A multi-stage phase change thermal storage and temperature control jacket for waste heat recovery from industrial equipment and workshop temperature regulation

By using a multi-stage phase change thermal storage and temperature regulation jacket, the problem of heat loss from the surface of medium-temperature industrial equipment is solved, achieving efficient thermal insulation and wide-temperature-range thermal storage, ensuring stable temperature control and long-term performance in the workshop.

CN123104207APending Publication Date: 2026-11-17SHANGHAI AIER ENTERPRISE DEVELOPMENT CO LTD +1
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611555315.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-09
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies cannot effectively prevent heat loss from the surface of medium-temperature industrial equipment to the workshop, and existing phase change materials melt rapidly at high temperatures or cannot effectively store heat at low temperatures, resulting in energy waste and failure of workshop temperature control.

Method used

A multi-stage phase change thermal storage and temperature regulation jacket is designed, comprising a thermal insulation layer, a porous aerogel composite coating, a high-temperature phase change thermal storage layer, and a low-temperature phase change buffer layer. Through a specific layer sequence design and an interface reinforcement layer, a tiered heat capacity network is formed to achieve efficient heat capture and slow release.

Benefits of technology

It achieves efficient heat insulation on the surface of medium-temperature industrial equipment, wide-temperature-range heat storage and delayed temperature regulation, reduces energy waste, maintains a comfortable temperature in the workshop, and ensures long-term stable performance.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

This invention belongs to the field of phase change technology, specifically relating to industrial waste heat recovery and thermal management, and more specifically to a multi-stage phase change thermal storage and temperature regulation jacket for waste heat recovery from industrial equipment and workshop temperature control. This invention provides a multi-stage phase change thermal storage and temperature regulation jacket through a specific layer sequence design. The insulation layer reduces heat flux density and forms a temperature gradient; the high-temperature phase change layer efficiently captures waste heat within a matched temperature range; and the low-temperature phase change layer performs secondary interception of penetrating heat and releases it directionally and slowly during cooling, constructing a nonlinear thermal resistance and tiered heat capacity network along the thickness direction. This synergistic mechanism enables the jacket to simultaneously possess the triple functions of instantaneous insulation, wide-temperature-range thermal storage, and delayed temperature regulation, far exceeding the effect achievable by simply superimposing the functions of each layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of phase change technology and relates to industrial waste heat recovery and thermal management, specifically to a multi-stage phase change thermal storage and temperature regulation jacket for industrial equipment waste heat recovery and workshop temperature control. Background Technology

[0002] In industries such as chemical engineering, a large number of medium-temperature industrial equipment (such as reactors, ovens, drying towers, and heat pipes) typically maintain a surface temperature of 50-100℃ during operation. This heat is continuously dissipated into the workshop environment through thermal radiation and natural convection, resulting in not only significant energy waste but also excessively high temperatures in the workshop operating area. This is particularly problematic in summer, severely impacting the comfort and work efficiency of workers and increasing the operating load on air conditioning systems.

[0003] Currently, the common methods for addressing the heat dissipation problem on the surface of industrial equipment are mainly as follows:

[0004] (1) Traditional passive insulation method

[0005] Traditional insulation materials such as rock wool, glass wool, and aluminum silicate fiber are used to wrap the outer walls of the equipment. While these materials can reduce steady-state heat conduction to some extent, their function is singular, merely serving as a "heat barrier" and unable to effectively recover and utilize lost heat. The blocked heat will eventually slowly seep into and dissipate into the workshop environment, failing to solve the long-term heat accumulation problem in the workshop. In addition, traditional insulation materials generally have drawbacks such as large thickness, easy moisture absorption and failure, and inconvenience in disassembly.

[0006] (2) Direct wrapping method for phase change materials

[0007] Phase change materials (PCMs) are used to replace or be added to traditional insulation layers to absorb heat emitted from the equipment surface through latent heat of phase change. However, existing solutions mostly use PCMs with a single phase change temperature, which has obvious application bottlenecks: if the phase change temperature is too low (e.g., close to room temperature), the PCM will quickly complete the phase change and reach thermal saturation during the high-temperature operation of the equipment, losing its continuous heat storage capacity; if the phase change temperature is too high, it is impossible to intercept the penetrating heat a second time, and it is also difficult to gently "slowly release heat" into the workshop environment after the equipment is shut down, thus failing to achieve the function of active temperature control in the workshop.

