A method for producing high-concentration SO2 from calcined gypsum
By moving the raw material preheating and dehydration process to an external preheating device in the gypsum-based acid production process and using low-temperature exhaust gas to dry the gypsum, the problem of low SO2 concentration in the kiln gas was solved, achieving stable production of high-concentration SO2 and cascade utilization of thermal energy, thus reducing equipment investment and energy consumption.
Patent Information
- Application Number
- CN202611565599.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-10
- Publication Date
- 2026-11-17
AI Technical Summary
In the existing gypsum-based acid production process, the SO2 concentration in the kiln gas discharged from the rotary kiln is low and fluctuates greatly, which leads to an increase in the size of the acid production system equipment, insufficient utilization of heat energy, and increased equipment investment and energy consumption.
The raw material preheating and dehydration process is separated from the rotary kiln and completed independently in an external preheating device. The low-temperature exhaust gas discharged from the preheating device is used to dry gypsum, and the hot air that cools the clinker is recovered and used to preheat the raw material. The kiln gas is separated from the preheating device and the drying system, and the SO2 concentration of the kiln gas is increased through waste heat recovery.
By stabilizing the SO2 concentration in the kiln gas, reducing the specifications of the acid production system equipment, decreasing investment and energy consumption, realizing the cascade utilization of thermal energy, and improving the operational stability and automation control level of the acid production system.
Smart Images

Figure CN123105558A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to gypsum-based acid production technology, specifically to a method for producing high-concentration SO2 from calcined gypsum. Background Technology
[0002] Gypsum-to-sulfuric acid co-production of cement is an industrial method that reduces and decomposes calcium sulfate in gypsum (including phosphogypsum, desulfurized gypsum, and natural gypsum) at high temperatures to generate SO2-containing kiln gas and cement clinker. The kiln gas is purified, converted, and absorbed to produce sulfuric acid, and the clinker is cooled to produce cement. This technology enables the resource utilization of industrial by-product gypsum, and has certain environmental and economic benefits.
[0003] The industrial application of gypsum-based sulfuric acid co-production of cement can be traced back to the Müller-Kühne process. Its basic steps involve mixing and grinding gypsum with auxiliary materials such as coke, clay, sand, and iron powder, then feeding the mixture into a rotary kiln for calcination. The calcium sulfate in the gypsum is reduced and decomposed at high temperatures, generating kiln gas containing SO2. This gas is then filtered, washed, and purified before being sent to the sulfuric acid production system. The sintered product obtained from calcination is cooled to produce cement clinker. This process remains the primary form of industrial application.
[0004] In existing processes, the SO2 volume concentration (dry basis) in the kiln gas discharged from rotary kilns is typically maintained at 4.5%~5.5%. Analysis of the causes reveals the following main factors: The rotary kiln must simultaneously perform three functions: raw material preheating and dehydration, decomposition, and calcination. To balance the removal of water vapor in the preheating section and the control of the weakly oxidizing atmosphere in the decomposition section, the kiln tail exhaust volume and the oxygen content within the kiln need to meet multiple demands, making the kiln atmosphere stability easily disturbed and affecting SO2 formation. Simultaneously, the large amount of water vapor released from the raw materials in the preheating section increases the total wet basis volume of the kiln gas. Although the effect of water vapor is deducted when the kiln gas concentration is measured on a dry basis, the increased wet basis volume increases the total gas volume that the acid production system needs to handle, resulting in a corresponding increase in equipment specifications. Furthermore, unavoidable mechanical air leakage exists at the pipelines and equipment interfaces between the kiln tail and the acid production system, and this air mixing further dilutes the SO2 concentration in the kiln gas. The combined effect of the above factors maintains the dry basis SO2 concentration of the kiln gas at a level of 4.5% to 5.5% under normal operating conditions. This lower SO2 concentration has the following impacts on the operation of the acid production system:
[0005] Firstly, the acid production system requires a larger volume of gas to be processed. Under the same sulfuric acid production, the total gas volume corresponding to low-concentration SO2 kiln gas is higher, which leads to a corresponding increase in the required specifications of equipment such as tail gas fans, waste heat recovery, purification electrostatic precipitators, SO2 blowers, heat exchangers, converters, and absorption towers, resulting in increased equipment investment.
[0006] Secondly, to ensure the thermal and water balance of the acid production system, low-concentration SO2 gas needs to undergo heat matching before entering the converter. Some processes add a basic sulfur combustion chamber before the acid production system to increase the SO2 concentration in the kiln gas to meet the acid production requirements by burning individual sulfur, which increases the additional consumption of sulfur resources.
