A processing technology to increase the compressive strength of aerated concrete blocks
By modifying raw material compounding and segmented temperature-controlled gas generation process, combined with gradient autoclaving and dry heat curing, the internal structure and crystal formation of aerated bricks are optimized, solving the problem of insufficient compressive strength of aerated bricks and achieving a synergistic improvement in high strength and thermal insulation performance.
Patent Information
- Application Number
- CN202611403695.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-10
- Publication Date
- 2026-11-17
AI Technical Summary
The existing aerated concrete block processing technology results in insufficient compressive strength, which cannot meet the requirements of high-rise buildings and heavy-duty walls. Furthermore, traditional reinforcement methods increase production costs or affect thermal insulation performance.
By employing modified raw material compounding and segmented temperature-controlled gas generation process, combined with gradient autoclaving and dry heat curing, the internal structure and crystal formation of aerated bricks are optimized. Modified basalt powder and composite adhesive powder enhance the interfacial bonding force of materials, control bubble nucleation and growth, and promote the formation of high-strength tobermorite crystals.
It significantly improves the compressive strength of aerated concrete blocks by 40%-60%, while maintaining their lightweight and thermal insulation properties, thus broadening their application range and making them suitable for high-rise buildings and heavy-duty walls.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention relates to the field of aerated concrete block processing technology, and specifically to a processing technology for increasing the compressive strength of aerated concrete blocks. Background Technology
[0002] Autoclaved aerated concrete (AAC) blocks are porous, lightweight wall building materials made primarily from siliceous and calcareous materials, along with foaming agents and additives. The process involves mixing, foaming, molding, pre-curing, cutting, and autoclaving. AAC blocks offer numerous advantages, including lightweight, heat insulation, sound insulation, fire resistance, energy efficiency, and environmental friendliness. They are widely used in wall filling and enclosure structure construction for civil and industrial buildings, and are currently one of the core building materials for prefabricated and green buildings.
[0003] Existing aerated concrete (AC) block processing technologies generally suffer from technical defects, which restrict the improvement of the product's compressive strength. Traditional production processes only employ conventional raw material mixing, natural gas generation, and single autoclaving. The resulting AC blocks have an uneven internal pore structure, often containing large-diameter pores, interconnected pores, and pore defects, leading to poor internal matrix density. Simultaneously, the raw material reaction is incomplete, resulting in insufficient formation and low crystallinity of strength-enhancing crystalline products such as hydrated calcium silicate and tobermorite. This results in generally low compressive strength in the finished product; the compressive strength of conventional B06 grade AC blocks is only 3.5-5.0 MPa, and the highest for B07 grade is no more than 6.0 MPa.
[0004] In high-intensity applications such as high-rise buildings, heavy-duty walls, and auxiliary load-bearing structures for exterior walls, existing aerated concrete blocks cannot meet the strength requirements of engineering loads, easily leading to quality problems such as wall cracking, deformation, and damage, significantly limiting the application range of aerated concrete blocks. Currently, many reinforcement processes in the industry achieve strength improvement by simply increasing the amount of cement and lime or adding ordinary fibers. This not only significantly increases production costs but also leads to increased weight of the aerated concrete blocks, decreased thermal insulation performance, and limited reinforcement effect, failing to fundamentally optimize the internal pore structure and crystal structure. Therefore, there is an urgent need for a processing technology that can increase the compressive strength of aerated concrete blocks. Summary of the Invention
[0005] The present invention aims to provide a processing technology to increase the compressive strength of aerated concrete blocks, thereby improving the compressive strength of aerated concrete blocks.
