A method for preparing the insulation layer of the expansion section of a solid rocket motor nozzle

By using needle punching and RTM closed-mold injection molding processes, the problems of long production cycle, low material utilization and weak interfacial bonding strength of the insulation layer of the nozzle expansion section of solid rocket motors have been solved, realizing a high-reliability, low-cost and high-efficiency preparation method.

CN123104109APending Publication Date: 2026-11-17SHAANXI PULIMEI MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611453267.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-18
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

The existing manufacturing process for the insulation layer of the nozzle expansion section of solid rocket motors suffers from problems such as long production cycle, low material utilization, weak interfacial bonding strength, and large performance dispersion, resulting in high product reliability and production cost.

Method used

Preforms are prepared using a needle punching process, combined with an RTM closed-mold injection molding process. A three-dimensional mesh structure is formed by needle punching layer by layer, and a thermosetting phenolic resin adhesive is used to achieve mechanical interlocking between the carbon fiber layer and the high silica layer. Near-net-shape forming process is combined to improve the interlayer bonding strength and material utilization.

Benefits of technology

It significantly improves the interlayer bonding strength and interface sealing, enhances the working reliability and material utilization of the product, reduces production costs, and ensures the uniformity and consistency of product performance and production efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123104109A_ABST
    Figure CN123104109A_ABST
Patent Text Reader

Abstract

This invention belongs to the technical field of solid rocket motor composite material component preparation, specifically relating to a method for preparing the insulation layer of the expansion section of a solid rocket motor nozzle. The method first prepares a preform composed of an acrylonitrile carbon fiber layer and a high-silica fiber layer using a needle-punching process. Then, after mold-fitting and airtightness testing, adhesive injection, stepped temperature curing, initial machining, bonding, and final machining, the finished expansion section insulation layer is obtained. This method exhibits high interlayer shear strength and excellent interfacial bonding performance, fundamentally solving the problems of air leakage and interlayer delamination at the composite interface. The product achieves near-net-shape forming, with small machining allowances, low production costs, and closed-mold molding reduces exhaust emissions, making it environmentally friendly.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of solid rocket engine composite material component preparation technology, specifically relating to a method for preparing a heat insulation layer of the nozzle expansion section of a solid rocket engine. Background Technology

[0002] Solid rocket engines are widely used in the aerospace and defense fields due to their advantages such as simple structure, high reliability, convenient maintenance, and long-term storage. The nozzle is the core energy conversion component of a solid rocket engine, converting the thermal and pressure energy of the high-temperature, high-pressure combustion gases generated in the combustion chamber into kinetic energy to produce thrust. The expander section, as a core component of the nozzle, is located downstream of the throat liner. Through gradual expansion of its profile, it accelerates the subsonic combustion gases to supersonic speeds. Its operating environment is extremely harsh, requiring it to withstand the scouring of high-temperature combustion gases (2500–3500°C), high-speed particle erosion, severe temperature gradients, and alternating stress. Therefore, the performance of the expander section's insulation layer directly determines the engine's operational reliability and service life.

[0003] Currently, the thermal insulation layer of the expansion section of high-performance solid rocket motors generally adopts a composite structure of "carbon fiber reinforced phenolic resin (ablation-resistant inner layer) + high silica fiber reinforced phenolic resin (thermal insulation outer layer)". The carbon fiber layer, with its excellent ablation and erosion resistance, directly withstands the high-temperature combustion gases, while the high silica layer, with its low thermal conductivity, provides thermal insulation protection, preventing the nozzle shell temperature from exceeding limits. Existing manufacturing processes for this type of composite expansion section are mainly divided into two categories: compression molding and fabric winding molding, corresponding to the aerospace industry standard QJ2727A-2014 "Specification for Carbon Fiber / Phenolic-High Silica Fiber / Phenolic Composite Compression Products" and the national military standard GJB3402-98 "Specification for Carbon Cloth / Phenolic-High Silica Cloth / Phenolic Composite Wound Products".

[0004] Compression molding uses short fibers or shredded cloth as reinforcement, which are premixed with phenolic resin and then cured under high temperature and pressure in a metal mold. While this process has low raw material costs, it has significant drawbacks: First, the molding process is complex, requiring multiple steps including premixing, pre-compression, molding, and post-curing, typically requiring 2-3 molding cycles to complete the composite structure, resulting in a long production cycle and low efficiency. Second, the interlayer bonding of the short fiber reinforcement is weak, and the fiber orientation is disordered, leading to significant dispersion in the mechanical properties and ablation resistance of the finished product. Third, the interface between the carbon fiber layer and the high-silica layer is physically bonded, resulting in low interfacial bonding strength. Under the thermal stress and airflow scouring during engine operation, interfacial delamination and debonding are highly likely to occur, leading to gas leakage along the interface and causing serious malfunctions such as nozzle shell burn-through, resulting in a high product scrap rate. Fourth, the near-net-shape of the molded product is poor, requiring large machining allowances, and the material utilization rate is typically less than 60%, resulting in high production costs.

[0005] The fabric winding process involves winding resin-impregnated prepreg fabric tape onto a mandrel at a predetermined angle, followed by curing to obtain the finished product. Products prepared using this process exhibit good fiber continuity and excellent mechanical properties, but it suffers from the following drawbacks: First, to ensure proper surface fit and uniform fiber tension during prepreg winding, the overlap must exceed one-third of the finished product thickness, resulting in high raw material consumption. Furthermore, matching the winding tension between high-silica fabric and carbon fabric is challenging, leading to wrinkles, slippage, and poor interlayer consistency at the interface. Second, controlling the resin content during winding is difficult, easily resulting in localized resin deficiency or excess, and high product porosity. Third, during long-term operation, interlayer delamination is prone to occur, especially under alternating temperature and vibration conditions, posing a high risk of interlayer failure. Fourth, the investment in winding equipment is substantial, the process debugging cycle is long, and the production cost for small-batch customized products is high. Summary of the Invention

[0006] The purpose of this invention is to provide a method for preparing the insulation layer of the expansion section of a solid rocket motor nozzle.

[0007] The implementation process of this invention is as follows: A method for preparing a heat insulation layer in the expansion section of a solid rocket motor nozzle includes the following steps: (S1) Preform preparation: (S11) Preparation of acrylonitrile carbon fiber layer: A layer of acrylonitrile carbon fiber cloth is laid on the outer periphery of the needle punching mold, and then a layer of acrylonitrile carbon fiber mesh is laid on the acrylonitrile carbon fiber cloth. The carbon fiber unit layer is formed by needle punching with a needle punching machine. The carbon fiber unit layer is laid layer by layer, and each carbon fiber unit layer is needle punched until the required thickness is reached, thus obtaining the acrylonitrile carbon fiber layer. (S12) Preparation of high silica fiber layer: A layer of high-silica fiber cloth is laid around the acrylonitrile carbon fiber layer, and then a layer of quartz mesh is laid on the high-silica fiber cloth. High-silica fiber unit layers are formed by needle punching. High-silica fiber unit layers are laid layer by layer, and each high-silica fiber unit layer is needle punched until the large end of the needle punching mold reaches the design thickness. High-silica fiber unit layers are laid layer by layer at the small end and middle section of the needle punching mold, and each high-silica fiber unit layer is needle punched until the thickness of the small end and middle section of the needle punching mold is 5-10 mm thicker than the thickness of the large end, thus obtaining the preform. (S2) Mold closing: Clean the mold and apply a release agent. Fit the preform onto the male mold and fix it in place. After installing the sealing strip, close the female mold. Install several ball valves connected to the mold cavity at the bottom and top of the mold. Close the remaining ball valves, open the first ball valve to connect the electronic pressure gauge, and open the second ball valve to connect the nitrogen source. Inject nitrogen into the mold cavity to test the airtightness. After the test is completed, close all ball valves. (S3) Injection of adhesive: Connect the mold inlet to the glue injection machine and the outlet to the negative pressure system. Load the thermosetting phenolic resin into the glue injection machine and preheat both the mold and the thermosetting phenolic resin. After preheating, close the glue injection machine and perform vacuum degassing on the thermosetting phenolic resin and vacuum the mold cavity. Then, open all the outlets of the mold and inject the resin into the mold cavity using nitrogen pressure from the glue injection machine. Maintain the mold temperature during the injection process and perform multiple glue-holding and glue-discharging operations. After completion, close all valves to finish the glue injection. (S4) Curing and preform machining: The mold with the glue injection completed is sent into the oven and the oven program is started to execute the stepped temperature rise curing program. After curing, it is cooled with the oven. When the mold temperature drops to below 50°C, it is demolded to obtain the expansion section composite material blank. Then, according to the design requirements of the insulation layer of the nozzle expansion section, the expansion section composite material blank is machined by CNC lathe to match the assembly dimensions of the inner surface of the nozzle shell. (S5) Bonding: The outer surface of the expanded section composite material blank after machining is roughened by grinding, the inner surface of the nozzle housing is sandblasted, epoxy adhesive is applied to the inner surface of the nozzle housing and the outer surface of the expanded section composite material blank, and it is fixed by bonding fixture. The adhesive is cured at room temperature. After removing the bonding fixture, the expanded section composite material bonded to the inner surface of the nozzle housing is obtained. (S6) Machining: According to the design requirements of the nozzle expansion section insulation layer, the large end face of the expansion section composite material bonded to the inner surface of the nozzle housing is machined by a CNC lathe to obtain the expansion section insulation layer bonded to the inner surface of the nozzle housing.

[0008] Furthermore, in step (S1), the areal density of the acrylonitrile carbon fiber fabric is 150–300 g / m². 2 The tread density of acrylonitrile carbon fiber mesh is 40–100 g / m². 2 The needle density per unit layer is 20–30 needles / cm. 2 .

