A low-temperature resistant metal hydraulic hose and its preparation method
By using a composite modified rubber compound and a four-layer brass-plated steel wire reinforcement, the problem of brittleness and leakage in metal hydraulic hoses under extremely cold environments has been solved. This has improved oil resistance, low-temperature flexibility, and weather aging resistance, thus extending service life.
Patent Information
- Application Number
- CN202611364789.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-04
- Publication Date
- 2026-11-17
AI Technical Summary
Existing metal hydraulic hoses are prone to brittleness and leakage in extremely cold environments. It is difficult to balance oil resistance and low-temperature resistance, and their weather resistance is insufficient, resulting in a short service life.
The compound modified rubber compound is made of low acrylonitrile butadiene rubber and low-temperature resistant cis-butadiene rubber, with special plasticizers, reinforcing fillers and aging resistant additives. The inner and outer rubber layers are prepared by high temperature and high pressure segmented mixing process in E-type internal mixer, and reinforced with four layers of brass-plated steel wire reinforcement.
It achieves no cracking or leakage in an environment of -55℃, with minimal decrease in pressure resistance, excellent resistance to hydraulic oil swelling, improved outdoor weather resistance, and extended service life.
Smart Images

Figure CN123104162A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of hydraulic hose technology, specifically relating to a low-temperature resistant metal hydraulic hose and its preparation method. Background Technology
[0002] High-pressure hydraulic oil delivery systems are core power transmission units in modern engineering machinery, mining equipment, aerospace equipment, and cold-region energy development facilities. Their operational reliability directly affects the safety and efficiency of the entire equipment system. Metal hydraulic hoses, as key flexible piping components connecting hydraulic elements in this system, typically consist of a rubber inner layer, a metal wire winding or braiding reinforcement layer, and an outer protective rubber layer. Under high-pressure conditions, they bear the responsibility of safely transmitting hydraulic oil. The rubber layer, as the core functional layer of the hose, directly determines the hose's pressure resistance, sealing reliability, service life, and environmental adaptability, making it the most critical technical component of metal hydraulic hoses.
[0003] Low-temperature resistance is a core performance indicator for the rubber layer in extremely cold operating environments. The glass transition temperature of rubber materials directly determines their flexibility and mechanical retention under low-temperature conditions, thus affecting the hose's bending adaptability, impact resistance, and sealing integrity in low-temperature environments. Furthermore, considering that metal hydraulic hoses are primarily used to transport hydraulic oil, the rubber layer must also possess excellent resistance to mineral hydraulic oil swelling to prevent softening, swelling, delamination, and even failure caused by prolonged contact with hydraulic oil. Outdoor service conditions also require the rubber layer to have excellent resistance to ozone and ultraviolet aging to meet the challenges of long-term service under harsh climatic conditions such as alternating day-night temperature differences, snow cover, and strong ultraviolet radiation at high altitudes.
[0004] In existing technologies, the rubber layer of commercial metal hydraulic hoses generally uses nitrile rubber with a single acrylonitrile content as the main rubber compound, which presents a difficult technical bottleneck to overcome. First, the low-temperature resistance limit of a single nitrile rubber compound is usually only about -40°C. When the ambient temperature is below this threshold, the glass transition temperature of the outer protective rubber is too high, and the molecular chains freeze at low temperatures, losing flexibility and becoming prone to low-temperature brittleness. The inner oil-resistant rubber hardens and breaks under extremely cold conditions, resulting in hydraulic oil leakage. The overall tensile strength and burst pressure resistance of the hose are significantly reduced, making it extremely prone to pipe bursting and leakage under high-pressure conditions, causing equipment shutdown or even safety accidents. Therefore, it cannot meet the usage requirements of extreme cold environments below -40°C, such as polar operations, open-pit oil fields in northern winters, and cold-region mines. Secondly, there is a natural technical contradiction in the rubber industry between oil resistance and low-temperature resistance: high-acrylonitrile nitrile rubber (NBR) contains a large number of polar cyano groups in its molecular chain, which provides excellent barrier properties and resistance to swelling of mineral hydraulic oils. However, its molecular chain is relatively rigid and prone to brittle fracture at low temperatures. On the other hand, low-acrylonitrile NBR, butadiene rubber, and EPDM rubber, while exhibiting good low-temperature toughness and lower glass transition temperatures, have poor resistance to mineral oils due to their molecular structure. After long-term transportation of hydraulic oil, significant swelling, softening, and delamination of the rubber layer can occur. Existing technologies are limited by the intrinsic properties of individual rubber compounds, allowing for a trade-off between oil resistance and low-temperature resistance. They cannot simultaneously meet multiple performance requirements, including long-term oil resistance, flexibility at -55°C, and resistance to outdoor weathering. Furthermore, existing rubber compound preparation processes mostly employ general-purpose plasticizers in combination with ordinary open mills or small internal mixers for room temperature mixing. This results in weak interfacial bonding between different types of rubber molecules, severe phase separation, uncontrollable crosslinking density distribution, and obvious stress concentration points within the rubber compound. Consequently, this leads to insufficient low-temperature impact strength, poor ozone aging resistance, and short long-term fatigue life, making the rubber prone to early cracking and failure under outdoor conditions with alternating day and night temperature differences. In addition, existing weather-resistant aging formulations are relatively crudely designed. Conventional hoses only add a single general-purpose antioxidant, without designing a composite anti-aging system to address the combined aging factors such as ultraviolet radiation, ozone corrosion, and high and low temperature alternating fatigue in extremely cold outdoor environments. After long-term outdoor use, problems such as surface powdering and cracking occur, and after the protective layer fails, the metal reinforcement layer corrodes, significantly shortening the overall service life of the hose. Summary of the Invention
[0005] To address the shortcomings of the existing technology, a low-temperature resistant metal hydraulic hose and its manufacturing method are provided to solve the aforementioned technical problems.
[0006] To solve the above-mentioned technical problems, the technical solution adopted by the present invention is a low-temperature resistant metal hydraulic hose, which consists of a low-temperature resistant and oil-resistant inner rubber layer, four layers of brass-plated steel wire reinforcement, and a low-temperature resistant protective outer rubber layer, arranged sequentially from the inside to the outside; the inner rubber layer and the outer rubber layer are both made of the same composite modified rubber compound vulcanized; the four layers of brass-plated steel wire reinforcement are formed by spirally winding brass-plated steel wire with a diameter of 0.6-0.9mm at a winding angle of 52°-58° with two positive and two negative cross spirals; The composite modified rubber compound comprises, by weight: 100 parts of blended raw rubber matrix, including 60-75 parts of low acrylonitrile butadiene rubber and 25-40 parts of low-temperature resistant cis-butadiene rubber; 12-22 parts of a special low-temperature resistant plasticizer, wherein the special low-temperature resistant plasticizer is diisooctyl adipate polyester low-temperature plasticizer; 45-65 parts of reinforcing filler, including 30-45 parts of carbon black N550 and 15-20 parts of precipitated silica; 3.5-6 parts of a vulcanization crosslinking system, including 1.0-1.8 parts of sulfur, 1.2-2.2 parts of accelerator CZ, 4-6 parts of zinc oxide, and 1-1.5 parts of stearic acid; 2.5-5 parts of a composite aging resistant additive, including 1-2 parts of hindered phenolic antioxidant, 0.5-1 parts of phosphite-assisted antioxidant, and 1-2 parts of ultraviolet absorber; and 1-3 parts of silane coupling agent.
