents to form a nanoscale thermally decomposable protective layer on the surface of the metal powder.

[0019] Taking benzimidazole (BIM) treatment of copper powder as an example, the nitrogen-containing groups in the benzimidazole molecule can adsorb or coordinate with the active sites on the copper surface:

[0020] Cu~surface~ + nBIM → Cu(BIM)~n~ (Formula 1)

[0021] In Formula 1, BIM represents a benzimidazole molecule, and n represents the coordination number. This forms a protective layer on the surface of the copper powder composed of a copper-benzimidazole complex, the structure of which can be represented as:

[0022] Cu core | Cu-BIM protective layer (Equation 2)

[0023] When the welding temperature rises to 150–300°C, the above-mentioned protective layer undergoes a thermal decomposition reaction:

[0024] Cu−BIM → Cu 0 + volatile organic species (Formula 3)

[0025] In Equation 3, "volatile organic species" represents gaseous small organic molecules (such as ammonia, hydrocarbon derivatives, etc.) released during the thermal decomposition of benzimidazole. After the thermal decomposition products volatilize and escape, the surface of the copper powder is re-exposed as a fresh metal surface, thereby promoting interfacial diffusion reactions between copper powders and between copper powder and the substrate during the subsequent hot pressing process.

[0026] The adhesive is polyvinyl butyral, and the plasticizer is dibutyl phthalate; by mass percentage, the content of polyvinyl butyral is 1.0% to 5.0%, and the content of dibutyl phthalate is 0.2% to 2.0%; the organic carrier also includes functional additives, which are one or more of hydrophobic fumed silica, dispersants, leveling agents, defoamers, coupling agents, and antioxidants.

[0027] Furthermore, the flexibility of the solder film of the present invention originates from the flexible bridging structure formed between adjacent metal particles by the organic continuous phase. The metal powder particles are not entirely connected by point contact, but rather by continuous or semi-continuous polymeric bridging structures formed between the particles by polymeric binders such as polyvinyl butyral, which can be illustrated as follows:

[0028] M1−P−M2 (Equation 4)

[0029] In this design, M1 and M2 represent adjacent metal particles, and P represents a polymer chain segment. When the film is subjected to bending, a small relative displacement occurs between adjacent metal particles. The polymer chain segment absorbs this relative displacement through stretching, bending, and conformational adjustments, thereby preventing the rigid metal particles from directly fractured. This bridging structure is the structural basis for the "self-supporting" performance of the solder film of this invention.

[0030] Furthermore, dibutyl phthalate, as a plasticizer, increases the free volume between polymer chain segments. This effect can be understood through the theory of polymer free volume: the total volume of a polymer material consists of the volume occupied by the molecular chains and the free volume between them. When plasticizer molecules insert into the spaces between polymer chain segments, they increase the space for chain movement, thus lowering the energy barrier required for the rotation and local movement of the polymer chain segments. Under external stress, the polymer chains can dissipate some mechanical energy through chain segment movement, macroscopically manifesting as good flexibility in the film.

[0031] σ~external~ → chain deformation → energy dissipation (Equation 5)

[0032] In Equation 5, σ~external~ represents the external stress applied to the film. Through this energy dissipation mechanism, the film is less prone to brittle fracture when bent or cut.

[0033] During the solder paste drying process, the organic solvent gradually evaporates. As the liquid phase volume fraction decreases, the average distance between metal particles decreases, while the polymer binder gradually fills the gaps between the particles. This process can be illustrated as follows:

[0034] M⋯M → M−Polymer−M (Equation 6)

[0035] In Equation 6, M⋯M represents the initial gap between adjacent metal particles, and M−Polymer−M represents the bridging structure formed by the polymer binder. This ultimately forms a dense metal-polymer composite network. This film formation method, which involves gradual solvent desolvation rather than instantaneous curing, reduces porosity, cracks, and localized stress concentration caused by rapid solvent escape within the film.