[0006] To achieve the above objectives, the present invention adopts the following technical solution: a processing method for increasing the compressive strength of aerated concrete blocks, comprising the following steps: S1, Raw material pretreatment: Select 45-55 parts by weight of siliceous raw material, 25-32 parts by weight of calcareous raw material, 8-12 parts by weight of modifying and reinforcing agent, 2-4 parts by weight of gypsum, 0.08-0.12 parts by weight of aluminum powder gas generator, and 30-38 parts by weight of water; grind the siliceous raw material, calcareous raw material, and gypsum separately, pass them through a 200-300 mesh sieve, and then send them into a drying equipment to dry at 105-115℃ until the moisture content is ≤1.5%; S2, graded mixing and slurry preparation: The pretreated siliceous raw materials, calcareous raw materials, and gypsum are put into the mixer and dry-mixed for 3-5 minutes; then 80% of the proportion of water is added and wet-mixed for 6-8 minutes to form a uniform base slurry; then the modified reinforcing agent is dispersed in the remaining 20% of water, the water temperature is controlled at 40-50℃, and after stirring and dispersing for 2 minutes, it is injected into the base slurry and stirred for another 4-6 minutes; finally, aluminum powder gas generator is added and stirred for 1-2 minutes to obtain a homogeneous and stable aerated brick slurry; S3, Segmented Temperature-Controlled Gas Generation and Molding: The prepared slurry is quickly injected into the mold, which is preheated to 35-45℃. A segmented temperature-controlled gas generation process is adopted: the first stage is kept at a constant temperature of 35-40℃ for 20-25 minutes to achieve initial gas generation and uniform bubble nucleation; the second stage is kept at a constant temperature of 45-50℃ for 30-35 minutes to complete stable bubble growth and slurry solidification. S4, Pre-curing and Precision Cutting: The formed blank, along with the mold, is sent into the pre-curing chamber and pre-cured for 2.5-3.5 hours at a temperature of 55-60℃ and a relative humidity of 85%-90% to allow the blank to initially harden and acquire the strength required for shaping. After demolding, the blank is precisely cut using CNC cutting equipment to remove edge waste and process it into standard-sized block blanks. S5, Gradient autoclaving: The cut billet is sent into the autoclave and subjected to three-stage autoclaving with gradient pressure increase, constant temperature and pressure, and gradient pressure decrease. S6, Post-construction dry heat curing: After autoclaving, the blocks are sent to a constant temperature curing chamber and dry heat cured at 90-110℃ for 12-24 hours to obtain the finished aerated brick product.
[0007] Preferably, as an improvement, the siliceous raw material is a mixture of fly ash and fine quartz sand powder in a mass ratio of 3:1; the calcareous raw material is a mixture of quicklime and ordinary silicate cement in a mass ratio of 2:1; the modified reinforcing agent is a mixture of modified basalt powder and composite adhesive powder in a mass ratio of 4:1, wherein the modified basalt powder is subjected to sodium hydroxide soaking, high-temperature calcination, and dilute hydrochloric acid activation modification treatment, and the composite adhesive powder is a mixture of redispersible latex powder with glass transition temperatures of 15℃ and -6℃.
[0008] Preferably, as an improvement, the modified basalt powder is prepared by soaking the basalt powder in a 1.2 mol / L sodium hydroxide solution for 1.2 h, drying it, calcining it at 650°C for 2 h, cooling it, soaking it in a 0.8 mol / L hydrochloric acid solution for 1.4 h, washing it until neutral, drying it, and grinding it to obtain the powder.
[0009] Preferably, as an improvement, the maintenance process in step S5 is as follows: A1, Gradient pressurization stage: The pressure is uniformly increased to 1.0-1.2MPa within 1.5-2.5h, and the temperature inside the reactor is simultaneously increased to 185-195℃ to slowly activate the hydration reaction of the raw materials and avoid sudden changes in pressure and temperature that could cause cracking of the internal structure of the billet. A2, Constant Temperature and Pressure Stage: Maintain a constant pressure of 1.0-1.2 MPa and a constant temperature of 185-195℃ for 6-8 hours; A3, Gradient depressurization stage: The pressure is uniformly reduced to normal pressure within 1.5-2.5 hours, and the temperature naturally drops to room temperature.
[0010] Preferably, as an improvement, during the autoclaving process in step S5, saturated water vapor is introduced into the autoclave to maintain 100% humidity throughout the process, ensuring that the hydration reaction proceeds fully.