[0007] The preferred weight ratio of the composite modified rubber compound in the aforementioned low-temperature resistant metal hydraulic hose is as follows: 70 parts low-acrylonitrile butadiene rubber, 30 parts low-temperature resistant cis-butadiene rubber; 18 parts diisooctyl adipate polyester low-temperature plasticizer; 38 parts carbon black N550, 17 parts precipitated silica; 1.5 parts sulfur, 1.8 parts accelerator CZ, 5 parts zinc oxide, 1.2 parts stearic acid; 1.5 parts hindered phenolic antioxidant, 0.8 parts phosphite auxiliary antioxidant, 1.7 parts ultraviolet absorber; and 2 parts silane coupling agent. The inner adhesive layer has a wall thickness of 1.2–2.0 mm, and the outer adhesive layer has a wall thickness of 1.5–2.5 mm. The overall glass transition temperature of the hose is ≤-62℃, and after being placed at a constant temperature of -55℃ for 72 hours, it shows no cracks or brittle fractures when bent at 180°.
[0008] The above-mentioned method for preparing low-temperature resistant metal hydraulic hose includes the following steps: Step 1: Use an E-type internal mixer to prepare composite modified rubber compound by high temperature and high pressure segmented mixing. The compound formula is as specified in the above composite modified rubber compound. The mixing is divided into three stages: raw rubber blending and plasticizing, auxiliary agent and filler compounding and dispersion, and low temperature final mixing and addition to the vulcanization system. After the mixing is completed, the rubber sheet is thinly passed through an open mill and left to mature at room temperature. Step 2: Extrude the cured composite modified rubber compound to form a tubular inner rubber layer; Step 3: Wrap four layers of brass-plated steel wire around the outside of the inner tubing core to form a steel wire reinforcement layer; Step 4: Extrude and coat the outside of the steel wire reinforcement layer with the same compound adhesive to form a protective outer adhesive layer; Step 5: The coated tube blank is sent into the vulcanization equipment for continuous steam vulcanization. After vulcanization, it is cooled by water, cut, and metal joints are assembled at both ends to obtain the finished hose.
[0009] In the above-mentioned method for preparing low-temperature resistant metal hydraulic hoses, in the first stage of the internal mixing and plasticizing of raw rubber, the filling coefficient of the E-type closed internal mixer is controlled within the range of 82% to 88%, the rotor speed is 55 to 65 revolutions per minute, cooling water is introduced into the jacket of the mixing chamber in advance for pre-cooling, the first mixing time is 3 to 4 minutes, and the discharge temperature is controlled within the range of 110 to 120 degrees Celsius.
[0010] In the above-mentioned method for preparing low-temperature resistant metal hydraulic hoses, in the two-stage mixing and filler compound dispersion stage of step one, zinc oxide, stearic acid, and silane coupling agent are added sequentially for low-speed mixing. Then, carbon black N550 and precipitated silica reinforcing fillers are added for further mixing. Finally, diisooctyl adipate polyester low-temperature plasticizer and ternary composite anti-aging agent are added for pressurized closed mixing for 3 to 5 minutes. The pressure in the mixing chamber is maintained at 0.4 to 0.6 MPa throughout the process, and the discharge temperature does not exceed 130 degrees Celsius.
[0011] In the above-mentioned method for preparing low-temperature resistant metal hydraulic hoses, in step one, during the three-stage final vulcanization system addition stage, after the second-stage compound rubber is cooled and left to stand for more than 12 hours, it is put back into the internal mixer, sulfur and accelerator CZ are added, and then it is mixed at low temperature and low pressure for 1.5 minutes, with the discharge temperature not exceeding 95 degrees Celsius.
[0012] In the above-mentioned method for preparing low-temperature resistant metal hydraulic hoses, in the first step of the open mill thin-pass sheeting stage, the temperature of the front and rear rollers of the open mill is controlled at 50 to 60 degrees Celsius. First, the thin pass is refined 6 times with a roller gap of 0.8 mm, and then the roller gap is adjusted to 1.8 mm for sheeting. The film is left to mature at room temperature for more than 24 hours.
[0013] In the above-mentioned method for preparing low-temperature resistant metal hydraulic hoses, the inner rubber layer wall thickness is controlled within the range of 1.2 to 2.0 mm during the extrusion molding of the inner rubber layer in step two. The extrusion temperature is 60 to 75°C for the machine body and 70 to 80°C for the die head. The extrusion speed is matched and linked with the linear speed of the subsequent steel wire winding process to achieve continuous production. The surface of the extruded inner rubber layer is free of air holes.
[0014] In the above-mentioned method for preparing low-temperature resistant metal hydraulic hose, step three, the steel wire winding reinforcement layer is made of four layers of brass-plated high-strength steel wire, which is wound in a cross spiral with two positive and two negative directions at a winding angle of 52 to 58 degrees. The diameter of the steel wire is 0.6 to 0.9 mm, the winding tension is uniform, and there are no gaps or gaps between the steel wire and the inner rubber layer, forming a complete composite structure.
[0015] The above-mentioned method for preparing low-temperature resistant metal hydraulic hoses involves extruding the outer rubber layer using the same formula as the inner rubber, with an outer rubber wall thickness of 1.5–2.5 mm completely encasing the steel wire layer; the vulcanization stage uses a horizontal continuous vulcanizing tank with a steam pressure of 0.35 MPa, a vulcanization temperature of 145°C, and a vulcanization time of 35–45 minutes; after vulcanization, the hose is water-cooled to room temperature, and then the metal fittings are cut and assembled.
[0016] The beneficial effects of this invention, a low-temperature resistant metal hydraulic hose and its manufacturing method, are that it extends the lower limit of the hose's stable operating temperature from -40℃ to -55℃. In extremely cold environments at -55℃, it exhibits no brittleness or leakage, and the pressure resistance attenuation is controlled within 7.2%. After being placed at a constant temperature of -55℃ for 72 hours, the finished hose shows no cracks or brittle fracture when bent at 180°, and the burst pressure decreases by only 7.2%. In contrast, existing conventional hoses develop surface micro-cracks at -40℃ and directly break and leak when bent below -40℃, with a pressure resistance attenuation exceeding 33%.
[0017] This invention simultaneously achieves excellent resistance to hydraulic oil swelling and low-temperature flexibility, eliminating the technical conflict between the two properties. After immersion in hydraulic oil for a preset period of time, the volumetric swelling rate of the rubber compound is controlled within a preset range, while the low-temperature impact toughness at a preset temperature is not lower than a preset value. In contrast, the swelling rate of existing single cold-resistant rubbers is not lower than a preset percentage, and the low-temperature impact toughness of existing single oil-resistant nitrile rubbers does not exceed a preset value.
[0018] The E-type intensive high-temperature and high-pressure mixing process improves the interfacial compatibility of the two rubbers, precisely controls the crosslinking density, and enhances the overall mechanical strength of the compound. After E-type high-temperature and high-pressure intensive mixing, the rubber two-phase interface is free of stratification, and the microstructure is uniformly dispersed. The tensile strength and elongation at break are not lower than the preset values. Conventional mixing processes, using the same raw materials, only achieve tensile strengths within the preset range and exhibit significant phase separation defects.