[0036] The activation layer comprises a reducing agent, micron-sized metal powder, and an organic carrier, wherein the organic carrier includes a binder, a plasticizer, and an organic solvent; by mass percentage, the micron-sized metal powder content is 30%–70%, the reducing agent content is 5%–20%, and the organic carrier content is 20%–60%; the reducing agent is one or more of formic acid, benzoic acid, ascorbic acid, citric acid, ammonium formate, or oxalic acid; the thickness of the activation layer is ≤20 μm. Preferably, the activation layer is disposed on both sides of the solder film body, forming an activation layer / solder film / activation layer sandwich structure.

[0037] Furthermore, when the solder film has an activation layer, the reducing components in the activation layer, such as formic acid, citric acid, ascorbic acid, ammonium formate, or oxalic acid, release active components during the soldering heating process, thereby removing oxides from the metal powder and the surface of the substrate to be soldered in situ. Taking formic acid as an example, the reduction reactions of copper oxide and zinc oxide can be represented as follows:

[0038] CuO + 2HCOOH → Cu + 2CO2↑ + 2H2O↑ (Equation 7)

[0039] ZnO + 2HCOOH → Zn + 2CO2↑ + 2H2O↑ (Formula 8)

[0040] As can be seen from Equations 7 and 8, formic acid, under heating conditions, reduces copper oxide and zinc oxide to metallic elements, while itself is oxidized to carbon dioxide and water and escapes. When local oxides are reduced, defect regions are formed inside the oxide film, reducing the effective diffusion resistance of the oxide film and increasing the area of ​​fresh metal, thereby promoting subsequent metal-metal contact and diffusion.

[0041] Secondly, the present invention provides a method for preparing a high-temperature solder film capable of being welded in air as described in any of the above-mentioned technical solutions, comprising the following steps:

[0042] (1) Preparation of organic carrier: Weigh the adhesive, plasticizer, organic solvent and optional functional additives according to the ratio, mix them evenly to obtain organic carrier;

[0043] (2) Metal powder surface treatment: The metal powder to be treated is dispersed in a solution containing benzimidazole compounds and stirred at 40-80℃ for 10-60 min to allow the benzimidazole compounds to be adsorbed or located on the surface of the metal powder. After solid-liquid separation and drying, modified metal powder with a thermally decomposable anti-oxidation protective layer is obtained.

[0044] (3) Preparation of solder paste: The metal powder obtained in step (2) and the organic carrier obtained in step (1) are mixed in a mass ratio, wherein the metal powder accounts for 60.0% to 72.0% and the organic carrier accounts for 28.0% to 40.0%. The mixture is stirred evenly under vacuum to obtain solder paste.

[0045] (4) Preparation of self-supporting solder film: The solder paste obtained in step (3) is coated on the surface of the release substrate, and the wet film thickness is controlled to be 200-1000 micrometers. After drying, a self-supporting high temperature solder film with a thickness of 50-300 micrometers is obtained.

[0046] Preferably, the drying process includes staged drying: the first stage is a heat preservation at 40-60°C, and the second stage is a heat preservation at 80-120°C.

[0047] Further, after step (4), step (5) is included: preparing an activation layer slurry, applying the activation layer slurry to one or both sides of the solder film by coating, and forming an activation layer after drying to obtain a single-sided activation structure or an activation layer / solder film / activation layer sandwich structure; the activation layer slurry is composed of a reducing agent, micron-sized metal powder and an organic carrier, and by mass percentage, the content of the micron-sized metal powder is 30% to 70%, the content of the reducing agent is 5% to 20%, and the content of the organic carrier is 20% to 60%.

[0048] The "self-supporting" in this invention refers to the ability of a film to maintain its complete sheet-like shape and undergo cutting, transfer, and stacking operations without breakage, thanks to its own mechanical strength and flexibility, without the support of a release substrate.