[0011] Compared with the prior art, the beneficial effects of the present invention are: 1. This invention optimizes the reaction system from the source of raw materials by combining modified raw materials with special reinforcing additives. Modified basalt powder can fill micropores and improve the strength of the matrix skeleton, while composite adhesive powder can enhance the bonding force of material interfaces and reduce internal microcracks. Compared with the traditional single raw material ratio, it greatly improves the structural stability of aerated brick matrix.
[0012] 2. This invention adopts a segmented temperature-controlled gas generation process to replace the traditional one-time constant temperature gas generation mode. It can accurately control the bubble nucleation and growth process, effectively eliminate large-diameter pores and interconnected pores, and form a uniform and dense closed microporous structure inside the block. This significantly reduces the negative impact of pore defects on compressive strength, while retaining the core performance of aerated bricks as lightweight and heat-insulating.
[0013] 3. The present invention adopts a three-stage gradient autoclaving process combined with a later dry heat curing process, which can gradually stimulate the hydration reaction of raw materials, promote the generation of a large number of high-strength tobermorite crystals, improve the crystallinity and interweaving tightness of crystals, significantly enhance the overall compressive strength of the blocks, and at the same time eliminate the structural residual stress during the production process, avoiding cracking and deformation during later use.
[0014] 4. The aerated concrete blocks prepared using the process of this invention have a dense and uniform internal structure and a compressive strength that is 40%-60% higher than that of traditional processes. They can be adapted to high-intensity use scenarios such as high-rise buildings and heavy-duty walls, greatly expanding the application range of the products. Detailed Implementation
[0015] The following detailed description illustrates the specific implementation method: Example 1 A processing method for increasing the compressive strength of aerated concrete blocks includes the following steps: S1, Raw material pretreatment: Select 50 parts by weight of siliceous raw material, 28 parts by weight of calcareous raw material, 10 parts by weight of modified reinforcing agent, 3 parts by weight of gypsum, 0.1 parts by weight of aluminum powder gas generator, and 35 parts by weight of water; grind the siliceous raw material, calcareous raw material, and gypsum separately, pass them through a 250-mesh sieve, and then send them to a drying equipment to dry at 110℃ until the moisture content is ≤1.5%; The siliceous raw material is a mixture of fly ash and fine quartz sand powder in a mass ratio of 3:1; the calcareous raw material is a mixture of quicklime and ordinary silicate cement in a mass ratio of 2:1; the modified reinforcing agent is a mixture of modified basalt powder and composite adhesive powder in a mass ratio of 4:1, wherein the modified basalt powder is treated by soaking in sodium hydroxide, high-temperature calcination, and activation modification with dilute hydrochloric acid, and the composite adhesive powder is a mixture of redispersible latex powder with glass transition temperatures of 15℃ and -6℃.
[0016] The modified basalt powder is prepared by soaking basalt powder in a 1.2 mol / L sodium hydroxide solution for 1.2 h, drying it, calcining it at 650℃ for 2 h, cooling it, soaking it in a 0.8 mol / L hydrochloric acid solution for 1.4 h, washing it until neutral, drying it, and grinding it.
