A core-reinforced wafer Notch groove chamfering grinding wheel and its preparation method

By employing a composite interface structure of integral titanium plating on a steel substrate and a dual-gradient metal buffer layer in the wafer notch chamfering grinding wheel, combined with a through-type core pillar reinforcement structure, the problems of brittle fracture and mass production of grinding wheels have been solved, realizing the preparation of high-strength, long-life grinding wheels suitable for notch processing of various semiconductor materials.

CN123103534APending Publication Date: 2026-11-17ZHENGZHOU SHINE MORE SUPERABRASIVES +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202611369437.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-04
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing wafer notch chamfering grinding wheels are prone to brittle fracture during grinding, have a short service life, and are difficult to mass-produce, affecting processing efficiency and wafer yield.

Method used

The composite interface structure of the steel substrate with overall titanium plating and double-gradient metal buffer layer is adopted, and the composite load-bearing structure is constructed by combining a through-type steel core column. The interface bonding force and grinding wheel strength are improved by batch preparation process of integral sintering of blank and wire cutting granulation.

Benefits of technology

It improves the ultimate bending load capacity of the grinding wheel, extends its service life, reduces the breakage rate, meets the needs of high-volume, high-precision supply, and is suitable for notch groove processing of various semiconductor materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123103534A_ABST
    Figure CN123103534A_ABST
Patent Text Reader

Abstract

This invention discloses a core-reinforced wafer notch chamfering grinding wheel and its preparation method. The grinding wheel sequentially comprises a substrate, a double-layer gradient metal buffer layer, and a grinding layer. The double-layer gradient metal buffer layer is located between the grinding layer and the substrate. The double-layer gradient metal buffer layer includes a metal buffer layer 1 disposed on the upper surface of the substrate and a metal buffer layer 2 disposed on the upper surface of the metal buffer layer 1. Both metal buffer layers 1 and 2 have a thickness of 1-2 mm. A core post is pre-embedded inside the substrate, extending through the double-layer gradient metal buffer layer into the grinding layer. The outer end face of the core post is flush with the outer end face of the grinding layer. This invention improves the ultimate load-bearing capacity of the grinding wheel by setting a steel core post inside the grinding wheel, forming a three-layer composite reinforcement structure of "abrasive layer-metal buffer layer-core post". The method employs a monolithic hot-pressing sintering molding process to prepare the entire blank, and then uses wire cutting to obtain multiple grinding wheels, increasing the single-furnace capacity by an order of magnitude and reducing production costs.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of semiconductor precision processing technology, specifically relating to a core-enhanced wafer Notch groove chamfering grinding wheel and its preparation method. Background Technology

[0002] A wafer is the physical substrate and core raw material for semiconductor chip manufacturing. It is mainly classified by diameter into 6-inch (150mm), 8-inch (200mm), and 12-inch (300mm) wafers, with 12-inch wafers currently being the mainstream size for advanced manufacturing processes. Silicon wafers are widely used in the manufacture of microprocessors, memory chips, and various integrated circuits due to their stable performance, abundant reserves, and relatively low cost. In recent years, silicon carbide (SiC) wafers have demonstrated significant advantages in high-frequency, high-power applications such as electric vehicles, power converters, and 5G communications due to their excellent high-temperature resistance, high-pressure resistance, and thermal conductivity.

[0003] A small notch or flat edge is typically found on the edge of a wafer to mark its crystal orientation and serve as a positioning reference in subsequent processing. For large wafers of 8 inches and above, a flat edge would waste wafer area; therefore, the industry commonly uses a small notch (i.e., a notch groove) at the wafer edge as a positioning marker. The position and shape accuracy of the notch groove directly affect the alignment accuracy of dozens of processes, including photolithography, thin film deposition, and etching, and has a crucial impact on chip yield. Precision chamfering of the notch groove requires the use of a small-sized dedicated grinding wheel (referred to in the industry as a "wafer chamfering grinding head" or "notch grinding wheel") to contour-grind the notch groove on the wafer edge using specialized chamfering equipment. The notch grinding wheel is tiny, typically only 30-40 mm in total length and a few millimeters in diameter, requiring extremely high shape accuracy and wear resistance. Its processing quality directly affects the microstructure of the wafer edge and the stability of subsequent processes.

[0004] In actual processing, Notch grinding wheels are prone to large bending moments and impact loads during grinding. The grinding wheels often experience brittle fracture at weak sections (such as the bottom of the groove), resulting in: (1) premature scrapping of the grinding head and short service life; (2) fracture fragments may damage the wafer surface, causing losses to customers; (3) increased tool changing frequency and reduced processing efficiency.