[0049] Compared with the prior art, the present invention has the following beneficial effects:

[0050] (1) The present invention uses metal powder and organic carrier to form a self-supporting flexible solder film. Compared with traditional solder paste, it has good shape retention ability and can be cut according to the size of the welding area to achieve precise quantitative supply of solder and avoid the problems of collapse, flow and uneven thickness in the solder paste printing process.

[0051] (2) By setting a thermally decomposable anti-oxidation protective layer formed by benzimidazole compounds on the surface of metal powder, the present invention can effectively reduce the oxidation of metal powder during storage and automatically remove the protective layer during welding at 150-300℃, thereby restoring the activity of the metal surface and significantly improving the interfacial diffusion reaction capability.

[0052] (3) By setting an activation layer structure, the present invention uses a reducing agent to remove metal oxides during the welding process, thereby further improving the contact quality between metal powders and between solder and substrate, and promoting the formation of a stable and reliable metallurgical connection.

[0053] (4) The solder film of the present invention can be hot-pressed in an air environment without the need for complex vacuum or protective atmosphere equipment. It also has the potential for low-cost metal material application, which is conducive to the large-scale application of highly reliable electronic packaging connection.

[0054] (5) This invention achieves a synergistic benefit between surface anti-oxidation treatment and film morphology, resulting in unexpected technical effects. Specifically, this invention utilizes benzimidazole compounds to form a nanoscale protective layer on the surface of copper / zinc powder, and combines it with the dense organic-inorganic composite structure of a self-supporting film, significantly improving the long-term storage stability of the solder film. As shown in the comparison between Examples 3 and 4 (see Table 2), the surface-treated solder film (Example 3) maintained a shear strength retention rate of 94.1% (from 67.22 MPa to 63.38 MPa) after 60 days of sealed storage at room temperature; while the control group (Example 4), which was not surface-treated but also had an activation layer, maintained a shear strength retention rate of only 87.2% (from 66.98 MPa to 58.41 MPa) under the same storage conditions. The difference between the two shows that the thermally decomposable anti-oxidation protective layer is not just a simple anti-oxidation coating. It forms a synergistic protection mechanism with the low-oxygen diffusion channels inside the film and the in-situ deoxygenation effect of the activation layer, enabling the film to maintain excellent welding activity after 60 days of storage. This significantly superior long-term stability compared to single methods (surface treatment only or activation layer only) is something that has not been revealed in the prior art. Attached Figure Description

[0055] Figure 1 This is a photograph of the solder film obtained in Example 1.

[0056] Figure 2 The cross-sectional morphology of the joints after welding with different sized pads ((a) 3×3, (b) 5×5, (c) 8×8, (d) 10×10, (e) Φ5) in Example 1 is shown.

[0057] Figure 3 This is a graph showing the average shear strength of pads of different sizes after soldering in Example 1.

[0058] Figure 4 The graph shows the change in shear strength of the welded joint in Example 1 after aging at 300°C.

[0059] Figure 5 The thermal conductivity diagrams of the welded joint in Example 1 after aging at 300°C at different test temperatures are shown.

[0060] The present invention will be further described in detail below through specific embodiments. These embodiments are for illustrative purposes only and should not be considered as limiting the scope of the invention. All technical solutions implemented based on the above description of the present invention fall within the protection scope of the present invention.

[0061] Example 1

[0062] A copper-zinc micron-sized mixed powder solder film, the raw materials of which, by mass percentage, comprise the following components:

[0063] Alloy powder: 63.03%, wherein the alloy powder is a physical-mechanical mixture of micron copper powder with an average particle size of 1 μm and micron zinc powder with an average particle size of 45 μm, which has been surface modified with benzimidazole, at a mass ratio of 7:3;

[0064] Organic carrier: 36.97%, the organic carrier is composed of the following components: polyvinyl butyral (PVB) 2.25%, dibutyl phthalate (DBP) 0.62%, modified hydrophobic fumed silica 1.0%, the balance being a mixed solvent composed of anhydrous ethanol and terpineol in a volume ratio of 17:10.