[0009] Furthermore, in step (S1), each layer of acrylonitrile carbon fiber cloth laid on the outer periphery of the needle punch is made of several fan-shaped acrylonitrile carbon fiber cloths spliced ​​together by bending needles. The overlap width of two adjacent acrylonitrile carbon fiber cloths is 30-80mm, the grout width along the overlap width direction is 5-20mm, and the stitch width between two adjacent bending needle hook points along the overlap direction is 20-70mm. Furthermore, in step (S1), the surface density of the high-silica fiber fabric is 200–300 g / m². 2 The density of quartz mesh tire tread is 40–120 g / m². 2The needle density is 20-30 needles / cm. 2 .

[0010] Further, in step (S1), the needle-punching mold is composed of a nylon mold core and an EVA foam layer bonded to the outer peripheral surface of the nylon mold core. The nylon mold core is a conical core mold, and the thickness of the EVA foam layer is 5-15mm. The outer surface of the needle-punching mold has the same dimensions as the inner surface of the expansion section insulation layer of the target product.

[0011] Further, in step (S2), the mold is cleaned by wiping with alcohol, and the release agent is applied three times, with an interval of 10-15 minutes between each application. The last application is left to dry for no less than 30 minutes. The male mold is consistent with the inner surface of the preform, and the female mold is consistent with the outer surface of the preform. Four ball valves are installed at the bottom of the mold's outlet and four ball valves are installed at the top of the mold's injection port. All ball valves are connected to the inside of the mold cavity. During the airtightness test, nitrogen gas is introduced at a pressure of 0.2-0.5 MPa. The airtightness qualification condition is that the pressure drop is no more than 0.005 MPa within 30 minutes.

[0012] Further, in step (S3), the preheating temperature of the mold is 80-85℃, and the preheating time is 30-90 min; the preheating temperature of the thermosetting phenolic resin is 80-85℃, and the preheating time is 10-15 min; the vacuum degassing pressure is -0.095 to -0.099 MPa, and the degassing time is 5-10 min; the vacuuming pressure of the mold cavity is -0.095 to -0.099 MPa, and the vacuuming time is 5-10 min; during the injection process, the injection rate is 1-5 g / s, the initial pressure of nitrogen pressurization is 0.3-0.4 MPa, and the pressure is increased by 0.05-0.1 MPa every 5-10 min, with the maximum injection pressure not exceeding 1 MPa; the temperature of the mold is not lower than 75℃ throughout the entire injection process.

[0013] Further, in step (S3), the glue-holding and discharging operation process is as follows: First, increase the glue injection pressure to 1-1.1 MPa for the first glue holding for 3-5 minutes. After the first glue holding is completed, open all glue outlets for the first glue discharging. After no air bubbles are discharged, close all glue outlets. Then, increase the glue injection pressure to 1.1-1.2 MPa for the second glue holding for 5-10 minutes. After the second glue holding is completed, open all glue outlets for the second glue discharging. After no air bubbles are discharged, close all glue outlets. Finally, increase the glue injection pressure to 1.2-1.5 MPa for the third glue holding for 10-20 minutes. After the second glue holding is completed, only open the top glue injection outlet for the final glue discharging. After no air bubbles are discharged, close all glue outlets, and the glue injection is completed.

[0014] Furthermore, in step (S4), the stepwise temperature curing procedure is as follows: First, the oven temperature is increased from room temperature to 80°C at a rate of 1–3°C / min, and held for 30–120 min; second, the temperature is increased from 80°C to 100°C at a rate of 0.5–1°C / min, and held for 30–120 min; third, the temperature is increased from 100°C to 120°C at a rate of 0.5–1°C / min, and held for 60–180 min; finally, the temperature is increased from 120°C to 165°C at a rate of 0.5–1°C / min, and held for 120–240 min.

[0015] Further, in step (S5), the process of sandblasting the inner surface of the nozzle housing involves rotating the spray gun at a uniform speed, keeping the nozzle 80-120mm away from the surface, and spraying at an angle of 30°-45°. 20-mesh diamond abrasive is used, and the surface is sanded for 30-40 seconds with compressed air at 0.5-0.6MPa. Then, the two bonding areas are wiped with a degreased cotton cloth soaked in ethyl acetate and allowed to air dry naturally. The adhesive cures for 24-48 hours.

[0016] The positive effects of this invention: (1) High interlayer bonding strength and good interface sealing. The present invention uses needle punching molding process to prepare preforms. Through layer-by-layer needle punching, the fibers form a three-dimensional network structure. The carbon fiber layer and the high silica layer are mechanically interlocked through needle punching. The interface bonding strength is much higher than that of physical bonding molding and winding processes. Combined with RTM closed mold injection molding process, thermosetting phenolic resin glue fully penetrates into the interlayer and interface under pressure to form a continuous resin bonding phase, which fundamentally solves the problems of composite interface delamination and air leakage, and significantly improves the reliability of the product.

[0017] (2) High near-net-shape forming degree and high material utilization rate. The present invention precisely controls the shape and size of the needle-punched preform and combines it with RTM closed mold forming. After the product is cured, the shape is close to the final product size. Only a small amount of machining allowance is required. The material utilization rate can reach more than 85%, which is much higher than the 60% of the molding process and the 70% of the winding process. This greatly reduces the consumption of expensive fiber raw materials and reduces the production cost by more than 30%.

[0018] (3) The product has good uniformity and consistency. The fiber distribution of the needle-punched preform is uniform and the density is controllable. The thermosetting phenolic resin adhesive flows stably and cures uniformly during the RTM injection process, avoiding the problems of interlayer wrinkles and uneven tension in the winding process, as well as the problem of short fiber performance dispersion in the molding process. The product batches have good consistency and stable performance.

[0019] (4) High production efficiency and good environmental protection. The process of this invention is simple. The composite structure can be formed by one closed mold injection, without the need for multiple molding or continuous winding. The production cycle is shortened by more than 40% compared with the traditional process. Moreover, the RTM process is a closed mold molding process, with less volatile matter from the thermosetting phenolic resin, which is environmentally friendly and meets the requirements of green manufacturing.

[0020] (5) It has strong process adaptability and can realize the precise preparation of variable thickness structures. By raising the ply unit layer, the variable thickness structure with thicker small end and thinner large end of the expansion section can be easily realized, which can meet the thermal protection requirements of different parts of the nozzle insulation layer. It has high forming accuracy, smooth surface transition, and no need for complex variable tension winding control. Attached Figure Description

[0021] Figure 1 This is a schematic cross-sectional view of the needle-punching mold. Figure 2 A cross-sectional schematic diagram of an acrylonitrile carbon fiber cloth laid on the outer periphery of a needle-punched die; Figure 3 for Figure 2 A cross-sectional view of a layer of acrylonitrile carbon fiber mesh covering the top layer; Figure 4 A schematic cross-sectional view of the mold for closing the mold. Figure 5 This is a schematic cross-sectional view of the preform after machining following curing. Figure 6 A cross-sectional schematic diagram of the bonding fixture in use; In the figure, 1 is a nylon mold core, 11 is a clamping handle, 2 is an EVA foam layer, 3 is an acrylonitrile carbon fiber layer, 4 is a high silica fiber layer, 21 is a mold base plate, 22 is a male mold, 23 is a female mold, 24 is a mold top plate, 25 is a guide post, 26 is a mold cavity, 27 is a glue injection port, 28 is a glue outlet, 29 is a temperature measuring hole, 30 is a ball valve, 31 is a screw, 32 is a sealing ring, 41 is a lower bonding plate, 42 is a higher bonding plate, 43 is a screw, 44 is a bolt, and 45 is a nozzle housing. Detailed Implementation

[0022] The present invention will be further described below with reference to the embodiments.

[0023] To facilitate a precise understanding of the technical solutions of this invention by those skilled in the art, the technical terms used in this document are explained below in conjunction with industry practice: Resin transfer molding (RTM) involves placing a dry fiber preform in a closed mold, sealing it, and then injecting low-viscosity liquid resin into the mold cavity under pressure and vacuum assistance. After the resin impregnates the fiber preform, it is cured and formed, resulting in products with high dimensional accuracy, smooth surfaces, low porosity, and good environmental performance.

[0024] Unit layer: The smallest structural unit of the needle-punched preform, which is formed by stacking a layer of fiber cloth and a layer of fiber mesh and then fixing them by needle punching; after stacking and needle punching multiple unit layers, a fiber preform with a set thickness is formed, which is the basic structure to ensure layer-by-layer bonding and uniform density.

[0025] Curved needle grouting: Using a hooked needle, the fiber cloth overlap seam is hooked and locked together to sew the two overlapping layers of fiber cloth into one piece. At the same time, the circumferential diameter of the precast body can be precisely controlled by adjusting the overlap amount to ensure the dimensional accuracy of the shape.

[0026] Overlap seams: When two adjacent fan-shaped fiber fabrics are spliced ​​together, the splicing area formed by the overlapping edges is a key structure to ensure the circumferential fiber continuity of the conical preform; evenly distributed overlap seams can avoid local performance weakness caused by concentrated seams.

[0027] Grout width: The total width of the grouting and locking area along the width direction of the overlap joint directly determines the locking strength of the overlap joint; if the width is too large, the forming efficiency will be low, and if it is too small, the locking will be insufficient and the joint will easily open.

[0028] Stitch width: The distance between two adjacent looper hooks along the lap joint direction, which affects the locking density and forming efficiency at the joint; the denser the stitches, the higher the locking strength, but the lower the production efficiency.

[0029] Glue holding-out: The core venting process in RTM glue injection. By increasing the injection pressure, the resin is kept under pressure and impregnated in the mold cavity, forcing the air in the pores to migrate to the outlet. Then the outlet is opened to release the resin containing air bubbles. Multiple cycles can fully remove residual air in the pores of the preform, significantly reducing the porosity of the product.

