A post-processing method to improve the dimensional accuracy of wax molds for spray-printed blades

By employing a multi-step collaborative control post-processing method, the problem of controlling the dimensional accuracy of wax molds for spray-printed blades was solved, enabling high-precision molding of complex thin-walled components and ensuring dimensional stability and accuracy of inspection.

CN123104070APending Publication Date: 2026-11-17SHANGHAI JIAOTONG UNIV
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611387120.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-08
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing wax spraying printing technology makes it difficult to control the dimensional accuracy of blade wax molds during the removal of support wax, resulting in cumulative errors and dimensional inconsistencies. This is especially true for complex thin-walled components, where conventional post-processing methods cannot effectively maintain the accuracy during the printing stage.

Method used

A multi-step, collaboratively controlled post-processing method, including baseline dimensional stabilization, isothermal pre-wetting, low-heat-load intermittent ultrasonic removal, controlled gradient rinsing and cooling, and uniform drying, establishes a stable dimensional baseline, limits the non-uniformity of heat load and solvent exchange, and avoids dimensional changes.

Benefits of technology

It significantly improves the final dimensional accuracy of the wax mold for spray-printed blades, controlling it within 0.1 mm, reducing bending, twisting, local shrinkage and measurement errors, and improving the reliability of 3D scanning and the authenticity of detection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123104070A_ABST
    Figure CN123104070A_ABST
Patent Text Reader

Abstract

This application provides a post-processing method to improve the dimensional accuracy of wax molds for spray-printed blades, comprising: maintaining the composite state of the molding wax and the support wax; placing the spray-printed blade wax mold in a first constant temperature environment for static treatment; completely immersing the static blade wax mold in a pretreatment solution at a first temperature; transferring the pretreated blade wax mold to a cleaning solution, controlling the cleaning temperature at a second temperature, and performing intermittent ultrasonic cleaning using a preset frequency and preset power density; transferring the ultrasonically cleaned blade wax mold to a rinsing solution at an initial temperature of a third temperature, and simultaneously cooling the wax mold and the rinsing solution to room temperature at a preset cooling rate; and placing the rinsed blade wax mold in a second constant temperature environment and drying it at a preset airflow rate until no residual liquid or oil film remains on the surface. This application, through multi-step coordinated control, reduces bending, shrinkage, swelling, and measurement deviations introduced by post-processing, thereby improving the dimensional accuracy of the final blade wax mold relative to the theoretical model.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of investment casting wax spraying printing technology, and more specifically, to a post-processing method for improving the dimensional accuracy of wax molds for spray-printed blades. Background Technology

[0002] 3D printing technology, also known as additive manufacturing technology, is a rapid prototyping manufacturing technology developed based on the principle of layer-by-layer deposition. Wax spray printing can directly produce wax models with high surface quality and complex structures, and is suitable for fields such as jewelry and precision investment casting.

[0003] Wax spray printing typically uses two materials: forming wax and support wax. Forming wax builds the blade body, while support wax fills suspended structures, thin-walled gaps, and areas of localized weakness. After printing, the support wax must be removed. However, the removal process involves solvent penetration, temperature changes, ultrasonic impact, gravitational loads, and drying shrinkage. These effects can further accumulate dimensional deviations already formed during the printing stage and may alter the blade's chord length, thickness, torsion angle, and local surface contours. For complex thin-walled components such as aero-engine blades, wax spray printing not only needs to achieve high forming accuracy but also needs to maintain this accuracy after the support wax is removed. Therefore, the post-processing stage essentially constitutes a crucial stage in the final dimensional formation of the wax model.

[0004] Existing wax support removal processes primarily aim for "clean removal" and "time reduction," typically employing steps such as heated immersion, continuous stirring, ultrasonic cleaning, direct rinsing, and natural evaporation. While these methods can remove supports from general wax molds, they lack continuous temperature and wetting control between processes. When thin-walled blades are repeatedly exposed to different media, they are prone to rapid heating and cooling, non-uniform swelling, and localized unloading, resulting in additional dimensional errors in post-processing.

[0005] For thin-walled, irregularly shaped wax models of blades, the final dimensions typically need to be controlled within the 0.1 mm range. The blade surface is continuous, with small local thickness and uneven stiffness. Furthermore, the structural constraints change before and after the removal of the supporting wax. Therefore, even with small dimensional deviations during the printing stage, conventional post-processing can still cause bending, twisting, localized depressions, shrinkage, and scanning errors, leading to the final wax model exceeding allowable tolerances. Defects such as cracking, pitting, white film, and oil film in existing processes also indirectly reduce the reliability of 3D scanning and dimensional evaluation.

[0006] A search revealed Chinese patent application CN119636073A, which discloses a 3D printing post-processing method for washing support wax and polishing surface textures of a model, including the following steps: mixing alcohol, alkane, and ester in a 1:1 ratio. 3:1 A mixture of 3 parts wax is thoroughly prepared to form a solution. The paraffin model is then immersed in the heated solution and removed. The model is then placed in a fume hood to allow the solvent on its surface to evaporate completely. This application aims to completely remove the supporting wax, but it cannot achieve precise control over the dimensional accuracy of the wax model. Summary of the Invention

[0007] In view of one of the defects in the prior art, the purpose of this application is to provide a post-processing method to improve the dimensional accuracy of wax molds for spray-printed blades.

[0008] Further analysis of existing processes reveals that the post-processing factors affecting the final dimensional accuracy of blade wax models mainly include the following two aspects: First, post-processing errors are cumulative and coupled. Delayed shrinkage after printing alters the initial dimensional baseline; rapid solvent immersion or evaporation causes localized swelling and shrinkage; continuous ultrasonic operation leads to temperature rise and localized impact; direct rinsing and rapid cooling generate thermal stress; and uneven drying introduces residual liquid on the surface and measurement errors. Optimizing only a single step is insufficient to stably control the final dimensions.

[0009] Second, existing technologies lack a complete set of parameter relationships aimed at achieving final dimensional accuracy. The settling temperature and time, pre-wetting degree, cleaning solution ratio, ultrasonic frequency and power, intermittent cycle time, rinsing cooling rate, cross-process transfer method, and drying conditions are usually determined separately. The continuity of temperature, wetting, and load between each step is not established, making it difficult to repeatedly obtain blade wax models with consistent dimensions.

[0010] Therefore, there is a need for a post-processing method that aims to reduce post-processing errors and improve the final dimensional accuracy of the blade wax model after the removal of the support wax. Through multi-step coordinated control, the wax model can maintain dimensional stability during the processes of support constraint release, solvent exchange, ultrasonic cleaning, cooling and drying.

[0011] This application provides a post-processing method for improving the dimensional accuracy of wax molds for spray-printed blades, including: Step 1, datum dimension stabilization: Maintain the composite state of molding wax and support wax, place the printed blade wax model in the first constant temperature environment and let it stand, so that the delayed shrinkage and residual stress after printing can be fully released under the support constraint, and establish a stable post-processing dimension datum. Step 2, Isothermal Pre-wetting and Support Softening: After standing (i.e. after dimensional stabilization), the blade wax mold is completely immersed in the pretreatment solution at the first temperature to soften the support wax evenly and allow the molding wax to slowly and evenly complete the solvent wetting balance, reducing local dimensional changes caused by inconsistent swelling rates in different areas during the subsequent ultrasonic stage. Step 3, Low-heat-load intermittent ultrasonic removal: The pretreated blade wax model is immersed in the cleaning solution and the cleaning temperature is controlled at the second temperature. Intermittent ultrasonic cleaning is performed using a preset frequency and preset power density. The support wax is removed by controlling the temperature, high frequency and low power and intermittent operation mode, and the heat accumulation and mechanical impact caused by the ultrasonic process are limited. Step 4, Controlled gradient rinsing and cooling: Immerse the ultrasonically treated blade wax model into a rinsing solution with an initial temperature of the third temperature. While removing residual cleaning solution and trace amounts of support wax, cool the wax model and rinsing solution to room temperature simultaneously and uniformly at a preset cooling rate to reduce thermal stress. Step 5, Constant Temperature and Uniform Drying: Place the rinsed blade wax model in a second constant temperature and ventilation environment and dry it at a preset wind speed until there is no residual liquid or oil film on the surface. This allows the residual solution to evaporate evenly, avoiding cooling shrinkage caused by local rapid evaporation and dimensional detection errors caused by the surface film layer. This results in a blade wax model with stable dimensions, a clean surface, and suitable for precision scanning.

[0012] This application provides a post-processing method for controlling cumulative dimensional changes and improving the final dimensional accuracy of the wax model of a spray-printed blade during the removal of support wax. This method does not simply pursue the rapid removal of support wax, but treats the support wax removal process as a wax model accuracy control link. By stabilizing the initial dimensional reference, balancing solvent wetting, limiting ultrasonic heat load, controlling the cooling rate, and uniform drying, the bending, shrinkage, swelling, and measurement deviations introduced by post-processing are reduced, thereby improving the dimensional accuracy of the final blade wax model relative to the theoretical model.

[0013] Optionally, in step 1, the temperature of the first constant temperature environment is 22-24°C, and the time spent standing in the first constant temperature environment is not less than 12 hours.

