A method for preparing disc-shaped ferric phosphate based on ferric phosphate slag, and the application of disc-shaped ferric phosphate.

By introducing exogenous monodisperse crystal nuclei under high acidity and low pH conditions, uniformly dispersed disc-shaped iron phosphate was prepared from iron phosphate slag, solving the problem of underutilization of iron phosphate slag and realizing high-value recycling of iron and phosphorus and improving the performance of lithium iron phosphate materials.

CN123105576APending Publication Date: 2026-11-17ZHEJIANG HUAYOU COBALT CO LTD +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611390750.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-08
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies have failed to effectively utilize the phosphorus-iron slag generated after lithium extraction from waste lithium iron phosphate batteries to prepare high-quality, low-cost battery-grade iron phosphate precursors. Furthermore, existing methods for preparing flake iron phosphate are not applicable to phosphorus-iron slag raw materials, making it difficult to achieve a closed-loop recycling process for iron and phosphorus.

Method used

By controlling the acid dissolution and precipitation conversion reactions of ferric phosphate slag, and introducing exogenous monodisperse crystal nuclei in a high acidity and low pH environment, uniformly dispersed disc-shaped ferric phosphate is prepared, avoiding spontaneous crystal nucleus formation and agglomeration. Using simple acid dissolution, granular dihydrate ferric phosphate seed crystals and precipitation conversion reactions, battery-grade ferric phosphate with low aluminum content is prepared.

Benefits of technology

This method enables the high-value recycling of iron phosphate slag, producing uniformly dispersed, non-agglomerated, spherical iron phosphate flakes. This improves the low-temperature performance and rate performance of lithium iron phosphate, reduces grinding energy consumption, and enhances the quality of lithium iron phosphate materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123105576A_ABST
    Figure CN123105576A_ABST
Patent Text Reader

Abstract

This invention provides a method for preparing disc-shaped ferric phosphate from ferrophosphate slag, as well as the disc-shaped ferric phosphate and its applications. The preparation method includes the following steps: adjusting the pH value and element concentration of the ferrophosphate leaching solution obtained by acid dissolution of ferrophosphate slag to obtain a ferrophosphate conditioning solution; the pH of the ferrophosphate conditioning solution is 0.2~1.2, and the ferrophosphate slag contains aluminum; mixing hydrogen peroxide and the ferrophosphate conditioning solution to obtain a solution containing ferric iron; then mixing granular ferric phosphate dihydrate and the solution containing ferric iron to carry out a precipitation conversion reaction to obtain a ferrophosphate reaction slurry; the ferrophosphate reaction slurry is sequentially subjected to solid-liquid separation, washing, and drying to obtain disc-shaped ferric phosphate with an average particle diameter of 200~500nm and an aluminum content ≤50ppm. This invention can utilize ferrophosphate slag to prepare high-quality, low-cost battery-grade ferric phosphate precursors, realizing a closed-loop recycling process and high-value recycling of iron and phosphorus.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of ferric phosphate materials technology, and in particular to a method for preparing disc-shaped ferric phosphate based on ferric phosphate slag, as well as the disc-shaped ferric phosphate and its applications. Background Technology

[0002] In the field of lithium iron phosphate battery recycling, lithium recovery technology is relatively mature, and lithium has been largely recycled at a high value. However, for iron and phosphorus, the phosphorus slag produced after lithium extraction from waste lithium iron phosphate materials is not fully utilized due to its complex composition, high Al content, poor batch stability, and low economic benefits. How to utilize the phosphorus slag produced after lithium extraction to prepare high-quality, low-cost battery-grade iron phosphate precursors, achieving a closed-loop recycling process and high-value recycling of iron and phosphorus, remains one of the key and challenging issues in the current recycling field.