[0017] S2, graded mixing and slurry preparation: The pretreated siliceous raw materials, calcareous raw materials, and gypsum are put into a forced mixer and dry-mixed for 4 minutes; then 80% of the proportion of water is added and wet-mixed for 7 minutes to form a uniform base slurry; then the modified reinforcing agent is dispersed in the remaining 20% of water, the water temperature is controlled at 45℃, and after stirring and dispersing for 2 minutes, it is slowly injected into the base slurry and stirred for another 5 minutes; finally, aluminum powder gas generator is added and quickly stirred for 1.5 minutes to obtain a homogeneous and stable aerated brick slurry; S3, segmented temperature-controlled gas generation molding: The prepared slurry is quickly injected into the mold, which is preheated to 40°C. The segmented temperature-controlled gas generation process is adopted: the first stage is kept at a constant temperature of 38°C for 22 minutes to achieve initial gas generation and uniform nucleation of bubbles; the second stage is kept at a constant temperature of 48°C for 32 minutes to complete the stable growth of bubbles and solidification of the slurry. S4, Pre-curing and Precision Cutting: The formed blank, along with the mold, is sent into the pre-curing chamber and pre-cured for 3 hours at a temperature of 58℃ and a relative humidity of 88% to allow the blank to initially harden and acquire the strength required for shaping. After demolding, the blank is precisely cut using CNC cutting equipment to remove edge waste and process it into standard-sized block blanks. S5, Gradient autoclaving: The cut billet is sent into an autoclave and cured using a three-stage autoclaving process: gradient pressurization, constant temperature and pressure, and gradient depressurization. The curing process steps are as follows: A1, Gradient pressurization stage: The pressure is uniformly increased to 1.1MPa within 2 hours, and the temperature inside the reactor is simultaneously increased to 190℃ to slowly activate the hydration reaction of the raw materials and avoid cracking of the internal structure of the billet caused by sudden changes in pressure and temperature. A2, Constant Temperature and Pressure Stage: Maintain a constant pressure of 1.1 MPa and a constant temperature of 190℃ for 7 hours; A3, Gradient depressurization stage: The pressure is reduced to normal pressure at a constant rate within 2 hours, and the temperature naturally drops to room temperature.
[0018] During the autoclaving process, saturated water vapor is introduced into the autoclave to maintain 100% humidity throughout the process, ensuring that the hydration reaction proceeds fully.
[0019] S6, Post-construction dry heat curing: After autoclaving, the blocks are sent to a constant temperature curing room and dry heat cured at 100℃ for 18 hours to obtain high-strength aerated brick finished products.
[0020] Example 2 A processing method for increasing the compressive strength of aerated concrete blocks includes the following steps: S1, Raw material pretreatment: Select 45 parts by weight of siliceous raw material, 25 parts by weight of calcareous raw material, 8 parts by weight of modified reinforcing agent, 2 parts by weight of gypsum, 0.08 parts by weight of aluminum powder gas generator, and 30 parts by weight of water; grind the siliceous raw material, calcareous raw material, and gypsum separately, pass them through a 200-mesh sieve, and then send them into a drying equipment to dry at 105℃ until the moisture content is ≤1.5%; The siliceous raw material is a mixture of fly ash and fine quartz sand powder in a mass ratio of 3:1; the calcareous raw material is a mixture of quicklime and ordinary silicate cement in a mass ratio of 2:1; the modified reinforcing agent is a mixture of modified basalt powder and composite adhesive powder in a mass ratio of 4:1, wherein the modified basalt powder is treated by soaking in sodium hydroxide, high-temperature calcination, and activation modification with dilute hydrochloric acid, and the composite adhesive powder is a mixture of redispersible latex powder with glass transition temperatures of 15℃ and -6℃.
[0021] The modified basalt powder is prepared by soaking basalt powder in a 1.2 mol / L sodium hydroxide solution for 1.2 h, drying it, calcining it at 650℃ for 2 h, cooling it, soaking it in a 0.8 mol / L hydrochloric acid solution for 1.4 h, washing it until neutral, drying it, and grinding it.