[0014] During the wax spraying process, the wax droplets undergo melting, spraying, spreading, and solidification. At the end of printing, the internal temperature and crystallization state are not yet completely uniform, and the wax mold may still experience delayed shrinkage. If the support wax is removed immediately, the blades lose their constraint before their dimensions stabilize, and subsequent solvent and temperature effects will amplify bending and twisting. This application retains the support wax at 22–24°C for at least 12 hours, allowing the molding wax and support wax to jointly achieve thermal equilibrium and subsequent shrinkage. This support structure restricts free deformation in thin-walled areas, reducing dimensional fluctuations before post-processing from the source.

[0015] Optionally, in step 2, the pretreatment solution is composed of 40–55 wt% ethanol, 25–35 wt% isopropanol and 20–30 wt% polypropylene glycol by mass percentage.

[0016] Traditional high-temperature, prolonged immersion or direct ultrasonic cleaning results in significant differences in the removal rate between thick and thin areas of the support wax. Thin areas lose support first, leading to a decrease in local blade stiffness, while thicker areas remain constrained, easily causing uneven unloading and localized deformation. Simultaneously, the sudden entry of solvent into the wax mold surface causes short-term, non-uniform volume changes. By incorporating a pretreatment process, the support wax is softened as a whole before ultrasonic cleaning, and the solvent exchange process changes from rapid impact to slow, even exchange, thereby gradually releasing the support constraints and reducing abrupt dimensional changes during post-processing.

[0017] The pretreatment solution is a blend of ethanol, isopropanol, and polypropylene glycol. Ethanol and isopropanol provide softening and dissolving capabilities for the supporting wax, while polypropylene glycol is used to adjust the solution viscosity, evaporation rate, and solvent diffusion rate. The synergistic effect of these three components allows the supporting wax to soften uniformly at lower temperatures, while avoiding localized swelling, shrinkage, and temperature fluctuations caused by the rapid penetration and evaporation of small-molecule solvents. The key function of this blend is to control the release rate of the supporting wax and the solvent exchange rate, rather than simply increasing the dissolution rate.

[0018] The first temperature is 35–37°C, and the immersion time in the pretreatment solution is 10–20 min. This temperature is higher than room temperature, which ensures that the supporting wax has an appropriate softening rate, while it is lower than the temperature range that easily causes significant softening and gravitational deformation of the blade wax model.

[0019] Optionally, during the pretreatment process, magnetic stirring is used to promote uniform flow of the pretreatment solution, and the blade wax model is fixed by a limiting structure or its spatial displacement is restricted by container space constraints to ensure that the blade wax model does not float, shift, tip over, or collide with the container with the flow field. A gentle and uniform liquid flow is used during the pretreatment process to avoid direct scouring or collision with the blade.

[0020] The limiting structures mainly include clamping limiting structures and holding limiting structures. Clamping limiting structures use pressure blocks on a flat machined surface to place the blade on the surface, using the pressure blocks to hold down the stronger, less deformable parts of the blade. Holding limiting structures use clamping components to hold the thicker, less deformable parts of the blade, such as the bottom and root. These limiting structures directly fix the blade through clamping force, holding force, and friction between the contact surfaces, thereby limiting the blade's translation, rotation, or tilting during post-processing and preventing deformation or surface damage due to movement or collision.

[0021] Container space constraints are primarily suitable for blades with irregular overall shapes, lacking smooth machined surfaces, or lacking easily deformable parts suitable for clamping and holding. Specifically, the blades can be placed within a plastic mesh frame, basket, or other confined container with sufficient space to accommodate them, ensuring the internal space of the container matches the blade's dimensions. The bottom and side walls of the container limit the maximum range of movement and rotation of the blades from different directions, allowing only small displacements within the container. This prevents large-scale movement, collisions, or concentrated clamping forces during post-processing, thereby reducing the risk of bending deformation and surface damage. When using a mesh frame or basket, the mesh openings also ensure normal flow and discharge of the post-processing medium.

[0022] It should be noted that limiting structures directly contact specific parts of the blade through compression or clamping, relatively fixing the blade and providing strong restraint. This is suitable for blades with flat surfaces or thick, non-deformable clamping parts. Container space constraints, on the other hand, limit the overall range of motion of the blade through the inner wall of the container. Generally, no large concentrated clamping force is applied to any part of the blade, allowing for slight movement within the confined space. This is suitable for blades lacking reliable compression surfaces or clamping parts, with low overall rigidity, and with complex shapes.

[0023] Optionally, in step 3, the second temperature is 33–36°C; the preset frequency is 80–120 kHz; and the preset power density is 15–25 W / L. The intermittent ultrasonic cleaning includes: a single ultrasonic cleaning session of 1 to 3 minutes, followed by a 1-minute rest interval and repeated 3 to 7 times.

[0024] The support wax and molding wax have a distinct color difference; the support wax is pure white, while the molding wax is another color. Therefore, visual inspection can be used to determine whether the support wax has been completely removed. Specifically, rotate the blade wax model in the cleaning solution and observe the surface under normal lighting conditions, paying particular attention to areas prone to support wax residue, such as grooves, corners, edges, and narrow gaps in the blades. When no visible white support wax residue is visible on the wax model surface or in the aforementioned areas, the support wax is considered to have been completely removed. Avoid removing the wax model from the cleaning solution as much as possible, as the evaporation of the cleaning solution can cause rapid cooling and deformation of the wax model.

[0025] The specific number of cycles was determined by checking each cycle. First, three cycles were completed, with each ultrasonic treatment lasting 1-3 minutes followed by a 1-minute rest period. After the third cycle, the blade wax model was visually inspected. If white support wax residue was still present, one more cycle was added, followed by another inspection. The number of cycles was increased sequentially in the above manner until no white residue was visible on the surface of the wax model.

[0026] It should be noted that the actual number of cycles required varies depending on the size, structural complexity, and amount of support wax used for different blades. Within the scope of the blades and process conditions covered in this application, blades with simpler structures or less support wax can usually be cleaned completely after 3 cycles; blades with more complex structures or more support wax require a slightly higher number of cycles, but can be cleaned completely after no more than 7 cycles. Therefore, the number of cycles is set at 3 to 7, with 3 being the minimum number of cycles. The actual number of cycles is terminated when no visible white support wax residue remains on the wax mold surface.

[0027] Optionally, the cleaning solution is composed of 50-65 wt% ethanol, 25-35 wt% isopropanol and 10-20 wt% polypropylene glycol by mass percentage.

[0028] This application treats the cleaning fluid ratio, ultrasonic frequency, power density, single working time, interval time, and cleaning temperature as interrelated precision control parameters, rather than as independent cleaning parameters.

[0029] Increasing the proportion of ethanol and appropriately decreasing the proportion of polypropylene glycol in the cleaning solution allows the softened support wax to be removed within a shorter ultrasonic time, reducing the cumulative time the blades are exposed to the solvent and acoustic field; at the same time, a certain proportion of polypropylene glycol is retained to suppress solvent diffusion and excessively rapid temperature changes.

[0030] Ultrasonic cavitation can accelerate the peeling of softened support wax, but cavitation impact and continuous temperature rise can also alter the dimensions of thin-walled wax molds. At lower frequencies, cavitation bubbles are larger and localized impacts are stronger; when the power is too high or the continuous working time is too long, the cleaning fluid temperature rises, the stiffness of the molded wax decreases, and the blades are easily deformed under the influence of gravity and fluid disturbance. Therefore, ultrasonic parameters must be matched with the degree of softening and temperature control in the preceding process.

[0031] The ultrasonic frequency is controlled between 80 and 120 kHz, preferably 120 kHz; the power density is controlled between 15 and 25 W / L, preferably 15 to 20 W / L. Higher frequencies can form finer and more uniformly distributed cavitation bubbles, while lower power can reduce localized impact. For blades with high dimensional accuracy requirements, using 120 kHz and 15 W / L can balance support removal with surface and dimensional preservation.

[0032] An intermittent ultrasonic cleaning method was employed, consisting of 1–3 minutes of single ultrasonic treatment, followed by 1 minute of rest, and repeated 3–7 times, with the cleaning solution temperature maintained at 33–36°C. The resting intervals were used to release the heat generated by the ultrasonic treatment and to re-homogenize the solution, thus avoiding temperature rise, stiffness reduction, and gravitational bending caused by continuous ultrasonic treatment. This ensured high dimensional stability of the blade wax model during the gradual removal of the support. High-frequency, low-power intermittent ultrasonic treatment at a controlled temperature was used to remove the support wax, suppressing dimensional changes caused by ultrasonic temperature rise and localized impacts.

[0033] Optionally, in step 4, the third temperature is 35-37°C, and the preset cooling rate is 0.8-1.2°C / min.

[0034] Optionally, the rinsing solution is composed of 35-50 wt% ethanol, 20-30 wt% isopropanol and 30-40 wt% polypropylene glycol by mass percentage.

[0035] The rinsing time is determined based on the initial rinsing temperature, ambient temperature, and preset cooling rate, and is not fixed at a specific time. In practice, the initial temperature of the rinsing solution is maintained at 35–37°C. During continuous rinsing, the temperature of the rinsing solution is gradually reduced at a rate of 0.8–1.2°C / min until the temperature of the leaf wax model and the rinsing solution drops to room temperature, which takes approximately 8–15 minutes. The actual rinsing time is terminated when the rinsing solution reaches room temperature.