[0005] Chinese invention patent "Application Publication No. CN 119427241A, Application Publication Date 2025.02.14" discloses a method for preparing a diamond grinding wheel for wafer notch grinding. It uses a metal binder and other additives to prepare a diamond grinding wheel for wafer notch grinding that takes into account both high life and high machining accuracy. However, its grinding wheel structure is only a simple structure of abrasive layer + metal matrix, lacking an effective internal reinforcement mechanism, and cannot solve the problem of easy brittle fracture at the bottom of the grinding wheel groove. Chinese invention patent CN 119501837A (publication date: February 25, 2025) discloses a wafer positioning groove chamfering grinding head and its manufacturing method for wafer notch chamfering. This method improves interfacial bonding by setting a metal powder transition layer between the substrate and the abrasive layer and applying a fluoroborate flux to the substrate before sintering. However, this approach has significant drawbacks: ① Residual impurities at the interface after high-temperature decomposition of the flux form brittle inclusions, weakening interlayer bonding; ② The large difference in thermal expansion coefficients between the steel substrate and the transition layer easily leads to microcracks at the interface due to thermal mismatch during sintering; ③ The consistency of manually applied flux is unstable, and interfacial bonding stability cannot be guaranteed during mass production. Furthermore, this invention also lacks an internal reinforcement structure, making it prone to groove bottom breakage during processing. Additionally, neither of these inventions addresses mass production methods, limiting single-furnace output to single-chip or small-batch production.

[0006] Therefore, in order to solve the above problems, the present invention provides a core-reinforced wafer Notch groove chamfering grinding wheel and a method for mass production thereof. Summary of the Invention

[0007] To address the problems of low sintering capacity, weak interfacial bonding between the substrate and abrasive layer, and brittle fracture during grinding in existing wafer notch chamfering grinding wheels, this invention provides a core-reinforced wafer notch chamfering grinding wheel and its preparation method. Through a batch production process combining integrated blank sintering and wire-cutting, the invention abandons the independent sintering mode of individual grinding wheels, increasing capacity, reducing production costs, and ensuring batch consistency in wheel size and performance, thus meeting the large-scale, stable supply demands of the semiconductor industry. A composite interface structure of integral titanium plating on a steel substrate and a dual-gradient metal buffer layer is adopted. Gradient composition matching and bidirectional metallurgical diffusion of the titanium plating layer reduce the difference in thermal expansion coefficients between interfaces, improving interfacial bonding and reducing the risk of microcracks or open fractures. A through-type steel core pillar is pre-embedded inside the grinding wheel to construct a composite load-bearing structure, changing the brittle fracture failure mode of the grinding wheel, improving its ultimate bending load-bearing capacity, preventing sudden wheel fracture during grinding, extending wheel life, and mitigating the risk of wafer scratches. Optimize the grinding wheel formulation system and sintering process to broaden the product's application scenarios. It is compatible with the chamfering of notch grooves on various semiconductor wafers such as silicon, silicon carbide, gallium nitride, and gallium arsenide, thereby improving the process's versatility and portability.

[0008] To achieve the above objectives, the technical solution adopted by the present invention is as follows:

[0009] A core-reinforced wafer notch chamfering grinding wheel, the grinding wheel structure comprising, in sequence, a substrate, a double-layer gradient metal buffer layer, and a grinding layer, wherein the double-layer gradient metal buffer layer is located between the grinding layer and the substrate, the double-layer gradient metal buffer layer comprising a metal buffer layer 1 (close to the substrate portion) disposed on the upper surface of the substrate, and a metal buffer layer 2 (close to the grinding layer portion) disposed on the upper surface of the metal buffer layer 1, the thickness of both the metal buffer layer 1 and the metal buffer layer 2 being 1~2 mm, wherein a core post is pre-embedded inside the substrate, the core post extending through the double-layer gradient metal buffer layer into the interior of the grinding layer, and the outer end face of the core post being flush with the outer end face of the grinding layer.

[0010] Furthermore, the core is inserted into the pre-embedded hole in the substrate, forming a clearance fit between the two.

[0011] Furthermore, the grinding wheel base material is 45# steel, and the core post material is preferably austenitic stainless steel.

[0012] Furthermore, the grinding wheel grinding layer formula is related to the wafer material. Taking silicon wafers as an example, the specific formula consists of the following raw materials in parts by weight: 20-40 parts abrasive, 60-80 parts metal binder, and 1-5 parts additives. The additives are one or more mixtures of reagent graphite or granular graphite. The metal binder consists of the following raw materials in parts by weight: 20-40 parts copper powder, 20-40 parts tin powder, and 40-60 parts cobalt powder.

[0013] Furthermore, the metal buffer layer 1 is composed of the following raw materials in parts by weight: 30-40 parts of ultrafine copper powder, 20-30 parts of ultrafine tin powder, 15-25 parts of nickel powder, 1-5 parts of titanium powder, 1-2 parts of phosphorus iron alloy powder, and 1-2 parts of bismuth powder.

[0014] Furthermore, the raw material composition of the metal buffer layer 2 is the same as that of the metal binder in the grinding layer.