[0007] Thirdly, in terms of thermal energy utilization, the existing process has room for insufficient matching between thermal energy of different grades. The high-temperature kiln gas generated by rotary kiln calcination is used for waste heat recovery, and the hot air released during the clinker cooling process is reused as combustion air. However, the above-mentioned methods of thermal energy utilization are relatively independent and lack multi-level matching and tiered utilization. Summary of the Invention
[0008] The purpose of this invention is to provide a production method for preparing high-concentration SO2 from calcined gypsum, in order to solve the problem that the SO2 concentration in the kiln gas discharged from the rotary kiln is low and the concentration fluctuates greatly during operation in the existing gypsum-based acid production process.
[0009] To achieve the above objectives, the present invention provides the following technical solution: a method for preparing high-concentration SO2 from calcined gypsum, comprising the following steps:
[0010] S1. Cool the high-temperature clinker after calcination in the rotary kiln and recover the hot air generated during the cooling process;
[0011] S2. The hot air is introduced into the preheating device to preheat and dehydrate the gypsum raw material that has not yet entered the rotary kiln, and the low-temperature exhaust gas containing water vapor obtained after heat exchange is extracted from the preheating device.
[0012] S3. Use the extracted low-temperature exhaust gas as a heat source to dry the raw gypsum.
[0013] S4. The preheated raw material is fed into a rotary kiln for decomposition and calcination, and the SO2-containing kiln gas discharged from the rotary kiln is separately extracted, and after waste heat recovery, it is sent to the acid production system.
[0014] The low-temperature exhaust gas does not enter the rotary kiln and acid production system, and the SO2-containing kiln gas does not enter the preheating device and the system used to dry raw gypsum.
[0015] Since the decomposed kiln gas does not undergo raw material preheating, it is easier to achieve automated control of clinker calcination and raw material decomposition, producing kiln gas with stable SO2 concentration and high-grade cement clinker.
[0016] Furthermore, the preheating device is a cyclone preheater.
[0017] Furthermore, the temperature of the hot air is 700–850°C; the temperature of the low-temperature exhaust gas is 130–150°C; and the temperature of the exhaust gas discharged after drying the raw gypsum is 80–90°C.
[0018] Furthermore, when the SO2-containing kiln gas enters the acid production system after waste heat recovery, the SO2 volume concentration therein is 5% to 10%.
[0019] Since the SO2-containing kiln gas volume concentration is 5% to 10%, the selection of equipment such as tail gas blowers, waste heat recovery, and acid production systems is reduced, thereby reducing the investment in the equipment.
[0020] Furthermore, it also includes a heat compensation step: when the heat of the low-temperature exhaust gas is insufficient to meet the drying requirements of the raw gypsum, the high-temperature flue gas generated by the boiling hot air furnace is added to the inlet of the drying system and mixed with the low-temperature exhaust gas, and the temperature of the mixed air is adjusted to 180-250°C.
[0021] Furthermore, the boiling hot air furnace is an energy-saving boiling hot air furnace.
[0022] Furthermore, it also includes a sulfur production mode: when switching to sulfur production mode, the air supply in the rotary kiln is reduced and the reducing agent ratio is increased to create a weak oxygen reducing atmosphere in the kiln, and the SO2-containing kiln gas discharged from the rotary kiln is switched to the sulfur reduction system.
[0023] Furthermore, the weak oxygen reducing atmosphere is characterized by an O2 volume concentration of less than 0.5% in the kiln tail flue gas.
[0024] Furthermore, the SO2-containing kiln gas is recovered from waste heat and then purified, converted, and absorbed in sequence to produce sulfuric acid.
[0025] Furthermore, the raw material gypsum is at least one of phosphogypsum, desulfurized gypsum, or natural gypsum.
[0026] Compared with the prior art, the present invention provides a method for producing high-concentration SO2 from calcined gypsum by separating the preheating and dehydration process of raw materials from the rotary kiln to be completed independently in an external preheating device. The low-temperature exhaust gas containing water vapor discharged from the preheating device is extracted and used to dry the gypsum, so that the water vapor generated by the preheating of raw materials no longer enters the rotary kiln, which is beneficial to the stable control of the weak oxidizing atmosphere. Under this condition, the reduction decomposition reaction pathway of calcium sulfate is more singular, and side reactions such as the formation of calcium sulfide and the precipitation of elemental sulfur are suppressed.