[0030] Stepped temperature curing: a curing regime that gradually increases temperature in stages. By controlling the heating rate and holding the temperature at each stage, the resin gradually completes the cross-linking reaction, avoiding problems such as concentrated exothermic reaction, excessive internal stress, product cracking, or uneven curing caused by rapid heating. It is a key process to ensure the curing quality of thermosetting resin-based composite materials.

[0031] Near-net-shape forming refers to the process where the dimensions of the formed product are close to the final product dimensions, requiring only a small amount of finishing to meet design requirements. This can significantly reduce machining allowances, reduce material waste, and shorten the production cycle, and is an important development direction for advanced composite material manufacturing.

[0032] The raw materials involved in the method of this invention are all commercially available industrial-grade products. Those skilled in the art can select appropriate types according to performance requirements, as detailed below: Acrylonitrile carbon fiber cloth: plain weave, areal density 150-300 g / m 2With a tensile strength ≥3500MPa and a tensile modulus ≥230GPa, it is used to prepare an ablation-resistant inner layer. Its high modulus and high strength can withstand the erosion of high-speed combustion gases.

[0033] Acrylonitrile carbon fiber mesh: Short fibers are randomly laid out, with an areal density of 40–100 g / m². 2 With a fiber length of 38–51 mm, it is a key raw material for forming a three-dimensional needled structure. During needled insertion, short fibers are carried into the thickness direction to form Z-axis fiber nails, which enhances the interlaminar shear strength.

[0034] High-silica fiber fabric: plain weave, areal density 200-300 g / m² 2 With a SiO2 content ≥96% and a thermal conductivity ≤0.08W / (m·K), the working temperature can reach over 1000℃. It is used to prepare thermal insulation outer layers and achieves thermal protection by virtue of its low thermal conductivity.

[0035] Quartz mesh: High-purity quartz short fibers are laid, with an areal density of 40-120 g / m². 2 The fiber purity is ≥99.9%, and it is used for needle-punching and consolidation of high silica layer unit layers to ensure the interlayer bonding of the insulation layer.

[0036] Thermosetting phenolic resin adhesive: A-stage phenolic resin with a solid content of ≥75%, it is a low-viscosity phenolic resin specifically for RTM potting, with high carbonization rate and excellent ablation resistance after curing.

[0037] Epoxy adhesive: Two-component modified epoxy structural adhesive, paste-like, non-flowing, cures at room temperature, shear strength ≥15MPa, resistant to damp heat aging, used for structural bonding of expansion section insulation layer and nozzle shell.

[0038] Release agent: Silicon-based high-temperature release agent, temperature resistance ≥200℃, uniform film formation, low release force, used for coating the mold surface, facilitates demolding after curing, and avoids product sticking and damage.

[0039] EVA foam: Cross-linked closed-cell foam with a Shore hardness of 35-45 degrees, a thickness of 5-15 mm, and a resilience of ≥70%. It is used for the surface layer of needle punching molds to provide space for needle punching retraction and protect the needles and rigid mold cores.

[0040] Nylon core: Made of PA66 material, tapered structure, precision machined by CNC, with dimensional accuracy ±0.1mm and surface roughness Ra≤1.6μm, providing rigid support for the needle-punched preform and ensuring the dimensional accuracy of the inner surface.

[0041] The main equipment involved in the method of this invention: The equipment used in this invention are all general-purpose equipment in the field of composite material manufacturing, as detailed below: Three-dimensional needle punching machine: needle punching frequency 200-600 times / minute, needle punching depth 0-50mm adjustable, equipped with curved needle hooking head, used for needle punching and forming of precast bodies.

[0042] RTM dispensing machine: Equipped with vacuum degassing and nitrogen pressurization functions, dispensing rate is continuously adjustable from 0.1 to 10 g / s, pressure range is 0 to 2 MPa, metering accuracy is ±1%, used for quantitative resin dispensing.

[0043] Programmable oven: room temperature to 200℃, heating rate adjustable from 0.1℃ to 5℃ / min, with multi-point temperature monitoring and programmable temperature control function, temperature control accuracy ±1℃, used for product curing.

[0044] CNC lathe: machining accuracy ±0.02mm, equipped with special tooling fixtures, used for precision machining of composite material blanks and end faces.

[0045] Sandblasting equipment: pressure adjustable from 0.3 to 0.8 MPa, equipped with a rotary table, used for roughening the bonding surface of metal shells.

[0046] Air tightness testing system: The pressure sensor has an accuracy of 0.001MPa and a data recording function, and is used for mold cavity sealing testing.

[0047] Example 1 Design parameters for the expansion section insulation layer: expansion section throat diameter 42mm, expansion ratio 12, finished product axial length 135mm; acrylonitrile carbon fiber layer thickness 8mm; high silica fiber layer small end thickness 20mm, large end thickness 10mm; finished product total thickness small end 27mm, large end 18mm.

[0048] A method for preparing a heat insulation layer in the expansion section of a solid rocket motor nozzle includes the following steps: (S1) Preform preparation: The core function of this step is to prepare a dry composite fiber preform with a three-dimensional fiber structure, precise dimensions, and strong interlayer bonding, providing a reinforcing skeleton for subsequent RTM glue injection. The preform consists of an inner acrylonitrile carbon fiber layer (ablation-resistant layer) and an outer high-silica fiber layer (thermal insulation layer), both formed using a unit-layer, layer-by-layer needle punching process.

[0049] (S11) Preparation of acrylonitrile carbon fiber layer: A layer of acrylonitrile carbon fiber cloth is laid around the outer periphery of the needle-punching die (see...). Figure 2 Then, a layer of acrylonitrile carbon fiber mesh is laid on the acrylonitrile carbon fiber cloth (see...). Figure 3 The carbon fiber unit layer is formed by needle punching with a needle punching machine. The carbon fiber unit layer is laid layer by layer, and each carbon fiber unit layer is needle punched until the designed thickness is reached to obtain an acrylonitrile carbon fiber layer. The acrylonitrile carbon fiber fabric has a surface density of 200 g / m.2 The tread density of acrylonitrile carbon fiber mesh is 80 g / m². 2 The needle density per unit layer is 25 needles / cm. 2 Each layer of acrylonitrile carbon fiber cloth laid on the outer periphery of the needle punch is made up of several fan-shaped acrylonitrile carbon fiber cloths spliced ​​together by bending needles. The overlap width of two adjacent acrylonitrile carbon fiber cloths is 50mm, the grout width along the overlap width direction is 15mm, and the stitch width between two adjacent bending needle hook points along the overlap direction is 40mm. The purpose of this step is to prepare an ablation-resistant inner layer facing high-temperature combustion gas. The three-dimensional needle-punched structure ensures the interlayer strength and ablation resistance, while the curved needle grouting ensures the circumferential dimensional accuracy.

[0050] The expansion section is conical and cannot be directly covered with a whole piece of fabric. Using fan-shaped fabric overlaps adapts to the conical variable-diameter structure, ensuring circumferential fiber continuity. Evenly distributed overlap seams avoid localized weakness caused by seams concentrated at the same generatrix position, ensuring uniform circumferential mechanical and ablation properties of the precast structure. Curved needle stitching mechanically hooks and locks the two overlapping layers of fiber fabric together, preventing slippage and scattering of the fabric during layup and needle punching, ensuring structural stability. On the laid-up and shaped acrylonitrile carbon fiber fabric, a layer of acrylonitrile carbon fiber mesh is smoothly laid, with the mesh edges aligned with the fiber fabric, free of wrinkles, stacking, and material shortages. The fiber mesh, composed of randomly laid short fibers, is the main source of thickness-direction (Z-direction) fibers during needle punching. During needle punching, the needle carries the short fibers of the mesh into the lower layer of fiber fabric, forming Z-direction fiber studs that connect the two-dimensional fibers in the plane into a three-dimensional whole, significantly improving interlayer shear strength. Needle-punching density is a core parameter affecting the density and interlayer strength of the preform. If the density is too low, there will be insufficient Z-axis fibers, resulting in weak interlayer bonding; if the density is too high, fiber damage will be severe, and the preform will be too dense, which is not conducive to resin impregnation. The needle-punching density of the unit layer is 25 needles / cm. 2 This process balances interlayer bonding strength and resin wettability, representing the optimal range verified through extensive process testing. The layer-by-layer needle punching process creates three-dimensional fiber connections between each unit layer, increasing interlayer shear strength by more than 40% compared to flat lay-up, thus preventing interlayer delamination from the structural root. At the same time, layer-by-layer lay-up allows for precise control of each layer's thickness, ensuring uniform density of the precast structure.

[0051] (S12) Preparation of high silica fiber layer: A layer of high-silica fiber cloth is laid around the acrylonitrile carbon fiber layer, and then a layer of quartz mesh is laid on the high-silica fiber cloth. The high-silica fiber unit layer is formed by needle punching. The high-silica fiber unit layer is laid layer by layer, and each high-silica fiber unit layer is needle punched until the large end of the needle punching mold reaches the design thickness. The high-silica fiber unit layer is laid layer by layer at the small end and middle section of the needle punching mold, and each high-silica fiber unit layer is needle punched until the thickness of the small end and middle section of the needle punching mold is 5-10 mm thicker than the thickness of the large end, thus obtaining the preform. The surface density of the high-silica fiber fabric is 250 g / m². 2 The density of the quartz mesh tread is 80g / m². 2 The needle density is 25 needles / cm². 2 The fabric splicing also adopts a structure of several fan-shaped high-silica fiber fabrics overlapping each other. The overlap seam width between two adjacent acrylonitrile carbon fiber fabrics is 50mm, the grout width along the overlap seam width direction is 15mm, and the stitch width between two adjacent bent needle hook points along the overlap seam direction is 40mm; and the overlap seam and the overlap seam of the carbon fiber layer are staggered by more than 30° in the circumferential direction.