[0015] Furthermore, the ultrafine copper powder and ultrafine tin powder have a particle size of 5~10 μm, the other metal powders (copper powder, tin powder, cobalt powder, nickel powder, titanium powder, ferrophosphorus alloy powder, bismuth powder) have a median particle size of ≤50 μm, and the reagent graphite or granular graphite has a particle size of ≤50 μm.

[0016] Furthermore, the abrasive in the grinding wheel layer is diamond, and the diamond mesh size varies from 800 to 3000 depending on the material of the object being processed and the processing requirements.

[0017] A method for preparing the above-mentioned core-reinforced wafer Notch groove chamfering grinding wheel includes the following steps:

[0018] S1. Weigh the required raw materials for metal buffer layer 1 according to the proportion, pour them into a mixing tank, add a certain proportion of steel balls and wetting agent, and mix them evenly using a three-dimensional mixer to obtain metal buffer layer 1 mixed powder.

[0019] S2. Weigh the raw materials required for metal buffer layer 2 according to the proportion, pour them into the mixing tank, and mix them according to the mixing method in S1 to obtain metal buffer layer 2 mixed powder. S3. Weigh out the raw materials required for the grinding layer according to the proportion, pour them into the mixing tank, and mix them in the same way as in S1 to obtain the grinding layer mixed powder.

[0020] Furthermore, in S1, S2, and S3, the mixing speed is 100~300 rpm, the mixing time is 2~3 h, the ball-to-material mass ratio is 1:(2~4), and the steel ball diameter is 2~10 mm; the wetting agent is paraffin wax, and the weight ratio of paraffin wax to powder is 1:(90~110).

[0021] S4. The steel substrate is processed and shaped according to the drawings, and multiple pre-embedded holes are machined on the surface. The diameter of the pre-embedded holes is 0.8~1.5mm and the depth is 8~15mm.

[0022] S5. Process core posts corresponding to the number of pre-embedded holes. The length of the core posts is 10~30 mm and the diameter is 0~0.02 mm smaller than that of the pre-embedded holes.

[0023] S6. The substrate and core are plated with Ti. All outer surfaces of the substrate and the core are covered with a titanium coating. After plating, the substrate is cleaned with acetone. The thickness of the titanium coating is 0.01~0.02 mm.

[0024] S7. Insert the core post into the pre-embedded hole in the base, and fix the two with a gap fit;

[0025] S8. Place the substrate with the core pillar from S7 at the bottom of the steel mold as the lower pressure head, with the core pillar facing upwards. Then, sequentially add the mixed powder of metal buffer layer 1, metal buffer layer 2, and grinding layer obtained from S1, S2, and S3. After each addition, vibrate the mixture 2-3 times on a vibrating platform, then use a scraper to spread the powder evenly and uniformly within the mold cavity. After leveling, pre-press the powder before adding the next type of powder. During the addition process, ensure that the top of the core pillar always protrudes from the powder surface. It is strictly forbidden for the powder to completely cover the core pillar, as this could cause the pressure head to directly press against the end face of the core pillar during subsequent cold pressing, leading to deformation of the core pillar.

[0026] S9. Use a multi-hole steel press head for cold pressing and pre-pressing - open through holes on the press head corresponding to the position of the core column. The diameter of the through holes is the same as the pre-embedded holes in the base body, so that the core column exposed on the surface of the powder extends into the hole. The press head has sufficient height to ensure that the press will not press the core column. During the pressing process, only the powder is pressed and the core column is not subjected to direct pressure. After cold pressing, a green blank of the grinding wheel block with the base body is obtained. S10. Place the green grinding wheel block obtained in S9 into a hot pressing sintering furnace. Use a porous graphite indenter (functionally the same as a cold-pressing porous steel indenter) to insert the portion of the core column above the powder surface into the through hole of the graphite indenter. This ensures that the core column does not bear direct pressure during the hot pressing process, preventing deformation of the core column. The matrix, core column, metal buffer layer, and abrasive layer are sintered into a single piece under high temperature and high pressure to obtain a complete grinding wheel blank.

[0027] Furthermore, the preloading pressure in S8 is 400~800 kg / cm². 2 The holding time is 3~6 s; the cold pressing pressure in S9 is 1000~2000 kg / cm³. 2 The holding time is 10~20 s; the sintering pressure in S10 is 200~400 kg / cm². 2 The sintering temperature is 600~700 ℃, and the holding time is 10~30 min;

[0028] S11. The grinding wheel blank block obtained in S10 is clamped on the wire EDM machine. The excess part of the core column that is higher than the end face of the grinding layer is removed to make the end face flat. Then, it is cut into equal parts along the axial direction. A single wire EDM can produce 90 to 108 grinding wheel units.

[0029] S12. The cut grinding wheel unit is processed. First, the grinding wheel base is machined, and then the grinding layer is precision dressed by electrical discharge machining to produce the required final contour shape and dimensional accuracy, thus obtaining the core-reinforced wafer Notch groove chamfering grinding wheel.