[0027] Using this method, after separating the preheating device from the kiln tail system, the kiln tail is only connected to the pipeline of the acid production system. The pipeline length and number of interfaces are reduced, the mechanical air leakage is controlled, and the SO2 concentration in the kiln gas is increased due to the reduced dilution by air leakage.
[0028] Meanwhile, by simplifying the function of the rotary kiln in this method, the number of operating variables is reduced, the control precision is improved, the operational stability of the SO2 concentration in the kiln gas is improved, and the average level is correspondingly increased.
[0029] This invention utilizes the high-temperature gas (approximately 700-850°C) from the kiln head after the raw material preheating and gypsum drying processes. The temperature of the raw material is reduced to around 140°C after preheating, while the actual temperature required for the drying process is around 140-200°C. This achieves the cascade utilization of thermal energy, and the thermal energy grade and application are effectively matched. Attached Figure Description
[0030] To more clearly illustrate the technical solutions in the embodiments of this application or the prior art, the drawings used in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in this invention. For those skilled in the art, other drawings can be obtained based on these drawings.
[0031] Figure 1 The process flow and heat balance diagram provided for embodiments of the present invention. Detailed Implementation
[0032] To enable those skilled in the art to better understand the technical solution of the present invention, the present invention will be further described in detail below with reference to the accompanying drawings.
[0033] As attached Figure 1 As shown:
[0034] The overall process flow of this method is as follows: High-temperature clinker discharged from the rotary kiln enters the clinker cooling unit. The hot air released during the cooling process (approximately 800°C) is sent to the cyclone preheater for preheating the raw meal. The low-temperature exhaust gas (approximately 140°C) discharged from the top of the cyclone preheater is drawn off and sent to the dryer for drying the raw gypsum. The drying exhaust gas (approximately 85°C) is discharged after dust removal. The preheated raw meal discharged from the bottom of the cyclone preheater is sent to the rotary kiln for decomposition and calcination. The SO2-containing kiln gas generated from decomposition is sent to the acid production system after waste heat recovery. The clinker obtained from calcination is sent to the cement system. When the drying system is insufficient in heat, the fluidized bed hot blast furnace supplements the heat to the dryer. The heat distribution between each unit (in kg coal / t clinker) is as follows: calcination and decomposition 65-80%, clinker cooling heat recovery 65-80%, preheated exhaust gas for drying 30-40%, waste heat for power generation 15-20%, and hot blast furnace supplementary heat 65-80%.
[0035] Example 1:
[0036] This invention provides a method for producing high-concentration SO2 from calcined gypsum.
[0037] This embodiment uses phosphogypsum as raw material and a cyclone preheater as a preheating device. The method is implemented according to the following steps.
[0038] (a) Raw material preparation
[0039] The phosphogypsum was obtained from a wet-process phosphoric acid production unit. Its main components (dry basis) are: CaSO4·2H2O content approximately 82%, SiO2 content approximately 6.5%, Al2O3 content approximately 1.8%, Fe2O3 content approximately 0.6%, P2O5 content approximately 1.2%, F content approximately 0.4%, and free water content approximately 18%. Metallurgical coke was used, with a fixed carbon content ≥82%, moisture content ≤1%, and fineness ≤3mm. The raw materials were mixed and ground in the following proportions: phosphogypsum (dry basis) 92%, coke 6.5%, clay 1.0%, and iron powder 0.5%. After mixing and grinding, the fineness was ≤10% residue on a 0.08mm standard sieve. Analysis of the ground raw meal showed a lime saturation coefficient KH of 1.02, a silica content n of 2.85, an iron content P of 2.60, and a carbon-sulfur ratio C / SO3 of 0.68.
[0040] (ii) Heat extraction from clinker cooling
[0041] After calcination in the rotary kiln, the cement clinker (exiting at approximately 1200℃) enters a grate cooler. Cooling air exchanges heat with the clinker in a counter-current flow. Hot air, at approximately 780~820℃, is extracted from the middle section of the cooler at a flow rate of approximately 1.8~2.2 Nm³. 3 / kg clinker. The hot air is sent to a cyclone preheater as a preheating medium.
[0042] (III) Raw material preheating and exhaust gas extraction
[0043] The cyclone preheater employs a multi-stage suspension heat exchange structure. Hot air at 780~820℃ enters the preheater from the bottom, undergoing counter-current suspension heat exchange with raw meal powder added from the top. The raw meal is heated to approximately 580~620℃ within the preheater, with a residence time of approximately 15~20 seconds. During this stage, some free water and water of crystallization in the raw meal are removed, and the removed moisture enters the gas phase. The gas, after heat exchange, exits from the top of the preheater at a temperature of approximately 135~145℃. This gas (i.e., low-temperature exhaust gas) contains water vapor, a small amount of dust, and air, with extremely low SO2 content (<0.05%). This low-temperature exhaust gas is piped to the gypsum drying system. The preheated raw meal exits from the bottom of the preheater via a lock-type discharge valve and is sent to the tail of the rotary kiln.