[0052] The needle-punching die consists of a nylon core 1 and an EVA foam layer 2 bonded to the outer peripheral surface of the nylon core (see...). Figure 1 The nylon core 1 has a clamping handle 11 at its large end, which is used to clamp it onto the needle punching machine. The nylon core is a conical core mold, and the EVA foam layer is 10mm thick. The outer surface of the needle punching mold is CNC-machined to match the inner surface dimensions of the expansion section insulation layer of the target product. The nylon core has high strength and high rigidity, providing stable internal support for the preform and ensuring the overall dimensional accuracy of the preform. The EVA foam is an elastic, puncture-resistant layer. During needle punching, the needle penetrates the fiber and then pierces the foam layer by 2-3mm, avoiding direct impact of the needle on the rigid nylon core that could cause needle breakage or mold damage. At the same time, the resilience of the foam helps the fiber maintain a loose, porous structure, which is beneficial for subsequent resin impregnation.

[0053] The purpose of this step is to prepare an outer insulating layer outside the carbon fiber layer. Variable thickness layup meets the insulation requirements of different parts of the expansion section, while interfacial needle punching achieves mechanical interlocking between the two layers. Staggered overlaps prevent seams from overlapping in the same radial position, preventing the formation of through-hole weak channels and significantly improving the overall airtightness and mechanical properties of the structure. If seams are aligned, cracks are prone to form and propagate along the seams during operation, leading to interfacial failure. During needle punching, the needle penetrates the interface between the two layers, bringing high-silica fibers into the carbon fiber layer and vice versa, forming a mechanical interlocking of fibers at the interface. Combined with subsequent RTM resin bonding, the composite interface strength is far higher than that of physically bonded interfaces, fundamentally solving the interfacial delamination and leakage problem of traditional processes. The heat load of the insulation layer in the expansion section is unevenly distributed along the axial direction. The smaller end, closer to the throat liner, has higher gas temperature and heat flux density, requiring a thicker insulation layer; the larger end has lower gas temperature, allowing for a thinner layer to reduce structural weight. Variable thickness layup is achieved by raising the layup unit, which eliminates the need to change the mold, simplifies the process, ensures smooth surface transition, and provides high dimensional accuracy. The 5-10mm thickness difference matches the heat flow distribution pattern of a typical expansion section, balancing thermal protection performance with lightweight structure.

[0054] (S2) Mold closing: Clean the mold and apply a release agent. Fit the preform onto the male mold and fix it in place. After installing the sealing strip, close the female mold. Install several ball valves connected to the mold cavity at the bottom and top of the mold. Close the remaining ball valves, open the first ball valve to connect the electronic pressure gauge, and open the second ball valve to connect the nitrogen source. Inject nitrogen into the mold cavity to test the airtightness. After the test is completed, close all ball valves. The process involved cleaning the mold with alcohol, applying the release agent three times with 12-minute intervals between each application, and allowing it to air dry for at least 30 minutes after the final application. The male mold was aligned with the inner surface of the preform, while the female mold was aligned with the outer surface of the preform. Four ball valves were installed at the bottom of the mold's outlet and four ball valves were installed at the top injection port, with all ball valves connected to the inside of the mold cavity. During the airtightness test, nitrogen gas was introduced at a pressure of 0.4 MPa, and the airtightness was deemed acceptable when the pressure drop was no more than 0.005 MPa within 30 minutes.

[0055] As shown in Figure 4, the mold consists of a mold base plate 21, a male mold 22, a female mold 23, and a mold top plate 24. The male mold 22 has an inverted conical structure, and the female mold 23 has a hollow cylindrical structure. The male mold 22 is installed in the middle of the mold base plate 21. In use, the preform is fitted onto the male mold 22. The female mold 23 is installed around the male mold 22. The lower end of the female mold 23 has a guide hole, which matches and has a clearance fit with the guide post 25 of the mold base plate 21. The mold top plate 26 is then placed on top, and the cavity formed between the male mold 22 and the female mold 23 is the mold cavity 26. The preform is placed inside the mold cavity. The mold top plate 24 is designed with four injection ports 27 communicating with the mold cavity 26, and the mold bottom plate 21 is designed with four outlet ports 28 communicating with the mold cavity. The mold top plate 24 is provided with a temperature measuring hole 29. Ball valves 30 are provided at the inlet of the injection ports 27 and the outlet of the outlet ports 28. The lower ends of the mold bottom plate 21 and the male mold 22 are fixedly connected by screws 31, and the upper ends of the mold top plate 24 and the female mold 23 are fixedly connected by screws 31. Both the mold bottom plate 21 and the female mold 23 are provided with sealing ring mounting grooves, and sealing rings 32 for sealing are installed in the sealing ring mounting grooves.

[0056] The core function of this step is to encapsulate the preform within a closed metal mold, establishing a sealed mold cavity environment. Airtightness testing verifies the reliability of the seal, providing a qualified sealed space for subsequent RTM infusion. Three coats ensure the release agent forms a continuous and uniform film, preventing mold sticking and material shortages on the product surface. Each coat is allowed to dry sufficiently, allowing the solvent to evaporate fully and ensuring the quality of the release agent film. Sufficient drying prevents release agent residue from contaminating the resin, affecting curing quality and interfacial bonding performance. The male mold conforms to the inner surface of the preform, providing internal support and preventing displacement or deformation during infusion. Trimming excess material prevents excess fiber from affecting mold closure and sealing surface fit. Silicone rubber sealing strips ensure the mold cavity is airtight, preventing resin leakage and pressure loss during infusion. Diagonally fastened bolts ensure even stress distribution on the mold and tight sealing surface fit, preventing leakage caused by localized gaps. The multi-point ball valve arrangement enables multi-point injection and discharge of resin, ensuring uniform resin flow within the mold cavity and preventing localized resin shortages or excesses. The bottom and top ball valve arrangements are adapted to the resin filling and flow patterns, facilitating the discharge of air bubbles with the resin flow. Air tightness testing is a critical quality control point in the RTM process. Mold cavity leakage can lead to insufficient injection pressure, inadequate resin wetting, and porosity defects. Using a test pressure higher than the actual injection pressure effectively verifies the reliability of the seal. A pressure drop of no more than 0.005 MPa over 30 minutes is a common acceptance standard for RTM injection processes in the aerospace field, ensuring stable pressure during the injection process.

[0057] (S3) RTM injection: Connect the mold inlet to the injection machine via a high-pressure metal hose, and connect the outlet to the negative pressure system via a high-pressure PU hose. Check that all pipe connections are secure and leak-free. Load the thermosetting phenolic resin into the injection machine and preheat both the mold and the thermosetting phenolic resin. After preheating, close the injection machine and perform vacuum degassing on the thermosetting phenolic resin. After evacuating the mold cavity, open all outlets of the mold and inject the resin into the mold cavity using nitrogen pressure from the injection machine. Maintain mold temperature during the injection process and perform multiple glue-holding and glue-discharging operations. After completion, close all valves to finish the injection process. The preheating temperature of the mold is 82℃, and the preheating time is 50 min; the preheating temperature of the thermosetting phenolic resin is 82℃, and the preheating time is 13 min; the vacuum degassing pressure is -0.095 to -0.099 MPa, and the degassing time is 7 min; the vacuuming pressure of the mold cavity is -0.095 to -0.099 MPa, and the vacuuming time is 7 min; during the injection process, the injection rate is 3 g / s, the initial pressure of nitrogen pressurization is 0.3 MPa, the pressure increases by 0.08 MPa every 7 min, and the maximum injection pressure is no more than 1 MPa; the temperature of the mold is no lower than 75℃ throughout the entire injection process.

[0058] The glue-holding and discharging operation process is as follows: First, increase the glue injection pressure to 1MPa for the first glue-holding for 4 minutes. After the first glue-holding is completed, open all glue outlets for the first glue discharging. After no air bubbles are discharged, close all glue outlets. Then, increase the glue injection pressure to 1.1MPa for the second glue-holding for 7 minutes. After the second glue-holding is completed, open all glue outlets for the second glue discharging. After no air bubbles are discharged, close all glue outlets. Finally, increase the glue injection pressure to 1.2MPa for the third glue-holding for 15 minutes. After the second glue-holding is completed, only open the top glue injection outlet for the final glue discharging. After no air bubbles are discharged, close all glue outlets, and the glue injection is completed.

[0059] The core function of this step is to uniformly inject liquid thermosetting resin into a closed mold cavity under vacuum assistance and nitrogen pressurization, fully impregnating the fiber preform. A stepped pressure-boosting and degassing process is used to thoroughly remove air bubbles from the pores, resulting in a low-porosity composite preform. The inlet uses a high-pressure-resistant metal hose to ensure stable injection pressure; the outlet uses a transparent PU tube for easy observation of resin flow and air bubble status; a unified connection allows for consistent injection and degassing, ensuring uniform pressure in each flow channel. Preheating the mold and resin to the same temperature prevents a sudden increase in resin viscosity due to temperature differences after injection, ensuring resin flowability and wettability. 82℃ is the optimal injection temperature for RTM phenolic resin, balancing low viscosity and curing stability. Slow stirring during resin preheating prevents premature gelation caused by localized overheating, ensuring stable resin processing performance. Resin vacuum degassing removes dissolved and entrained air bubbles from the resin itself, preventing them from entering the mold cavity and causing internal defects. Mold cavity vacuuming removes air from the preform pores and the mold cavity, reducing resin filling resistance and minimizing product porosity. A high vacuum of -0.095 MPa or higher ensures effective venting while preventing excessive solvent evaporation due to a decrease in resin boiling point. Nitrogen pressurization drives the resin, providing stable and controllable pressure and avoiding the pulsation issues associated with mechanical pumps. Low-pressure, low-speed initial injection prevents preform displacement and fiber deformation caused by rapid resin erosion. An injection rate of 1–5 g / s adapts to the wetting speed of preforms with varying thicknesses, ensuring uniform resin propagation and preventing flow front traps that encapsulate air bubbles. Gradual pressurization allows the resin to penetrate the preform's micropores gradually, preventing short-circuiting ("finding") along surface channels caused by rapid high pressure, ensuring sufficient fiber wetting. A maximum pressure not exceeding 1 MPa balances wetting effect and mold sealing requirements. Full mold insulation ensures stable resin viscosity and uniform filling. The core technological innovation of this invention is the three-stage pressure-pressurization-expulsion process. Low-pressure pressurization primarily removes large-pore air bubbles, medium-pressure pressurization penetrates into small pores, and high-pressure pressurization achieves final wetting and compaction. The step-by-step pressure increase conforms to the gas discharge pattern from large pores to small pores, resulting in a much higher venting efficiency than a single-stage pressure-holding process, which can control the porosity of the product to within 1%. The final expulsion only opens the top injection port, utilizing the principle of gas buoyancy to allow any remaining air bubbles to escape from the highest point, ensuring that there are no air bubbles at the top of the mold cavity. The criterion of a liquid level above 40cm ensures that the resin fills the mold cavity with sufficient pressure, avoiding insufficient resin.