[0036] The above-mentioned time and cooling rate settings ensure that the residual support wax and cleaning fluid on the surface of the blade wax mold are thoroughly rinsed. On the other hand, they prevent the blade wax mold from experiencing large internal and external temperature differences and uneven shrinkage due to a sudden drop in temperature, thereby reducing the risk of warping, microcracks, and dimensional changes.

[0037] After the support wax is removed, the blade structure has low stiffness, and the overall temperature of the wax model remains above room temperature. If it is removed directly and rinsed with cold liquid or cooled with air, a large temperature difference will form between the surface and the interior, which can easily cause warping, shrinkage, and localized cracking. This application uses immersion rinsing to allow the wax model to complete the temperature transition in a uniform liquid environment.

[0038] The rinsing solution is prepared by appropriately reducing the proportions of ethanol and isopropanol and increasing the proportion of polypropylene glycol to slow down solvent evaporation and heat exchange. The rinsing solution is cooled from 35–37°C to room temperature at a rate of 0.8–1.2°C / min to maintain a similar cooling rate across all areas of the blade, reducing dimensional changes caused by temperature gradients and simultaneously removing residual support wax and cleaning solution.

[0039] Optionally, in step 5, the temperature of the second constant temperature environment is 22-24℃, and the preset wind speed is 0.45-0.55 m / s; a uniform and continuous ventilation method is used for drying until there is no oil film or solution residue on the surface of the blade wax model, and the temperature is kept balanced in an environment of 22-24℃ before dimensional detection.

[0040] The oil film on the surface of the blade wax mold is mainly formed by residual liquid containing polypropylene glycol. Because polypropylene glycol is somewhat oily and not easily volatile, when it remains on the wax mold surface, it will exhibit continuous or localized oily sheen under light. Drying is carried out using a uniform and continuous ventilation method at a temperature of 22–24℃ and a wind speed of 0.45–0.55 m / s to gradually remove moisture and other volatile components from the wax mold surface until the specified surface dryness is achieved.

[0041] The determination of an oil film involves a combination of visual inspection and lint-free paper inspection. Under uniform lighting conditions, the surface of the leaf wax model is observed from different angles, paying particular attention to areas prone to liquid accumulation such as the leaf roots, grooves, corners, and edges. If no continuous or localized abnormal oily reflections are observed on the wax model surface, it is preliminarily determined that there is no oil film. Subsequently, clean, dry lint-free paper is used to gently press non-critical surfaces of the wax model. If no transparent or translucent oil spots appear on the lint-free paper, and the wax model surface does not feel noticeably sticky, it is determined that there is no oil film on the surface.

[0042] The determination of solution residue is mainly made through visual inspection. When there are no visible droplets, wet marks, drip marks, or liquid accumulation on the surface of the blade wax model and its grooves, corners, and edges, and no wet marks appear after lightly pressing with clean, lint-free paper, it is determined that there is no solution residue on the surface.

[0043] Uniform ventilation can make the volatilization rates on both sides of the blade and different curved areas similar, reducing micro-deformation caused by asymmetric drying; sufficient drying can also prevent oil film or residual liquid from changing the powder coating thickness and scanning reflection state, thereby improving the reliability of final size detection.

[0044] Optionally, during the pretreatment, intermittent ultrasonic cleaning, and rinsing processes, the blade wax model is always completely immersed in the corresponding solution; the wax model is transferred between adjacent solution treatment steps using a container with liquid, ensuring it is not exposed to air during the transfer, and that the blade wax model remains completely immersed throughout, with the temperature difference between solutions in adjacent steps not exceeding 4°C. This operation avoids the rapid evaporation of solvent from the wax model surface in the air, which would cause a sudden drop in temperature, and also avoids a rapid rise in temperature upon re-immersion, thus maintaining a continuous temperature and immersion state for the wax model across processes.

[0045] The pretreatment process is both a support wax softening step and a dimensional accuracy control step. By uniformly softening the support, establishing solvent wetting balance in advance, and maintaining temperature continuity, it allows all areas of the blade to release constraints synchronously during subsequent ultrasonic cleaning, reducing local bending, surface peeling, and dimensional abrupt changes.

[0046] The liquid transfer container can be a rectangular plastic box, or a cylindrical container, trough-shaped container, barrel-shaped container, or other container capable of holding the treatment solution; its shape is not particularly limited. The internal dimensions of the container should be slightly larger than the external dimensions of the blade wax model, so that the blade wax model can be completely placed inside without being squeezed against the inner wall of the container; the depth and liquid volume of the container should ensure that the liquid level is always slightly higher than the highest point of the blade wax model during the transfer process, so that the blade wax model remains completely submerged and the impact on the solution in the next step is minimized.

[0047] During the transfer process, the blade wax model is placed in a transfer container containing the corresponding solution, below the solution level of the previous processing step. The entire transfer container, including the solution and the blade wax model, is then carefully removed and moved to the next processing step. Upon arrival at the next processing container, the container is slowly immersed in the solution of the next step until its opening is below the solution level. The blade wax model is then transferred below the solution level, ensuring that it is not directly exposed to air between adjacent processing steps. During transfer, the container should be kept relatively level and handled gently, avoiding sudden acceleration, stopping, tilting, or violent shaking to prevent the blade wax model from colliding with the container wall or being subjected to significant liquid flow impact.

[0048] The phrase "the temperature difference between adjacent process solutions is no more than 4℃" refers to the temperature difference between the solutions used in two adjacent processing steps before transfer. Specifically, the temperature difference between the pretreatment solution and the intermittent ultrasonic cleaning solution is no more than 4℃, and the temperature difference between the intermittent ultrasonic cleaning solution and the rinsing solution is no more than 4℃. The temperature of each solution is measured and adjusted before transfer to ensure that the above temperature difference requirement is met before the transfer.

[0049] Because the cleaning solution is volatile, traditional methods of directly removing the blade wax model from the solution and exposing it to air for transfer can easily cause a rapid drop in temperature due to the rapid evaporation of the surface solution; upon re-immersion in the next process solution, a rapid temperature rise may occur. Using a container with the liquid attached for transfer, and controlling the temperature difference between adjacent process solutions within 4°C, can significantly reduce temperature fluctuations of the blade wax model during inter-process transfer, reducing warping, microcracks, and dimensional deviations caused by rapid temperature changes and uneven shrinkage, thereby improving the dimensional accuracy of the blade wax model.

[0050] This application aims for "final dimensional accuracy" by establishing a continuous precision control chain that includes stabilizing the reference dimensions, isothermal pre-wetting, intermittent ultrasonication under low heat load, controlled gradient cooling, and uniform drying. Each step controls different sources of error and achieves synergy through liquid-laden transfer and temperature continuity, significantly improving the final dimensional accuracy after removing the support wax. By retaining the support and allowing it to stand, a stable dimensional reference is established; pre-wetting ensures uniform release of support constraints; intermittent ultrasonication limits heat and impact; gradient rinsing reduces thermal stress; and uniform drying minimizes evaporation shrinkage. These steps collectively suppress bending, torsion, localized shrinkage, and swelling, thereby controlling the accumulation and coupling of post-processing errors. This application limits the solution ratio, temperature, time, ultrasonic parameters, transfer state, cooling rate, and drying environment, reducing dimensional fluctuations caused by operational differences. This facilitates the formation of a standardized blade wax model post-processing procedure, improving dimensional consistency and process repeatability. Rinsing and thorough drying reduce white film, oil film, and residual liquid, resulting in a more uniform distribution of developer or scanning powder. This reduces interference from surface conditions on point cloud acquisition, leading to detection results that more closely approximate the true dimensions of the wax model and improving the realism of 3D detection. Pretreatment shortens the effective ultrasonic time, and intermittent ultrasonication avoids prolonged high-temperature immersion. While improving the final dimensional accuracy, it reduces cracking, pitting, and surface erosion, balancing support removal efficiency with blade integrity. This method is suitable for complex thin-walled blades and other high-precision wax-printed models.

[0051] The post-processing method provided in this application for improving the dimensional accuracy of wax molds for printed blades establishes a stable dimensional benchmark by maintaining a composite state at a constant temperature; pre-wetting ensures uniform release of support constraints, avoiding local unloading; intermittent ultrasonication limits heat and impact; gradient rinsing reduces thermal stress; and uniform drying minimizes evaporation shrinkage. These methods synergistically suppress bending, torsion, and local depressions, effectively controlling error accumulation. Simultaneously, the pre-processing shortens the ultrasonic time and avoids high-temperature immersion, ensuring that the final dimensional deviation is stably controlled within 0.10 mm while reducing cracking and erosion, balancing removal efficiency and blade integrity. Furthermore, thorough rinsing and drying eliminate white film, oil film, and residual liquid, resulting in more uniform powder spraying during scanning, reducing interference from point cloud acquisition, and improving the accuracy of 3D detection and dimensional evaluation.

[0052] Furthermore, by optimizing dissolution efficiency through specific solution formulations and combining magnetic stirring with limiting constraints to avoid flow field impact and wax model displacement, and by using liquid-carrying transfer and strict temperature difference control between adjacent processes, additional stress caused by air exposure and sudden temperature changes during medium alternation is completely eliminated. These features further eliminate dimensional fluctuations caused by operational differences and sudden environmental changes, significantly improving the dimensional consistency and process repeatability of wax models for complex thin-walled blades, and facilitating the formation of standardized post-processing procedures.