[0065] Its preparation method includes the following steps:

[0066] (1) Preparation of organic carrier: Weigh PVB, anhydrous ethanol, terpineol and DBP. First, add PVB to anhydrous ethanol and stir until completely dissolved. Then add DBP and hydrophobic fumed silica. After vacuum degassing and stirring, a clear and transparent organic carrier is obtained.

[0067] (2) Surface treatment of metal powder: Copper powder with an average particle size of 1 μm is dispersed in an ethanol solution containing benzimidazole and stirred at 80°C for 60 minutes. After washing and drying, modified copper powder with a thermally decomposable anti-oxidation protective layer is obtained. The modified copper powder is mechanically mixed with zinc powder with an average particle size of 45 μm at a mass ratio of 7:3 to obtain a uniform copper-zinc mixed alloy powder.

[0068] (3) Preparation of solder slurry: The copper-zinc mixed powder obtained in step (2) is mixed with the organic carrier obtained in step (1) at a mass ratio of 63.03:36.97, and vacuum stirred in a vacuum mixer to obtain a uniform slurry;

[0069] (4) Preparation of self-supporting solder film: The slurry is coated onto release paper by a scraping method, and the wet film thickness is controlled to be 500 μm; the wet film is placed in a drying oven and heated to 100°C at a rate of 0.8°C / min, and kept at the temperature for 100 minutes for drying; after drying, the release paper is peeled off to obtain a self-supporting flexible high-temperature solder film with a film thickness of about 150 μm.

[0070] Welding method: The obtained solder film is punched to the size corresponding to the oxygen-free copper substrate to be welded (sizes are 3×3, Φ5, 5×5, 8×8, 10×10 respectively), and placed in a three-layer stacked structure of "copper substrate / solder film / copper substrate"; the above assembly is placed in a hot press, and under an air atmosphere, a pressure of 10MPa is applied, heated to 250℃ and held for 10 minutes, and then cooled to achieve the welding connection.

[0071] Post-weld test results are as follows Figures 2 to 5 As shown, the joint has good shear strength, and its strength is further improved after aging at 300℃. Its thermal conductivity meets the requirements for high-temperature packaging.

[0072] Example 2

[0073] To verify the rationality of the composition range of the solder film of the present invention, while maintaining consistent welding temperature, pressure, holding time, film thickness, base material, and metal powder particle size, only the mass ratio of metal powder to organic carrier was changed to prepare solder films with metal powder contents of 58%, 60%, 63.03%, 68%, 72%, and 74%. The 63.03% group adopted the composition described in Example 1, while the other groups only adjusted the ratio of metal powder to organic carrier, with the proportions of other components calculated according to the same ratio. All solder films were prepared according to the method described in Example 1 and welded under the same air hot-pressing conditions. The film integrity, flexibility, post-weld shear strength, weld thickness, and interface microstructure of each group of films were tested to evaluate the rationality of the metal powder content range.

[0074] Table 1. Comparison of properties of solder films with different ratios (5mm×5mm pads)

[0075] Metal powder / wt% Organic carrier / wt% flexibility Shear strength / MPa 58 42 high 26.33 60 40 high 44.68 63.03 36.97 high 50.35 68 32 higher 52.31 72 28 brittle 38.11 74 26 crisp 39.17

[0076] Based on the above comparison results, it can be seen that when each component and its content are within the range defined by the present invention, the resulting solder film can take into account both good flexibility and welding performance, and achieve a good balance between film integrity, bending adaptability and welding joint bonding performance, resulting in excellent overall performance.

[0077] Example 3

[0078] This embodiment further incorporates an activation layer on the solder film obtained in Example 1 to enhance soldering activity in an air environment.

[0079] (1) Preparation of activated slurry: Weigh 50% micron copper powder, 10% formic acid, 2% PVB, and 0.8% DBP by mass percentage, with the remainder being a mixed solvent of anhydrous ethanol and terpineol; first dissolve PVB in the mixed solvent, then add DBP for plasticization, add micron copper powder and disperse at high speed to make the copper powder evenly distributed, and finally add formic acid, and obtain the activated slurry by vacuum stirring.