[0060] (S4) Curing and preform machining: The mold with the glue applied is placed in an oven, and the oven program is started to execute the stepped temperature curing program; after curing, it is cooled with the oven, and when the mold cools down to below 50°C, it is demolded to obtain the expanded section composite material blank; then, according to the design requirements of the insulation layer of the nozzle expanded section, the expanded section composite material blank is machined on a CNC lathe. Figure 5 This allows it to match the assembly dimensions of the nozzle housing's inner surface. The step-by-step curing procedure is as follows: First, the oven temperature is increased from room temperature to 80℃ at a rate of 2℃ / min, and held for 90 min; then, the temperature is increased from 80℃ to 100℃ at a rate of 0.8℃ / min, and held for 90 min; next, the temperature is increased from 100℃ to 120℃ at a rate of 0.8℃ / min, and held for 110 min; finally, the temperature is increased from 120℃ to 165℃ at a rate of 0.8℃ / min, and held for 180 min.

[0061] The core function of this step is to fully cross-link and cure the resin through a stepped temperature curing regime, forming a composite material preform with excellent mechanical and heat resistance properties. Preliminary processing then ensures it meets assembly dimensional requirements. Stepped temperature curing is crucial for ensuring resin curing quality. The low-temperature stage (80℃) allows the resin to flow slowly, further eliminating micro-bubbles and initiating a preliminary cross-linking reaction. The medium-temperature stage (100-120℃) carries out the main cross-linking reaction; slow heating avoids excessive internal stress and product cracking caused by concentrated exothermic reactions. The high-temperature stage (165℃) completes final curing, achieving a cross-linking degree of over 90%, ensuring the product's mechanical and heat resistance properties. The precise matching of heating rates and holding times at each stage to the curing kinetics of phenolic resin prevents uneven curing or over-curing. Slow cooling in the furnace reduces temperature stress, preventing cracking and deformation due to rapid cooling. Demolding below 50℃ avoids demolding damage caused by insufficient strength at high temperatures, while also ensuring operational safety. Preliminary processing ensures the assembly accuracy of the blank and the shell. Appropriate fitting clearance ensures smooth assembly and uniform adhesive layer thickness. The near-net-shape forming process of this invention results in a machining allowance of only 10% to 15%, which is much smaller than the more than 30% of the traditional process, greatly reducing machining and material waste.

[0062] (S5) Bonding: The outer surface of the machined expansion section composite material blank is roughened by grinding, the inner surface of the nozzle housing is sandblasted, epoxy adhesive is applied to the inner surface of the nozzle housing and the outer surface of the machined expansion section composite material blank, and fixed by bonding fixtures. The adhesive is cured at room temperature. After removing the bonding fixtures, the expansion section composite material bonded to the inner surface of the nozzle housing is obtained. The process of sandblasting the inner surface of the nozzle housing is as follows: the spray gun rotates at a constant speed, the distance between the nozzle and the surface is 100mm, the spray angle is 30°, 20-mesh diamond abrasive is used to polish with 0.5MPa compressed air for 40s, and then the two bonding areas are wiped with degreased cotton cloth soaked in ethyl acetate and allowed to air dry naturally; the curing time of the adhesive is 36h.

[0063] The core function of this step is to firmly bond the expansion section insulation layer to the nozzle shell using epoxy structural adhesive, ensuring interfacial bonding strength and sealing performance to meet the engine's operating requirements. Roughening the bonding surface increases the actual bonding area, creating a mechanical interlocking effect and significantly improving bonding strength. Precise control of sandblasting parameters ensures uniform surface roughness of the shell, avoiding dimensional deviations due to over-blasting or insufficient bonding due to under-blasting. Ethyl acetate wiping thoroughly removes oil and dust, ensuring good wetting of the adhesive and substrate and preventing weak boundary layers at the interface. Using a paste-like epoxy adhesive avoids dripping when applying to vertical conical surfaces, ensuring uniform adhesive layer thickness. Positioning with bonding fixtures ensures assembly coaxiality, preventing uneven adhesive layer thickness caused by eccentricity, which affects bonding strength and sealing performance. Room temperature curing eliminates the need for heating, avoiding the impact of high temperatures on the performance of the phenolic insulation layer. The process is simple and suitable for bonding large-size components. A 36-hour curing time ensures the adhesive reaches maximum bonding strength, meeting structural stress requirements.

[0064] like Figure 6 The bonding fixture consists of a lower bonding plate 41, an upper bonding plate 42, a screw 43, and bolts 44. The nozzle housing 45 is placed on the lower bonding plate 41, the machined expansion section composite material blank is placed on the inner surface of the nozzle housing, the upper bonding plate 42 is placed on the expansion section composite material blank, the lower bonding plate 41 and the upper bonding plate 42 are connected by the screw 43, the bolts 44 are tightened and cured at room temperature, and the bonding fixture is removed after 36 hours.

[0065] (S6) Machining: According to the design requirements of the nozzle expansion section insulation layer, the large end face of the expansion section composite material bonded to the inner surface of the nozzle housing is machined using a CNC lathe to obtain the expansion section insulation layer bonded to the inner surface of the nozzle housing. The density of the expansion section insulation layer is 1.55 g / cm³. 3 .

[0066] The core function of this step is to perform precision machining on the end faces of the components, ensuring that the end faces are flush and that the aerodynamic profile is accurate, thus meeting the overall assembly requirements of the engine. Flush end faces prevent eddies and localized scouring of the gas flow at the outlet, ensuring the integrity of the aerodynamic profile; precision machining ensures the flatness of the end faces, meeting the assembly and sealing requirements with downstream components and preventing gas leakage.

[0067] Performance test results: The average value of the three parallel test samples was 27.9 MPa. There was no leakage at the composite interface under a gas pressure of 1.15 MPa. The porosity of the product was 0.82%. The material utilization rate was 87.2%. The single batch product qualification rate was 97.8%.

[0068] Example 2 A method for preparing a heat insulation layer in the expansion section of a solid rocket motor nozzle includes the following steps: (S1) Preform preparation: (S11) Preparation of acrylonitrile carbon fiber layer: A layer of acrylonitrile carbon fiber cloth is laid on the outer periphery of the needle punching mold, and then a layer of acrylonitrile carbon fiber mesh is laid on the acrylonitrile carbon fiber cloth. The carbon fiber unit layer is formed by needle punching with a needle punching machine. The carbon fiber unit layer is laid layer by layer, and each carbon fiber unit layer is needle punched until the required thickness is reached, thus obtaining the acrylonitrile carbon fiber layer. The acrylonitrile carbon fiber fabric has a surface density of 150 g / m². 2 The tread density of acrylonitrile carbon fiber mesh is 40 g / m². 2 The needle density per unit layer is 20 needles / cm. 2 Each layer of acrylonitrile carbon fiber cloth laid on the outer periphery of the needle punch is made up of several fan-shaped acrylonitrile carbon fiber cloths spliced ​​together by bending needles. The overlap width of two adjacent acrylonitrile carbon fiber cloths is 30mm, the grout width along the overlap width direction is 5mm, and the stitch width between two adjacent bending needle hook points along the overlap direction is 20mm. (S12) Preparation of high silica fiber layer: A layer of high-silica fiber cloth is laid around the acrylonitrile carbon fiber layer, and then a layer of quartz mesh is laid on the high-silica fiber cloth. The high-silica fiber unit layer is formed by needle punching. The high-silica fiber unit layer is laid layer by layer, and each high-silica fiber unit layer is needle punched until the large end of the needle punching mold reaches the design thickness. The high-silica fiber unit layer is laid layer by layer at the small end and middle section of the needle punching mold, and each high-silica fiber unit layer is needle punched until the thickness of the small end and middle section of the needle punching mold is 5-10 mm thicker than the thickness of the large end, thus obtaining the preform. The surface density of the high-silica fiber fabric is 200 g / m². 2 The density of the quartz mesh tread is 40g / m². 2 The needle density is 20 needles / cm². 2 The fabric splicing also adopts a structure of several fan-shaped high silica fiber fabrics overlapping each other. The overlap seam width between two adjacent acrylonitrile carbon fiber fabrics is 30mm, the grout width along the overlap seam width direction is 5mm, and the stitch width between two adjacent bent needle hook points along the overlap seam direction is 20mm; and the overlap seam and the overlap seam of the carbon fiber layer are staggered by more than 30° in the circumferential direction.

[0069] The needle-punching mold consists of a nylon mold core and an EVA foam layer bonded to the outer peripheral surface of the nylon mold core. The nylon mold core is a cone-shaped core mold, and the thickness of the EVA foam layer is 5mm. The outer surface of the needle-punching mold has the same dimensions as the inner surface of the expansion section insulation layer of the target product.