[0022] S2, graded mixing and slurry preparation: The pretreated siliceous raw materials, calcareous raw materials, and gypsum are put into a forced mixer and dry-mixed for 3 minutes; then 80% of the proportion of water is added and wet-mixed for 6 minutes to form a uniform base slurry; then the modified reinforcing agent is dispersed in the remaining 20% of water, the water temperature is controlled at 40℃, and after stirring and dispersing for 2 minutes, it is slowly injected into the base slurry and stirred for another 4 minutes; finally, aluminum powder gas generator is added and quickly stirred for 1 minute to obtain a homogeneous and stable aerated brick slurry; S3, segmented temperature-controlled gas generation molding: The prepared slurry is quickly injected into the mold, which is preheated to 35°C. The segmented temperature-controlled gas generation process is adopted: the first stage is kept at a constant temperature of 35°C for 20 minutes to achieve initial gas generation and uniform bubble nucleation; the second stage is kept at a constant temperature of 45°C for 30 minutes to complete the stable growth of bubbles and solidification of the slurry. S4, Pre-curing and Precision Cutting: The formed blank, along with the mold, is sent into the pre-curing chamber and pre-cured for 2.5 hours at a temperature of 55℃ and a relative humidity of 85% to allow the blank to initially harden and acquire the strength required for shaping. After demolding, the blank is precisely cut using CNC cutting equipment to remove edge waste and process it into standard-sized block blanks. S5, Gradient autoclaving: The cut billet is sent into an autoclave and cured using a three-stage autoclaving process: gradient pressurization, constant temperature and pressure, and gradient depressurization. The curing process steps are as follows: A1, Gradient pressurization stage: The pressure is uniformly increased to 1.0MPa within 1.5h, and the temperature inside the reactor is simultaneously increased to 185℃ to slowly activate the hydration reaction of the raw materials and avoid cracking of the internal structure of the billet caused by sudden changes in pressure and temperature. A2, Constant Temperature and Pressure Stage: Maintain a constant pressure of 1.0 MPa and a constant temperature of 185℃ for 6 hours; A3, Gradient depressurization stage: The pressure is reduced to normal pressure at a constant rate within 1.5 hours, and the temperature naturally drops to room temperature.
[0023] During the autoclaving process, saturated water vapor is introduced into the autoclave to maintain 100% humidity throughout the process, ensuring that the hydration reaction proceeds fully.
[0024] S6, Post-construction dry heat curing: After autoclaving, the blocks are sent to a constant temperature curing room and dry heat cured at 90℃ for 12 hours to obtain high-strength aerated brick finished products.
[0025] Example 3 A processing method for increasing the compressive strength of aerated concrete blocks includes the following steps: S1, Raw material pretreatment: Select 55 parts by weight of siliceous raw material, 32 parts by weight of calcareous raw material, 12 parts by weight of modified reinforcing agent, 4 parts by weight of gypsum, 0.12 parts by weight of aluminum powder gas generator, and 38 parts by weight of water; grind the siliceous raw material, calcareous raw material, and gypsum separately, pass them through a 300-mesh sieve, and then send them into a drying equipment to dry at 115℃ until the moisture content is ≤1.5%; The siliceous raw material is a mixture of fly ash and fine quartz sand powder in a mass ratio of 3:1; the calcareous raw material is a mixture of quicklime and ordinary silicate cement in a mass ratio of 2:1; the modified reinforcing agent is a mixture of modified basalt powder and composite adhesive powder in a mass ratio of 4:1, wherein the modified basalt powder is treated by soaking in sodium hydroxide, high-temperature calcination, and activation modification with dilute hydrochloric acid, and the composite adhesive powder is a mixture of redispersible latex powder with glass transition temperatures of 15℃ and -6℃.
[0026] The modified basalt powder is prepared by soaking basalt powder in a 1.2 mol / L sodium hydroxide solution for 1.2 h, drying it, calcining it at 650℃ for 2 h, cooling it, soaking it in a 0.8 mol / L hydrochloric acid solution for 1.4 h, washing it until neutral, drying it, and grinding it.