[0030] The aforementioned core-enhanced wafer notch chamfering grinding wheel can be used in semiconductor precision machining for notch machining of wafers made of semiconductor materials such as silicon (Si), silicon carbide (SiC), germanium (Ge), gallium nitride (GaN), and gallium arsenide (GaAs).

[0031] It should be noted that the above technical solutions are only an overview of the present invention. In order to make the features, objectives and innovations of the present invention clearer and easier to understand, the present invention will be further described below in conjunction with specific embodiments.

[0032] Compared with the prior art, the present invention has the following significant advantages:

[0033] This invention employs a monolithic hot-pressing and sintering process to prepare the blank, which is then divided into multiple grinding wheels by wire cutting. This increases the single-furnace capacity by an order of magnitude and reduces production costs. The cold / hot pressing stage utilizes a multi-hole clearance pressure head, preventing external force deformation of the core column, ensuring uniform core column positioning accuracy, and achieving high batch-to-batch consistency in grinding wheel size and performance, thus meeting the semiconductor industry's requirements for high-volume, high-precision supply.

[0034] This invention employs a composite interface structure consisting of a steel substrate with a vacuum-plated titanium-modified layer and a diamond-free metal buffer layer. The titanium plating undergoes bidirectional elemental diffusion with both the steel substrate and the metal buffer layer, constructing a continuous metallurgical interface. The pure metal buffer layer, free of diamond particles, exhibits good plasticity and can synergistically buffer multi-layer thermal expansion stress with the titanium plating, forming a multi-layer system with gradually varying thermal expansion coefficients, thus reducing the risk of microcracks or cracking at the interface after high-temperature sintering. The buffer layer utilizes ultrafine metal powder with high sintering activity, allowing for thorough wetting and diffusion with the titanium plating substrate, further enhancing interfacial bonding. Phosphorus-iron alloy powder lowers the sintering activation temperature and promotes elemental interdiffusion between the titanium plating and the metal powder. The addition of low-melting-point bismuth fills the gaps between the powder particles in the liquid phase during sintering, improving the density of the buffer layer and reducing internal porosity.

[0035] This invention enhances the ultimate load-bearing capacity of a grinding wheel by incorporating a steel core pillar inside the wheel, forming a three-layer composite reinforcement structure of "abrasive layer - metal buffer layer - core pillar". The core pillar is made of austenitic stainless steel with a higher coefficient of thermal expansion. Utilizing the difference in thermal expansion between dissimilar materials, an interference fit is actively formed during the sintering heating stage. Simultaneously, the synergistic effects of mechanical interlocking and metallurgical diffusion significantly improve the bonding strength between the core pillar and the substrate. Bending tests demonstrate that the average ultimate load-bearing capacity of the grinding wheel of this invention is approximately 57% higher than that of conventional grinding wheels without a core pillar. Furthermore, only slight distortion of the substrate occurs when the load limit is reached, with no cracks or fractures in the grinding layer. In addition, processing results show that under the same processing conditions, the fracture rate of the grinding wheel of this invention is 0%, while the fracture rate of conventional grinding wheels is 13.3%. This extends the wheel's service life while ensuring processing accuracy, reducing tool change frequency and the risk of wafer damage.

[0036] The process of this invention is highly versatile and widely applicable. This invention can be adapted to the grinding of notch grooves on wafers of different materials such as silicon, silicon carbide, germanium, gallium nitride, and gallium arsenide by adjusting the diamond grit size and binder formulation of the grinding layer. The metal dual-gradient buffer layer, titanium plating process, and core pillar reinforcement structure can be universally applied without significant adjustments, demonstrating strong process portability. Attached Figure Description

[0037] To more clearly illustrate the embodiments or technical solutions of the present invention, the embodiments and related drawings will be briefly described below. It should be understood that the drawings described below are only some embodiments of the present invention, and those skilled in the art can obtain other drawings without creative effort.

[0038] Figure 1 This is a schematic diagram of the notch grinding process on a wafer.

[0039] Figure 2 This is a flowchart illustrating the grinding wheel preparation process of Embodiment 1 of the present invention;

[0040] Figure 3 This is a schematic diagram of the grinding wheel structure in Embodiment 1 of the present invention;

[0041] Figure 4 This is a diagram of the grinding wheel substrate according to Embodiment 1 of the present invention;

[0042] Figure 5 This is a diagram of the steel core column of Embodiment 1 of the present invention;

[0043] Figure 6 This is a schematic diagram of cold pressing molding according to Embodiment 1 of the present invention;

[0044] Figure 7 This is a schematic diagram of the grinding wheel structure of Comparative Example 1 of the present invention;

[0045] Figure 8This is a bar chart comparing the average maximum bending strength of the grinding wheels in the comparative test 1 of this invention with the average values ​​of the comparative test.