[0008] To further broaden the operating temperature range, existing technologies have attempted to stack two or more PCMs with different phase transition temperatures. However, this simple sequential stacking reveals the following key drawbacks in practical applications:

[0009] First, there is the problem of "simultaneous melting" due to the lack of heat flux gradient control. Under conditions close to a high-temperature heat source, if high and low phase change temperature PCM layers are simply stacked sequentially, the lack of an effective thermal insulation gradient design will cause heat flux to penetrate each layer simultaneously at a high density. As a result, the low-temperature phase change layer may completely melt and become thermally saturated before the high-temperature thermal insulation layer completes its phase change and heat absorption, losing its function as a "secondary interception" and "buffer for heat release." This causes the entire structure to degenerate into behavior similar to a single PCM layer, and the synergistic effect of tiered thermal storage is completely lost.

[0010] Secondly, the direction of heat release is uncontrollable, and temperature control fails. In simple layered structures, during equipment shutdown or cooling phases, the heat release from the solidification of each PCM layer is bidirectional and indiscriminate—some heat is dissipated in the reverse direction towards the equipment, while only a portion is released into the workshop environment. This significantly undermines the design goal of "slowly releasing heat to the operating area to maintain a comfortable temperature," making proactive workshop temperature control impossible.

[0011] Third, performance degradation is caused by liquid phase leakage and interlayer permeation. During repeated melt-solidification cycles, liquid phase components in PCMs with different phase change temperatures easily permeate and migrate between layers, leading to uncontrollable drift in the phase change temperature of each layer. Macroscopically, this manifests as a decrease in heat storage capacity and a loss of temperature regulation accuracy. Simple stacked structures lack effective interface isolation and anti-seepage mechanisms, making it difficult to meet the requirements for long-term stable operation in industrial environments.

[0012] (3) Active heat recovery method

[0013] Waste heat from equipment can be recovered and utilized through active systems such as heat exchangers and heat pumps. While these systems offer high recovery efficiency, they typically require fans, pumps, piping, and control systems, resulting in complex structures, high investment costs, and significant challenges in retrofitting existing equipment. Consequently, they are not suitable for the flexible deployment of small to medium-sized equipment. Summary of the Invention

[0014] To address the challenge of achieving synergistic effects of "efficient heat insulation" and "tiered heat storage" on the surface of medium-temperature industrial equipment—preventing rapid heat loss into the workshop while effectively capturing and storing waste heat over a wide temperature range—this invention aims to overcome the aforementioned shortcomings of existing technologies and provide a multi-stage phase change heat storage and temperature regulation jacket.

[0015] To solve the above-mentioned technical problems, the present invention provides a multi-stage phase change thermal storage and temperature regulation jacket, the technical solution of which is as follows:

[0016] A multi-stage phase change thermal storage and temperature regulation jacket, comprising, from the inside out:

[0017] A thermal insulation layer is used to contact the surface of a heat source, reduce the rate of heat conduction, and create a temperature gradient;

[0018] A high-temperature phase change heat storage layer is disposed on the outside of the insulation layer and contains a first phase change material. Its phase change temperature is matched with the operating temperature range of the heat source to capture and store waste heat in the high-temperature section.

[0019] A low-temperature phase change buffer layer is disposed on the outside of the high-temperature phase change heat storage layer. It contains a second phase change material, the phase change temperature of which is lower than that of the first phase change material. This layer is used to absorb the heat penetration and release it slowly during cooling.

[0020] A flexible encapsulation layer is disposed outside the low-temperature phase change buffer layer to provide mechanical protection and overall encapsulation.

[0021] Furthermore, the heat insulation layer is a nanoporous aerogel composite coating with a thickness of 0.5-2 mm and a thermal conductivity of less than 0.025 W / m·K. Preferably, the nanoporous aerogel composite coating is formed by a coating process using an aerogel coating adhesive.