[0070] (S2) Mold closing: Clean the mold and apply a release agent. Fit the preform onto the male mold and fix it in place. After installing the sealing strip, close the female mold. Install several ball valves connected to the mold cavity at the bottom and top of the mold. Close the remaining ball valves, open the first ball valve to connect the electronic pressure gauge, and open the second ball valve to connect the nitrogen source. Inject nitrogen into the mold cavity to test the airtightness. After the test is completed, close all ball valves. The process involves cleaning the mold with alcohol, applying the release agent three times with 10-minute intervals between each application, and allowing it to air dry for at least 30 minutes after the final application. The male mold is aligned with the inner surface of the preform, while the female mold is aligned with the outer surface of the preform. Four ball valves are installed at the bottom of the mold's outlet and four ball valves are installed at the top injection port, with all ball valves connected to the inside of the mold cavity. During the airtightness test, nitrogen gas is introduced at a pressure of 0.2 MPa, and the airtightness is deemed acceptable when the pressure drop is no more than 0.005 MPa within 30 minutes.

[0071] (S3) Injection of adhesive: Connect the mold inlet to the glue injection machine and the outlet to the negative pressure system. Load the thermosetting phenolic resin into the glue injection machine and preheat both the mold and the thermosetting phenolic resin. After preheating, close the glue injection machine and perform vacuum degassing on the thermosetting phenolic resin and vacuum the mold cavity. Then, open all the outlets of the mold and inject the resin into the mold cavity using nitrogen pressure from the glue injection machine. Maintain the mold temperature during the injection process and perform multiple glue-holding and glue-discharging operations. After completion, close all valves to finish the glue injection. The preheating temperature of the mold is 80℃, and the preheating time is 90 min; the preheating temperature of the thermosetting phenolic resin is 80℃, and the preheating time is 10 min; the vacuum degassing pressure is -0.095 to -0.099 MPa, and the degassing time is 5 min; the vacuuming pressure of the mold cavity is -0.095 to -0.099 MPa, and the vacuuming time is 5 min; during the injection process, the injection rate is 1 g / s, the initial pressure of nitrogen pressurization is 0.3 MPa, the pressure increases by 0.05 MPa every 5 min, and the maximum injection pressure is not greater than 1 MPa; the temperature of the mold is not lower than 75℃ throughout the entire injection process.

[0072] The glue-holding and discharging operation process is as follows: First, increase the glue injection pressure to 1MPa for the first glue-holding for 5 minutes. After the first glue-holding is completed, open all glue outlets for the first glue discharging. After no air bubbles are discharged, close all glue outlets. Then, increase the glue injection pressure to 1.1MPa for the second glue-holding for 10 minutes. After the second glue-holding is completed, open all glue outlets for the second glue discharging. After no air bubbles are discharged, close all glue outlets. Finally, increase the glue injection pressure to 1.2MPa for the third glue-holding for 20 minutes. After the second glue-holding is completed, only open the top glue injection outlet for the final glue discharging. After no air bubbles are discharged, close all glue outlets, and the glue injection is completed.

[0073] (S4) Curing and preform machining: The mold with the glue injection completed is sent into the oven and the oven program is started to execute the stepped temperature rise curing program. After curing, it is cooled with the oven. When the mold temperature drops to below 50°C, it is demolded to obtain the expansion section composite material blank. Then, according to the design requirements of the insulation layer of the nozzle expansion section, the expansion section composite material blank is machined by CNC lathe to match the assembly dimensions of the inner surface of the nozzle shell. The step-by-step curing procedure is as follows: First, the oven temperature is increased from room temperature to 80℃ at a rate of 1℃ / min, and held for 120 min; then, the temperature is increased from 80℃ to 100℃ at a rate of 0.5℃ / min, and held for 120 min; next, the temperature is increased from 100℃ to 120℃ at a rate of 0.5℃ / min, and held for 180 min; finally, the temperature is increased from 120℃ to 165℃ at a rate of 0.5℃ / min, and held for 240 min.

[0074] (S5) Bonding: The outer surface of the expanded section composite material blank after machining is roughened by grinding, the inner surface of the nozzle housing is sandblasted, epoxy adhesive is applied to the inner surface of the nozzle housing and the outer surface of the expanded section composite material blank, and it is fixed by bonding fixture. The adhesive is cured at room temperature. After removing the bonding fixture, the expanded section composite material bonded to the inner surface of the nozzle housing is obtained. The process of sandblasting the inner surface of the nozzle housing is as follows: the spray gun rotates at a constant speed, the distance between the nozzle and the surface is 80mm, the spray angle is 45°, 20-mesh diamond abrasive is used to polish with 0.6MPa compressed air for 30s, and then the two bonding areas are wiped with degreased cotton cloth soaked in ethyl acetate and allowed to air dry naturally; the curing time of the adhesive is 24h.

[0075] (S6) Machining: According to the design requirements of the nozzle expansion section insulation layer, the large end face of the expansion section composite material bonded to the inner surface of the nozzle housing is machined by a CNC lathe to obtain the expansion section insulation layer bonded to the inner surface of the nozzle housing.

[0076] Example 3 A method for preparing a heat insulation layer in the expansion section of a solid rocket motor nozzle includes the following steps: (S1) Preform preparation: (S11) Preparation of acrylonitrile carbon fiber layer: A layer of acrylonitrile carbon fiber cloth is laid on the outer periphery of the needle punching mold, and then a layer of acrylonitrile carbon fiber mesh is laid on the acrylonitrile carbon fiber cloth. The carbon fiber unit layer is formed by needle punching with a needle punching machine. The carbon fiber unit layer is laid layer by layer, and each carbon fiber unit layer is needle punched until the required thickness is reached, thus obtaining the acrylonitrile carbon fiber layer. The acrylonitrile carbon fiber fabric has a surface density of 300 g / m. 2 The tread density of acrylonitrile carbon fiber mesh is 100g / m². 2 The needle density per unit layer is 30 needles / cm. 2 Each layer of acrylonitrile carbon fiber cloth laid on the outer periphery of the needle punch is made up of several fan-shaped acrylonitrile carbon fiber cloths spliced ​​together by bending needles. The overlap width of two adjacent acrylonitrile carbon fiber cloths is 80mm, the grout width along the overlap width direction is 20mm, and the stitch width between two adjacent bending needle hook points along the overlap direction is 70mm. (S12) Preparation of high silica fiber layer: A layer of high-silica fiber cloth is laid around the acrylonitrile carbon fiber layer, and then a layer of quartz mesh is laid on the high-silica fiber cloth. The high-silica fiber unit layer is formed by needle punching. The high-silica fiber unit layer is laid layer by layer, and each high-silica fiber unit layer is needle punched until the large end of the needle punching mold reaches the design thickness. The high-silica fiber unit layer is laid layer by layer at the small end and middle section of the needle punching mold, and each high-silica fiber unit layer is needle punched until the thickness of the small end and middle section of the needle punching mold is 5-10 mm thicker than the thickness of the large end, thus obtaining the preform. The surface density of the high-silica fiber fabric is 300 g / m². 2 The density of the quartz mesh tread is 120g / m². 2 The needle density is 30 needles / cm². 2 The fabric splicing also adopts a structure of several fan-shaped high-silica fiber fabrics overlapping each other. The overlap seam width between two adjacent acrylonitrile carbon fiber fabrics is 80mm, the grout width along the overlap seam width direction is 20mm, and the stitch width between two adjacent bent needle hook points along the overlap seam direction is 70mm; and the overlap seam and the overlap seam of the carbon fiber layer are staggered by more than 30° in the circumferential direction.

[0077] The needle-punching mold consists of a nylon mold core and an EVA foam layer bonded to the outer peripheral surface of the nylon mold core. The nylon mold core is a cone-shaped core mold, and the thickness of the EVA foam layer is 15mm. The outer surface of the needle-punching mold has the same dimensions as the inner surface of the expansion section insulation layer of the target product.

[0078] (S2) Mold closing: Clean the mold and apply a release agent. Fit the preform onto the male mold and fix it in place. After installing the sealing strip, close the female mold. Install several ball valves connected to the mold cavity at the bottom and top of the mold. Close the remaining ball valves, open the first ball valve to connect the electronic pressure gauge, and open the second ball valve to connect the nitrogen source. Inject nitrogen into the mold cavity to test the airtightness. After the test is completed, close all ball valves. The process involves cleaning the mold with alcohol, applying the release agent three times with 15-minute intervals between each application, and allowing it to air dry for at least 30 minutes after the final application. The male mold is aligned with the inner surface of the preform, while the female mold is aligned with the outer surface of the preform. Four ball valves are installed at the bottom of the mold's outlet and four ball valves are installed at the top injection port, with all ball valves connected to the inside of the mold cavity. During the airtightness test, nitrogen gas is introduced at a pressure of 0.5 MPa, and the airtightness is deemed acceptable when the pressure drop is no more than 0.005 MPa within 30 minutes.

[0079] (S3) Injection of adhesive: Connect the mold inlet to the glue injection machine and the outlet to the negative pressure system. Load the thermosetting phenolic resin into the glue injection machine and preheat both the mold and the thermosetting phenolic resin. After preheating, close the glue injection machine and perform vacuum degassing on the thermosetting phenolic resin and vacuum the mold cavity. Then, open all the outlets of the mold and inject the resin into the mold cavity using nitrogen pressure from the glue injection machine. Maintain the mold temperature during the injection process and perform multiple glue-holding and glue-discharging operations. After completion, close all valves to finish the glue injection. The preheating temperature of the mold is 85℃, and the preheating time is 30 min; the preheating temperature of the thermosetting phenolic resin is 85℃, and the preheating time is 10 min; the vacuum degassing pressure is -0.095 to -0.099 MPa, and the degassing time is 10 min; the vacuuming pressure of the mold cavity is -0.095 to -0.099 MPa, and the vacuuming time is 10 min; during the injection process, the injection rate is 5 g / s, the initial pressure of nitrogen pressurization is 0.4 MPa, the pressure increases by 0.1 MPa every 10 min, and the maximum injection pressure is not greater than 1 MPa; the temperature of the mold is not lower than 75℃ throughout the entire injection process.