[0019] The combination of a complex antioxidant and UV-stabilized formula significantly improves outdoor weather resistance and ozone aging resistance, extending the service life of the hose. After a preset time of accelerated UV-ozone aging test, the rubber surface showed no cracking, and the tensile strength retention rate was no less than the preset percentage. Conventional single-antioxidant formulas, after the same aging process, only retain the preset percentage of strength, exhibit large-area surface cracking, and the metal wires are prone to corrosion and failure.
[0020] The entire mixing, extrusion, and vulcanization process can be implemented by modifying existing hydraulic hose production lines without replacing large equipment, thus improving production efficiency. The overall cost of raw materials only increases moderately, balancing performance improvement with mass production economics. Attached Figure Description
[0021] Figure 1 This is a process flow diagram of the present invention; Figure 2 This is a flow chart of the high-temperature and high-pressure segmented mixing process of the E-type internal mixer. Detailed Implementation
[0022] The present invention will now be described in detail with reference to the accompanying drawings and specific embodiments. Example 1
[0023] A low-temperature resistant metal hydraulic hose comprises, from the inside out, a low-temperature resistant and oil-resistant inner rubber layer, four layers of brass-plated steel wire reinforcement, and a low-temperature resistant protective outer rubber layer; both the inner and outer rubber layers are vulcanized from the same composite modified rubber compound; the four layers of brass-plated steel wire reinforcement are formed by spirally winding brass-plated steel wire with a diameter of 0.6-0.9 mm at a winding angle of 52°-58° with two positive and two negative cross spirals. The composite modified rubber compound comprises, by weight, the following components: 100 parts of blended raw rubber matrix. This matrix is composed of low-acrylonitrile butadiene rubber and low-temperature resistant butadiene rubber blended in a specific ratio. The low-acrylonitrile butadiene rubber accounts for 60 to 75 parts, and the low-temperature resistant butadiene rubber accounts for 25 to 40 parts. The low-acrylonitrile butadiene rubber contains a suitable amount of cyano groups in its molecular chain. These polar groups can form a barrier effect with mineral hydraulic oil molecules, effectively inhibiting the penetration and swelling of hydraulic oil into the rubber compound, thereby ensuring the dimensional stability and structural integrity of the inner rubber layer of the hose under long-term contact with hydraulic oil. The low-temperature resistant butadiene rubber has extremely high flexibility in its molecular chain, with a glass transition temperature as low as -100 degrees Celsius. When the hose is in an extremely cold environment, this rubber phase can maintain the mobility of chain segments, giving the rubber compound excellent low-temperature impact toughness, absorbing the energy of microcrack propagation caused by low-temperature stress concentration, and preventing brittle fracture. When two types of rubber are blended within a specific ratio range, they can form a composite structure of continuous and dispersed phases at the microscale: the low acrylonitrile butadiene rubber forms a continuous oil-resistant network, and the cis-butadiene rubber microphase is uniformly dispersed in the network. When the rubber compound is subjected to low-temperature impact, the dispersed phase particles can effectively passivate the crack tip and prevent the rapid propagation of the crack, thereby solving the contradiction of oil resistance and low-temperature resistance that is difficult to balance in traditional technologies at the molecular level.
[0024] A specialized low-temperature resistant plasticizer is used, with a dosage of 12 to 22 parts. This invention selects diisooctyl adipate polyester low-temperature plasticizer. This plasticizer belongs to the long-chain polyester compound category. Its long-chain alkyl groups can insert into the segments of rubber macromolecules, reducing van der Waals forces and entanglement density between molecular chains, thereby significantly lowering the overall glass transition temperature of the composite rubber compound. Compared with conventional phthalate plasticizers, diisooctyl adipate polyester plasticizer exhibits excellent compatibility with nitrile rubber and butadiene rubber, and is less prone to exudation migration or plasticizing efficiency degradation at extremely low temperatures. When the temperature drops to -55 degrees Celsius, the rubber compound modified with this plasticizer still maintains a highly elastic state; the chain movement of the rubber macromolecules is not frozen, fundamentally eliminating the risk of low-temperature brittleness.
[0025] The reinforcing filler, in total quantities of 45 to 65 parts, is composed of carbon black N550 and precipitated silica. Carbon black N550, at 30 to 45 parts, primarily functions to form a complete filler network structure within the rubber matrix, providing the main reinforcing effect and significantly improving the tensile strength, tear resistance, and abrasion resistance of the rubber compound. Precipitated silica, at 15 to 20 parts, has a fine particle size and large specific surface area, filling the voids between carbon black aggregates, improving the dispersion of the filler in the rubber matrix, and reducing stress concentration defects caused by filler agglomeration. Simultaneously, the silanol groups on the silica surface can chemically react with silane coupling agents to form chemical bonds, further enhancing the bonding force between the filler and the rubber interface. The synergistic effect of carbon black and silica creates a three-dimensional network structure in the reinforcing filler system, effectively hindering the free movement of rubber molecular chains. While improving the strength of the rubber compound, it also moderately adjusts the hardness and tensile stress at a given elongation, resulting in balanced mechanical properties in the final hose product.
[0026] The total amount of the vulcanization crosslinking system is 3.5 to 6 parts. This system includes four compounding agents: sulfur, accelerator CZ, zinc oxide, and stearic acid. Sulfur is used in amounts of 1.0 to 1.8 parts, acting as a vulcanization crosslinking agent. Under heating conditions, it undergoes an addition reaction with the double bonds of rubber macromolecules to form a polysulfide crosslinking network, connecting linear rubber molecules into a three-dimensional network structure, giving the rubber compound permanent elastic memory and shape stability. Accelerator CZ is used in amounts of 1.2 to 2.2 parts. Its function is to accelerate the reaction rate between sulfur and rubber, lower the activation energy required for the vulcanization reaction, and ensure that the crosslinking reaction is completed quickly within the process-controllable temperature range. It also promotes the uniform distribution of crosslinking bonds, preventing excessively high local crosslinking density that could lead to hardening and brittleness of the rubber compound. Zinc oxide is used in amounts of 4 to 6 parts, acting as a vulcanization activator. On one hand, it reacts with stearic acid to form zinc stearate, a compound that is an excellent activator carrier for accelerator CZ. On the other hand, it neutralizes trace amounts of acidic substances generated during rubber mixing and storage, preventing premature aging of the rubber compound. The amount of stearic acid used is 1 to 1.5 parts. One end of its molecule is a long-chain alkyl group and the other end is a carboxyl functional group. This amphiphilic structure allows stearic acid to be uniformly dispersed in the rubber system. Its carboxyl group reacts with zinc oxide to generate zinc stearate activator, while its alkyl chain plays an internal lubricating role, improving the processing fluidity and demolding performance of the rubber compound.