[0027] S2, graded mixing and slurry preparation: The pretreated siliceous raw materials, calcareous raw materials, and gypsum are put into a forced mixer and dry-mixed for 5 minutes; then 80% of the proportion of water is added and wet-mixed for 8 minutes to form a uniform base slurry; then the modified reinforcing agent is dispersed in the remaining 20% of water, the water temperature is controlled at 40℃, and after stirring and dispersing for 2 minutes, it is slowly injected into the base slurry and stirred for another 4 minutes; finally, aluminum powder gas generator is added and quickly stirred for 1 minute to obtain a homogeneous and stable aerated brick slurry; S3, segmented temperature-controlled gas generation molding: The prepared slurry is quickly injected into the mold, which is preheated to 45°C. The segmented temperature-controlled gas generation process is adopted: the first stage is kept at a constant temperature of 40°C for 25 minutes to achieve initial gas generation and uniform nucleation of bubbles; the second stage is kept at a constant temperature of 50°C for 35 minutes to complete the stable growth of bubbles and solidification of the slurry. S4, Pre-curing and Precision Cutting: The formed blank, along with the mold, is sent into the pre-curing chamber and pre-cured for 3.5 hours at a temperature of 60℃ and a relative humidity of 90% to allow the blank to initially harden and acquire the strength required for shaping. After demolding, the blank is precisely cut using CNC cutting equipment to remove edge waste and process it into standard-sized block blanks. S5, Gradient autoclaving: The cut billet is sent into an autoclave and cured using a three-stage autoclaving process: gradient pressurization, constant temperature and pressure, and gradient depressurization. The curing process steps are as follows: A1, Gradient pressurization stage: The pressure is uniformly increased to 1.2MPa within 2.5h, and the temperature inside the reactor is simultaneously increased to 195℃ to slowly activate the hydration reaction of the raw materials and avoid cracking of the internal structure of the billet caused by sudden changes in pressure and temperature. A2, Constant Temperature and Pressure Stage: Maintain a constant pressure of 1.2 MPa and a constant temperature of 195℃ for 8 hours; A3, Gradient depressurization stage: The pressure is uniformly reduced to normal pressure within 2.5 hours, and the temperature naturally drops to room temperature.
[0028] During the autoclaving process, saturated water vapor is introduced into the autoclave to maintain 100% humidity throughout the process, ensuring that the hydration reaction proceeds fully.
[0029] S6, Post-construction dry heat curing: After autoclaving, the blocks are sent to a constant temperature curing room and dry heat cured at 110℃ for 24 hours to obtain high-strength aerated brick finished products.
[0030] Comparative Example The traditional aerated concrete block processing technology is adopted, and the raw materials are conventional fly ash, lime and cement in a conventional ratio. The process involves simple mixing, constant temperature gas generation, and conventional uniform speed autoclaving. There are no modified reinforcing additives or subsequent dry heat curing processes. The rest of the production environment is the same as in Example 1.
[0031] Performance test results The compressive strength, dry density, and thermal conductivity of the B06 grade aerated concrete blocks prepared in each embodiment and comparative example were tested. The test results are shown in the table below:
[0032] The test data shows that the aerated bricks prepared by the process of this invention have a dry density that is basically the same as that of traditional products, no reduction in thermal insulation performance, and significantly improved compressive strength compared with traditional processes, with an improvement of 47.9%-64.6%, perfectly achieving the synergistic effect of high strength, lightweight and thermal insulation.
[0033] The above descriptions are merely embodiments of the present invention, and common knowledge such as specific technical solutions and / or characteristics are not described in detail here. It should be noted that those skilled in the art can make various modifications and improvements without departing from the technical solutions of the present invention, and these should also be considered within the scope of protection of the present invention. These modifications and improvements will not affect the effectiveness of the implementation of the present invention or the practicality of the patent. The scope of protection claimed in this application should be determined by the content of its claims, and the specific embodiments described in the specification can be used to interpret the content of the claims.