[0080] The glue-holding and discharging operation process is as follows: First, increase the glue injection pressure to 1.1MPa for the first glue-holding for 3 minutes. After the first glue-holding is completed, open all glue outlets for the first glue discharging. After no air bubbles are discharged, close all glue outlets. Then, increase the glue injection pressure to 1.2MPa for the second glue-holding for 5 minutes. After the second glue-holding is completed, open all glue outlets for the second glue discharging. After no air bubbles are discharged, close all glue outlets. Finally, increase the glue injection pressure to 1.5MPa for the third glue-holding for 10 minutes. After the second glue-holding is completed, only open the top glue injection outlet for the final glue discharging. After no air bubbles are discharged, close all glue outlets, and the glue injection is completed.

[0081] (S4) Curing and preform machining: The mold with the glue injection completed is sent into the oven and the oven program is started to execute the stepped temperature rise curing program. After curing, it is cooled with the oven. When the mold temperature drops to below 50°C, it is demolded to obtain the expansion section composite material blank. Then, according to the design requirements of the insulation layer of the nozzle expansion section, the expansion section composite material blank is machined by CNC lathe to match the assembly dimensions of the inner surface of the nozzle shell. The step-by-step curing process is as follows: First, the oven temperature is increased from room temperature to 80℃ at a rate of 3℃ / min, and held for 30 minutes; then, the temperature is increased from 80℃ to 100℃ at a rate of 1℃ / min, and held for 30 minutes; next, the temperature is increased from 100℃ to 120℃ at a rate of 1℃ / min, and held for 60 minutes; finally, the temperature is increased from 120℃ to 165℃ at a rate of 1℃ / min, and held for 120 minutes.

[0082] (S5) Bonding: The outer surface of the expanded section composite material blank after machining is roughened by grinding, the inner surface of the nozzle housing is sandblasted, epoxy adhesive is applied to the inner surface of the nozzle housing and the outer surface of the expanded section composite material blank, and it is fixed by bonding fixture. The adhesive is cured at room temperature. After removing the bonding fixture, the expanded section composite material bonded to the inner surface of the nozzle housing is obtained. The process of sandblasting the inner surface of the nozzle housing is as follows: the spray gun rotates at a constant speed, the distance between the nozzle and the surface is 120mm, the spray angle is 30°, 20-mesh diamond abrasive is used to polish with 0.6MPa compressed air for 30s, and then the two bonding areas are wiped with degreased cotton cloth soaked in ethyl acetate and allowed to air dry naturally; the curing time of the adhesive is 48h.

[0083] (S6) Machining: According to the design requirements of the nozzle expansion section insulation layer, the large end face of the expansion section composite material bonded to the inner surface of the nozzle housing is machined by a CNC lathe to obtain the expansion section insulation layer bonded to the inner surface of the nozzle housing.

[0084] Comparative Example 1 (Traditional short fiber molding process, according to QJ2727A-2014 process specification) Using the exact same design parameters, raw material grades, and finished product size requirements as in Example 1, and employing the short fiber molding process commonly used in the aerospace industry, the specific process is as follows: Carbon fiber chopped short fibers and high-silica chopped short fibers were mixed with phenolic resin in a kneader at a mass ratio of 65:35 to obtain molding materials. The mixing temperature was 60℃ and the mixing time was 20min. First, carbon fiber molding material is added to the mold cavity of the molding die and pre-pressed for 5 minutes under a pressure of 10MPa and a temperature of 80℃ to form the inner layer blank. Add high-silica molding compound, close the mold and heat to 155℃, then mold and cure at 15MPa for 120 minutes; After demolding, the product is transferred to an oven and cured at 180°C for 4 hours. After natural cooling, it is machined to the finished size by removing excess material using a CNC lathe.

[0085] Performance test results: The average value of the three parallel test samples was 15.7 MPa for interlaminar shear strength, and leakage along the interface occurred at a composite interface airtight pressure of 0.45 MPa. The porosity of the product was 3.64%, the material utilization rate was 57.3%, and the single batch product qualification rate was 71.5%.

[0086] Comparative Example 2 (Prepreg tape winding process, according to GJB3402-98 process specification) Using the exact same design parameters, raw material grades, and finished product size requirements as in Example 1, and employing a military-standard prepreg tape winding process, the specific process is as follows: Carbon fiber cloth and high silica cloth were impregnated with phenolic resin to prepare prepreg tapes with a resin content controlled at 35±2% and stored at low temperature. First, wind a layer of carbon fiber onto the conical mandrel. The fabric tape is wound obliquely with an overlap of 40% of the finished thickness and a winding tension of 25N. Wrap layer by layer until the designed thickness is reached. Then wrap the outer layer with high-silica prepreg tape at a tension of 20N, and overlap it to the designed thickness. After winding, the product is placed into the outer mold, heated and pressurized for curing, and then machined to remove excess material at both ends and the outer shape to the finished size after demolding.

[0087] Performance test results: The average value of the three parallel test samples was 20.3 MPa for interlaminar shear strength, 0.65 MPa for composite interface airtightness pressure, and leakage along the interface was observed. The porosity of the product was 2.21%, the material utilization rate was 68.5%, and the single batch product qualification rate was 80.2%. There were obvious wrinkles at the composite interface and poor uniformity of interlaminar thickness.

[0088] Performance Comparison and Analysis: The following comparative data are all original measured data obtained through parallel comparative tests under the same raw material system, the same product design dimensions, and the same environmental conditions. The mechanical property test is based on the three-point bending interlaminar shear strength test method specified in QJ2727A-2014. The air tightness test is based on the general specification for air pressure air tightness test of aerospace composite material components. The porosity test adopts the metallographic microsection statistical method. The material utilization rate is calculated as the ratio of the net weight of the finished product to the total weight of the raw materials input. All data are the arithmetic mean of 3 valid samples. The data distribution conforms to the performance law and test accuracy requirements of the aerospace composite material industry.

[0089] The main performance indicators of Example 1 were compared with those of Comparative Example 1 and Comparative Example 2, and the results are shown in the table below: Based on the comparative results and the analysis of the process mechanism, the following conclusions can be drawn: (1) Significantly improved interlayer bonding strength and interfacial sealing performance: The interlaminar shear strength of the products prepared by the process of this invention is 77.7% higher than that of the traditional short fiber molding process and 37.4% higher than that of the prepreg tape winding process; the composite interface can withstand 1.15MPa air pressure without leakage, which is more than 2.5 times that of the molding process and more than 1.7 times that of the winding process.

[0090] The core reason for the performance improvement lies in the fact that the needle punching process creates continuous Z-axis fiber bridging in the thickness direction. The carbon fiber layer and the high-silica layer achieve mechanical interlocking of fibers through needle punching, rather than the simple physical stacking of traditional processes. Combined with RTM closed-mold pressure infusion, the resin fully penetrates the interface pores and fiber gaps under pressure, forming a composite interface of "fiber mechanical interlocking + resin chemical bonding", fundamentally eliminating the channels for interface delamination and leakage. In contrast, in the molding process, short fibers are stacked randomly, and there is no continuous fiber connection between layers, with the interface relying solely on physical bonding with resin. In the winding process, the layers are stacked in two dimensions, relying solely on interlayer resin bonding, and uneven tension of the fabric tape easily causes interface wrinkles. Therefore, the interface bonding strength and sealing performance are significantly lower than those of the process of this invention.

[0091] (2) The internal quality and uniformity of the product have been greatly improved: The porosity of the product of this invention is only 0.82%, which is 77.5% lower than that of the molding process and 62.9% lower than that of the winding process. It has very few internal defects and good performance uniformity.

[0092] The reason is that this invention employs a combined venting process of "resin vacuum degassing + mold cavity pre-vacuuming + three-stage step-up pressure suffocation and discharge." First, it removes air bubbles trapped in the resin itself, then extracts air from the pores of the preform and the mold cavity. Through step-by-step pressure suffocation, the resin is forced to penetrate deeper into each level of pore, gradually driving residual air bubbles to the discharge port. This venting efficiency is far higher than traditional processes. In contrast, compression molding involves closed-mold pressure forming, making it difficult to completely expel air from the mold cavity, easily leading to pore formation. In the winding process, air easily gets trapped at the overlap of the fabric tape, and the volatile components of the prepreg are difficult to completely expel; therefore, the porosity of both processes is significantly higher than that of the RTM needle punching process of this invention.

[0093] (3) Significant advantages in material utilization and economic benefits: The method of this invention achieves a near-net-shape forming process with a material utilization rate of 87.2%, which is 29.9 percentage points higher than the molding process and 18.7 percentage points higher than the winding process, significantly reducing the consumption of expensive carbon fiber and high-silica fiber raw materials.

[0094] The reasons are as follows: needle-punched preforms allow for precise control of external dimensions, and the dimensions of the finished product after RTM closed molding are close to those of the final product; while molding processes result in large amounts of flash and excess adhesive, and require significant machining allowances for both internal and external surfaces, leading to substantial material waste; and winding processes require an overlap of more than 1 / 3 of the finished product thickness to ensure the performance of the overlap area, with all excess overlap layers ultimately being removed, resulting in significant raw material waste. Meanwhile, this invention increases the product qualification rate to 97.8%, a 26.3 percentage point improvement over molding and a 17.6 percentage point improvement over winding, further reducing scrap costs.