[0053] Other technical effects resulting from the additional features will be further illustrated in the corresponding embodiments. Attached Figure Description

[0054] Other features, objects, and advantages of this application will become more apparent from the following detailed description of non-limiting embodiments with reference to the accompanying drawings: Figure 1 This is a flowchart of a post-processing method for improving the dimensional accuracy of wax molds for spray-printed blades, as described in an embodiment of this application. Figure 2 This is a diagram showing the out-of-tolerance dimensions of the blade defects in Comparative Example 9. Detailed Implementation

[0055] The present application will now be described in detail with reference to specific embodiments / comparative examples. These embodiments will help those skilled in the art to further understand the present application. It should be understood that the following are merely some examples and are not intended to limit the present application. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of the present application, and these all fall within the protection scope of the present application. Parts not described in detail in the following embodiments can be implemented using existing technology.

[0056] Unless otherwise specified, the equipment and raw materials used in this application are commercially available or commonly used in the field. Unless otherwise specified, the methods in the following embodiments are conventional methods in the field.

[0057] Performance testing and dimensional accuracy evaluation methods: 1. Surface Quality Evaluation: Observe whether the final wax model has residual support wax, white film or oil film, as well as defects such as micro-pits, cracks and localized erosion. Surface defects serve as an auxiliary evaluation indicator that may affect the true dimensions and scanning reliability.

[0058] 2. Final Dimensional Accuracy Evaluation: The dried and room-temperature equilibrated blade wax model was scanned using an OptimScan 5M Plus 3D scanner from Hangzhou Shining 3D Technology Co., Ltd. The measured point cloud was then optimally fitted and registered with the theoretical model. The maximum absolute value of the dimensional deviation across all detected areas was used as the "maximum dimensional deviation after post-processing." A smaller value indicates less dimensional change introduced by post-processing and higher final dimensional accuracy.

[0059] 3. Time Recording: Record the stabilization time after printing, the treatment time of each solution, the cooling time, the drying time, and the total time from printing completion to final size inspection. This is used to evaluate the balance between improved accuracy and production cycle time. This application utilizes a ProJet MJP 2500W wax printer from 3D Systems, employing SJTU-005 and SJTU-003 support waxes from Jiaxing Zhunwei Additive Manufacturing Technology Co., Ltd. The blade model's outline dimensions are 60 × 40 × 15 mm, with a minimum thickness of 1 mm. Samples were prepared using the same printing parameters, and the maximum dimensional deviation under support after printing was controlled within 0.05 mm. After completing different post-processing schemes, the final blade wax model was again subjected to 3D scanning to compare the impact of each post-processing scheme on the final dimensional accuracy.

[0060] Example 1 Reference Figure 1 The post-processing method for improving the dimensional accuracy of the wax mold for spray-printed blades in this embodiment specifically includes the following steps: Step 1: Place the printed blade wax model in a constant temperature environment for 12 hours. The ambient temperature of the constant temperature room is set to 23℃. Step 2: Prepare a 5 kg pretreatment solution consisting of 45 wt% ethanol, 30 wt% isopropanol, and 25 wt% polypropylene glycol. The ethanol purity is 99.5%, the isopropanol purity is 99.9%, and the polypropylene glycol is PPG400. Immerse the dimensionally stable blade wax model in the pretreatment solution at 36℃. Use a 40 mm cylindrical stirring rotor for magnetic stirring at 500 r / min for 15 min. Step 3: Prepare a 5 kg cleaning solution consisting of 55 wt% ethanol, 30 wt% isopropanol, and 15 wt% polypropylene glycol. The ethanol purity is 99.5%, the isopropanol purity is 99.9%, and the polypropylene glycol is PPG400. Transfer the pretreated wax model to an ultrasonic cleaner using a 65 × 45 × 20 mm rectangular plastic box and immerse it in the cleaning solution. The initial ultrasonic cleaning temperature is set to 33℃. During the cleaning process, the solution temperature is monitored in real time, and a temperature interlock control is used: when the solution temperature rises to 36℃, ultrasonic cleaning is immediately paused, and ultrasonic cleaning resumes after the solution temperature drops to 33℃. Additional pauses triggered by temperature protection are not included in the effective ultrasonic working time. The ultrasonic frequency is 120 kHz, the ultrasonic power is 20 W / L, and an intermittent ultrasonic method is used: 2 min of ultrasonic work, 1 min of rest, repeated 5 times, until the supporting wax is completely removed. Step 4: Prepare 5 kg of rinsing solution, consisting of 40 wt% ethanol, 25 wt% isopropanol, and 35 wt% polypropylene glycol. The ethanol purity is 99.5%, the isopropanol purity is 99.9%, and the polypropylene glycol is PPG400. Transfer the ultrasonically cleaned wax model to the rinsing solution using a 65 × 45 × 20 mm rectangular plastic box. Set the rinsing solution temperature to 36℃. After immersing the leaf in the rinsing solution, begin cooling at a rate of 1℃ / min until it reaches room temperature. Step 5: Remove the wax model and place it in a fume hood with the air velocity set to 0.55 m / s and the room temperature set to 24℃. Allow the rinsing solution to evaporate until there is no oil film on the surface of the wax model. Once the solution on the surface of the wax model has evaporated, a blade wax model with sufficient removal of the supporting wax, stable dimensions, and suitable for precision testing can be obtained.

[0061] Example 2 The post-processing method for improving the dimensional accuracy of wax molds for spray-printed blades in this embodiment includes the following steps: Step 1: Place the printed blade wax model in a constant temperature environment for 12 hours. The ambient temperature of the constant temperature room is set to 23℃. Step 2: Prepare a 5 kg pretreatment solution consisting of 55 wt% ethanol, 25 wt% isopropanol, and 20 wt% polypropylene glycol. The ethanol purity is 99.5%, the isopropanol purity is 99.9%, and the polypropylene glycol is PPG400. Immerse the dimensionally stable blade wax model in the pretreatment solution at a temperature of 36℃. Use a 40 mm cylindrical stirring rotor for magnetic stirring at a speed of 500 r / min for 15 min. Step 3: Prepare a 5 kg cleaning solution consisting of 65 wt% ethanol, 25 wt% isopropanol, and 10 wt% polypropylene glycol. The ethanol purity is 99.5%, the isopropanol purity is 99.9%, and the polypropylene glycol is PPG400. Transfer the pretreated wax model to an ultrasonic cleaner using a 65 × 45 × 20 mm rectangular plastic box and immerse it in the cleaning solution. The initial ultrasonic cleaning temperature is set to 33℃. During the cleaning process, the solution temperature is monitored in real time, and a temperature interlock control is used: when the solution temperature rises to 36℃, ultrasonic cleaning is immediately paused, and ultrasonic cleaning resumes after the solution temperature drops to 33℃. Additional pauses triggered by temperature protection are not included in the effective ultrasonic working time. The ultrasonic frequency is 120 kHz, the ultrasonic power is 20 W / L, and an intermittent ultrasonic method is used: ultrasonic work for 2 minutes, rest for 1 minute, repeated 5 times, until the supporting wax is completely removed. Step 4: Prepare 5 kg of rinsing solution, consisting of 50 wt% ethanol, 20 wt% isopropanol, and 30 wt% polypropylene glycol. The ethanol purity is 99.5%, the isopropanol purity is 99.9%, and the polypropylene glycol is PPG400. Use a 65 × 45 × 20 mm rectangular plastic box to transfer the ultrasonically cleaned wax model into the rinsing solution. Set the rinsing solution temperature to 36℃. After immersing the leaf in the rinsing solution, begin cooling at a rate of 1℃ / min until it reaches room temperature. Step 5: Remove the wax model and place it in a fume hood with the air velocity set to 0.55 m / s and the room temperature set to 24℃. Allow the rinsing solution to evaporate until there is no oil film on the surface of the wax model. Once the solution on the surface of the wax model has evaporated, a blade wax model with sufficient removal of the supporting wax, stable dimensions, and suitable for precision testing can be obtained.

[0062] Example 3 The post-processing method for improving the dimensional accuracy of wax molds for spray-printed blades in this embodiment includes the following steps: Step 1: Place the printed blade wax model in a constant temperature environment for 12 hours. The ambient temperature of the constant temperature room is set to 23℃. Step 2: Prepare a 5 kg pretreatment solution consisting of 45 wt% ethanol, 35 wt% isopropanol, and 20 wt% polypropylene glycol. The ethanol purity is 99.5%, the isopropanol purity is 99.9%, and the polypropylene glycol is PPG400. Immerse the dimensionally stable blade wax model in the pretreatment solution at 36℃. Use a 40 mm cylindrical stirring rotor for magnetic stirring at 500 r / min for 15 min. Step 3: Prepare a 5 kg cleaning solution consisting of 55 wt% ethanol, 35 wt% isopropanol, and 10 wt% polypropylene glycol. The ethanol purity is 99.5%, the isopropanol purity is 99.9%, and the polypropylene glycol is PPG400. Transfer the pretreated wax model to an ultrasonic cleaner using a 65 × 45 × 20 mm rectangular plastic box and immerse it in the cleaning solution. The initial ultrasonic cleaning temperature is set to 33℃. During the cleaning process, the solution temperature is monitored in real time, and a temperature interlock control is used: when the solution temperature rises to 36℃, ultrasonic cleaning is immediately paused, and ultrasonic cleaning resumes after the solution temperature drops to 33℃. Additional pauses triggered by temperature protection are not included in the effective ultrasonic working time. The ultrasonic frequency is 120 kHz, the ultrasonic power is 20 W / L, and an intermittent ultrasonic method is used: 2 min of ultrasonic work, 1 min of rest, repeated 5 times, until the supporting wax is completely removed. Step 4: Prepare 5 kg of rinsing solution, consisting of 40 wt% ethanol, 30 wt% isopropanol, and 30 wt% polypropylene glycol. The ethanol purity is 99.5%, the isopropanol purity is 99.9%, and the polypropylene glycol is PPG400. Transfer the ultrasonically cleaned wax model to the rinsing solution using a 65 × 45 × 20 mm rectangular plastic box. Set the rinsing solution temperature to 36℃. After immersing the leaf in the rinsing solution, begin cooling at a rate of 1℃ / min until it reaches room temperature. Step 5: Remove the wax model and place it in a fume hood with the air velocity set to 0.55 m / s and the room temperature set to 24℃. Allow the rinsing solution to evaporate until there is no oil film on the surface of the wax model. Once the solution on the surface of the wax model has evaporated, a blade wax model with sufficient removal of the supporting wax, stable dimensions, and suitable for precision testing can be obtained.