[0027] A composite anti-aging additive, with a total amount of 2.5 to 5 parts. This system is composed of three components: hindered phenolic antioxidant, phosphite co-antioxidant, and UV-531 ultraviolet absorber. The hindered phenolic antioxidant is used in an amount of 1 to 2 parts. The hindered phenolic hydroxyl groups in its molecular structure can capture free radicals generated during the thermo-oxidative aging of rubber, interrupt the free radical chain reaction, thereby inhibiting the oxidative degradation of rubber macromolecules and extending the thermo-aging life of the rubber compound. The phosphite co-antioxidant is used in an amount of 0.5 to 1 part. Its main function is to decompose the hydroperoxides generated during the rubber oxidation process, reducing harmful peroxides to harmless alcohol compounds, and avoiding the autocatalytic degradation reaction caused by the accumulation of peroxides. The hindered phenolic antioxidant and the phosphite co-antioxidant form a synergistic effect in the anti-aging mechanism. The former blocks the free radical chain reaction, and the latter eliminates the hidden danger of hydroperoxides. The combination of the two can significantly improve the thermo-oxidative aging resistance of the rubber compound under high temperature and low temperature alternating environments. The UV-531 ultraviolet absorber is used in quantities of 1 to 2 parts. Its molecular structure can efficiently absorb ultraviolet light with wavelengths of 290 to 400 nanometers, converting the energy of ultraviolet photons into harmless heat energy. This prevents ultraviolet light from directly acting on rubber macromolecules and causing photo-oxidation reactions that lead to surface powdering and cracking. This ternary composite anti-aging system provides a comprehensive protection solution for rubber products that may suffer from thermo-oxidative aging, ozone corrosion, and ultraviolet radiation in extremely cold outdoor environments.
[0028] A silane coupling agent is used in an amount of 1 to 3 parts. This invention selects silane coupling agent KH-550 as a processing aid. One end of the molecule of this coupling agent has an ethoxysilane functional group, which can undergo hydrolysis in the presence of water to generate silanol groups. These silanol groups further undergo condensation and dehydration reactions with silanol groups on the surface of silica to form strong siloxane covalent bonds. The other end has an amino functional group, which can physically entangle with rubber macromolecules and exhibit certain chemical interactions. Through the bridging effect of the silane coupling agent, a dual interfacial bond of chemical bonding and physical entanglement is formed between the silica filler and the rubber matrix, effectively enhancing the reinforcing efficiency of the filler on the rubber, while improving the processing fluidity of the rubber compound and reducing mixing energy consumption and extrusion resistance.
[0029] In a preferred embodiment, the specific weight parts of each component are as follows: 70 parts of low-acrylonitrile butadiene rubber, 30 parts of low-temperature resistant cis-butadiene rubber, 18 parts of diisooctyl adipate low-temperature plasticizer, 38 parts of carbon black N550, 17 parts of precipitated silica, 1.5 parts of sulfur, 1.8 parts of accelerator CZ, 5 parts of zinc oxide, 1.2 parts of stearic acid, 1.5 parts of hindered phenolic antioxidant, 0.8 parts of phosphite, 1.7 parts of UV-531 ultraviolet absorber, and 2 parts of silane coupling agent KH-550. This preferred ratio achieves an optimal balance of synergistic effects among the components, ensuring good oil resistance, low-temperature flexibility, and weather aging resistance while possessing good processing adaptability and economy.
[0030] The core technological innovation of this invention lies in the use of a high-temperature, high-pressure, segmented mixing process with an E-type internal mixer to prepare composite modified rubber compounds. This process achieves uniform blending of two rubbers with different polarities, efficient dispersion of fillers and plasticizers, and precise control of crosslinking density by precisely controlling the operating parameters of the internal mixer and the segmented operation process, thereby obtaining a composite rubber compound with uniform microstructure and excellent macroscopic properties.
[0031] Step 1: Equipment Pre-treatment Stage. Before starting the formal mixing operation, the E-type closed internal mixer needs to undergo thorough equipment condition debugging and pre-preparation. The filling coefficient of the internal mixer should be precisely controlled within the optimal process window of 82% to 88%. The filling coefficient refers to the ratio of the total volume of the material fed into the mixing chamber to the effective volume of the mixing chamber. This parameter directly affects the tumbling, shearing, and dispersion efficiency of the material during the mixing process. When the filling coefficient is too low, the number of shearing operations of the mixing rotor on the material decreases, and the mixing uniformity declines; when the filling coefficient is too high, the material in the mixing chamber becomes too crowded, and the shearing stress cannot be effectively transferred, which also leads to the deterioration of the mixing quality. Through extensive process experiments, this invention has verified that a filling coefficient range of 82% to 88% can enable the material to form the optimal tumbling and shearing motion state in the mixing chamber. The rotor speed of the internal mixer should be set to 55 to 65 revolutions per minute. This speed range can provide sufficient shearing and mixing energy without causing excessive temperature rise and premature scorching of the material due to excessive speed. Cooling water should be introduced into the mixing chamber jacket for pre-cooling before the mixing operation begins, so that the temperature of the mixing chamber wall is reduced to the initial state required by the process, avoiding material adhesion to the chamber wall and affecting heat transfer efficiency and mixing uniformity. The closed chamber structure of the E-type internal mixer can maintain a constant internal pressure of 0.4 to 0.6 MPa during the mixing process. The high-pressure environment forces the material to generate strong extrusion and shearing action between the rotor gap, the chamber wall and the material interior, promoting full mixing and interfacial fusion between different components.
[0032] The first stage is the internal mixing, also known as the raw rubber blending and plasticizing stage. After equipment pretreatment, low-acrylonitrile nitrile rubber and low-temperature resistant butadiene rubber are fed into the internal mixer according to a preset ratio. The two rubbers are plasticized and blended under closed pressure for 3 to 4 minutes. The core objective of this stage is to ensure that the macromolecules of the two rubbers fully interpenetrate and fuse under high temperature and high pressure, eliminating the tendency for macromolecular phase separation caused by the polarity difference between the two rubbers. The mechanical shear force and thermal effect during the mixing process give the rubber macromolecular chain segments sufficient activation energy, enabling them to intertwine and penetrate across the rubber phase interface. The discharge temperature should be strictly controlled within the range of 110 to 120 degrees Celsius. This temperature ensures that the rubber macromolecules have sufficient mobility to complete the interfacial fusion, while preventing thermal degradation of the rubber molecular chains or premature volatilization of plasticizers due to excessive temperature. When the internal mixer discharges the rubber, the material presents a homogeneous blend state, and the two rubbers have completed preliminary mixing on a macroscopic scale, laying the foundation for fine dispersion in subsequent stages.
[0033] The second stage is the compounding and dispersion stage of additives and fillers. The raw rubber blending masterbatch obtained from the first stage is fed back into the E-type internal mixer, and various compounding agents are added sequentially according to a specific feeding order. The operation process and feeding order of this stage have a decisive influence on the properties of the final rubber compound.
[0034] First, zinc oxide, stearic acid, and silane coupling agent KH-550 are added and mixed at low speed for 1 minute to ensure uniform dispersion of the activator and coupling agent in the rubber matrix. Zinc oxide and stearic acid react rapidly under high-temperature mixing conditions to generate zinc stearate activator, which is diffusely distributed within the rubber system, providing necessary catalytic active centers for subsequent vulcanization and crosslinking reactions. The ethoxy group of silane coupling agent KH-550 undergoes hydrolysis under the action of water vapor generated during mixing, generating active silanol groups, preparing for subsequent chemical bonding with silica filler.