[0022] Further, the phase transition temperature of the first phase change material is 55-65°C, and it is selected from at least one of n-alkanes, fatty acids, or eutectic salts; the phase transition temperature of the second phase change material is 26-32°C. Preferably, the first phase change material is n-octacosane, and the second phase change material is n-octadecane.

[0023] Furthermore, the high-temperature phase change thermal storage layer also includes a porous adsorption framework and a thermally conductive enhanced filler; wherein, the first phase change material is adsorbed in the porous adsorption framework, and the thermally conductive enhanced filler forms a thermally conductive pathway along the in-plane direction within the high-temperature phase change thermal storage layer. Through this structural design, heat, after being captured, can rapidly diffuse and be stored within the layer along the in-plane direction, rather than continuing to be conducted inward along the thickness direction, thus forming a heat flow "interception and diffusion" mechanism in conjunction with the insulation layer.

[0024] Furthermore, the low-temperature phase change buffer layer is a flexible foam or sponge with an open-cell structure, and the second phase change material is adsorbed into the pores of the flexible foam or sponge through vacuum impregnation. Preferably, the flexible foam with an open-cell structure is temperature-regulating memory foam.

[0025] Furthermore, an interface strengthening and anti-seepage layer is provided between the high-temperature phase change thermal storage layer and the low-temperature phase change buffer layer, and / or between the low-temperature phase change buffer layer and the flexible encapsulation layer; the interface strengthening and anti-seepage layer is a hot melt adhesive film or a nanofiber film, formed by a hot-pressing composite process. This interface layer can effectively prevent phase change temperature drift caused by interpenetration of liquid phase PCM between layers, while enhancing the integrity and peel strength of the multilayer structure.

[0026] Furthermore, the flexible encapsulation layer is a waterproof fabric with a hydrophobic finish and is provided with an openable fastener so that the entire outer cover can be detachably wrapped around the heat source surface.

[0027] Compared with the prior art, the present invention has the following significant advantages:

[0028] (1) Through a specific layer sequence design, the present invention reduces the heat flux density and forms a temperature gradient in the insulation layer, the high-temperature phase change layer efficiently captures residual heat within the matched temperature range, and the low-temperature phase change layer intercepts the penetrating heat a second time and releases it directionally during cooling, thus constructing a nonlinear thermal resistance and tiered heat capacity network along the thickness direction. This synergistic mechanism enables the outer jacket to simultaneously possess the triple functions of instantaneous heat insulation, wide-temperature-range heat storage, and delayed temperature regulation, far exceeding the effect that can be achieved by simply superimposing the functions of each layer.

[0029] (2) The insulation layer creates conditions for the high-temperature phase change layer to carry out solid-liquid phase change for a long time and with high efficiency in a narrow temperature range close to its phase change point, avoiding the "heat penetration" effect caused by the rapid melting of the surface of the high-temperature phase change layer when there is no insulation design.

[0030] (3) The phase change temperature of the low-temperature phase change buffer layer is set at 26-32℃, which is close to the human body's comfortable temperature range. When the equipment is shut down or cooled down, the heat stored in this layer is slowly released to the workshop environment through the flexible encapsulation layer, maintaining the comfortable temperature of the surrounding operating area without any external energy input, thus realizing workshop temperature control.

[0031] (4) By adding an interface strengthening and anti-seepage layer, the liquid interpenetration and phase change temperature drift of different PCM layers during repeated melting-solidification cycles are effectively prevented, ensuring the independence of the heat storage performance of each layer under long-term use. At the same time, the vacuum impregnation process and flexible packaging design make the PCM firmly locked in the porous skeleton, avoiding the risk of PCM leakage in traditional macro packaging. Detailed Implementation

[0032] The technical solution of the present invention will be described in detail below with reference to embodiments, but this does not limit the present invention to the scope of the embodiments described. Process parameters not specified in the embodiments of this application can be performed according to conventional methods, and all raw materials used can be obtained through commercial channels.

[0033] Comparative Example 1

[0034] (1) Polyester woven fabric (thickness 0.3 mm, weight 200 g / m²) was selected as the flexible substrate. Aerogel coating adhesive (thermal conductivity less than 0.025 W / m·K) was applied to the substrate surface by scraping. After coating, it was surface dried at room temperature for 30 minutes, and then placed in an oven at 80℃ for 10 minutes to obtain an aerogel coating with a dry film thickness of about 0.9 mm and a thermal conductivity of 0.02 W / m·K.