[0063] Example 4 The post-processing method for improving the dimensional accuracy of wax molds for spray-printed blades in this embodiment includes the following steps: Step 1: Place the printed blade wax model in a constant temperature environment for 12 hours. The ambient temperature of the constant temperature room is set to 23℃. Step 2: Prepare a 5 kg pretreatment solution consisting of 40 wt% ethanol, 30 wt% isopropanol, and 30 wt% polypropylene glycol. The ethanol purity is 99.5%, the isopropanol purity is 99.9%, and the polypropylene glycol is PPG400. Immerse the dimensionally stable blade wax model in the pretreatment solution at 36℃. Use a 40 mm cylindrical stirring rotor for magnetic stirring at 500 r / min for 15 min. Step 3: Prepare a 5 kg cleaning solution consisting of 50 wt% ethanol, 30 wt% isopropanol, and 20 wt% polypropylene glycol. The ethanol purity is 99.5%, the isopropanol purity is 99.9%, and the polypropylene glycol is PPG400. Transfer the pretreated wax model to an ultrasonic cleaner using a 65 × 45 × 20 mm rectangular plastic box and immerse it in the cleaning solution. The initial ultrasonic cleaning temperature is set to 33℃. During the cleaning process, the solution temperature is monitored in real time, and a temperature interlock control is used: when the solution temperature rises to 36℃, ultrasonic cleaning is immediately paused, and ultrasonic cleaning resumes after the solution temperature drops to 33℃. Additional pauses triggered by temperature protection are not included in the effective ultrasonic working time. The ultrasonic frequency is 120 kHz, the ultrasonic power is 20 W / L, and an intermittent ultrasonic method is used: 2 min of ultrasonic work, 1 min of rest, repeated 5 times, until the supporting wax is completely removed. Step 4: Prepare 5 kg of rinsing solution, consisting of 40 wt% ethanol, 20 wt% isopropanol, and 40 wt% polypropylene glycol. The ethanol purity is 99.5%, the isopropanol purity is 99.9%, and the polypropylene glycol is PPG400. Use a 65 × 45 × 20 mm rectangular plastic box to transfer the ultrasonically cleaned wax model into the rinsing solution. Set the rinsing solution temperature to 36℃. After immersing the leaf in the rinsing solution, begin cooling at a rate of 1℃ / min until it reaches room temperature. Step 5: Remove the wax model and place it in a fume hood with the air velocity set to 0.55 m / s and the room temperature set to 24℃. Allow the rinsing solution to evaporate until there is no oil film on the surface of the wax model. Once the solution on the surface of the wax model has evaporated, a blade wax model with sufficient removal of the supporting wax, stable dimensions, and suitable for precision testing can be obtained.

[0064] Example 5 The post-processing method for improving the dimensional accuracy of wax molds for spray-printed blades in this embodiment includes the following steps: Step 1: Place the printed blade wax model in a constant temperature environment for 12 hours. The ambient temperature of the constant temperature room is set to 24℃. Step 2: Prepare a 5 kg pretreatment solution consisting of 45 wt% ethanol, 30 wt% isopropanol, and 25 wt% polypropylene glycol. The ethanol purity is 99.5%, the isopropanol purity is 99.9%, and the polypropylene glycol is PPG400. Immerse the dimensionally stable blade wax model in the pretreatment solution at 36℃. Use a 40 mm cylindrical stirring rotor for magnetic stirring at 500 r / min for 15 min. Step 3: Prepare a 5 kg cleaning solution consisting of 55 wt% ethanol, 30 wt% isopropanol, and 15 wt% polypropylene glycol. The ethanol purity is 99.5%, the isopropanol purity is 99.9%, and the polypropylene glycol is PPG400. Transfer the pretreated wax model to an ultrasonic cleaner using a 65 × 45 × 20 mm rectangular plastic box and immerse it in the cleaning solution. The initial ultrasonic cleaning temperature is set to 33℃. During the cleaning process, the solution temperature is monitored in real time, and a temperature interlock control is used: when the solution temperature rises to 36℃, ultrasonic cleaning is immediately paused, and ultrasonic cleaning resumes after the solution temperature drops to 33℃. Additional pauses triggered by temperature protection are not included in the effective ultrasonic working time. The ultrasonic frequency is 120 kHz, the ultrasonic power is 20 W / L, and an intermittent ultrasonic method is used: 1 min of ultrasonic work, 1 min of rest, repeated 7 times, until the supporting wax is completely removed. Step 4: Prepare 5 kg of rinsing solution, consisting of 40 wt% ethanol, 25 wt% isopropanol, and 35 wt% polypropylene glycol. The ethanol purity is 99.5%, the isopropanol purity is 99.9%, and the polypropylene glycol is PPG400. Transfer the ultrasonically cleaned wax model to the rinsing solution using a 65 × 45 × 20 mm rectangular plastic box. Set the rinsing solution temperature to 36℃. After immersing the leaf in the rinsing solution, begin cooling at a rate of 1℃ / min until it reaches room temperature. Step 5: Remove the wax model and place it in a fume hood with the air velocity set to 0.55 m / s and the room temperature set to 24℃. Allow the rinsing solution to evaporate until there is no oil film on the surface of the wax model. Once the solution on the surface of the wax model has evaporated, a blade wax model with sufficient removal of the supporting wax, stable dimensions, and suitable for precision testing can be obtained.

[0065] Example 6 The post-processing method for improving the dimensional accuracy of wax molds for spray-printed blades in this embodiment includes the following steps: Step 1: Place the printed blade wax model in a constant temperature environment for 12 hours. The ambient temperature of the constant temperature room is set to 22℃. Step 2: Prepare a 5 kg pretreatment solution consisting of 45 wt% ethanol, 30 wt% isopropanol, and 25 wt% polypropylene glycol. The ethanol purity is 99.5%, the isopropanol purity is 99.9%, and the polypropylene glycol is PPG400. Immerse the dimensionally stable blade wax model in the pretreatment solution at 36℃. Use a 40 mm cylindrical stirring rotor for magnetic stirring at 500 r / min for 15 min. Step 3: Prepare a 5 kg cleaning solution consisting of 55 wt% ethanol, 30 wt% isopropanol, and 15 wt% polypropylene glycol. The ethanol purity is 99.5%, the isopropanol purity is 99.9%, and the polypropylene glycol is PPG400. Transfer the pretreated wax model to an ultrasonic cleaner using a 65 × 45 × 20 mm rectangular plastic box and immerse it in the cleaning solution. The initial ultrasonic cleaning temperature is set to 33℃. During the cleaning process, the solution temperature is monitored in real time, and a temperature interlock control is used: when the solution temperature rises to 36℃, ultrasonic cleaning is immediately paused, and ultrasonic cleaning resumes after the solution temperature drops to 33℃. Additional pauses triggered by temperature protection are not included in the effective ultrasonic working time. The ultrasonic frequency is 120 kHz, the ultrasonic power is 20 W / L, and an intermittent ultrasonic method is used: ultrasonic work for 3 minutes, rest for 1 minute, repeated 3 times, until the supporting wax is completely removed. Step 4: Prepare 5 kg of rinsing solution, consisting of 40 wt% ethanol, 25 wt% isopropanol, and 35 wt% polypropylene glycol. The ethanol purity is 99.5%, the isopropanol purity is 99.9%, and the polypropylene glycol is PPG400. Transfer the ultrasonically cleaned wax model to the rinsing solution using a 65 × 45 × 20 mm rectangular plastic box. Set the rinsing solution temperature to 36℃. After immersing the leaf in the rinsing solution, begin cooling at a rate of 1℃ / min until it reaches room temperature. Step 5: Remove the wax model and place it in a fume hood with the air velocity set to 0.55 m / s and the room temperature set to 24℃. Allow the rinsing solution to evaporate until there is no oil film on the surface of the wax model. Once the solution on the surface of the wax model has evaporated, a blade wax model with sufficient removal of the supporting wax, stable dimensions, and suitable for precision testing can be obtained.