[0035] Subsequently, carbon black N550 and precipitated silica reinforcing fillers were added, and mixing continued for 2 minutes. Under the strong shearing action of the internal mixer rotor, the carbon black filler was forcibly broken into primary aggregates and torn apart and dispersed into the rubber matrix. The silica filler, through pretreatment with a silane coupling agent, formed an organosilane coating on its surface. This coating effectively reduced the adsorption of highly polar silanol groups on the silica surface onto rubber macromolecules, improving the compatibility between silica and rubber, allowing it to be uniformly dispersed in the rubber matrix without severe agglomeration. The carbon black and silica fillers interpenetrate and fill each other in the rubber matrix, forming a three-dimensional reinforcing network structure.
[0036] Finally, the special low-temperature resistant plasticizer diisooctyl adipate polyester and the ternary composite anti-aging additive are added, followed by 3 to 5 minutes of pressurized closed mixing. During this stage, the pressure in the mixing chamber is maintained at 0.4 to 0.6 MPa throughout. This high-pressure environment forces the long-chain polyester plasticizer molecules to rapidly penetrate into the spaces between the rubber macromolecular chains, effectively reducing the interaction forces between rubber molecular chains and preventing the plasticizer from being lost due to volatilization during high-temperature mixing. Under high-pressure mixing, the anti-aging additive system is uniformly embedded in the interstitial spaces of the rubber macromolecular network, providing a guarantee for the long-term weather resistance and aging protection of subsequent hose products. The discharge temperature of the second-stage mixing should be strictly controlled within the range of no more than 130 degrees Celsius to prevent thermal oxidative degradation of the rubber macromolecular chains or thermal volatilization loss of the plasticizer caused by high temperatures.
[0037] The compound obtained from the two-stage internal mixing was cooled and allowed to stand at room temperature for 12 hours. This standing process allows the polymer chains inside the compound sufficient time to relax, eliminating residual stress accumulated during mixing and enabling the compounding agents to achieve uniform concentration equilibrium diffusion within the rubber matrix. Simultaneously, the standing process lowers the compound temperature to room temperature, creating safe conditions for the subsequent low-temperature addition of vulcanizing agents and preventing premature cross-linking reactions of sulfur and accelerator CZ at high temperatures, which could lead to scorching and spoilage of the compound.
[0038] After cooling and resting, the second-stage compound is re-input into the E-type internal mixer, along with sulfur and accelerator CZ. After input, it is mixed at low speed and low pressure for 1.5 minutes to ensure the vulcanization system is uniformly dispersed in the rubber matrix. The key process control point in the third-stage final mixing stage is that the discharge temperature must not exceed 95 degrees Celsius. This temperature limit aims to prevent premature dissolution and activation of sulfur at higher temperatures, which could lead to premature cross-linking and vulcanization reactions in the rubber compound during storage or subsequent processing, resulting in the so-called "scorching" phenomenon. Accelerator CZ can slowly and uniformly disperse in the rubber system under low temperature and low pressure conditions, providing a controllable reserve of vulcanization activity for subsequent hose forming and vulcanization processes.
[0039] The final compound from the three-stage final mixing stage is fed into a two-roll mill for thin-pass plasticizing and refining. The temperatures of both the front and rear rolls of the mill should be controlled within a process window of 50 to 60 degrees Celsius. This temperature range maintains the rubber in a suitable viscoelastic state, providing sufficient plasticity for thin-pass plasticizing without causing sticking or scorching due to excessive temperature. First, the mill roll gap is set to a narrow 0.8 mm, and the final compound is repeatedly rolled between the two rolls six times. The purpose of this thin-pass operation is to utilize the powerful shearing and stretching action of the mill to further refine the rubber's blending and dispersion, breaking down rubber phase aggregates that were not completely eliminated during the intensive mixing stage. This further strengthens the blending interface between the two rubbers and further breaks down and disperses filler agglomerates. After the thin-pass operation, the roll gap is adjusted to a large 1.8 mm, and the compound is pressed into sheets of the specified thickness and discharged. The rubber compound is left to stand at room temperature for 24 hours for curing treatment, which allows the molecular chain segments inside the rubber compound to fully relax and reach equilibrium. The concentration of each compounding agent component continues to be uniformly diffused, and the interfacial condensation reaction of the silane coupling agent is further completed, ultimately obtaining a composite modified rubber compound with stable and uniform performance.
[0040] Step two involves feeding the cured composite modified rubber compound into a cold-feed extruder for extrusion molding of the inner rubber layer. The hopper temperature of the cold-feed extruder is controlled at room temperature, and the rubber compound is fed into the screw compression section in a solid state at room temperature. The extruder body temperature is set to 60-75 degrees Celsius, and the die head temperature is set to 70-80 degrees Celsius. This gradual temperature distribution in the body ensures that the rubber compound gradually warms and softens during screw conveying, compression, and plasticizing, preventing the formation of air bubbles or surface scorching defects due to sudden temperature increases. The die head temperature is slightly higher than the body temperature to ensure that the rubber compound maintains optimal melt flow during the extrusion molding stage, allowing the filler network to align under the extrusion shearing action, forming a dense skin structure.
[0041] The extruder's specialized die shapes the plasticized rubber melt into a tubular inner rubber layer of specified dimensions. The die size is designed according to the standard specifications of the target product to ensure that the inner rubber layer meets the final product's inner diameter tolerance requirements after subsequent wire winding and vulcanization processes. The wall thickness of the inner rubber layer should be precisely controlled within a process window of 1.2 to 2.0 mm. Too thin a wall will reduce the inner rubber layer's oil barrier properties and mechanical strength, affecting the hose's long-term reliability; too thick a wall will increase raw material consumption and production costs, while also reducing the hose's flexibility. The extruded inner rubber layer surface should be uniform and continuous, free of pores, impurities, fisheyes, and other surface defects, ensuring a smooth and dense interface with the hydraulic oil for long-term contact. The extrusion speed should be matched and synchronized with the linear speed of the subsequent wire winding process to achieve continuous production of the extrusion and winding processes.
[0042] Step three: The extruded inner tubing core is continuously fed into the wire winding machine under the action of the traction device. Four layers of brass-plated high-strength steel wire are cross-spirally wound at this station to form a metal reinforcement layer structure. The diameter of the steel wire is controlled within the range of 0.6 to 0.9 mm. This diameter specification provides sufficient tensile strength to withstand axial tensile loads under high-pressure conditions, while avoiding excessively thick wires that would result in an excessively large bending radius of the hose, affecting the flexibility of actual installation and use.
[0043] The four layers of steel wire are arranged in a crisscross spiral winding pattern with two positive and two negative windings. Specifically, the first and third layers of steel wire are wound around the inner core surface at a positive winding angle, while the second and fourth layers are wound around the surface of the previous layer at a negative winding angle, forming a cross-shaped mesh reinforcement skeleton structure. The winding angle of the steel wires should be precisely controlled within the process range of 52 to 58 degrees. The size of the winding angle directly affects the balance between the hose's pressure resistance and flexibility: when the winding angle is too small, the hose has a higher burst pressure resistance, but its flexibility decreases; when the winding angle is too large, the hose's flexibility improves, but its pressure resistance decreases. Through extensive testing, this invention has determined that a winding angle range of 52 to 58 degrees achieves the optimal balance between high-pressure resistance and low-temperature deformation flexibility.