[0035] (2) After the aerogel coating is completely dry, apply PCM coating adhesive (containing n-octacosane powder, 70-80 wt%; phase change temperature about 60℃, latent heat of fusion about 240 J / g) to the surface of the substrate, with a dry film thickness of about 2.0 mm.

[0036] (3) Cover with waterproof fabric and sew the edges together.

[0037] Comparative Example 2 (An attempt to add thermally conductive filler and improve interfacial bonding)

[0038] (1) Add 3 parts by weight of graphene nanosheets (GNP, sheet diameter 5-10 μm, thickness less than 5 nm) to 100 parts by weight of PCM coating adhesive. First, ultrasonically disperse for 30 minutes, and then disperse at 3000 rpm for 15 minutes using a high-speed shear disperser to obtain PCM coating slurry containing thermally conductive filler.

[0039] (2) Apply the aerogel coating according to the process of Comparative Example 1, the difference being that: after the aerogel coating is surface dry at room temperature for 30 minutes, the PCM layer is scraped in the semi-dry state before it is fully cured, and then dried at low temperature of 50°C for 6 hours.

[0040] (3) Cover with waterproof fabric and sew the edges together.

[0041] Comparative Example 3 (An Attempt to Introduce a Low-Temperature PCM Layer – A Simple Stack-Up Scheme)

[0042] The aerogel coating and the GNP-containing PCM coating were prepared according to steps (1) and (2) of Comparative Example 2. The difference is that the aerogel coating was completely dried before the PCM layer was coated (to avoid the pinhole problem that occurred in Comparative Example 2). The interface bonding problem will be addressed later.

[0043] After the PCM coating is completely dry, n-octadecane (phase change temperature about 28-30℃, latent heat about 237kJ / kg) is heated and melted, and coated onto the release film through a slit. After cooling, a dense PCM sheet about 3mm thick is obtained, and nonwoven fabric is hot-pressed on both sides as support and leak prevention.

[0044] It is covered with waterproof fabric and the edges are sewn together.

[0045] Example 1 (The final breakthrough solution of the present invention)

[0046] Preparation steps

[0047] Preparation of aerogel insulation layer

[0048] Polyester woven fabric (0.3 mm thickness, 200 g / m²) was selected as the flexible substrate. An aerogel coating adhesive was applied to the substrate surface using a blade coating method. The gap between the blade and the substrate was set to 1.0 mm, and the coating speed was 2 m / min. After coating, the coating was allowed to dry at room temperature for 30 minutes, followed by drying in an oven at 80°C for 10 minutes to obtain a fully cured aerogel coating. The dry film thickness was approximately 0.9 mm, and the thermal conductivity was 0.022 W / m·K.

[0049] Fabrication of high-temperature phase change thermal storage layer (including anisotropic thermal conductivity design)

[0050] Add 3 parts by weight of graphene nanosheets (GNP, 5-10 μm in diameter and less than 5 nm in thickness) to 100 parts by weight of PCM coating adhesive. First, ultrasonically disperse for 30 minutes, then disperse at 3000 rpm for 15 minutes using a high-speed shear disperser to obtain a uniform PCM slurry containing thermally conductive filler.

[0051] The above slurry was applied to the completely dried aerogel coating surface from step (1) using a blade coating method. During the blade coating process, the shear force applied to the slurry by the blade induced the high aspect ratio graphene nanosheets to align along the blade coating direction (i.e., the in-plane direction). After coating, the nanosheets were placed in a 50°C oven for low-temperature drying for 6 hours to obtain a high-temperature phase change thermal storage layer. The dry film thickness was approximately 2.0 mm, and the effective PCM content was 70-80 wt%.

[0052] Tests showed that the in-plane thermal conductivity of this layer is 3.8 W / m·K, the normal thermal conductivity is 0.32 W / m·K, and the anisotropy ratio (in-plane / normal) is approximately 12:1.