[0044] (iv) Drying of gypsum
[0045] Low-temperature exhaust gas (approximately 140°C) drawn from the top of the cyclone preheater enters the rotary dryer, where it undergoes co-current contact drying with the phosphogypsum raw material containing approximately 18% moisture. The dryer is a 2.2m diameter, 18m long rotary drum dryer equipped with internal lifting plates. The contact time between the low-temperature exhaust gas and the wet gypsum within the dryer is approximately 25-30 minutes. After drying, the gypsum exits the dryer at approximately 90-100°C, with a moisture content reduced to 5.0%-5.5%. The drying exhaust gas, at approximately 83-87°C, is discharged from the tail end of the dryer and, after dust removal by a bag filter, is discharged with a dust concentration ≤30mg / Nm³. 3 .
[0046] During the drying process, when the heat from the low-temperature exhaust gas is insufficient to completely remove all free water from the gypsum, an energy-saving fluidized bed hot air furnace is activated for heat compensation. The fluidized bed hot air furnace uses pulverized coal as fuel, generating high-temperature flue gas of approximately 750-850°C, which is added to the dryer inlet pipe and mixed with the 140°C exhaust gas. By adjusting the fuel dosage of the hot air furnace, the mixed air temperature is controlled at approximately 200-220°C. Based on heat balance calculations, approximately 9.8 × 10⁻⁶ heat is required to process one ton of wet gypsum (initial water content 18%). 5 kJ, of which approximately 6.2 × 10 kJ is provided by exhaust gas at 140°C. 5 kJ, hot air furnace replenishment approximately 3.6 × 10 kJ. 5 kJ.
[0047] (v) Raw material decomposition and kiln gas collection
[0048] The preheated raw material is fed into the rotary kiln via a kiln tail airlock feeder. The rotary kiln rotates at a speed of 0.8~1.2 r / min, and the residence time of the raw material in the kiln is approximately 80~100 minutes. Pulverized coal is injected from the kiln head for combustion and heating, with the kiln head temperature controlled at 950~1000℃ and the kiln tail temperature controlled at 450~500℃. The material decomposition zone temperature is approximately 1050~1150℃. By adjusting the air supply at the kiln head, the O2 content in the flue gas at the kiln tail is controlled at 0.8%~1.2% (volume fraction) to maintain a weakly oxidizing atmosphere.
[0049] Inside the rotary kiln, calcium sulfate is reduced and decomposed by coke, generating SO2 which enters the gas phase. CaO reacts with SiO2, Al2O3, Fe2O3, etc., to form cement clinker minerals. The SO2-containing kiln gas discharged from the rotary kiln is extracted from the kiln tail and enters the waste heat recovery system directly without passing through the preheating device and drying system. The kiln gas temperature is approximately 450~550℃, and the SO2 volume concentration is approximately 8.2%~9.0% (measured values are shown in the table below).
[0050] Main components of rotary kiln gas (volume fraction, standard state)
[0051] Components <![CDATA[SO2]]> <![CDATA[CO2]]> <![CDATA[N2]]> <![CDATA[O2]]> <![CDATA[H2O]]> content(%) 8.2~9.0 18~22 66~70 0.8~1.2 1.5~2.5
[0052] (vi) Waste heat recovery and acid production
[0053] SO2-containing kiln gas first enters the waste heat boiler, where its temperature drops from approximately 480℃ to approximately 310-330℃. The recovered heat is used to generate saturated steam (approximately 1.6 MPa, approximately 201℃), which is then integrated into the plant's steam network or used for power generation. After waste heat recovery, the kiln gas sequentially enters a dry dust removal system (sedimentation chamber + cyclone dust collector + electrostatic precipitator), achieving a dust content ≤50 mg / Nm³ after dust removal. 3 After dust removal, the kiln gas undergoes wet purification via an empty tower, a scrubbing tower, and a two-stage electrostatic precipitator, with the scrubbing liquid recycled. After purification, the kiln gas temperature drops to approximately 28-32℃. After passing through a demister to remove entrained droplets, it enters a drying tower where it is dried and dehydrated with 93%-98% sulfuric acid, ensuring a moisture content of ≤0.1g / Nm³. 3 .