[0066] Example 7 The post-processing method for improving the dimensional accuracy of wax molds for spray-printed blades in this embodiment includes the following steps: Step 1: Place the printed blade wax model in a constant temperature environment for 12 hours. The ambient temperature of the constant temperature room is set to 23℃. Step 2: Prepare a 5 kg pretreatment solution consisting of 45 wt% ethanol, 30 wt% isopropanol, and 25 wt% polypropylene glycol. The ethanol purity is 99.5%, the isopropanol purity is 99.9%, and the polypropylene glycol is PPG400. Immerse the dimensionally stable blade wax model in the pretreatment solution at 36℃. Use a 40 mm cylindrical stirring rotor for magnetic stirring at 500 r / min for 15 min. Step 3: Prepare a 5 kg cleaning solution consisting of 55 wt% ethanol, 30 wt% isopropanol, and 15 wt% polypropylene glycol. The ethanol purity is 99.5%, the isopropanol purity is 99.9%, and the polypropylene glycol is PPG400. Transfer the pretreated wax model to an ultrasonic cleaner using a 65 × 45 × 20 mm rectangular plastic box and immerse it in the cleaning solution. The initial ultrasonic cleaning temperature is set to 33℃. During the cleaning process, the solution temperature is monitored in real time, and a temperature interlock control is used: when the solution temperature rises to 36℃, ultrasonic cleaning is immediately paused, and ultrasonic cleaning resumes only after the solution temperature drops to 33℃. Any additional pauses triggered by temperature protection are not included in the effective ultrasonic working time. The ultrasonic frequency is 80 kHz, and the ultrasonic power is 25 W / L. An intermittent ultrasonic method is used: 2 min of ultrasonic work, 1 min of rest, repeated 5 times, until the supporting wax is completely removed. Step 4: Prepare 5 kg of rinsing solution, consisting of 40 wt% ethanol, 25 wt% isopropanol, and 35 wt% polypropylene glycol. The ethanol purity is 99.5%, the isopropanol purity is 99.9%, and the polypropylene glycol is PPG400. Transfer the ultrasonically cleaned wax model to the rinsing solution using a 65 × 45 × 20 mm rectangular plastic box. Set the rinsing solution temperature to 36℃. After immersing the leaf in the rinsing solution, begin cooling at a rate of 1℃ / min until it reaches room temperature. Step 5: Remove the wax model and place it in a fume hood with the air velocity set to 0.55 m / s and the room temperature set to 24℃. Allow the rinsing solution to evaporate until there is no oil film on the surface of the wax model. Once the solution on the surface of the wax model has evaporated, a blade wax model with sufficient removal of the supporting wax, stable dimensions, and suitable for precision testing can be obtained.

[0067] Example 8 The post-processing method for improving the dimensional accuracy of wax molds for spray-printed blades in this embodiment includes the following steps: Step 1: Place the printed blade wax model in a constant temperature environment for 12 hours. The ambient temperature of the constant temperature room is set to 23℃. Step 2: Prepare a 5 kg pretreatment solution consisting of 45 wt% ethanol, 30 wt% isopropanol, and 25 wt% polypropylene glycol. The ethanol purity is 99.5%, the isopropanol purity is 99.9%, and the polypropylene glycol is PPG400. Immerse the dimensionally stable blade wax model in the pretreatment solution at 36℃. Use a 40 mm cylindrical stirring rotor for magnetic stirring at 500 r / min for 15 min. Step 3: Prepare a 5 kg cleaning solution consisting of 55 wt% ethanol, 30 wt% isopropanol, and 15 wt% polypropylene glycol. The ethanol purity is 99.5%, the isopropanol purity is 99.9%, and the polypropylene glycol is PPG400. Transfer the pretreated wax model to an ultrasonic cleaner using a 65 × 45 × 20 mm rectangular plastic box and immerse it in the cleaning solution. The initial ultrasonic cleaning temperature is set to 33℃. During the cleaning process, the solution temperature is monitored in real time, and a temperature interlock control is used: when the solution temperature rises to 36℃, ultrasonic cleaning is immediately paused, and ultrasonic cleaning resumes after the solution temperature drops to 33℃. Additional pauses triggered by temperature protection are not included in the effective ultrasonic working time. The ultrasonic frequency is 120 kHz, the ultrasonic power is 15 W / L, and an intermittent ultrasonic method is used: 2 min of ultrasonic work, 1 min of rest, repeated 5 times, until the supporting wax is completely removed. Step 4: Prepare 5 kg of rinsing solution, consisting of 40 wt% ethanol, 25 wt% isopropanol, and 35 wt% polypropylene glycol. The ethanol purity is 99.5%, the isopropanol purity is 99.9%, and the polypropylene glycol is PPG400. Transfer the ultrasonically cleaned wax model to the rinsing solution using a 65 × 45 × 20 mm rectangular plastic box. Set the rinsing solution temperature to 36℃. After immersing the leaf in the rinsing solution, begin cooling at a rate of 1℃ / min until it reaches room temperature. Step 5: Remove the wax model and place it in a fume hood with the air velocity set to 0.55 m / s and the room temperature set to 24℃. Allow the rinsing solution to evaporate until there is no oil film on the surface of the wax model. Once the solution on the surface of the wax model has evaporated, a blade wax model with sufficient removal of the supporting wax, stable dimensions, and suitable for precision testing can be obtained.

[0068] Comparative Example 1: The difference from Example 1 is that the constant temperature static stabilization process after printing is cancelled, and the support wax removal operation is carried out directly after the wax model is printed; the wax model is scanned and detected immediately after cleaning, and scanned and detected again at 3 h, 6 h and 9 h respectively to observe the changes in dimensional stability.

[0069] Comparative Example 2: The difference from Example 1 is that the 99.5% pure ethanol in all process solutions of this application is replaced with 97% pure ethanol, while the other components and process parameters remain unchanged.

[0070] Comparative Example 3: The difference from Example 1 is that the 99.9% pure isopropanol in all process solutions of this application is uniformly replaced with 99% pure isopropanol, while the other components and process parameters remain unchanged.

[0071] Comparative Example 4: The difference from Example 1 is that the polypropylene glycol PPG 400 in all process solutions of this application is replaced with polypropylene glycol PPG 800 with a higher molecular weight, while the other components and process parameters remain unchanged.

[0072] Comparative Example 5: The difference from Example 1 is that the polypropylene glycol component in the original composite solution is removed, and all process solution ratios are adjusted to a binary compound system of 50% ethanol + 50% isopropanol, while the other process parameters remain unchanged.

[0073] Comparative Example 6: The difference from Example 1 is that the isopropanol component in the original composite solution is removed, and all process solution ratios are adjusted to a binary compound system of 50% ethanol + 50% polypropylene glycol, while the other process parameters remain unchanged.

[0074] Comparative Example 7: The difference from Example 1 is that the pretreatment softening process is eliminated. After the wax mold size is stabilized, it is directly placed in the ultrasonic cleaning solution for ultrasonic dewaxing.

[0075] Comparative Example 8: The difference from Example 1 is that the wax model was frequently removed during the cleaning process to observe the removal status of the support wax, and no liquid-sealed container was used for protection when transferring it across processes, resulting in the wax model being exposed to air multiple times.

[0076] Comparative Example 9: The difference from Example 1 is that the high-frequency parameters of the ultrasonic cleaning process are replaced with 40 kHz low-frequency ultrasound, while the other ultrasonic parameters, solution ratios and process flow remain unchanged.

[0077] Comparative Example 10: The difference from Example 1 is that the ultrasonic cleaning power density is adjusted from 15-25 W / L to a high-power condition of 40 W / L, while the other ultrasonic parameters, solution ratio and process flow remain unchanged.

[0078] Comparative Example 11: The difference from Example 1 is that the intermittent ultrasonic cleaning mode is cancelled, and continuous ultrasonic cleaning is used for 10 minutes without temperature control intermittent buffering process.

[0079] Comparative Example 12: The difference from Example 1 is that the constant temperature slow rinsing and cooling process is cancelled, and the wax mold is directly rinsed and cooled with 99.5% pure ethanol after ultrasonic cleaning.

[0080] Comparative Example 13: The difference from Example 1 is that the constant temperature ventilation and drying process in the fume hood is cancelled, and after the wax model is rinsed, no residual liquid and oil film evaporation treatment is performed. Instead of letting it stand, it is wiped with a lint-free cloth and powder coating scanning test is carried out directly.

[0081] The surface morphology and final dimensional accuracy of the blade wax models obtained in Examples 1-8 and Comparative Examples 1-13 were observed and tested. The results are shown in Table 1.

[0082] Table 1 Performance Comparison of Examples and Comparative Examples The "immersion time" in Table 1 actually refers to the total time that the blade wax model is in contact with the solutions used in each process. The timing starts when the blade wax model is completely immersed in the pretreatment solution and ends when it is rinsed and removed from the rinsing solution. This includes the pretreatment immersion time, intermittent ultrasonic cleaning time, settling time, rinsing time, and the time spent transferring the wax model while still submerged in the solution. This indicator is set because excessively long solution treatment times may increase the risk of surface defects and dimensional changes in the wax model.

[0083] The "Total Post-Processing Time" in Table 1 refers to the total time elapsed after the blade wax model is printed, including pre-processing, intermittent ultrasonic cleaning, rinsing, ventilation drying, and constant temperature equilibration, until the wax model reaches a state suitable for dimensional inspection or subsequent use. This time includes the processing time for the five steps, as well as the transfer, inspection, and waiting time between each step. "Soaking Time" is a part of the "Total Post-Processing Time".