[0053] Interface reinforcement and anti-seepage layer setting

[0054] A TPU hot melt adhesive film (50 μm thick) was selected and laid on the surface of the high-temperature phase change thermal storage layer as an interface reinforcement and anti-seepage layer.

[0055] Preparation and composite of low-temperature phase change buffer layer

[0056] Temperature-regulating memory foam (made of open-cell polyurethane foam with a porosity of about 85%, prepared by adsorbing n-octadecane through vacuum impregnation process, with a phase change temperature of 28-30℃, a latent heat of phase change of about 237 kJ / kg, and a thickness of 3.0 mm) was used. It was cut to the same size as the aforementioned coating and laid on the TPU hot melt adhesive film in step (3) (for specific methods, refer to Example 1 in CN117777709A).

[0057] On the other side of the low-temperature phase change buffer layer (the side facing the encapsulation layer), a layer of TPU hot melt adhesive film is also laid.

[0058] A one-time integral hot-pressing composite is performed using a hot press: hot pressing temperature 80℃, pressure 0.3 MPa, and holding time 30 seconds. After hot pressing, the layers are mechanically interlocked by molten TPU hot melt adhesive, achieving integrated composite bonding.

[0059] Example 2 Performance Testing Method

[0060] The following unified testing method was used to evaluate the performance of each scheme.

[0061] DSC test phase transition temperature and latent heat

[0062] Differential scanning calorimetry (DSC) was used under a nitrogen atmosphere (50 mL / min) at a heating / cooling rate of 5 °C / min, within a temperature range of 0 °C to 80 °C. Sample sizes ranged from 5 to 10 mg. The phase transition temperature and latent heat of phase transition of the PCM layers in each scheme were measured. For schemes containing multilayer PCM, layer-by-layer sampling was performed to observe the independence of the phase transition peaks in the DSC curves of each PCM layer and the presence of any new impurity peaks.

[0063] Thermal conductivity test

[0064] The normal thermal conductivity was tested using a Hot Disk thermal constant analyzer, and the in-plane thermal conductivity was tested using the laser flash method at a test temperature of 25℃.

[0065] Thermal shock simulation test

[0066] A constant-temperature heating plate (temperature controllable 65±1℃, size 300 mm × 300 mm) was used as a simulated heat source and placed in an environmental test chamber (temperature 28±1℃, relative humidity 50±5%). Samples (300 mm × 300 mm) were laid flat on the surface of the heating plate, and the temperatures of each interface and the center point of the outer surface were collected in real time using a multi-channel temperature recorder and K-type thermocouples (accuracy ±0.1℃). The thermocouples were positioned as follows: T1 is the surface of the heating plate (heat source temperature); T2 is the interface between the insulation layer (aerogel coating) and the adjacent PCM layer or intermediate layer; T3 is the center point of the PCM layer closest to the heat source; T4 is the interface between the high-temperature PCM layer and the low-temperature PCM layer (if present); T5 is the interface between the outermost PCM layer or buffer layer and the encapsulation layer; and T6 is the center point of the outer surface of the encapsulation layer.

[0067] In addition, five miniature thermocouples (one at the center and four at the top, bottom, left, and right, 2 cm from the center) are pre-embedded inside the high-temperature PCM layer to test the temperature uniformity within the layer.

[0068] Test procedure: After the heating plate is preheated to 65℃ and stabilized for 30 minutes, the sample is placed in the heating plate and the temperature at each point is recorded continuously for 4 hours (heating stage). Then the heating plate is turned off and the sample is allowed to cool naturally for 8 hours (cooling stage). The test is repeated 3 times and the average value is taken.

[0069] Aging resistance test

[0070] Samples from each design were placed in a high-low temperature alternating test chamber for accelerated aging testing. Each cycle was performed under the following conditions: heating to 65°C and holding for 2 hours → natural cooling to 25°C and holding for 2 hours. Samples were taken after 0, 50, 100, and 200 cycles for visual inspection and DSC testing. The latent heat retention rate of each layer was calculated (based on the latent heat value at 0 cycles).