[0003] On the other hand, the differentiated needs of customers regarding winter driving and fast charging are driving lithium iron phosphate batteries to continuously improve their low-temperature performance and rate performance. Reducing the size of lithium iron phosphate to the nanometer scale can significantly reduce charge transfer resistance and shorten the diffusion distance of lithium ions within solid particles, allowing lithium ions to be inserted and extracted more quickly, thereby effectively improving the rate performance and low-temperature performance of lithium iron phosphate.

[0004] Therefore, obtaining nano-lithium iron phosphate particles with uniform particle size, high crystallinity, and low agglomeration is one of the hot research directions that manufacturers are committed to.

[0005] The morphology of the precursor iron phosphate has a significant impact on lithium iron phosphate. Two-dimensional sheet-like iron phosphate sheets are typically only tens or even hundreds of nanometers thick, making it easier to fabricate nanoscale lithium iron phosphate materials. Therefore, many researchers have proposed technical solutions for preparing ultrafine lithium iron phosphate based on sheet-like iron phosphate. Currently, the main technical solutions for preparing sheet-like iron phosphate include the iron-based process, the surfactant-induced method, and the hydrothermal method.

[0006] (1) Iron-based methods or their derivative processes: For example, related technologies have proposed a method for preparing nanosheet iron phosphate using iron black (Fe3O4) and phosphoric acid as raw materials. By controlling the rotation speed, phosphoric acid concentration, and reaction temperature, iron phosphate is preferentially crystallized and grown on one crystal plane, thus preparing nanosheet iron phosphate with a diameter of 600~800nm. Related technologies have also proposed a method for preparing flake iron phosphate using iron red (Fe2O3) and phosphoric acid as raw materials. By adjusting process parameters such as phosphoric acid concentration, the molar ratio of iron red to phosphoric acid, and reaction temperature, flake iron phosphate was obtained.

[0007] (2) Surfactant-induced method: Related technologies disclose a method for preparing spherical iron phosphate based on ferric phosphate slag, as well as the application and uses of spherical iron phosphate. This method introduces nonionic, cationic, or amphoteric surfactants during the synthesis of iron phosphate to obtain spherical iron phosphate with uniform size and an average diameter of 0.3~0.5μm. Related technologies disclose a battery-grade spherical hydrated iron phosphate and its preparation method, which introduces surfactants such as hexadecyltrimethylammonium bromide to obtain spherical iron phosphate with a diameter of 0.3~2μm. Related technologies disclose a spherical dihydrate iron phosphate and its preparation method, which uses morphology control agents such as 1,7-heptanediamine and terephthalic acid to obtain iron phosphate with primary particles in the form of spherical particles and secondary particles in the form of petals.

[0008] (3) Hydrothermal method: Related technologies disclose a method for preparing flake ferric phosphate from titanium dioxide slag, using ferrous sulfate, phosphoric acid, ammonia, and hydrogen peroxide as raw materials and performing a hydrothermal reaction at 120-180℃ to prepare uniformly dispersed flake ferric phosphate. Related technologies disclose a flake ferric phosphate and its preparation method and application, in which oleic alcohol, lower alcohol, iron salt, and phosphate are mixed and subjected to a hydrothermal reaction at 80-180℃ to obtain flake ferric phosphate. Related technologies disclose a morphology-controllable battery-grade ferric phosphate and its preparation method, which is based on a polyol system and obtains spherical flake ferric phosphate with a diameter of approximately 4μm through a hydrothermal reaction.

[0009] However, there is currently no proposed technical solution for preparing flaky iron phosphate from lithium iron phosphate residue after lithium extraction. Existing technical solutions for preparing flaky iron phosphate, such as the iron method, surfactant-induced method, and hydrothermal method, all have certain limitations and are not suitable for iron phosphate residue raw materials. Summary of the Invention

[0010] To address the shortcomings of existing technologies, the present invention aims to provide a method for preparing disc-shaped iron phosphate based on ferrophosphate slag, as well as the disc-shaped iron phosphate and its applications. This method enables the preparation of high-quality, low-cost battery-grade iron phosphate precursors from ferrophosphate slag, achieving a closed-loop recycling process and high-value recycling of iron and phosphorus.