[0084] The aforementioned defects are primarily identified through visual inspection under uniform conditions, low-magnification observation, and necessary lint-free paper inspection. The specific identification methods are as follows: Pits: After the leaf wax model has been cleaned, rinsed and dried, observe the front and back surfaces, leaf roots, corners and edges of the leaf from different angles under uniform light conditions. If necessary, use low magnification for observation. If there are local depressions on the surface that are visible to the naked eye or under low magnification and are significantly lower than the surrounding surface, it is judged as "having pits"; if no such local depressions are found, it is judged as "no pits".

[0085] Cracks: Visually inspect the surface of the blade wax model and observe it under low magnification. If there are continuous or discontinuous linear cracks on the surface, including fine cracks, obvious cracks, or cracks with local openings, it is judged as "cracked"; if no linear cracks are found, it is judged as "no crack".

[0086] White film on the surface: There is a clear color difference between the wax model and the white film-like residue. After drying, observe the surface of the wax model under uniform lighting conditions; if there is a continuous, sheet-like, or localized white film layer visible to the naked eye, it is judged as "having a white film"; if no white film-like substance is found on the surface, it is judged as "not having a white film".

[0087] Surface oil film: Under uniform lighting conditions, observe the surface of the leaf wax model from different angles. If there is continuous or localized abnormal oily reflection, it is preliminarily determined that an oil film exists. Then, gently press the non-critical surfaces of the wax model with clean, dry, lint-free paper; if transparent or semi-transparent oil spots appear on the lint-free paper, it is determined that "an oil film exists". When there is no abnormal oily reflection on the surface of the wax model, and no oil spots appear after gentle pressing with lint-free paper, it is determined that "no oil film exists".

[0088] Support wax residue: Support wax is pure white, unlike the color of molding wax. After cleaning and rinsing, pay special attention to areas where support wax is likely to remain, such as blade grooves, corners, edges, and narrow gaps. If visible white lumps, flakes, or dots are present, it is considered "support wax residue present"; if no white support wax is found on any visible surface of the wax model, it is considered "no support wax residue." The white film appears as a thin layer adhering to the surface of the molding wax, while support wax residue mainly appears as lumps, flakes, or dots of a certain thickness; the two can be distinguished by their morphology.

[0089] Table 1 shows that the maximum dimensional deviation after post-processing for Examples 1-8 was ±0.06 to ±0.10 mm, all controlled within 0.10 mm; the maximum dimensional deviation for the comparative examples was ±0.13 to ±0.35 mm. This demonstrates that the technical effect of this application is not merely in removing the support wax, but in significantly reducing post-processing errors through multi-step synergistic control, thereby improving the final dimensional accuracy of the blade wax model after support wax removal. Surface defect results further illustrate that cracking, pitting, white film, and oil film are typically accompanied by larger dimensional deviations or detection errors.

[0090] A comparison of Example 1 and Example 2 with increased ethanol content shows that increasing the ethanol ratio can accelerate the removal of support wax and shorten the soaking time. However, excessively rapid solvent exchange increases the risk of local swelling, shrinkage, and crack propagation, causing the final maximum dimensional deviation to increase from ±0.08 mm to ±0.10 mm. Therefore, a balance needs to be struck between the ethanol ratio and dimensional stability.

[0091] A comparison of Example 1 and Example 3, which increased the isopropanol content, shows that isopropanol can regulate the solubility and permeation characteristics of the composite solution. However, excessively high content alters the solvent diffusion balance, accelerating local solvent exchange and causing cracks, ultimately increasing the maximum dimensional deviation to ±0.10 mm. This indicates that isopropanol should be used in conjunction with ethanol and polypropylene glycol, rather than pursuing a high content alone.

[0092] A comparison of Example 1 and Example 4, which increased the polypropylene glycol content, shows that increasing the polypropylene glycol content increases solution viscosity and prolongs processing time, but it slows down the diffusion of small molecule solvents and temperature changes, reducing the maximum dimensional deviation to ±0.06 mm. The trade-off is increased drying time and the potential formation of an oil film; therefore, the polypropylene glycol content needs to balance dimensional accuracy, cleaning efficiency, and drying conditions.

[0093] As can be seen from Examples 1-4, ethanol and isopropanol in the composite solution determine the softening and dissolution rate of the support wax, while polypropylene glycol determines the buffering degree of solvent exchange and evaporation. The synergy of the three components is not simply to pursue the fastest dewaxing, but to control the release of support constraints and the solvent wetting rate, so that the final dimensional deviation is stabilized within 0.10 mm.

[0094] A comparison of Example 1 with Example 5, which uses a short-duration intermittent ultrasonic mode, shows that when the intermittent ultrasonic mode is adjusted to 1 minute of ultrasonic operation followed by 1 minute of rest, the duration of a single continuous ultrasonic action is shortened, the removal rate of the support wax decreases, and the post-processing time is correspondingly extended. However, the resting phase helps release local heat and cavitation impact, reducing wax mold softening and cumulative deformation in thin-walled areas, ultimately reducing the maximum dimensional deviation to ±0.06 mm. This result indicates that, within the limits of production cycle time, using a gentler intermittent ultrasonic mode is beneficial for improving the dimensional accuracy and surface integrity of the blade wax mold.

[0095] A comparison of Example 1 with Example 6, which uses a long-duration intermittent ultrasonic mode, shows that when the intermittent ultrasonic mode is adjusted to 3 minutes of ultrasonic operation followed by 1 minute of rest, the effective ultrasonic action time per unit time increases, the support wax peeling speed accelerates, and the post-processing time can be shortened. However, the longer continuous cavitation effect increases the solution temperature rise and local impact, increasing the risk of wax softening and deformation of thin-walled areas, ultimately increasing the maximum dimensional deviation to ±0.10 mm. Therefore, the intermittent ultrasonic parameters should not only be based on the support wax removal efficiency, but also take into account the surface quality and dimensional stability of the blade wax model.

[0096] A comparison of Example 1 with Example 7, which involved the highest ultrasonic intensity, shows that when the ultrasonic frequency was reduced from 120kHz to 80kHz and the ultrasonic power increased from 20W / L to 25W / L, the cavitation effect and the ability to peel off the support wax were significantly enhanced, and the support wax removal time was shortened. However, the strong cavitation impact had an adverse effect on the surface of the blade wax model and thin-walled areas, resulting in numerous pits on the surface, with the maximum dimensional deviation ultimately being ±0.09 mm. These results indicate that while excessively strong ultrasonic action can improve cleaning efficiency, it is detrimental to maintaining the surface integrity and local contour accuracy of the blade wax model.

[0097] A comparison of Example 1 with Example 8, which uses the lowest ultrasonic intensity, shows that when the ultrasonic power is reduced from 20 W / L to 15 W / L, the local impact caused by the generation and collapse of cavitation bubbles is weakened, resulting in a decrease in the removal rate of the support wax and a corresponding increase in the time required for complete removal. However, the weaker ultrasonic action can reduce pitting on the blade surface and deformation in thin-walled areas, with the final maximum dimensional deviation being ±0.08 mm. These results indicate that weaker ultrasonic parameters are beneficial for protecting the wax mold surface, but the cleaning efficiency is relatively low. Therefore, a comprehensive selection should be made based on the support wax removal efficiency, surface quality, and dimensional accuracy.

[0098] The ultrasonic strategy, frequency, and power collectively determine the removal rate of the support wax and the dimensional changes in the post-processing. Too low a frequency, too high a power, or continuous ultrasonication can increase localized impact, heat accumulation, and softening of the wax. This application limits the ultrasonic frequency to 80–120 kHz, preferably 120 kHz, and the power density to 15–25 W / L, preferably 15–20 W / L, achieving a balance between support removal efficiency and final dimensional accuracy through intermittent operation.

[0099] It should be noted that, within the process scope defined in this application, the ambient temperature, constant temperature placement time, pretreatment temperature, pretreatment soaking time, stirring speed, stirring rotor size, initial temperature of ultrasonic cleaning solution, initial temperature of rinsing solution, fume hood airflow, and rinsing cooling rate are mainly used to maintain the stability of temperature, mass transfer, flow, and drying conditions at each processing stage. When the above parameters vary within the defined range, the impact on the removal effect of the supporting wax on the blade wax mold, the maximum dimensional deviation, and defects such as cracks, pits, white films, or oil films on the surface is relatively small, and will not substantially change the dimensional stability and surface quality improvement effects achieved by the technical solution of this application.

[0100] Therefore, in each embodiment of this application, representative values ​​of the above-mentioned auxiliary process parameters are selected and kept basically consistent. No endpoint values ​​and intermediate values ​​are set for each parameter separately. Each embodiment focuses on examining the influence of major influencing factors such as the composition of the composite solution, the intermittent ultrasonic working mode, and the ultrasonic intensity on the support wax removal efficiency, wax mold dimensional accuracy, and surface integrity.

[0101] A comparison of Example 1 and Comparative Example 1 shows that canceling the constant temperature resting period after printing causes the wax model to undergo solvent treatment before its dimensions have stabilized, resulting in a maximum dimensional deviation of ±0.23 mm after post-treatment. Retaining the supporting wax and resting it at 22–24°C for at least 12 hours allows delayed shrinkage to complete under constraints, establishing a stable dimensional reference, which is the primary step in improving the final accuracy.