[0071] Example 3: Summary of Performance Test Results

[0072] 1. DSC testing of phase transition temperature and latent heat

[0073] Test Project GNP-free (for comparison example 1) Contains 3% GNP (used in Example 1) Temperature-regulating memory foam (low-temperature phase change buffer layer, containing n-octadecane) Comparative Example 3: Low-Temperature PCM Layer Melting peak temperature Tm (°C) 60.2 60.5 29.5 29.2 Latent heat of fusion ΔHm (J / g) 238.5 228.2 235.2 (approximately 235 J / g) 241.5 Solidification peak temperature Tc (°C) 57.8 57.2 26.8 27.5 Latent heat of solidification ΔHc (J / g) 225.3 216.8 228.6 233.8 Supercooling (Tm-Tc) (°C) 2.4 3.3 2.7 1.7

[0074] 2. Thermal conductivity test

[0075] Normal thermal conductivity: A Hot Disk thermal constant analyzer (TPS 2500S model) was used according to ISO 22007-2 standard, probe model C5501 (radius 6.4 mm), test power 20 mW, test time 10 s, each sample was tested 5 times and the average value was taken, and the test temperature was 25℃.

[0076] In-plane thermal conductivity: Laser flash method (LFA) was used according to ASTM E1461 standard. The sample diameter was 25.4 mm, and the surface was coated with graphite to eliminate reflectivity differences. Each sample was tested 3 times and the average value was taken. The in-plane thermal conductivity λ = α × ρ × Cp (α is the thermal diffusivity, ρ is the density, and Cp is the specific heat capacity), and the test temperature was 25℃.

[0077] The proposed solution In-plane thermal conductivity (W / m·K) Normal thermal conductivity (W / m·K) Anisotropy ratio Scheme containing all aerogel layers — 0.022 — Comparative Example 1: PCM coating (no filler) 0.28 0.26 1.08:1 Comparative Examples 2, 3, and Example 1: PCM coating (containing 3% GNP) 3.8 0.32 11.9:1 Example 1: Temperature-Regulating Memory Foam (Solid Phase) 0.08 0.07 1.14:1 Example 1: Temperature-Regulating Memory Foam (Liquid Phase) 0.21 0.19 1.11:1 Comparative Example 3: Conventional Low-Temperature PCM Layer (Solid Phase) 0.22 0.21 1.05:1 Comparative Example 3: Conventional Low-Temperature PCM Layer (Liquid Phase) 0.24 0.23 1.04:1

[0078] 3. Thermal shock simulation test

[0079] (1) Steady-state data of each measuring point during the heating stage (temperature of each measuring point at 4 hours)

[0080] measuring point Comparative Example 1 Comparative Example 2 Comparative Example 3 Example 1 T1 Heat source (°C) 65.0 65.0 65.0 65.0 T2 outer side of insulation layer (°C) 62.3 62.1 62.2 61.5 T3 PCM layer internal center (°C) 61.0 60.8 60.6 60.5 T4 Interface between two PCM layers (°C) — — 59.2 60.3 T5 Outermost layer (°C) 48.5 44.3 41.8 34.2 T6 Outer surface center (°C) 46.2 42.1 39.8 32.5 Steady-state heat flux density (W / m²) 226 192 178 52 Heat flux attenuation rate (%) 55.4 62.8 66.3 89.9

[0081] (2) Temperature homogeneity data inside the high-temperature PCM layer (after 4 hours)

[0082] Measurement point location Comparative Example 1 Comparative Example 2 Comparative Example 3 Example 1 Center point (°C) 65.0 64.2 64.0 61.5 2cm (°C) above 60.2 62.8 62.5 61.0 2cm (°C) below 58.5 62.2 62.0 60.5 2cm left (℃) 59.5 62.5 62.3 60.8 Right 2cm (℃) 59.0 62.0 61.8 60.3 Maximum temperature difference within the layer (°C) 6.5 2.2 2.2 1.2 PCM effective utilization rate (%) 58 72 70 94

[0083] (3) Cooling process of T6 outer surface

[0084] Time Node Comparative Example 1 Comparative Example 2 Comparative Example 3 Example 1 0 h (downtime) 46.2 42.1 39.8 32.5 0.5 h 40.5 37.8 36.2 31.8 1.0 h 35.8 34.2 33.5 31.2 1.5 h 32.0 31.2 31.0 30.5 2.0 h 30.0 29.5 29.2 30.0 3.0 h 28.5 28.2 28.0 29.5 4.0 h 28.0 28.0 28.0 29.2 5.0 h 28.0 28.0 28.0 28.8 6.0 h 28.0 28.0 28.0 28.5 7.0 h 28.0 28.0 28.0 28.2 8.0 h 28.0 28.0 28.0 28.0