[0011] To achieve this objective, the present invention adopts the following technical solution:

[0012] In a first aspect, the present invention provides a method for preparing disc-shaped ferric phosphate based on ferric phosphate slag, the method comprising the following steps:

[0013] The pH value and the concentration of each element in the ferrophosphorus leaching solution obtained by acid dissolution of ferrophosphorus slag are adjusted to obtain a ferrophosphorus conditioning solution; the pH value of the ferrophosphorus conditioning solution is 0.2~1.2; the ferrophosphorus slag contains aluminum.

[0014] Hydrogen peroxide and the ferric phosphorus conditioning solution are mixed to obtain a solution containing ferric iron. Granular ferric phosphate dihydrate is then mixed with the ferric iron solution to undergo a precipitation conversion reaction, yielding a ferric phosphorus reaction slurry. The ferric phosphorus reaction slurry is subsequently subjected to solid-liquid separation, washing, and drying to obtain disc-shaped ferric phosphate. The average diameter of the primary particles of the disc-shaped ferric phosphate is 200-500 nm, and the aluminum content in the disc-shaped ferric phosphate is ≤50 ppm.

[0015] The principle behind this invention for preparing uniformly dispersed, disc-shaped ferric phosphate lies in controlling the reaction under a high-acidity, low-pH environment. High acidity inhibits the precipitation reaction of ferric phosphate and reduces supersaturation, resulting in the system spontaneously generating very few, or even none, crystal nuclei. By adding externally distributed monodisperse crystal nuclei, ions in the solution continuously deposit and aggregate on the surface of the nuclei, inducing primary particles to assemble along a specific two-dimensional direction through directional attachment, gradually forming a disc-shaped morphology. Compared to spontaneously formed nuclei, the externally distributed monodisperse crystal nuclei have the characteristics of larger primary particle size and are less prone to agglomeration into secondary irregular aggregates. Therefore, the disc-shaped particles formed by the attachment and growth of primary particles on the external crystal nuclei are also less prone to agglomeration.

[0016] Preferably, the preparation of the phosphorus iron slag acid dissolution to obtain the phosphorus iron leaching solution includes: acid dissolution of the phosphorus iron slag produced after lithium extraction, followed by solid-liquid separation to obtain the phosphorus iron leaching solution.

[0017] Preferably, the acid that is acid-soluble includes sulfuric acid and / or hydrochloric acid.

[0018] Preferably, the molar ratio of iron to sulfuric acid in the phosphorus-iron slag is controlled to be n(Fe):n(H2SO4) = 1:1.5~1:4.5.

[0019] Preferably, during the acid dissolution process, the solid content of the ferrophosphate slag is controlled to be 5-30 wt%.

[0020] Preferably, the acid dissolution temperature is 80~100℃.

[0021] Preferably, when the acid to be dissolved is sulfuric acid, the temperature of acid dissolution is 80~100℃; when the acid to be dissolved is hydrochloric acid, the temperature of acid dissolution is 80~90℃.

[0022] Preferably, the acid dissolution time is 0.5 to 5 hours.

[0023] Preferably, the pH adjuster used to adjust the pH of the ferrophosphate leaching solution obtained by acid dissolution of ferrophosphate slag includes any one or a combination of at least two of phosphoric acid, iron powder, or sulfuric acid.

[0024] Preferably, the concentrations of each element include iron concentration, phosphorus concentration, and titanium concentration.

[0025] Preferably, the phosphorus source used to adjust the phosphorus concentration includes phosphoric acid.

[0026] Preferably, the titanium source used to adjust the titanium concentration includes any one or a combination of at least two of titanium sulfate, titanium oxysulfate, citric acid chelated titanium, metatitanic acid solution, or titanic acid solution.