[0080] (2) Formation of activation layer: The activation slurry is coated on one or both sides of the solder film obtained in Example 1 by scraping, and the thickness of the activation layer is controlled to be 5 to 20 μm. After drying at 80 to 120°C, a single-sided activated solder film or an activated layer / solder film / activated layer sandwich structure solder film is obtained.

[0081] To investigate the surface oxidation resistance and welding performance stability of solder films after storage, solder films prepared in the same batch were divided into an immediate welding group and a storage welding group. The immediate welding group was welded immediately after preparation, while the storage welding group was sealed and stored at room temperature for 10 days, 30 days, and 60 days before welding. Both welding processes were performed according to the welding method described in Example 1. The base material used in both groups was a copper block with a trace oxide layer on its surface. The shear strength and interface microstructure of the welded joints were analyzed.

[0082] Example 4

[0083] This embodiment serves as a comparison with Example 3, verifying the effect of the activation layer on welding in air by only setting an activation layer on the metal powder without surface treatment.

[0084] (1) Solder film preparation: No metal surface treatment is performed, and the remaining steps are the same as in Example 1.

[0085] (2) Preparation and formation of activated slurry: Same as in Example 3.

[0086] To investigate the surface oxidation resistance and welding performance stability of solder films after storage, solder films prepared in the same batch were divided into an immediate welding group and a storage welding group. The immediate welding group was welded immediately after preparation, while the storage welding group was sealed and stored at room temperature for 10 days, 30 days, and 60 days before welding. Both welding processes were carried out according to the welding method described in Example 1. The base material used in both groups was a copper block with a trace oxide layer on its surface. The shear strength and interface microstructure of the welded joints were analyzed.

[0087] Table 2 Comparison of welding performance between Example 3 and Example 4 (5mm×5mm pad)

[0088] Storage time (days) 0 10 30 60 Example 3 67.22MPa 66.63MPa 65.31MPa 63.38MPa Example 4 66.98MPa 64.14MPa 62.72MPa 58.41MPa

[0089] The above comparison results show that the solder film of the present invention maintains good welding performance and exhibits good storage stability even after long-term storage. Specifically, the surface-treated solder film demonstrates superior welding performance after storage, indicating that surface treatment effectively reduces oxidation and activity loss on the solder film surface during storage, thus improving its long-term storage stability. Furthermore, for the untreated solder film, activation treatment with an activation layer before welding still yields a weld joint strength similar to that of the surface-treated solder film with the activation layer. This demonstrates that the activation layer effectively restores or enhances the interfacial reactivity of the solder film, thereby reducing the adverse effects of surface oxidation on welding performance. Therefore, the present invention, by combining surface treatment with a pre-welding activation layer, can balance the long-term storage stability and welding performance of the solder film.

[0090] Example 5

[0091] A copper powder sintered high-temperature solder film, the raw materials of which, by mass percentage, comprise the following components:

[0092] Metal powder: 60%, wherein the metal powder is micron copper powder with an average particle size of 1 μm that has been surface modified with benzimidazole;

[0093] Organic carrier: 40%, the organic carrier is composed of the following components: PVB 1.0%, DBP 0.2%, hydrophobic fumed silica 0.5%, polyvinylpyrrolidone (PVP) 1.0%, the balance being a mixed solvent of anhydrous ethanol and terpineol.

[0094] The preparation and welding methods are the same as in Example 1, with the base material being an oxide-free copper substrate. After welding, a copper sintered bonding layer is formed, and the average shear strength of the welded joint is 46.17 MPa.

[0095] Example 6

[0096] A zinc powder sintered high-temperature solder film, the raw materials of which, by mass percentage, comprise the following components:

[0097] Metal powder: 67.23%, wherein the metal powder is elemental zinc powder without surface modification treatment, with an average particle size of 1–10 μm.