Claims
1. A processing method for increasing the compressive strength of aerated concrete blocks, characterized in that, Includes the following steps: S1, Raw material pretreatment: Select 45-55 parts by weight of siliceous raw material, 25-32 parts by weight of calcareous raw material, 8-12 parts by weight of modifying and reinforcing agent, 2-4 parts by weight of gypsum, 0.08-0.12 parts by weight of aluminum powder gas generator, and 30-38 parts by weight of water; grind the siliceous raw material, calcareous raw material, and gypsum separately, pass them through a 200-300 mesh sieve, and then send them into a drying equipment to dry at 105-115℃ until the moisture content is ≤1.5%; S2, graded mixing and slurry preparation: The pretreated siliceous raw materials, calcareous raw materials, and gypsum are put into the mixer and dry-mixed for 3-5 minutes; then 80% of the proportion of water is added and wet-mixed for 6-8 minutes to form a uniform base slurry; then the modified reinforcing agent is dispersed in the remaining 20% of water, the water temperature is controlled at 40-50℃, and after stirring and dispersing for 2 minutes, it is injected into the base slurry and stirred for another 4-6 minutes; finally, aluminum powder gas generator is added and stirred for 1-2 minutes to obtain a homogeneous and stable aerated brick slurry; S3, Segmented Temperature-Controlled Gas Generation and Molding: The prepared slurry is quickly injected into the mold, which is preheated to 35-45℃. A segmented temperature-controlled gas generation process is adopted: the first stage is kept at a constant temperature of 35-40℃ for 20-25 minutes to achieve initial gas generation and uniform bubble nucleation; the second stage is kept at a constant temperature of 45-50℃ for 30-35 minutes to complete stable bubble growth and slurry solidification. S4, Pre-curing and Precision Cutting: The formed blank, along with the mold, is sent into the pre-curing chamber and pre-cured for 2.5-3.5 hours at a temperature of 55-60℃ and a relative humidity of 85%-90% to allow the blank to initially harden and acquire the strength required for shaping. After demolding, the blank is precisely cut using CNC cutting equipment to remove edge waste and process it into standard-sized block blanks. S5, Gradient autoclaving: The cut billet is sent into the autoclave and subjected to three-stage autoclaving with gradient pressure increase, constant temperature and pressure, and gradient pressure decrease. S6, Post-construction dry heat curing: After autoclaving, the blocks are sent to a constant temperature curing chamber and dry heat cured at 90-110℃ for 12-24 hours to obtain the finished aerated brick product.
2. The processing technology for increasing the compressive strength of aerated concrete blocks according to claim 1, characterized in that: The siliceous raw material is a mixture of fly ash and fine quartz sand powder in a mass ratio of 3:1; the calcareous raw material is a mixture of quicklime and ordinary silicate cement in a mass ratio of 2:1; the modified reinforcing agent is a mixture of modified basalt powder and composite adhesive powder in a mass ratio of 4:1, wherein the modified basalt powder is treated by soaking in sodium hydroxide, high-temperature calcination, and activation modification with dilute hydrochloric acid, and the composite adhesive powder is a mixture of redispersible latex powder with glass transition temperatures of 15℃ and -6℃.
3. The processing technology for increasing the compressive strength of aerated concrete blocks according to claim 2, characterized in that: The modified basalt powder is prepared by soaking basalt powder in a 1.2 mol / L sodium hydroxide solution for 1.2 h, drying it, calcining it at 650℃ for 2 h, cooling it, soaking it in a 0.8 mol / L hydrochloric acid solution for 1.4 h, washing it until neutral, drying it, and grinding it.
4. The processing technology for increasing the compressive strength of aerated concrete blocks according to claim 3, characterized in that: The maintenance process steps in step S5 are as follows: A1, Gradient pressurization stage: The pressure is uniformly increased to 1.0-1.2MPa within 1.5-2.5h, and the temperature inside the reactor is simultaneously increased to 185-195℃ to slowly activate the hydration reaction of the raw materials and avoid sudden changes in pressure and temperature that could cause cracking of the internal structure of the billet. A2, Constant Temperature and Pressure Stage: Maintain a constant pressure of 1.0-1.2 MPa and a constant temperature of 185-195℃ for 6-8 hours; A3, Gradient depressurization stage: The pressure is uniformly reduced to normal pressure within 1.5-2.5 hours, and the temperature naturally drops to room temperature.
5. The processing technology for increasing the compressive strength of aerated concrete blocks according to claim 4, characterized in that: During step S5, the autoclave is filled with saturated steam to maintain 100% humidity throughout the process, ensuring that the hydration reaction proceeds fully.