[0027] Preferably, the iron source used to adjust the iron concentration includes ferrous sulfate.

[0028] Preferably, the molar ratio of iron to phosphorus in the phosphorus-iron conditioning solution is 1:1 to 1:1.2.

[0029] Preferably, the molar concentration of iron in the phosphorus-iron conditioning solution is 0.1~1.2 mol / L.

[0030] Preferably, the molar ratio of titanium to iron in the phosphorus-iron conditioning solution is 0.0016:1 to 0.016:1.

[0031] Preferably, the aluminum content in the phosphorus-iron conditioning solution is 30~500ppm.

[0032] Preferably, the molar ratio of hydrogen peroxide to ferrous iron in the phosphorus-iron conditioning solution is (0.55~0.8):1.

[0033] Preferably, the particle size D50 of the ferric phosphate dihydrate is 150~300nm.

[0034] Preferably, the molar ratio of iron in the ferric phosphate dihydrate to iron in the ferric phosphate conditioning solution is 1:100 to 15:100.

[0035] Preferably, the temperature of the precipitation conversion reaction is 80~100℃.

[0036] Preferably, the holding time for the precipitation conversion reaction is 1 to 5 hours.

[0037] Preferably, the ferric phosphorus reaction slurry is subjected to solid-liquid separation to obtain ferric phosphorus mother liquor and a solid phase containing ferric phosphorus in the form of discs.

[0038] Preferably, the ferric phosphate mother liquor is subjected to impurity removal treatment, and the resulting purified ferric phosphate mother liquor is recycled to the acid dissolution step.

[0039] Preferably, the impurity removal treatment includes any one or a combination of at least two of the following: aluminum phosphate precipitation, fluoride precipitation, solvent extraction, or ion exchange.

[0040] Preferably, when the impurity removal method is aluminum phosphate precipitation, the aluminum phosphate precipitation method includes: mixing ferric phosphate mother liquor and iron powder, adjusting the pH to 1.2~1.6, heating to 85~95℃ to form AlPO4 precipitate, and then separating the solid and liquid to obtain purified ferric phosphate mother liquor.

[0041] Preferably, when the impurity removal method is a fluoride precipitation method, the fluoride precipitation method includes: adding fluoride salts to the iron phosphate mother liquor to form AlF3 precipitate, and then performing solid-liquid separation to obtain purified iron phosphate mother liquor.

[0042] Preferably, the fluoride salt comprises ammonium fluoride and / or potassium fluoride.

[0043] As a preferred technical solution of the present invention, a method for preparing disc-shaped ferric phosphate based on ferric phosphate slag is provided, the method comprising the following steps:

[0044] S1. The phosphorus iron slag produced after lithium extraction is acid-dissolved with sulfuric acid at 80~100℃ for 0.5~5h. The solid content of the phosphorus iron slag is controlled at 5~30wt%, and the molar ratio of iron element to sulfuric acid in the phosphorus iron slag is controlled at n(Fe):n(H2SO4)=1:1.5~1:4.5. After solid-liquid separation, phosphorus iron leachate is obtained.

[0045] S2. Adjust the pH of the ferrophosphate leaching solution obtained by acid dissolution of ferrophosphate slag to 0.2~1.2, and adjust the concentrations of phosphorus, iron and titanium. Specifically, adjust the molar ratio of iron to phosphorus to 1:1~1:1.2, the molar concentration of iron to 0.1~1.2 mol / L, and the molar ratio of titanium to iron to 0.0016:1~0.016:1 to obtain the ferrophosphate conditioning solution.