[0054] The dried kiln gas has a SO2 volume concentration of approximately 7.5%–8.5% (due to a small amount of air intake from the system's negative pressure). After preheating to approximately 410–420°C by a heat exchanger, it enters the converter. The converter employs a three-stage vanadium catalyst bed, with inlet temperatures for each stage: stage one 420–425°C, stage two 425–430°C, and stage three 380–390°C. The maximum bed temperature does not exceed 610°C. The overall SO2 conversion rate is approximately 95.5%–97.0%. After cooling, the converted gas enters an absorption tower where SO3 is absorbed by 98% sulfuric acid, with an absorption rate ≥99.8%, yielding 93% or 98% industrial sulfuric acid or fuming sulfuric acid.
[0055] The total sulfur yield (from sulfur in raw gypsum to sulfur in finished sulfuric acid) is approximately 90% to 93%.
[0056] (vii) Cement preparation
[0057] Cement clinker discharged from the rotary kiln is cooled to approximately 80-120°C by a grate cooler before being sent to the clinker silo. The clinker is tested according to GB / T 21372-2008 standard, with a free calcium oxide content ≤1.5% and a weight per liter ≥1200g / L. Approximately 5% dihydrate gypsum, approximately 4% granulated blast furnace slag, and approximately 2% zeolite are added to the clinker and ground together to a specific surface area ≥320m². 2 / kg yields ordinary Portland cement. Testing shows that the cement has a three-day compressive strength ≥22MPa and a twenty-eight-day compressive strength ≥48MPa, meeting the requirements of grade 42.5 cement.
[0058] Example 2:
[0059] This embodiment uses desulfurized gypsum as raw material and a cyclone preheater as the preheating device. The raw material, desulfurized gypsum, is taken from a wet flue gas desulfurization unit of a coal-fired power plant. Its main components (dry basis) are: CaSO4·2H2O content approximately 88%, SiO2 content approximately 3.5%, Al2O3 content approximately 0.8%, Fe2O3 content approximately 0.3%, CaCO3 content approximately 2.5%, and free water content approximately 14%. The coke ratio is adjusted to 6.0%, and no clay or iron powder is added. The raw meal ratio is: desulfurized gypsum (dry basis) 94%, coke 6.0%. After grinding, the fineness is ≤8% residue on a 0.08mm standard sieve. The raw meal ratio is: KH 0.98, n 2.92, P 2.89, C / SO3 0.70.
[0060] The clinker cooling air, at a temperature of approximately 750-790°C, is fed into a multi-stage cyclone preheater. The raw material is heated to approximately 570-600°C within the preheater. The low-temperature exhaust gas discharged from the top of the preheater, at a temperature of approximately 138-142°C and containing approximately 12%-15% water vapor (by volume), is pumped to a dryer for drying the desulfurized gypsum raw materials.
[0061] The desulfurized gypsum initially contains about 14% moisture. After being dried for about 28 minutes in contact with low-temperature exhaust gas at 140°C (with supplemental hot air from a mixed hot air furnace to about 210°C), the moisture content at the outlet drops to 4.5%~5.0%, and the outlet temperature is about 92~98°C. The exhaust gas temperature is about 82~86°C.
[0062] After preheating, the raw material is fed into the rotary kiln via an airlock feeding device. The rotary kiln speed is 0.7~1.1 r / min, the kiln head temperature is 960~1020℃, the kiln tail temperature is 460~510℃, and the material decomposition temperature is approximately 1050~1180℃. The kiln atmosphere is controlled as a weakly oxidizing atmosphere, with an O2 content of 0.7%~1.3% at the kiln tail. The SO2-containing kiln gas discharged from the rotary kiln has a temperature of approximately 460~530℃ and is directly fed into the waste heat boiler. The SO2 volume concentration in the kiln gas (before waste heat recovery) is approximately 8.6%~9.5%.
[0063] After waste heat recovery, the kiln gas temperature drops to approximately 315~335℃. After dry dust removal (settling chamber + multi-tube cyclone dust collector + electrostatic precipitator), the dust content is ≤40mg / Nm³. 3 After dust removal, the kiln gas is purified through an empty tower, a scrubbing tower, and an electrostatic precipitator, reaching a temperature of approximately 28-32℃. Before entering the converter, the SO2 concentration is approximately 7.8%-8.6%, the conversion rate is approximately 96.0%-97.2%, and the absorption rate is ≥99.85%, yielding 98% industrial sulfuric acid or fuming sulfuric acid.