[0085] 4. Aging resistance test

[0086] (1) Appearance

[0087] Loop count Comparative Example 1 Comparative Example 2 Comparative Example 3 Example 1 0 times No abnormalities No abnormalities No abnormalities No abnormalities 50 times No abnormalities No abnormalities No abnormalities No abnormalities 100 times Slight peeling at the edges No abnormalities Slight seepage at the edge No abnormalities 200 times Local peeling A small number of pinholes Obvious seepage marks, localized adhesion between layers No obvious abnormalities

[0088] (2) Latent heat retention rate of each PCM phase change layer (%)

[0089] Layer 0 times 50 times 100 times 200 times Comparative Example 1 High-temperature PCM layer 100 91.8 85.5 82.0 Comparative Example 2 High-temperature PCM (GNP) layer 100 92.0 86.3 80.5 Comparative Example 3 High-temperature PCM (GNP) layer 100 94.5 87.3 78.5 Comparative Example 3 Low-temperature PCM layer (conventional dense) 100 90.8 82.1 68.7 Example 1 High-temperature PCM (GNP) layer 100 98.2 96.6 93.8 Example 1 Low-temperature PCM sponge layer 100 97.6 95.8 92.4

[0090] As can be seen from the above test results, from Comparative Examples 1, 2, and 3 to Example 1 of the present invention.

[0091] Comparative Example 1 introduced an aerogel layer, which extended the effective working time of the PCM, but led to serious interfacial bonding problems and PCM temperature uniformity problems.

[0092] Comparative Example 2 partially solved the above problems by adding thermally conductive fillers and using a semi-dry coating process, but the semi-dry process introduced pinhole defects, and the increase in normal thermal conductivity offset part of the insulation effect.

[0093] Comparative Example 3 introduced a low-temperature PCM layer (simple stacking), but the low-temperature layer saturated and failed in the early stages of heating, resulting in a weak slow-release effect; moreover, interpenetration of PCM between layers led to severe long-term performance degradation. Although the temperature rise of the outer surface was somewhat delayed in the early stages of heating, the overall improvement was far below expectations. DSC analysis and intralayer temperature monitoring revealed that n-octadecane completely melted after only 45 minutes of heating. The reason is that although the high-temperature PCM layer intercepted some heat, the heat flux density that penetrated was still sufficient to cause the low-temperature layer, which was only 3 mm thick, to quickly reach the phase transition temperature and saturate. After saturation, the low-temperature layer not only lost its ability to continue absorbing heat, but also accelerated the outward transfer of heat due to the increased thermal conductivity of the liquid-phase PCM, resulting in extremely limited improvement compared to Comparative Example 2.

[0094] Since the cryogenic layer is saturated in the early stages of heating, most of the heat stored in it is gradually dissipated through heat conduction in the latter half of the heating phase (from saturation to shutdown). After shutdown, very little latent heat remains that can be used for sustained release, and the sustained release duration is far shorter than designed.

[0095] Interlayer PCM interpenetration leads to severe performance degradation: After 200 thermal cycling aging tests, DSC detected a splitting of the phase transition peak in the low-temperature layer, indicating that interpenetration occurred between n-octacosane (phase transition temperature 60℃) in the high-temperature layer and n-octacosane (phase transition temperature 28-30℃) in the low-temperature layer during repeated melting-solidification. After 200 cycles, the latent heat retention rate of the low-temperature layer decreased significantly, and the system's thermal storage performance severely degraded.

[0096] In Embodiment 1 of the present invention, graphene nanosheets are oriented in the in-plane direction by a scraping process, thereby constructing an anisotropic thermal conductivity structure with an in-plane / normal thermal conductivity ratio of 12:1. This enables the high-temperature phase change thermal storage layer to fully disperse heat in the in-plane direction and maintain it near the phase change temperature for a long time.