[0095] (4) Better production efficiency and process adaptability: This invention achieves a single-batch production cycle of only 3 days, which is 57.1% shorter than the molding process and 40% shorter than the winding process. The molding process requires multiple steps, including mixing, pre-pressing, molding, and post-curing, and involves a long mold heating and cooling cycle. The winding process involves long tape cutting and winding tension adjustment cycles and requires specialized winding equipment. This invention features a simple process, completing the double-layer composite structure molding in a single mold-closing injection, eliminating the need for specialized winding equipment. Furthermore, variable thickness structures can be easily achieved by adjusting the number of lay-up layers, making it particularly suitable for the efficient preparation of small-batch customized expanded section products.

[0096] (5) Improved environmental friendliness in production: The RTM injection molding process of this invention is a fully closed mold molding process. The resin volatiles are sealed in the mold cavity and only a small amount is collected and processed in an orderly manner during the glue discharge stage. The VOC concentration in the working environment is much lower than that of open mold molding and open mold winding processes, which meets the requirements of green manufacturing and occupational health.

[0097] The above description is merely a preferred embodiment of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention. For example, applying the method of the present invention to other sizes or types of nozzle insulation components, or making conventional adjustments to process parameters, are all equivalent embodiments of the present invention.

Claims

1. A method for preparing a heat insulation layer in the expansion section of a solid rocket motor nozzle, characterized in that, Includes the following steps: (S1) Preform preparation: (S11) Preparation of acrylonitrile carbon fiber layer: A layer of acrylonitrile carbon fiber cloth is laid on the outer periphery of the needle punching mold, and then a layer of acrylonitrile carbon fiber mesh is laid on the acrylonitrile carbon fiber cloth. The carbon fiber unit layer is formed by needle punching with a needle punching machine. The carbon fiber unit layer is laid layer by layer, and each carbon fiber unit layer is needle punched until the required thickness is reached, thus obtaining the acrylonitrile carbon fiber layer. (S12) Preparation of high silica fiber layer: A layer of high-silica fiber cloth is laid around the acrylonitrile carbon fiber layer, and then a layer of quartz mesh is laid on the high-silica fiber cloth. High-silica fiber unit layers are formed by needle punching. High-silica fiber unit layers are laid layer by layer, and each high-silica fiber unit layer is needle punched until the large end of the needle punching mold reaches the design thickness. High-silica fiber unit layers are laid layer by layer at the small end and middle section of the needle punching mold, and each high-silica fiber unit layer is needle punched until the thickness of the small end and middle section of the needle punching mold is 5-10 mm thicker than the thickness of the large end, thus obtaining the preform. (S2) Mold closing: Clean the mold and apply a release agent. Fit the preform onto the male mold and fix it in place. After installing the sealing strip, close the female mold. Install several ball valves connected to the mold cavity at the bottom and top of the mold. Close the remaining ball valves, open the first ball valve to connect the electronic pressure gauge, and open the second ball valve to connect the nitrogen source. Inject nitrogen into the mold cavity to test the airtightness. After the test is completed, close all ball valves. (S3) Injection of adhesive: Connect the mold inlet to the glue injection machine and the outlet to the negative pressure system. Load the thermosetting phenolic resin into the glue injection machine and preheat both the mold and the thermosetting phenolic resin. After preheating, close the glue injection machine and perform vacuum degassing on the thermosetting phenolic resin and vacuum the mold cavity. Then, open all the outlets of the mold and inject the resin into the mold cavity using nitrogen pressure from the glue injection machine. Maintain the mold temperature during the injection process and perform multiple glue-holding and glue-discharging operations. After completion, close all valves to finish the glue injection. (S4) Curing and preform machining: The mold with the glue injection completed is sent into the oven and the oven program is started to execute the stepped temperature rise curing program. After curing, it is cooled with the oven. When the mold temperature drops to below 50°C, it is demolded to obtain the expansion section composite material blank. Then, according to the design requirements of the insulation layer of the nozzle expansion section, the expansion section composite material blank is machined by CNC lathe to match the assembly dimensions of the inner surface of the nozzle shell. (S5) Bonding: The outer surface of the expanded section composite material blank after machining is roughened by grinding, the inner surface of the nozzle housing is sandblasted, epoxy adhesive is applied to the inner surface of the nozzle housing and the outer surface of the expanded section composite material blank, and it is fixed by bonding fixture. The adhesive is cured at room temperature. After removing the bonding fixture, the expanded section composite material bonded to the inner surface of the nozzle housing is obtained. (S6) Machining: According to the design requirements of the nozzle expansion section insulation layer, the large end face of the expansion section composite material bonded to the inner surface of the nozzle housing is machined by a CNC lathe to obtain the expansion section insulation layer bonded to the inner surface of the nozzle housing.

2. The method for preparing the insulation layer of the expansion section of the solid rocket motor nozzle according to claim 1, characterized in that: In step (S1), the areal density of the acrylonitrile carbon fiber cloth is 150 to 300 g / m 2 , the areal density of the acrylonitrile carbon fiber web is 40 to 100 g / m 2 , and the needling density of the unit layer is 20 to 30 needles / cm 2 .

3. The method for preparing the insulation layer of the expansion section of the solid rocket motor nozzle according to claim 1, characterized in that: In step (S1), each layer of acrylonitrile carbon fiber cloth laid on the outer periphery of the needle punch is made up of several fan-shaped acrylonitrile carbon fiber cloths spliced ​​together by bending needles. The overlap width of two adjacent acrylonitrile carbon fiber cloths is 30-80mm, the grout width along the overlap width direction is 5-20mm, and the stitch width between two adjacent bending needle hook points along the overlap direction is 20-70mm.

4. The method for preparing the insulation layer of the solid rocket motor nozzle expansion section according to claim 1, characterized in that: In step (S1), the surface density of the high-silica fiber fabric is 200–300 g / m². 2 The density of quartz mesh tire tread is 40–120 g / m². 2 The needle density is 20-30 needles / cm. 2 .

5. The method for preparing the insulation layer of the expansion section of the solid rocket motor nozzle according to claim 1, characterized in that: In step (S1), the needle-punching mold consists of a nylon mold core and an EVA foam layer bonded to the outer peripheral surface of the nylon mold core. The nylon mold core is a cone-shaped core mold, and the thickness of the EVA foam layer is 5-15mm. The outer surface of the needle-punching mold has the same dimensions as the inner surface of the expansion section insulation layer of the target product.

6. The method for preparing the insulation layer of the expansion section of the solid rocket motor nozzle according to claim 1, characterized in that: In step (S2), the mold is cleaned by wiping with alcohol. The release agent is applied three times, with an interval of 10-15 minutes between each application. The last application is left to dry for at least 30 minutes. The male mold is aligned with the inner surface of the preform, and the female mold is aligned with the outer surface of the preform. Four ball valves are installed at the bottom of the mold's outlet and four ball valves are installed at the top of the mold's injection port. All ball valves are connected to the inside of the mold cavity. During the airtightness test, nitrogen gas is introduced at a pressure of 0.2-0.5 MPa. The airtightness is deemed acceptable when the pressure drop is no more than 0.005 MPa within 30 minutes.

7. The method for preparing the insulation layer of the expansion section of the solid rocket motor nozzle according to claim 1, characterized in that: In step (S3), the preheating temperature of the mold is 80-85℃, and the preheating time is 30-90 min; the preheating temperature of the thermosetting phenolic resin is 80-85℃, and the preheating time is 10-15 min; the vacuum degassing pressure is -0.095 to -0.099 MPa, and the degassing time is 5-10 min; the vacuuming pressure of the mold cavity is -0.095 to -0.099 MPa, and the vacuuming time is 5-10 min; during the injection process, the injection rate is 1-5 g / s, the initial pressure of nitrogen pressurization is 0.3-0.4 MPa, the pressure is increased by 0.05-0.1 MPa every 5-10 min, and the maximum injection pressure is no more than 1 MPa; The temperature of the mold should not be lower than 75℃ throughout the entire injection process.

8. The method for preparing the heat insulation layer of the expansion section of the solid rocket motor nozzle according to claim 1, characterized in that: In step (S3), the glue-holding and discharging operation process is as follows: First, increase the glue injection pressure to 1-1.1 MPa for the first glue holding for 3-5 minutes. After the first glue holding is completed, open all glue outlets for the first glue discharging. After no air bubbles are discharged, close all glue outlets. Then, increase the glue injection pressure to 1.1-1.2 MPa for the second glue holding for 5-10 minutes. After the second glue holding is completed, open all glue outlets for the second glue discharging. After no air bubbles are discharged, close all glue outlets. Finally, increase the glue injection pressure to 1.2-1.5 MPa for the third glue holding for 10-20 minutes. After the second glue holding is completed, only open the top glue injection outlet for the final glue discharging. After no air bubbles are discharged, close all glue outlets, and the glue injection is completed.

9. The method for preparing the heat insulation layer of the expansion section of the solid rocket motor nozzle according to claim 1, characterized in that, In step (S4), the stepwise temperature curing procedure is as follows: First, the oven temperature is increased from room temperature to 80℃ at a rate of 1-3℃ / min, and held for 30-120 min; then, the temperature is increased from 80℃ to 100℃ at a rate of 0.5-1℃ / min, and held for 30-120 min; next, the temperature is increased from 100℃ to 120℃ at a rate of 0.5-1℃ / min, and held for 60-180 min; finally, the temperature is increased from 120℃ to 165℃ at a rate of 0.5-1℃ / min, and held for 120-240 min.

10. The method for preparing the heat insulation layer of the expansion section of the solid rocket motor nozzle according to claim 1, characterized in that: In step (S5), the process of sandblasting the inner surface of the nozzle housing involves rotating the spray gun at a constant speed, keeping the nozzle 80-120mm away from the surface, and spraying at an angle of 30°-45°. 20-mesh diamond abrasive is used, and the surface is sanded for 30-40 seconds with compressed air at 0.5-0.6MPa. Then, the two bonding areas are wiped with a degreased cotton cloth soaked in ethyl acetate and allowed to air dry naturally. The adhesive cures for 24-48 hours.