[0098] Organic carrier: 32.77%, the organic carrier is composed of the following components: PVB 1.2%, DBP 0.1%, hydrophobic fumed silica 0.3%, polyvinylpyrrolidone (PVP) 1.0%, polyether modified polysiloxane 0.02%, and the balance is a mixed solvent of anhydrous ethanol and terpineol.

[0099] The preparation and welding methods are the same as in Example 1, with the base material being an oxide-free copper substrate. During the welding process, zinc powder and the copper substrate undergo an interfacial reaction to form a copper-zinc intermetallic compound bonding layer. The average shear strength of the welded joint is 27.99 MPa.

[0100] Comparative Example 1

[0101] This comparative example uses a copper-zinc mixed powder with the same composition and ratio as in Example 1 (average copper particle size 1 μm, average zinc particle size 45 μm, mass ratio 7:3). However, the copper powder is not subjected to benzimidazole surface modification treatment, and the mixed powder is used directly as solder for air atmosphere soldering without adding any organic carrier, slurry preparation, or casting. The soldering method is the same as in Example 1.

[0102] The test results are shown in Table 3. The room temperature shear strength and the shear strength after aging at 300℃ of Comparative Example 1 are significantly lower than those of Example 1, and the weld thickness is uneven and greater than 300μm. This indicates that the surface protective layer and film morphology provided by the present invention have a significant effect on improving welding performance.

[0103] Table 3 Comparison of welding performance using CuZn powder and CuZn solder thin film (Φ5 pad)

[0104] Group Shear strength at room temperature Shear strength after aging at 300℃ weld thickness Example 1 50.35MPa 68.06MPa Approximately 100 micrometers Comparative Example 1 31.98MPa 51.32MPa Greater than 300 micrometers

[0105] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of this application and not to limit the technical solutions. Although the applicant has described this application in detail with reference to preferred embodiments, those skilled in the art should understand that any modifications or equivalent substitutions to the technical solutions of this application without departing from the spirit and scope of this technical solution should be covered within the scope of the claims of this application.

Claims

1. A high-temperature solder film that can be welded in air, characterized in that, The invention includes a self-supporting solder film body, which is composed of metal powder and an organic carrier; The metal powder comprises 60.0% to 72.0% by mass percentage, and the organic carrier comprises 28.0% to 40.0% by mass percentage. The metal powder is at least one of copper powder and zinc powder, or a mixture of copper powder and zinc powder; The surface of the metal powder is formed with a thermally decomposable anti-oxidation protective layer composed of benzimidazole compounds. The organic carrier includes adhesives, plasticizers, and organic solvents; The thermally decomposable anti-oxidation protective layer decomposes, volatilizes, or desorbs during hot-press welding at 150–300°C, thereby exposing the fresh metal surface and promoting interfacial diffusion reaction.

2. The high-temperature solder film that can be welded in air according to claim 1, characterized in that, An activation layer is provided on one or both sides of the solder film body. The activation layer contains a reducing agent and metal powder. During the hot pressing welding process at 150-300°C, the activation layer releases reducing components to remove oxides from the interface to be welded and the surface of the metal powder.

3. A high-temperature solder film that can be welded in air according to claim 2, characterized in that, The activation layer is disposed on both sides of the solder film body, forming an activation layer / solder film / activation layer sandwich structure.

4. A high-temperature solder film that can be welded in air according to any one of claims 1-3, characterized in that, The copper powder has an average particle size of 0.5–10 μm, and the zinc powder has an average particle size of 0.5–45 μm.

5. A high-temperature solder film that can be welded in air according to any one of claims 1-4, characterized in that, The thermally decomposable anti-oxidation protective layer is formed by the adsorption, coordination or chemical reaction between the surface treatment agent and the surface of the metal powder; the surface treatment agent is a benzimidazole compound, and its addition amount is 0.1% to 5.0% of the mass of the metal powder; the thickness of the thermally decomposable anti-oxidation protective layer is 1 to 100 nanometers.