[0097] By fully utilizing the self-adaptive properties of solid-phase thermal insulation and liquid-phase thermal conductivity provided by the sponge skeleton in temperature-regulating memory foam, and combining it with the TPU hot melt adhesive film interface anti-seepage layer, problems such as adaptive heat capacity buffering, interface bonding, and interlayer anti-seepage are solved.

[0098] The above embodiments are preferred embodiments of the present invention, but the embodiments of the present invention are not limited to the above embodiments. Any changes, modifications, substitutions, combinations, or simplifications made without departing from the spirit and principle of the present invention shall be considered equivalent substitutions and shall be included within the protection scope of the present invention.

Claims

1. A multi-stage phase change thermal storage and temperature regulation jacket, characterized in that, From the inside out, the following are arranged sequentially: A thermal insulation layer is used to contact the surface of a heat source, reduce the rate of heat conduction, and create a temperature gradient; A high-temperature phase change heat storage layer is disposed on the outside of the insulation layer and contains a first phase change material. Its phase change temperature is matched with the operating temperature range of the heat source to capture and store waste heat in the high-temperature section. A low-temperature phase change buffer layer is disposed on the outside of the high-temperature phase change heat storage layer. It contains a second phase change material, the phase change temperature of which is lower than that of the first phase change material. This layer is used to absorb the heat penetration and release it slowly during cooling. A flexible encapsulation layer is disposed outside the low-temperature phase change buffer layer to provide mechanical protection and overall encapsulation.

2. The multi-stage phase change thermal storage and temperature regulation jacket as described in claim 1, characterized in that, The heat insulation layer is a nanoporous aerogel composite coating with a thickness of 0.5-2 mm and a thermal conductivity of less than 0.025 W / m·K.

3. The multi-stage phase change thermal storage and temperature regulation jacket as described in claim 2, characterized in that, The nanoporous aerogel composite coating is formed by a coating process using aerogel coating adhesive.

4. The multi-stage phase change thermal storage and temperature regulation jacket as described in claim 1, characterized in that, The phase transition temperature of the first phase change material is 55-65℃, and it is selected from at least one of n-alkanes, fatty acids, or eutectic salts; the phase transition temperature of the second phase change material is 26-32℃.

5. The multi-stage phase change thermal storage and temperature regulation jacket as described in claim 4, characterized in that, The first phase change material is n-octacosane, and the second phase change material is n-octacosane.

6. The multi-stage phase change thermal storage and temperature regulation jacket as described in claim 4 or 5, characterized in that, The high-temperature phase change thermal storage layer also includes a porous adsorption framework and a thermally conductive enhanced filler; wherein, the first phase change material is adsorbed in the porous adsorption framework, and the thermally conductive enhanced filler forms a thermally conductive pathway in the in-plane direction within the high-temperature phase change thermal storage layer.

7. The multi-stage phase change thermal storage and temperature regulation jacket as described in claim 1, characterized in that, The low-temperature phase change buffer layer is a flexible foam or sponge with an open-cell structure, and the second phase change material is adsorbed into the pores of the flexible foam or sponge through vacuum impregnation.

8. The multi-stage phase change thermal storage and temperature regulation jacket as described in claim 7, characterized in that, The flexible foam with an open-cell structure is temperature-regulating memory foam.

9. The multi-stage phase change thermal storage and temperature regulation jacket as described in claim 1, characterized in that, An interface strengthening and anti-seepage layer is further provided between the high-temperature phase change heat storage layer and the low-temperature phase change buffer layer, and / or between the low-temperature phase change buffer layer and the flexible encapsulation layer; the interface strengthening and anti-seepage layer is a hot melt adhesive film or a nanofiber film, formed by a hot-pressing composite process.

10. The multi-stage phase change thermal storage and temperature regulation jacket as described in claim 1, characterized in that, The flexible encapsulation layer is a waterproof fabric with a hydrophobic finish and is equipped with an openable fastener so that the entire outer cover can be detachably wrapped around the heat source surface.

Citation Information

Patent Citations

  • Composite heat-storage temperature-regulation energy-storage product for household articles and preparation method of composite heat-storage temperature-regulation energy-storage product

    CN117777709A