[0044] During the wire winding process, the winding tension should be precisely controlled to ensure that each wire has a constant tension value when wound to the specified position. Insufficient tension will cause the wire to slack after winding, failing to adhere tightly to the inner rubber layer surface and creating gaps. Under high pressure conditions, stress concentration at these gaps can lead to localized bulging or even breakage. Excessive tension, on the other hand, may cause the wire to leave excessively deep indentations on the inner rubber layer surface, affecting its integrity. The four layers of wound wire should be tightly adhered to the outer wall of the inner rubber layer, with no gaps between the wires and no gaps between the wires and the inner rubber layer, ensuring a complete composite structure between the metal reinforcement layer and the rubber inner layer.
[0045] Step four: After the core is wrapped with the steel wire reinforcement layer, the outer rubber layer is extruded using the same composite modified rubber compound as the inner rubber layer. The outer rubber layer extrusion adopts a cold-feed extrusion process similar to that of the inner rubber layer, and the extrusion temperature parameters are set in the same principle. The main function of the outer rubber layer is to form an outer protective barrier for the hose, resisting the erosion of moisture, oxygen, ozone, and ultraviolet rays in the external environment, and protecting the internal metal reinforcement layer from corrosion failure. The wall thickness of the outer rubber layer should be precisely controlled within a process window of 1.5 to 2.5 mm. Too thin a wall will weaken the protective performance of the outer rubber layer and accelerate the erosion rate of the metal steel wire layer by external aging factors; too thick a wall will increase the overall weight and bending rigidity of the hose, reducing the ease of installation and use. The outer rubber layer should completely wrap the metal steel wire layer, and the ends of the steel wires should not be exposed on the surface of the outer rubber layer, forming a continuous protective cover.
[0046] Step 5: The formed tube blank, after the outer rubber layer has been extruded and coated, enters the continuous vulcanization process. The tube blank is continuously fed into the internal channel of a horizontal continuous vulcanizing tank. Saturated steam is introduced into the vulcanizing tank as the heat source medium for vulcanization, with the steam pressure controlled at 0.35 MPa, corresponding to a vulcanization temperature of 145 degrees Celsius. Under these temperature and pressure conditions, the tube blank undergoes heating and vulcanization. The rubber macromolecular chains and sulfur undergo a cross-linking reaction under the catalysis of accelerator CZ, forming a three-dimensional network structure, transforming the soft raw rubber material into a vulcanized rubber product with high elasticity, high strength, and high heat resistance.
[0047] The vulcanization time is set within a process window of 35 to 45 minutes. This vulcanization time directly affects the crosslinking density and mechanical properties of the rubber compound: too short a vulcanization time will lead to insufficient crosslinking reaction, resulting in suboptimal tensile strength, tensile stress at a given elongation, and heat resistance; too long a vulcanization time may lead to over-vulcanization, causing the crosslinking bonds within the rubber compound to break and rearrange, resulting in performance degradation or even thermal decomposition. This invention, through process experiments, has determined that a vulcanization time range of 35 to 45 minutes allows the composite modified rubber compound to achieve the optimal crosslinking density distribution and comprehensive mechanical properties.
[0048] After vulcanization, the tube blank enters the water cooling section. In the water cooling tank, the tube blank is sprayed or immersed in room temperature cooling water to rapidly reduce its temperature to room temperature. The purpose of water cooling is twofold: first, to rapidly cool and fix the cross-linked network structure after vulcanization, preventing further cross-linking reactions at high temperatures that could lead to over-vulcanization; second, to shrink the hose to its final dimensions at room temperature, ensuring product dimensional stability. The hose, cooled to room temperature, is then cut to the specified length at the cutting station, and metal fitting assemblies are assembled at both ends. The metal fittings use crimping or threaded connections to achieve a reliable seal with the hose ends, completing the manufacturing of the finished low-temperature resistant metal hydraulic hose.
[0049] The finished low-temperature resistant metal hydraulic hose prepared using the above-mentioned optimized ratio and process parameters underwent systematic performance testing and verification by a third-party authoritative testing institution in accordance with relevant national standards. The key performance indicators are as follows: the glass transition temperature of the rubber compound is -62 degrees Celsius; after being placed in a constant temperature environment of -55 degrees Celsius for 72 hours, the hose underwent a 180-degree bending test, and no cracks or brittle fractures were observed; the burst pressure decay rate of the hose at -55 degrees Celsius was only 7.2%; the volume swelling rate of the inner rubber layer of the hose after immersion in hydraulic oil for 72 hours was 2.8%; the low-temperature impact toughness of the hose at -55 degrees Celsius reached 131 kJ / m²; after 500 hours of accelerated aging test with ultraviolet ozone, the tensile strength retention rate was 88%. These performance data fully demonstrate that the technical solution of this invention has achieved the expected design goals in multiple dimensions, including low-temperature resistance, oil resistance, and aging resistance.
[0050] At the molecular level, this invention creates a unique island structure in the blend of low-acrylonitrile nitrile rubber (NBR) and low-temperature resistant butadiene rubber (BR): NBR forms a continuous, oil-resistant marine phase, while BR micro-regions act as low-temperature resistant, dispersed island phases uniformly distributed within this marine phase. When the fluid medium inside the hose is hydraulic oil, the continuous NBR phase forms a dense barrier layer, effectively preventing the penetration and swelling of oil molecules. When the ambient temperature drops sharply to -55 degrees Celsius, the BR micro-regions distributed in the continuous phase still maintain chain segment mobility, absorbing low-temperature shrinkage stress and passivating stress concentration at crack tips, preventing crack propagation throughout the entire rubber layer. Under E-type internal mixing conditions of high temperature and high pressure, the two-phase interface achieves full molecular chain intercalation and fusion, significantly improving the interfacial bonding strength. External loads can be effectively transferred and distributed through the two-phase interface.
[0051] At the rubber compound formulation level, the addition of diisooctyl adipate polyester low-temperature plasticizer further enhances the low-temperature toughness of the blended rubber compound. After the plasticizer molecules insert between the rubber macromolecular chains, they lower the barrier to chain segment movement, significantly improving the overall chain segment relaxation ability of the composite rubber compound. Even at temperatures as low as -55 degrees Celsius, the rubber macromolecular chains can still undergo a certain degree of micro-Brownian motion, without experiencing glass transition caused by chain segment freezing. Traditional phthalate plasticizers, due to their low molecular weight and poor compatibility with rubber, easily migrate and leach from the rubber matrix at low temperatures, leading to a sharp decline in plasticizing efficiency. The polyester plasticizer selected in this invention has a moderate molecular weight and excellent compatibility with both types of rubber, maintaining stable plasticizing efficiency throughout the entire operating temperature range.
[0052] At the process level, the high-temperature, high-pressure, staged mixing process of the E-type internal mixer plays a decisive role in improving the final rubber compound performance. The closed chamber of the E-type internal mixer can maintain a high-pressure environment of 0.4 to 0.6 MPa during the mixing process. This pressure forces the material to undergo intense compression and shearing between the rotor and the chamber wall. Compared to the thin-pass mixing under normal pressure using a conventional open mill, the high-pressure environment of the E-type internal mixer allows for the full expulsion of air and volatile components from the material, eliminating bubble defects. Simultaneously, the high-pressure conditions subject the filler aggregates to stronger mechanical shearing and crushing effects, significantly improving the filler dispersion. More importantly, the high-pressure conditions promote the interpenetration and penetration of macromolecular chains of two different polarities of rubber, strengthening the physical bonding strength at the two-phase interface. The three-stage step-by-step feeding process ensures that each compounding agent component is added at the optimal time and dispersed and mixed, avoiding the defects of uneven dispersion or excessively high local concentrations caused by simultaneous feeding. Example 2
[0053] This embodiment demonstrates the technical solution of the lower limit of the compound ratio range of the present invention.