[0046] In the diagram, 1 is the grinding wheel layer, 2 is the metal buffer layer 1, 3 is the metal buffer layer 2, 4 is the grinding wheel base, 5 is the mandrel, 6 is the steel porous pressure head, and 7 is the steel mold. Detailed Implementation

[0047] The technical solution of the present invention will be further described below with reference to the embodiments. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without inventive effort are within the scope of protection of the present invention.

[0048] Example 1

[0049] A core-reinforced wafer notch chamfering grinding wheel, such as Figure 3 As shown, it includes a grinding layer 1, a metal buffer layer 1 (marked 2 in the figure), a metal buffer layer 2 (marked 3 in the figure), a substrate 4, and a core pillar 5. It is worth noting that, in order to ensure the structural strength of the substrate, the substrate 4 is made of 45# steel, and the core pillar 5 is made of 304 stainless steel.

[0050] The grinding layer is formulated from the following raw materials in parts by weight: 30 parts diamond, 65 parts metal binder, and 5 parts additives. The additive is reagent graphite, and the metal binder is composed of the following raw materials in parts by weight: 25 parts copper powder, 25 parts tin powder, and 50 parts cobalt powder.

[0051] The metal buffer layer 1 is composed of the following raw materials in parts by weight: 40 parts of ultrafine copper powder, 30 parts of ultrafine tin powder, 25 parts of nickel powder, 3 parts of titanium powder, 1 part of trace phosphorus-iron alloy powder (FeP24 grade phosphorus-iron alloy powder is selected: phosphorus 24wt%, iron 73wt%, and the remaining 3wt% is trace impurities such as silicon and manganese), and 1 part of bismuth powder.

[0052] The metal buffer layer 2 is composed of the following raw materials in parts by weight: 25 parts copper powder, 25 parts tin powder, and 50 parts cobalt powder.

[0053] The ultrafine copper powder and ultrafine tin powder have a particle size of 5-10 μm. Other metal powders need to be sieved under a combined sieve to obtain metal powder with a particle size of 30-50 μm. The particle size of the reagent graphite is ≤50 μm, and the diamond particle size is 800 mesh.

[0054] The above-mentioned method for preparing the core-reinforced wafer Notch groove chamfering grinding wheel, such as Figure 2 As shown, it includes the following steps:

[0055] S1. Weigh out ultrafine copper powder, ultrafine tin powder, nickel powder, titanium powder, phosphorus iron alloy powder and bismuth powder according to the proportion and pour them into a mixing tank. Add steel balls (10 mm in diameter) and wetting agent, and put them on a three-dimensional mixer for mixing. The ball-to-material mass ratio is 1:3, the rotation speed is 200 rpm, and the time is 2 hours. After mixing, metal buffer layer 1 mixed powder is obtained.

[0056] S2. Weigh out copper powder, tin powder, and cobalt powder according to the proportion, pour them into a mixing tank, add steel balls and wetting agent, and keep the mixing process consistent with S1. After mixing, metal buffer layer 2 mixed powder is obtained.

[0057] S3. Weigh out copper powder, tin powder, cobalt powder, reagent graphite and diamond abrasive according to the proportion, pour them into a mixing tank, add steel balls and wetting agent, put them on a three-dimensional mixer for mixing, ball-to-powder ratio 1:3, rotation speed 300 rpm, time 3 h, and after mixing, the grinding layer mixed powder is obtained.

[0058] It is worth noting that the wetting agent mentioned in S1, S2 and S3 is paraffin wax, and the weight ratio of paraffin wax to powder is 1:100.

[0059] S4. The steel substrate 4 is machined and formed according to the drawings, and multiple pre-embedded holes are machined on its surface. In this embodiment, the dimensions of the steel substrate 4 are 50 mm * 80 mm * 30 mm, the depth of the pre-embedded holes is 8 mm, and the diameter is Ф1 mm (tolerance range: 0 to 0.02 mm). A schematic diagram of the machined steel substrate 4 is attached. Figure 4 ;

[0060] S5. Separately machine steel core posts 5 corresponding to the number of pre-embedded holes. The core post 5 has a diameter of Ф1 mm (tolerance range: -0.02 to 0 mm) and a length of 20 mm. See the attached diagram for a schematic diagram of the core post 5. Figure 5 ;

[0061] S6. Plate the core 5 and the substrate 4 together with Ti for 20 minutes, with a plating thickness of 0.02 mm. After plating, ultrasonically clean with acetone for 10 minutes to ensure that there is no oil or other impurities on the surface. Then insert the core 5 into the pre-embedded hole in the substrate 4, and fix the two with a gap fit.