6. A high-temperature solder film that can be welded in air according to any one of claims 1-5, characterized in that, The adhesive is polyvinyl butyral, and the plasticizer is dibutyl phthalate. The content of polyvinyl butyral is 1.0% to 5.0% by mass percentage, and the content of dibutyl phthalate is 0.2% to 2.0%. The organic carrier also includes functional additives, which are one or more of hydrophobic fumed silica, dispersants, leveling agents, defoamers, coupling agents, and antioxidants.

7. A high-temperature solder film that can be welded in air according to claim 6, characterized in that, The amount of hydrophobic fumed silica added is 0.2% to 1.5%, its specific surface area is 150 to 250 m² / g, and its surface is hydrophobically modified by hexamethyldisilazane. The dispersant is one or more of polyvinylpyrrolidone, polyethylene glycol, polyacrylate, or polycarboxylate, and its total addition amount is 0.05% to 1.0%. The leveling agent is a polyether-modified polysiloxane, and its addition amount is 0.02% to 0.05%. The coupling agent is γ-aminopropyltriethoxysilane, γ-glycidoxypropyltrimethoxysilane or γ-methacryloyloxypropyltrimethoxysilane, and its addition amount is 0.05% to 0.5%.

8. A high-temperature solder film that can be welded in air according to any one of claims 2-7, characterized in that, The organic carrier in the activation layer includes an adhesive, a plasticizer, and an organic solvent; the adhesive is polyvinyl butyral, and the plasticizer is dibutyl phthalate. By mass percentage, the content of the micron-sized metal powder is 30%–70%, the content of the reducing agent is 5%–20%, and the content of the organic carrier is 20%–60%. The reducing agent is one or more of formic acid, benzoic acid, ascorbic acid, citric acid, ammonium formate, or oxalic acid. The thickness of the activation layer is ≤20μm.

9. A method for preparing a high-temperature solder film capable of air soldering as described in any one of claims 1-8, characterized in that, Includes the following steps: (1) Preparation of organic carrier: Weigh the adhesive, plasticizer, organic solvent and optional functional additives according to the ratio, mix them evenly to obtain organic carrier; (2) Metal powder surface treatment: The metal powder to be treated is dispersed in a solution containing benzimidazole compounds and stirred at 40-80℃ for 10-60 min to allow the benzimidazole compounds to be adsorbed or located on the surface of the metal powder. After solid-liquid separation and drying, modified metal powder with a thermally decomposable anti-oxidation protective layer is obtained. (3) Preparation of solder paste: The metal powder obtained in step (2) and the organic carrier obtained in step (1) are mixed in a mass ratio, wherein the metal powder accounts for 60.0% to 72.0% and the organic carrier accounts for 28.0% to 40.0%. The mixture is stirred evenly under vacuum to obtain solder paste. (4) Preparation of self-supporting solder film: The solder paste obtained in step (3) is coated on the surface of the release substrate, and the wet film thickness is controlled to be 200-1000 micrometers. After drying, a self-supporting high temperature solder film with a thickness of 50-300 micrometers is obtained.

10. The method for preparing a high-temperature solder film that can be soldered in air according to claim 9, characterized in that, Step (5) is included after step (4): An activation layer slurry is prepared and coated onto one or both sides of the solder film. After drying, an activation layer is formed, resulting in a single-sided activation structure or an activation layer / solder film / activation layer sandwich structure. The activated layer slurry is composed of a reducing agent, micron-sized metal powder, and an organic carrier. By mass percentage, the micron-sized metal powder content is 30%–70%, the reducing agent content is 5%–20%, and the organic carrier content is 20%–60%.

11. A method for preparing a high-temperature solder film that can be soldered in air according to claim 9 or 10, characterized in that, The drying in step (4) includes segmented drying: Phase 1: Insulation at 40-60℃; Second stage: Insulation at 80-120℃.

Citation Information

Patent Citations

  • Low temperature sintered metal solder paste and method of making and use thereof

    CN119426848B

  • High-performance copper-based metal composite soldering lug and preparation method thereof

    CN121363026A