[0064] After the clinker is cooled, the clinker, retarder, and active materials are mixed and ground in a certain proportion according to product requirements. In this embodiment, the clinker is mixed and ground in a proportion of 92%, gypsum dihydrate 5%, and slag 3% to obtain cement. The cement has a three-day compressive strength ≥23MPa and a twenty-eight-day compressive strength ≥49MPa, meeting the 42.5 grade standard.
[0065] The sulfur recovery rate of the entire process is approximately 91%~94%. The coal consumption (including coal for rotary kiln and hot blast stove) for processing one ton of dry desulfurized gypsum is approximately 105~115 kgce / t gypsum.
[0066] Example 3:
[0067] This embodiment uses natural dihydrate gypsum as raw material and a cyclone preheater as the preheating device. The natural dihydrate gypsum is obtained from a mine, in block form, and is used after being crushed to ≤25mm. Its main components (dry basis) are: CaSO4·2H2O content approximately 92%, SiO2 content approximately 4.2%, Al2O3 content approximately 1.1%, Fe2O3 content approximately 0.4%, and free water content approximately 2% (the natural gypsum has been partially dehydrated after being stored in the open air). Since the natural gypsum has a low water content, deep drying with a dryer is not required; only the 140℃ exhaust gas extracted from the top of the preheater needs to be used as an auxiliary drying medium.
[0068] The raw material ratio is: 90.5% natural gypsum (dry basis), 5.5% coke, 2.5% clay, and 1.5% iron powder. The fineness after grinding is ≤9% residue on a 0.08mm standard sieve. The raw material ratio is: KH 0.99, n 3.10, P 2.65, C / SO3 0.72.
[0069] The temperature of the hot air used for clinker cooling is approximately 780~820℃. After the raw material is preheated by a multi-stage cyclone preheater, the low-temperature exhaust gas discharged from the top of the preheater has a temperature of approximately 140~148℃. This exhaust gas is only partially used for auxiliary drying of natural gypsum (the moisture content of natural gypsum is already very low, so the deep drying step can be omitted), and the remaining exhaust gas can be directly discharged after dust removal. In this embodiment, because the moisture content of natural gypsum is low, the hot air furnace can maintain low-load operation or be shut down, and the system has good heat self-balance.
[0070] After preheating, the raw material is fed into the rotary kiln via an airlock feeding device. The rotary kiln speed is 0.9~1.3 r / min, the kiln head temperature is 940~990℃, the kiln tail temperature is 440~490℃, and the material decomposition temperature is approximately 1050~1150℃. The O2 content inside the kiln is controlled at 0.6%~1.2%. The SO2 volume concentration in the SO2-containing kiln gas discharged from the rotary kiln is approximately 8.9%~9.8%, significantly higher than in Examples 1 and 2 (due to the low impurity content of natural gypsum).
[0071] After waste heat recovery (temperature reduced from approximately 470℃ to approximately 320℃), dust removal, and purification, the SO2 concentration entering the converter is approximately 8.0%~9.0%. The SO2 conversion rate is approximately 96.5%~97.5%, and the absorption rate is approximately 99.9%. Two grades of industrial sulfuric acid or fuming sulfuric acid, 93% and 98%, are produced.
[0072] After clinker is batched and ground, the cement has a three-day compressive strength ≥24MPa and a twenty-eight-day compressive strength ≥50MPa, with some batches reaching the 52.5 grade standard.
[0073] The sulfur yield of the entire process is approximately 92% to 94%. Due to the low water content and few impurities of natural gypsum, and the elimination of heat consumption from deep drying, the overall energy consumption of this embodiment is the lowest among the three embodiments, with a comprehensive coal consumption of approximately 120 to 130 kgce per ton (per ton of sulfuric acid + per ton of cement).
[0074] Example 4:
[0075] In this embodiment, phosphogypsum is used as raw material, and a vertical preheater is used instead of a cyclone preheater as a preheating device to verify the replaceability of the preheating device.
[0076] The source and composition of phosphogypsum are the same as in Example 1, as are the raw meal ratio and rate values. The hot air for cooling the clinker, at a temperature of approximately 760-800°C, is introduced from the bottom of the vertical preheater and exchanges heat with the raw meal added from the top in a counter-current manner. The vertical preheater is a tubular structure, with air flowing inside the tubes and material flowing between them, or it employs a gravity settling gas-solid heat exchange structure. The raw meal is heated to approximately 560-600°C in the vertical preheater, with a residence time of approximately 30-40 seconds. After heat exchange, the gas is discharged from the top of the preheater at a temperature of approximately 136-143°C, and this low-temperature exhaust gas is drawn into the drying system.