[0062] S7. Place the core-pillar 5 substrate 4 from S6 at the bottom of the steel mold 7, with the core 5 facing upwards. First, add the metal buffer layer 1 mixed powder obtained in S1. After adding the powder, vibrate it 2-3 times on the vibrating platform. Then, slowly scrape the powder with a scraper to ensure that the powder is evenly distributed and of uniform height within the mold cavity. After leveling, use a porous steel pressure head for pre-pressing. After pre-pressing, continue adding the metal buffer layer 2 mixed powder obtained in S2, repeating the above steps. Finally, add the grinding layer mixed powder obtained in S3. During the feeding process, ensure that the top of the core pillar is always exposed above the powder surface to avoid the pressure head directly pressing on the end face of the core pillar during subsequent cold pressing, which could cause deformation of the core pillar. The pre-pressing pressure is 600 kg / cm². 2 The pressure holding time is 3 seconds.

[0063] S8. A through hole corresponding to the position of the core column is made on the steel cold pressing head 6. The diameter and tolerance of the through hole are consistent with the pre-embedded hole in the grinding wheel base 4. The part of the core column exposed on the powder surface extends into the through hole during cold pressing. The cold pressing head needs to be high enough, which can be the same as or slightly lower than the length of the core column 5, to ensure that the top of the core column 5 is always lower than the upper surface of the pressing head during the cold pressing process. During the pressing process, only the powder is subjected to pressure, and the core column 5 is not subjected to force. A schematic diagram of cold pressing is attached. Figure 6 After cold pressing, a green grinding wheel block with a substrate is obtained. The cold pressing pressure is 1500 kg / cm². 2 The pressure holding time is 10 seconds.

[0064] S9. Place the green grinding wheel block obtained in S8 into a graphite mold, and sinter it under high temperature and pressure using a porous graphite indenter (functioning the same as a cold-pressed porous steel indenter). The matrix, core, metal buffer layer, and grinding layer are bonded together in one step during the sintering process, resulting in a complete grinding wheel blank. The sintering temperature is 700 ℃, and the sintering pressure is 300 kg / cm². 2 Hold at this temperature and pressure for 30 minutes;

[0065] S10. The grinding wheel blank block obtained in S9 is clamped on the wire EDM machine. The excess part of the core column that is higher than the end face of the grinding layer is removed to make the end face flat. Then, it is cut into equal parts along the axial direction to cut out 99 grinding wheel units at one time.

[0066] S11. The cut grinding wheel base is machined by turning, and the grinding layer is then precision dressed by electrical discharge machining. Finally, the required contour shape and dimensional accuracy are obtained, thus producing the core-reinforced wafer Notch groove chamfering grinding wheel.

[0067] It is worth noting that in other embodiments of the present invention, the steel substrate size and the number of wire cuts can be selected from other values. The number of cuts is determined according to the blank size and the size and specifications of the grinding wheel. Those skilled in the art can make corresponding adjustments according to the actual situation.

[0068] It is worth noting that in other embodiments of the present invention, the size of the pre-embedded hole and the size of the core post can be other values, but the distance between the core post and the bottom of the groove should not be less than 0.5 mm;

[0069] The core-reinforced wafer notch chamfering wheel obtained in this embodiment is used for chamfering of notch grooves on silicon (Si) wafers.

[0070] Example 2

[0071] The core-reinforced wafer Notch groove chamfering grinding wheel prepared in this embodiment has the following adjusted parameters compared with Embodiment 1: the depth of the substrate pre-embedded hole in S4 is 10 mm, the diameter is Ф0.8 mm (tolerance range: 0 to 0.02 mm), the core column diameter is Ф0.8 mm (tolerance range: -0.02 to 0 mm), and the length is 10 mm;

[0072] The grinding layer is composed of the following raw materials in parts by weight: 20 parts diamond abrasive, 75 parts metal binder, 3 parts reagent graphite, and 2 parts granular graphite. The metal binder is composed of the following raw materials in parts by weight: 30 parts copper powder, 30 parts tin powder, and 40 parts cobalt powder.

[0073] The metal buffer layer 2 is composed of the following raw materials in parts by weight: 30 parts copper powder, 30 parts tin powder, and 40 parts cobalt powder.

[0074] The mixing speed in S1, S2, and S3 is 250 rpm, and the mixing time is 2 hours.

[0075] The sintering temperature in S9 is 650 ℃, and the sintering pressure is 300 kg / cm². 2 The heat preservation and pressure holding time is 20 minutes.

[0076] The other steps in this embodiment are the same as in Embodiment 1, and will not be repeated here.

[0077] The core-reinforced wafer Notch groove chamfering grinding wheel prepared in this embodiment is used for chamfering of Notch grooves in silicon carbide (SiC) wafers;

[0078] Comparative Example 1

[0079] The wafer Notch chamfering grinding wheel prepared in this comparative example is shown in the schematic diagram below. Figure 7 As shown, compared with Example 1, the preparation method is adjusted as follows: the preparation of the metal buffer layer in S2 and S3 is cancelled; the processing of the pre-embedded hole in the substrate in S4 is cancelled; the processing of the steel core column in S5 is cancelled; and the processing of the through holes of the cold pressing head and the hot pressing head in S8 and S9 is cancelled. The remaining manufacturing steps are the same as in Example 1, and will not be repeated here.