[0054] In the preparation of the composite rubber compound, the ratio of the blended raw rubber matrix is: 60 parts of low acrylonitrile butadiene rubber and 40 parts of low-temperature resistant cis-butadiene rubber, totaling 100 parts. At this ratio, the amount of cis-butadiene rubber reaches its upper limit, maximizing the low-temperature toughness of the compound, while the amount of nitrile rubber is correspondingly reduced, resulting in a slight sacrifice in oil resistance, but still remaining within an acceptable range. The amount of the special low-temperature resistant plasticizer, diisooctyl adipate polyester, is set at 12 parts, which is at the lower limit of the ratio range. This amount of plasticizer can meet the basic low-temperature plasticizing requirements of the compound, but the plasticizing efficiency is lower than the preferred ratio. The ratios of the reinforcing filler system, vulcanization crosslinking system, composite aging-resistant additive system, and processing aids are all consistent with those in Example 1.
[0055] The process parameters of the E-type internal mixer are exactly the same as those in Example 1: filling factor 85%, rotor speed 60 rpm, first stage internal mixing 3.5 minutes, discharge temperature 115°C, second stage internal mixing 4 minutes, chamber pressure 0.5 MPa, discharge temperature 128°C, third stage final mixing 1.5 minutes, discharge temperature 92°C, open mill thin pass 6 times, room temperature curing for 24 hours. The parameters for the hose forming and vulcanization processes are also consistent with those in Example 1.
[0056] Hose samples prepared using the lower limit of this formulation were verified through performance testing. The glass transition temperature was -57°C, and the hoses maintained normal bending performance without cracking at -55°C. After immersion in hydraulic oil for 72 hours, the volume swelling rate was 3.5%, and the low-temperature impact toughness at -55°C was 118 kJ / m². Although these performance indicators are slightly lower than the preferred formulation in Example 1, they still fully meet the requirements for hydraulic hoses used in extremely cold environments, demonstrating that the technical solution of this invention has good performance tolerance within the formulation range. Example 3
[0057] This embodiment demonstrates the technical solution of the upper limit of the compound ratio range of the present invention.
[0058] In the preparation of the composite rubber compound, the ratio of the blended raw rubber matrix is: 75 parts of low acrylonitrile butadiene rubber and 25 parts of low-temperature resistant butadiene rubber, totaling 100 parts. At this ratio, the amount of butadiene rubber reaches its upper limit, maximizing the compound's resistance to hydraulic oil swelling, while the amount of butadiene rubber is correspondingly reduced, resulting in a slight sacrifice in low-temperature toughness, but still remaining within an acceptable range. The amount of the special low-temperature resistant plasticizer, diisooctyl adipate polyester, is set at 22 parts, at the upper limit of the ratio range. This amount of plasticizer allows the compound to achieve the best low-temperature plasticizing effect, forming a synergistic effect with the higher proportion of butadiene rubber, offsetting the loss of low-temperature toughness caused by the reduced amount of butadiene rubber. The ratios of the reinforcing filler system, vulcanization crosslinking system, composite aging-resistant additive system, and processing aids are all consistent with those in Example 1.
[0059] The process parameters of the E-type internal mixer are exactly the same as those in Example 1, and the operation steps and process control requirements of each process remain unchanged. The parameters of the hose forming and vulcanization processes are also consistent with those in Example 1.
[0060] Hose samples prepared using the upper limit of this formulation ratio were verified through performance testing. The glass transition temperature was -60°C, the compressive strength at -55°C decreased by only 7.9%, and the volume swelling rate after immersion in hydraulic oil for 72 hours was only 2.6%. These performance data indicate that when the amount of nitrile rubber is at its upper limit, the oil resistance of the compound is significantly improved, while the low-temperature performance does not show significant deterioration. The glass transition temperature remains below -60°C, fully meeting the requirements for use in extremely cold environments down to -55°C. This further verifies the balanced optimization characteristics of the performance indicators within the formulation range of this invention.
[0061] Comparative Example Comparative Example 1 used a conventional single high-acrylonitrile nitrile rubber as the main compound, combined with a general-purpose dibutyl phthalate plasticizer, and employed a conventional open-milling mixing process, with only a general-purpose antioxidant added. The hose sample prepared in this comparative example had a minimum temperature resistance of only -40°C. When the temperature dropped to -42°C, microcracks appeared on the sample surface, and when the temperature further decreased to -50°C, the sample experienced brittle fracture. Although its volume swelling rate after immersion in hydraulic oil for 72 hours was only 2.1%, exhibiting excellent oil resistance, its low-temperature impact toughness at -40°C was only 42 kJ / m², and its compressive strength decay rate was as high as 33%, failing to meet the requirements for use in extremely cold environments. This comparative example confirms that a single nitrile rubber system cannot overcome the low-temperature resistance limit.
[0062] Comparative Example 2 used a single cold-resistant butadiene rubber as the main compound, combined with a conventional low-temperature plasticizer, without any nitrile rubber blend. Although the hose sample prepared in this comparative example exhibited excellent low-temperature toughness with a glass transition temperature as low as -65 degrees Celsius, its volume swelling rate after immersion in hydraulic oil for 72 hours reached as high as 13.6%, indicating significant swelling and delamination of the rubber layer. This failed to guarantee the sealing reliability for long-term hydraulic media transport. This comparative example confirms that a single cold-resistant rubber system cannot overcome the technical defects in oil resistance.
[0063] Comparative Example 3 used the exact same blending compound formulation as Example 1 of this invention, but replaced the E-type internal mixing high-temperature and high-pressure segmented mixing process with a conventional two-roll open mill mixing process, without the segmented high-pressure internal mixing process. Under an electron microscope, the rubber sample prepared in this comparative example showed obvious two-phase separation, with significant gaps and defects at the rubber two-phase interface. Mechanical property tests showed that its tensile strength was only 15.3 MPa, significantly lower than the 22 MPa or higher level of Example 1. In a bending test at -55 degrees Celsius, the sample showed fine interfacial cracks, indicating that insufficient interfacial bonding caused low-temperature cracks to propagate along the interface. This comparative example confirms that the E-type internal mixing high-temperature and high-pressure segmented mixing process is a key and necessary step to achieve uniform blending of the two phases and improve interfacial bonding strength.
[0064] Comparative Example 4 used the exact same blending compound formulation and E-type internal mixing process as Example 1 of this invention, but replaced the diisooctyl adipate polyester low-temperature plasticizer with general-purpose dioctyl phthalate. The rubber sample prepared in this comparative example had a glass transition temperature of only -46 degrees Celsius. When the temperature dropped to -52 degrees Celsius, the rubber compound became hard and brittle, failing to achieve the target of stable use at -55 degrees Celsius. This comparative example confirms that a dedicated low-temperature polyester plasticizer is a key technical element for reducing the glass transition temperature of composite rubber compounds and achieving ultra-low temperature toughness.