[0102] A comparison of Example 1 and Comparative Example 2 shows that as the purity of ethanol decreases, the water content in the solution increases, the removal time of the supporting wax is significantly prolonged, the cumulative residence time of the blades in the solvent increases, and the final maximum dimensional deviation increases to ±0.18 mm. This result indicates that solution purity not only affects cleaning efficiency but also amplifies post-treatment dimensional changes by extending the solvent exposure time.

[0103] A comparison of Example 1 and Comparative Example 3 shows that reduced isopropanol purity alters the polarity and diffusion characteristics of the composite solution, leading to slower removal of the support wax and the presence of residue, ultimately increasing the maximum dimensional deviation to ±0.13 mm. Therefore, stable solvent purity helps ensure dimensional consistency across different batches of post-processing.

[0104] A comparison of Example 1 and Comparative Example 4 shows that replacing PPG400 with the higher viscosity PPG800 significantly reduced solution diffusion, rinsing, and drying rates, resulted in the formation of an oil film on the surface, and ultimately increased the maximum dimensional deviation to ±0.13 mm. This indicates that excessively high viscosity can cause uneven residual liquid and measurement interference, and that PPG400 is more suitable for balancing solvent buffering and final dimensional detection.

[0105] A comparison of Example 1 and Comparative Example 5 shows that, after removing polypropylene glycol, the exchange and evaporation rates of small molecule solvents were too rapid, resulting in cracks, white film, and dimensional deviations in the blades, with the maximum dimensional deviation ultimately reaching ±0.15 mm. The buffering effect of polypropylene glycol on solvent diffusion and evaporation is an important factor in reducing swelling, shrinkage, and measurement errors.

[0106] A comparison of Example 1 and Comparative Example 6 shows that removing isopropanol and increasing the proportion of polypropylene glycol significantly prolonged the removal time of the support wax, resulted in a small amount of residue and oil film, and ultimately achieved a maximum dimensional deviation of ±0.15 mm. This indicates that excessively reducing the solubility will prolong the post-processing load time, which is also detrimental to the final dimensional accuracy.

[0107] A comparison of Example 1 and Comparative Example 7 shows that when pretreatment was omitted and ultrasonication was performed directly, the support wax of different thicknesses could not be released synchronously. Local areas suffered excessive cavitation impact, resulting in cracks and pits, and the maximum dimensional deviation eventually increased to ±0.17 mm. Pretreatment, through uniform softening and pre-wetting, allows for the gradual and synchronous release of the support constraint, which is key to suppressing sudden changes in local dimensions.

[0108] A comparison of Example 1 and Comparative Example 8 shows that frequent removal for observation and transfer to air during the treatment process causes rapid solvent evaporation and repeated rapid cooling and heating, resulting in cracks in the blades and a maximum dimensional deviation of ±0.27 mm. Transferring the blades with liquid and complete immersion throughout the process maintains continuous temperature and wetting conditions, which is a crucial operational feature for improving the accuracy of this method.

[0109] A comparison of Example 1 and Comparative Example 9 shows that 40 kHz low-frequency ultrasound generates larger cavitation bubbles and stronger localized impacts, leading to severe pitting and surface material loss, with a final maximum dimensional deviation reaching ±0.35 mm. Using 80–120 kHz high-frequency ultrasound, especially 120 kHz, can significantly reduce localized erosion and contour errors. Figure 2 As shown, using the post-processing method of Comparative Example 9, the actual dimensions of the blade wax model deviate from the design model, and some local dimensions exceed the allowable tolerance.

[0110] A comparison of Example 1 and Comparative Example 10 shows that high-power ultrasound at 40 W / L significantly increases cavitation impact and surface damage, with a final maximum dimensional deviation of ±0.27 mm. Limiting the power density to 15–25 W / L, preferably 15–20 W / L, can reduce local contour deviations while removing the support wax.

[0111] A comparison of Example 1 and Comparative Example 11 shows that continuous ultrasound causes a sustained increase in the temperature of the cleaning fluid, leading to a decrease in the stiffness of the blade wax material and thermal deformation, with the maximum dimensional deviation eventually reaching ±0.32 mm. Using intermittent ultrasound while maintaining a temperature of 33–36°C can limit heat accumulation and is key to controlling overall bending and torsional errors.

[0112] A comparison of Example 1 and Comparative Example 12 shows that eliminating controlled rinsing and cooling and directly rinsing with high-purity ethanol causes rapid evaporation and a sudden drop in temperature, resulting in blade cracks and ultimately increasing the maximum dimensional deviation to ±0.14 mm. Using a rinsing solution with a high proportion of polypropylene glycol and cooling at 0.8–1.2 °C / min can reduce thermal stress and solvent evaporation shrinkage.

[0113] A comparison of Example 1 and Comparative Example 13 shows that, without constant-temperature uniform drying, the surface oil film and residual liquid cause uneven powder coating thickness and scanning reflection, with a maximum dimensional deviation of ±0.26 mm after post-processing. Thorough drying reduces subsequent dimensional changes caused by residual liquid and improves the accuracy of 3D detection results.

[0114] In summary, this application utilizes a continuous technical chain of "stabilizing dimensional reference—equal wetting and support release—limiting ultrasonic thermal load—controlling cooling gradient—uniform drying" to systematically control shrinkage, swelling, bending, impact erosion, and detection interference during the post-processing of blade wax models. The maximum dimensional deviation in the final embodiment stabilized at ±0.06 to ±0.10 mm, significantly better than the comparative example (±0.13 to ±0.35 mm) where key precision control steps were changed or eliminated. This demonstrates that the method can significantly reduce additional dimensional errors caused by post-processing, improving the final dimensional accuracy of the spray-printed blade wax model while simultaneously removing the support wax, achieving a stable accuracy level of less than 0.10 mm for the final wax model.

[0115] The foregoing has described some specific embodiments of this application. It should be understood that this application is not limited to the specific embodiments described above, and those skilled in the art can make various modifications or variations within the scope of the claims, which do not affect the substantive content of this application. The above-described preferred features can be used in any combination without conflict.

Claims

1. A post-processing method for improving the dimensional accuracy of wax molds for spray-printed blades, characterized in that, include: Maintain the composite state of molding wax and support wax, and place the spray-printed blade wax model in the first constant temperature environment to stand. The wax model of the blade after it has been left to stand is completely immersed in the pretreatment solution at the first temperature; The pretreated blade wax model was immersed in the cleaning solution, and the cleaning temperature was controlled at the second temperature. Intermittent ultrasonic cleaning was performed using a preset frequency and preset power density. After ultrasonication, the leaf wax model was immersed and transferred to a rinsing solution with an initial temperature of the third temperature. The wax model and the rinsing solution were cooled to room temperature simultaneously at a preset cooling rate. After rinsing, place the blade wax model in a second constant temperature environment and dry it at a preset wind speed until there is no residual liquid or oil film on the surface.

2. The method according to claim 1, characterized in that, The temperature of the first constant temperature environment is 22-24℃, and the time spent standing in the first constant temperature environment is not less than 12 hours.

3. The method according to claim 1, characterized in that, The first temperature is 35-37°C, and the immersion time in the pretreatment solution is 10-20 min; The pretreatment solution is composed of 40-55 wt% ethanol, 25-35 wt% isopropanol and 20-30 wt% polypropylene glycol by mass percentage.

4. The method according to claim 1, characterized in that, During the pretreatment process, magnetic stirring is used to promote the flow of the pretreatment solution, and the blade wax model is fixed by a limiting structure or the spatial displacement of the blade wax model is restricted by a container space constraint method.

5. The method according to claim 1, characterized in that, The second temperature is 33–36°C; the preset frequency is 80–120 kHz; and the preset power density is 15–25 W / L. The intermittent ultrasonic cleaning includes: a single ultrasonic cleaning session of 1 to 3 minutes, followed by a 1-minute rest interval and repeated 3 to 7 times.

6. The method according to claim 1, characterized in that, The cleaning solution is composed of 50-65 wt% ethanol, 25-35 wt% isopropanol and 10-20 wt% polypropylene glycol by mass percentage.

7. The method according to claim 1, characterized in that, The third temperature is 35-37℃, and the preset cooling rate is 0.8-1.2℃ / min.

8. The method according to claim 1, characterized in that, The rinsing solution is composed of 35-50 wt% ethanol, 20-30 wt% isopropanol and 30-40 wt% polypropylene glycol by mass percentage.

9. The method according to claim 1, characterized in that, The temperature of the second constant temperature environment is 22-24℃, and the preset wind speed is 0.45-0.55 m / s; The blade wax model was dried using a uniform and continuous ventilation method until there was no oil film or solution residue on the surface, and the temperature was kept balanced in an environment of 22-24℃ before dimensional inspection.

10. The method according to claim 1, characterized in that, During the pretreatment, intermittent ultrasonic cleaning and rinsing processes, the blade wax model is always completely immersed in the corresponding solution; the wax model is transferred between adjacent solution treatment processes using a container with liquid, and the wax model is not exposed to air during the transfer process, and the temperature difference between the solutions in adjacent processes is no more than 4°C.

Citation Information

Patent Citations

  • 3D printing post-processing method for washing supporting wax and polishing model surface layer lines

    CN119636073A