[0080] Comparative Experiment 1

[0081] The grinding wheels prepared according to Examples 1, 2 and Comparative Example 1 of the present invention were subjected to bending strength tests on a universal testing machine with a feed rate of 0.1 mm / min.

[0082] To improve the accuracy of the test results, four grinding wheels were tested in each of Examples 1, 2 and Comparative Example 1, and the average value was taken as the final test result.

[0083] The maximum and average forces experienced by the grinding wheel when it bent or broke were recorded, and the results are shown in Table 1 and... Figure 8 As shown:

[0084] Table 1 Comparison of average bending strength of different grinding wheel samples

[0085]

[0086] Bending strength tests revealed that the grinding wheel in Comparative Example 1 had the lowest bending strength, and the bottom of the groove near the substrate of the grinding wheel experienced a sudden, overall fracture after the test. The bending strength of the grinding wheels in Examples 1 and 2 was essentially the same, both significantly higher than that of the grinding wheel in Comparative Example 1, with a maximum stress value increased by about 56%. Furthermore, after the test, only the substrate of the grinding wheel experienced slight distortion, and no cracks or fractures appeared in the grinding layer. This indicates that the core post, as an internal reinforcing structure, effectively shared the load borne by the grinding layer, reducing the risk of sudden fracture of the grinding wheel during processing.

[0087] Comparative Experiment 2

[0088] The grinding wheels prepared in Example 1 and Comparative Example 1 of this invention were respectively tested in actual machine grinding on a Tokyo Seimitsu W-GM-4200 dedicated wafer chamfering machine. Figure 1 As shown, the object being processed was an 8-inch silicon wafer notch, and the grinding wheel speed was set to 3000 rpm. Thirty grinding wheels each from Example 1 and Comparative Example 1 were used for continuous processing under the same cutting feed rate, grinding pressure, and coolant flow rate. The processing effects of the two types of grinding wheels were compared, and the results are shown in Table 2.

[0089] Table 2 Comparison of machining effects of different grinding wheels

[0090]

[0091] Compared with the actual processing results, the grinding wheel in Comparative Example 1 had a higher probability of breakage during processing, which further led to a decrease in product yield and lifespan. The grinding wheel in Example 1 can completely eliminate the problem of sudden breakage failure during grinding, reducing the breakage rate from 13.3% to 0, reducing the frequency of equipment downtime for tool changes, and improving the yield and lifespan of wafer notch processing.

Claims

1. A core-reinforced wafer notch chamfering grinding wheel, characterized in that, The grinding wheel comprises a base, a double-layer gradient metal buffer layer, and a grinding layer. The double-layer gradient metal buffer layer is located between the grinding layer and the base. The double-layer gradient metal buffer layer includes a metal buffer layer 1 disposed on the upper surface of the base and a metal buffer layer 2 disposed on the upper surface of the metal buffer layer 1. The thickness of both the metal buffer layer 1 and the metal buffer layer 2 is 1~2 mm. A core post is pre-embedded inside the base. The core post extends through the double-layer gradient metal buffer layer into the grinding layer. The outer end face of the core post is flush with the outer end face of the grinding layer.

2. The core-reinforced wafer Notch groove chamfering grinding wheel according to claim 1, characterized in that, The grinding wheel base is made of 45# steel, and the core is made of austenitic stainless steel.

3. The core-reinforced wafer Notch groove chamfering grinding wheel according to claim 1, characterized in that, The grinding wheel grinding layer is composed of the following raw materials in parts by weight: 20-40 parts abrasive, 60-80 parts metal binder, and 1-5 parts additives, wherein the additives are one or more mixtures of reagent graphite or granular graphite; the metal binder is composed of the following raw materials in parts by weight: 20-40 parts copper powder, 20-40 parts tin powder, and 40-60 parts cobalt powder.

4. The core-reinforced wafer Notch groove chamfering grinding wheel according to claim 1, characterized in that, The metal buffer layer 1 is composed of the following raw materials in parts by weight: 30-40 parts of ultrafine copper powder, 20-30 parts of ultrafine tin powder, 15-25 parts of nickel powder, 1-5 parts of titanium powder, 1-2 parts of phosphorus iron alloy powder, and 1-2 parts of bismuth powder.

5. The core-reinforced wafer Notch groove chamfering grinding wheel according to claim 3, characterized in that, The composition of the metal buffer layer 2 is the same as that of the metal binder in the grinding layer.

6. The core-reinforced wafer Notch groove chamfering grinding wheel according to any one of claims 3 to 5, characterized in that, The ultrafine copper powder and ultrafine tin powder have a particle size of 5~10 μm. The median particle size of the copper powder, tin powder, cobalt powder, nickel powder, titanium powder, ferrophosphorus alloy powder, and bismuth powder is ≤50 μm. The reagent graphite or granular graphite has a particle size of ≤50 μm. The abrasive in the grinding wheel grinding layer is diamond, and the diamond particle size is 800~3000 mesh.