[0077] The operating parameters for the remaining steps (gypsum drying, rotary kiln decomposition, waste heat recovery, acid production, and cement preparation) are basically the same as in Example 1. This example verifies that when using a vertical preheater, gas separation for preheating and decomposition can also be achieved, and the SO2 volume concentration of the kiln gas discharged from the rotary kiln is approximately 7.8%~8.7%, which is at the same level as in Example 1.
[0078] This embodiment shows that the specific structure of the preheating device is not a necessary limiting condition for achieving the core objective of this method. As long as sufficient heat exchange between the high-temperature hot air and the raw material can be achieved and the low-temperature exhaust gas containing water vapor can be effectively extracted, the technical effect of this method can be achieved.
[0079] Example 5:
[0080] This embodiment uses phosphogypsum as raw material, employs a cyclone preheater, and operates in sulfur production mode.
[0081] The raw materials and proportions are the same as in Example 1. After stable operation in normal sulfuric acid production mode (weak oxidizing atmosphere in the kiln, O2 0.8%~1.2%), the mode is switched. The switching operation includes: gradually reducing the primary air supply of the rotary kiln by about 20%~30%, and at the same time increasing the coke proportion in the raw material batching from 6.5% to 7.5%~8.0% to increase the reducing atmosphere in the kiln. After adjustment, the O2 volume concentration in the kiln tail flue gas drops to 0.3%~0.5% (i.e., weak oxygen reducing atmosphere). At this time, the decomposition path of calcium sulfate in the kiln changes, and some SO2 is further reduced to elemental sulfur vapor. In addition to SO2, the kiln gas also contains a small amount of elemental sulfur vapor and reducing components such as H2S.
[0082] The kiln gas discharged from the rotary kiln is not sent to the sulfuric acid purification system, but is instead switched to the sulfur reduction system via a valve group. The kiln gas first undergoes dust removal (cyclone dust collector + electrostatic precipitator) to remove dust, then enters a sulfur condenser to be cooled to approximately 130-150°C. Elemental sulfur vapor condenses into liquid sulfur, which is then purified by distillation to obtain industrial sulfur (purity ≥99.5%). Uncondensed SO2-containing tail gas is discharged after desulfurization treatment.
[0083] During the switch to sulfur production mode, the main operating parameters of the rotary kiln were adjusted as follows: the kiln head temperature was maintained at 950~1000℃, the kiln tail temperature was slightly reduced to 430~480℃, and the material residence time in the kiln was extended to 100~120 minutes. When switching back from sulfur production mode to sulfuric acid production mode, the air supply was gradually restored and the coke ratio was reduced to the original level. The O2 content at the kiln tail rose back to 0.8%~1.2%, and the kiln gas was switched back to the sulfuric acid purification system. The mode switching operation took approximately 30~60 minutes. During the switching period, the system operated stably, and no abnormal phenomena such as ring formation or scaling occurred.
[0084] This embodiment demonstrates that the method can switch between sulfuric acid and sulfur production modes without changing the main equipment, and the product plan can be flexibly adjusted according to market demand.
[0085] The key parameters for each embodiment are summarized in the table below.
[0086] project Example 1 Example 2 Example 3 Example 4 Example 5 Raw material type phosphogypsum Desulfurized gypsum Natural gypsum phosphogypsum phosphogypsum Preheating device Cyclone preheater Cyclone preheater Cyclone preheater Vertical preheater Cyclone preheater Moisture content of raw materials entering the kiln (%) 5.0~5.5 4.5~5.0 ~4.0 5.0~5.5 5.0~5.5 Clinker cooling hot air temperature (°C) 780~820 750~790 780~820 760~800 780~820 Temperature of exhaust gas after preheating (°C) 135~145 138~142 140~148 136~143 135~145 Temperature of raw material after preheating (°C) 580~620 570~600 — 560~600 580~620 <![CDATA[Kiln gas SO2 concentration (volume %, before waste heat recovery)]]> 8.2~9.0 8.6~9.5 8.9~9.8 7.8~8.7 7.0~7.8* <![CDATA[SO₂ concentration entering the acid making system (volume %)]]> 7.5~8.5 7.8~8.6 8.0~9.0 7.2~8.0 — <![CDATA[Total SO2 conversion rate (%)]]> 95.5~97.0 96.0~97.2 96.5~97.5 95.5~96.8 — Sulfur yield (%) of the entire process 90~93 91~94 92~94 89~92 — Cement grade 42.5 42.5 42.5 / 52.5 42.5 42.5 Product Model sulfuric acid + cement sulfuric acid + cement sulfuric acid + cement sulfuric acid + cement Sulfur + Cement
[0087] Note: Example 5 is a sulfur production mode. Sulfur in the kiln gas mainly exists in the form of a mixture of elemental sulfur and SO2. The values in the table are estimated values of SO2 volume concentration.