[0065] The above description is only a preferred embodiment of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.
Claims
1. A low-temperature resistant metal hydraulic hose, characterized in that: The material consists of, from the inside out, a low-temperature resistant and oil-resistant inner rubber layer, four layers of brass-plated steel wire reinforcement, and a low-temperature resistant protective outer rubber layer. Both the inner and outer rubber layers are vulcanized from the same composite modified rubber compound. The four layers of brass-plated steel wire reinforcement are formed by spirally winding brass-plated steel wire with a diameter of 0.6-0.9 mm at a winding angle of 52°-58° with two positive and two negative cross spirals. The composite modified rubber compound comprises, by weight: 100 parts of blended raw rubber matrix, including 60-75 parts of low acrylonitrile butadiene rubber and 25-40 parts of low-temperature resistant cis-butadiene rubber; 12-22 parts of a special low-temperature resistant plasticizer, wherein the special low-temperature resistant plasticizer is diisooctyl adipate polyester low-temperature plasticizer; 45-65 parts of reinforcing filler, including 30-45 parts of carbon black N550 and 15-20 parts of precipitated silica; 3.5-6 parts of a vulcanization crosslinking system, including 1.0-1.8 parts of sulfur, 1.2-2.2 parts of accelerator CZ, 4-6 parts of zinc oxide, and 1-1.5 parts of stearic acid; 2.5-5 parts of a composite aging resistant additive, including 1-2 parts of hindered phenolic antioxidant, 0.5-1 parts of phosphite-assisted antioxidant, and 1-2 parts of ultraviolet absorber; and 1-3 parts of silane coupling agent.
2. The low-temperature resistant metal hydraulic hose according to claim 1, characterized in that, The preferred weight ratio of the composite modified rubber compound is as follows: 70 parts of low acrylonitrile butadiene rubber, 30 parts of low-temperature resistant cis-butadiene rubber, 18 parts of diisooctyl adipate polyester low-temperature plasticizer, 38 parts of carbon black N550, 17 parts of precipitated silica, 1.5 parts of sulfur, 1.8 parts of accelerator CZ, 5 parts of zinc oxide, and 1.2 parts of stearic acid. 1.5 parts hindered phenolic antioxidant, 0.8 parts phosphite co-antioxidant, 1.7 parts ultraviolet absorber; 2 parts silane coupling agent; The inner adhesive layer has a wall thickness of 1.2–2.0 mm, and the outer adhesive layer has a wall thickness of 1.5–2.5 mm. The overall glass transition temperature of the hose is ≤-62℃, and after being placed at a constant temperature of -55℃ for 72 hours, it shows no cracks or brittle fractures when bent at 180°.
3. A method for preparing a low-temperature resistant metal hydraulic hose according to any one of claims 1-2, characterized in that: Includes the following steps: Step 1: Use an E-type internal mixer to prepare composite modified rubber compound by high temperature and high pressure segmented mixing. The compound formula is as specified in the above composite modified rubber compound. The mixing is divided into three stages: raw rubber blending and plasticizing, auxiliary agent and filler compounding and dispersion, and low temperature final mixing and addition to the vulcanization system. After the mixing is completed, the rubber sheet is thinly passed through an open mill and left to mature at room temperature. Step 2: Extrude the cured composite modified rubber compound to form a tubular inner rubber layer; Step 3: Wrap four layers of brass-plated steel wire around the outside of the inner tubing core to form a steel wire reinforcement layer; Step 4: Extrude and coat the outside of the steel wire reinforcement layer with the same compound adhesive to form a protective outer adhesive layer; Step 5: The coated tube blank is sent into the vulcanization equipment for continuous steam vulcanization. After vulcanization, it is cooled by water, cut, and metal joints are assembled at both ends to obtain the finished hose.
4. The method for preparing the low-temperature resistant metal hydraulic hose according to claim 3, characterized in that, In the first step of the mixing and plasticizing stage of raw rubber, the filling coefficient of the E-type closed mixer is controlled within the range of 82% to 88%, the rotor speed is 55 to 65 revolutions per minute, cooling water is introduced into the jacket of the mixing chamber in advance for pre-cooling, the mixing time is 3 to 4 minutes, and the discharge temperature is controlled within the range of 110 to 120 degrees Celsius.
5. The method for preparing the low-temperature resistant metal hydraulic hose according to claim 4, characterized in that, In the two-stage mixing process of Step 1, zinc oxide, stearic acid, and silane coupling agent are added sequentially for low-speed mixing. Then, carbon black N550 and precipitated silica reinforcing fillers are added for further mixing. Finally, diisooctyl adipate polyester low-temperature plasticizer and ternary composite aging resistant additives are added for pressurized closed mixing for 3 to 5 minutes. The pressure in the mixing chamber is maintained at 0.4 to 0.6 MPa throughout the process, and the discharge temperature does not exceed 130 degrees Celsius.
6. The method for preparing the low-temperature resistant metal hydraulic hose according to claim 5, characterized in that, In step one, during the three-stage final vulcanization system addition stage, after the second-stage compound rubber has been cooled and left to stand for more than 12 hours, it is put back into the internal mixer. After adding sulfur and accelerator CZ, it is mixed at low temperature and low pressure for 1.5 minutes, and the discharge temperature does not exceed 95 degrees Celsius.
7. The method for preparing the low-temperature resistant metal hydraulic hose according to claim 6, characterized in that, In step one, during the thin-pass film extrusion stage of the open mill, the temperature of the front and rear rollers of the open mill is controlled at 50 to 60 degrees Celsius. The film is first refined 6 times with a roller gap of 0.8 mm, and then the roller gap is adjusted to 1.8 mm for film extrusion. The film is then left to mature at room temperature for more than 24 hours.
8. The method for preparing the low-temperature resistant metal hydraulic hose according to claim 7, characterized in that, In step two, the inner rubber layer is extruded and molded. The wall thickness of the inner rubber layer is controlled within the range of 1.2 to 2.0 mm. The extrusion temperature is 60 to 75°C for the machine body and 70 to 80°C for the die head. The extrusion speed is matched and linked with the linear speed of the subsequent wire winding process to achieve continuous production. The surface of the extruded inner rubber layer is free of air holes.
9. The method for preparing the low-temperature resistant metal hydraulic hose according to claim 8, characterized in that, The third step involves wrapping the steel wire reinforcing layer with four layers of brass-plated high-strength steel wire, which is wound in a cross spiral with two positive and two negative directions at a winding angle of 52 to 58 degrees. The diameter of the steel wire is 0.6 to 0.9 mm, and the winding tension is uniform. There are no gaps or gaps between the steel wire and the inner adhesive layer, forming a complete composite structure.
10. The method for preparing the low-temperature resistant metal hydraulic hose according to claim 9, characterized in that, The outer rubber layer is extruded using the same formula as the inner rubber, and the outer rubber wall thickness is 1.5-2.5mm, completely covering the steel wire layer; the vulcanization stage uses a horizontal continuous vulcanizing tank, with a steam pressure of 0.35MPa, a vulcanization temperature of 145℃, and a vulcanization time of 35-45min. After vulcanization, it is water-cooled to room temperature and then cut and assembled into metal joints.