7. A method for preparing a core-reinforced wafer Notch groove chamfering grinding wheel according to any one of claims 1 to 6, characterized in that, Includes the following steps: S1. Weigh the required raw materials for metal buffer layer 1 according to the proportion, pour them into a mixing tank, add a certain proportion of steel balls and wetting agent, and mix them evenly using a three-dimensional mixer to obtain metal buffer layer 1 mixed powder. S2. Weigh the raw materials required for metal buffer layer 2 according to the proportion, pour them into the mixing tank, and mix them according to the mixing method in S1 to obtain metal buffer layer 2 mixed powder. S3. Weigh out the raw materials required for the grinding layer according to the proportion, pour them into the mixing tank, and mix them in the same way as in S1 to obtain the grinding layer mixed powder. S4. The steel substrate is processed and shaped according to the drawings, and multiple pre-embedded holes are machined on the surface. The diameter of the pre-embedded holes is 0.8~1.5 mm and the depth is 8~15 mm. S5. Process core posts corresponding to the number of pre-embedded holes. The length of the core posts is 10~30 mm and the diameter is 0~0.02 mm smaller than that of the pre-embedded holes. S6. The substrate and core are plated with Ti. All outer surfaces of the substrate and the core are covered with titanium plating. After plating, they are cleaned with acetone. S7. Insert the core post into the pre-embedded hole in the base, and fix the two with a gap fit; S8. Place the substrate with the core column in S7 at the bottom of the steel mold as the lower pressure head, with the core column facing upwards. Then, sequentially feed in the mixed powder of metal buffer layer 1, metal buffer layer 2 and grinding layer obtained in S1, S2 and S3. After each feeding, vibrate on the vibrating platform 2 to 3 times. Then, use a scraper to flatten and pre-press. After pre-pressing, continue to feed in the next powder. During the feeding process, ensure that the top of the core column is always exposed on the powder surface. S9. A multi-hole steel press head is used for cold pressing and pre-pressing. A through hole is opened on the press head corresponding to the position of the core column. The diameter of the through hole is the same as the pre-embedded hole of the base body, so that the core column exposed on the surface of the powder extends into the through hole of the press head. During the pressing process, only the powder is pressed and the core column is not subjected to direct pressure. After cold pressing, a green blank of the grinding wheel block with the base body is obtained. S10. Place the green grinding wheel block obtained in S9 into a hot pressing sintering furnace and use a graphite press head. A through hole corresponding to the position of the core column is opened on the graphite press head. The diameter of the through hole is the same as the pre-embedded hole in the substrate. The part of the core column above the powder surface extends into the through hole of the graphite press head to ensure that the core column does not bear direct pressure during the hot pressing process. The substrate, core column, metal buffer layer and abrasive layer are sintered into one piece under high temperature and high pressure to obtain a whole grinding wheel blank. S11. The grinding wheel blank block obtained in S10 is clamped on the wire EDM machine. The excess part of the core column that is higher than the end face of the grinding layer is removed to make the end face flat. Then, it is cut into equal parts along the axial direction. A single wire EDM can produce 90 to 108 grinding wheel units. S12. The cut grinding wheel unit is processed. First, the grinding wheel base is machined, and then the grinding layer is precision dressed by electrical discharge machining to produce the required final contour shape and dimensional accuracy, thus obtaining the core-reinforced wafer Notch groove chamfering grinding wheel.

8. The preparation method according to claim 7, characterized in that, In S1, S2, and S3, the mixing speed is 100~300 rpm, the mixing time is 2~3 h, and the ball-to-powder mass ratio is 1:(2~4); the wetting agent is paraffin wax, and the weight ratio of paraffin wax to powder is 1:(90~110); in S6, the titanium coating thickness is 0.01~0.02 mm.

9. The preparation method according to claim 7, characterized in that, The pre-compression pressure in S8 is 400~800 kg / cm². 2 The holding time is 3~6 s; the cold pressing pressure in S9 is 1000~2000 kg / cm³. 2 The holding time is 10~20 s; the sintering pressure in S10 is 200~400 kg / cm². 2 The sintering temperature is 600~700 ℃, and the holding time is 10~30 min.

10. The application of the core-reinforced wafer Notch groove chamfering grinding wheel according to any one of claims 1 to 6 in semiconductor precision machining, characterized in that, Notch groove processing for wafers of silicon (Si), silicon carbide (SiC), germanium (Ge), gallium nitride (GaN), and gallium arsenide (GaAs) semiconductor materials.

Citation Information

Patent Citations

  • Preparation method of diamond grinding wheel for wafer Notch groove grinding

    CN119427241A

  • Wafer positioning groove chamfering grinding head for wafer Notch notch chamfering and manufacturing method

    CN119501837A