[0088] Industrial applicability
[0089] This invention can be used to construct new gypsum-based acid production and cement co-production plants, as well as to upgrade existing traditional gypsum-based acid production plants. Using this method, without significantly increasing investment in core equipment, the SO2 concentration in the acid production kiln gas can be effectively increased, the equipment specifications of the acid production system can be reduced, the unit product investment and operating energy consumption of the plant can be decreased, the automation control level of the plant can be improved, and the stability and qualification rate of raw materials can be enhanced, thereby achieving long-term stable operation of the plant. Simultaneously, this invention can utilize industrial by-product gypsum such as phosphogypsum and desulfurization gypsum, which helps solve the environmental problems caused by solid waste treatment and stockpiling in related industries, demonstrating good industrial practical value and promising prospects for widespread application.
[0090] The foregoing has only described certain exemplary embodiments of the present invention by way of illustration. Undoubtedly, those skilled in the art can modify the described embodiments in various ways without departing from the spirit and scope of the present invention. Therefore, the foregoing drawings and descriptions are illustrative in nature and should not be construed as limiting the scope of protection of the claims of the present invention.
Claims
1. A method for producing high-concentration SO2 from calcined gypsum, characterized in that, Includes the following steps: S1. Cool the high-temperature clinker after calcination in the rotary kiln and recover the hot air generated during the cooling process; S2. The hot air is introduced into the preheating device to preheat and dehydrate the gypsum raw material that has not yet entered the rotary kiln, and the low-temperature exhaust gas containing water vapor obtained after heat exchange is extracted from the preheating device. S3. Use the extracted low-temperature exhaust gas as a heat source to dry the raw gypsum. S4. The preheated raw material is fed into a rotary kiln for decomposition and calcination, and the SO2-containing kiln gas discharged from the rotary kiln is separately extracted, and after waste heat recovery, it is sent to the acid production system. The low-temperature exhaust gas does not enter the rotary kiln and acid production system, and the SO2-containing kiln gas does not enter the preheating device and the system used to dry raw gypsum.
2. The method of claim 1, wherein the method is characterized by, The preheating device is a cyclone preheater.
3. The method of claim 1, wherein the method is characterized by, The temperature of the hot air is 700-850℃; the temperature of the low-temperature exhaust gas is 130-150℃; and the temperature of the exhaust gas discharged after drying the raw gypsum is 80-90℃.
4. The method of claim 1, wherein the method is characterized by, When the SO2-containing kiln gas enters the acid production system after waste heat recovery, the SO2 volume concentration is 5% to 10%.
5. The method of claim 1, wherein the method is characterized by, It also includes a heat compensation step: when the heat of the low-temperature exhaust gas is insufficient to meet the drying requirements of the raw gypsum, the high-temperature flue gas generated by the boiling hot air furnace is added to the inlet of the drying system and mixed with the low-temperature exhaust gas, and the temperature of the mixed air is adjusted to 180-250°C.
6. A method for producing high-concentration SO2 from calcined gypsum according to claim 5, characterized in that, The boiling hot air furnace is an energy-saving boiling hot air furnace.
7. The method for producing high-concentration SO2 from calcined gypsum according to claim 1, characterized in that, It also includes a sulfur production mode: when switching to sulfur production mode, the air supply in the rotary kiln is reduced and the reducing agent ratio is increased, so that the kiln is in a weak oxygen reducing atmosphere, and the SO2-containing kiln gas discharged from the rotary kiln is switched to the sulfur reduction system.
8. The method of claim 7, wherein the method is characterized by, The weak oxygen reducing atmosphere is defined as an O2 volume concentration of less than 0.5% in the kiln tail flue gas.
9. The method of claim 1, wherein the method is characterized by, The SO2-containing kiln gas is recovered from waste heat and then purified, converted, and absorbed to produce sulfuric acid.
10. The method of claim 1, wherein the method is characterized by, The raw material gypsum is at least one of phosphogypsum, desulfurized gypsum, or natural gypsum.