[0046] S3. Mix hydrogen peroxide and the ferric phosphorus conditioning solution, wherein the molar ratio of ferrous iron in the hydrogen peroxide to ferric phosphorus conditioning solution is (0.55~0.8):1, so as to convert all the iron in the ferric phosphorus solution into ferric trivalent ions, thereby obtaining a solution containing ferric trivalent ions; then mix granular ferric dihydrate with a particle size D50 of 150~300nm and the solution containing ferric trivalent ions, wherein the molar ratio of iron in ferric dihydrate to iron in the ferric phosphorus conditioning solution is 1:100~15:100, and heat to 80~100℃ to carry out a precipitation conversion reaction for 1~5h, thereby obtaining a ferric phosphorus reaction slurry;

[0047] S4. The ferric phosphate reaction slurry is subjected to solid-liquid separation to obtain ferric phosphate mother liquor and ferric phosphate solid phase containing disc-shaped ferric phosphate. The ferric phosphate solid phase containing disc-shaped ferric phosphate is washed and dried to obtain disc-shaped ferric phosphate.

[0048] S5. The ferric phosphate mother liquor is treated to remove impurities, and the purified ferric phosphate mother liquor is recycled to the acid dissolution step in step S1.

[0049] In a second aspect, the present invention provides a disc-shaped ferric phosphate, wherein the disc-shaped ferric phosphate is prepared by the method for preparing disc-shaped ferric phosphate based on ferric phosphate slag as described in the first aspect.

[0050] Preferably, the primary particles of the ferric phosphate in the disc shape are disc-shaped or elliptical.

[0051] Preferably, the average diameter of the primary particles of the disc-shaped iron phosphate is 200~500 nm.

[0052] Preferably, the thickness of the disc-shaped iron phosphate is 1~30 nm.

[0053] Preferably, the aluminum content in the disc-shaped iron phosphate is ≤50ppm.

[0054] Preferably, the disc-shaped iron phosphate is doped with titanium.

[0055] Preferably, the titanium content in the disc-shaped iron phosphate is 500~3000ppm.

[0056] Preferably, the iron-phosphorus molar ratio of the disc-shaped iron phosphate is (97.0~98.0):100.

[0057] Preferably, the half-peak width of the disc-shaped iron phosphate in the main XRD peak is between 0.175 and 0.185.

[0058] Thirdly, the present invention provides an application of the disc-shaped iron phosphate described in the second aspect in a battery.

[0059] The circular iron phosphate provided by this invention can be made into nano-lithium iron phosphate material with rounded particles, clear boundaries, and non-adhesive particles by high-temperature solid-state method. The primary average particle size of the nano-lithium iron phosphate material is 200~500nm.

[0060] Compared with the prior art, the present invention has at least the following beneficial effects:

[0061] (1) The method for preparing spherical iron phosphate based on ferric phosphate slag provided by the present invention is simple, has few control parameters, and can obtain spherical iron phosphate with regular morphology, uniform dispersion and no need for any surfactant.

[0062] (2) The method for preparing spherical iron phosphate based on ferrophosphate slag provided by the present invention can prepare battery-grade iron phosphate with low aluminum content using ferrophosphate slag. The aluminum content in the spherical iron phosphate obtained is less than 26 ppm, preferably less than 25 ppm, and it has high compatibility with ferrophosphate slag raw materials.

[0063] (3) The disc-shaped iron phosphate provided by the present invention has the characteristics of uniform dispersion and non-agglomeration of particles. When preparing lithium iron phosphate, it has the advantages of high grinding efficiency and low grinding energy consumption. There is no obvious hard agglomeration between particles. After being made into lithium iron phosphate, it can still maintain the characteristics of monodispersity, which has a significant effect on improving the low temperature performance and rate performance of lithium iron phosphate. Attached Figure Description

[0064] Figure 1 This is a schematic diagram of the process for preparing disc-shaped iron phosphate based on iron phosphate slag according to a specific embodiment of the present invention.

[0065] Figure 2 This is a schematic diagram illustrating the principle of preparing disc-shaped ferric phosphate based on ferric phosphate slag provided by the present invention.

[0066] Figure 3 This is an SEM image of the ferric phosphate seed crystals before grinding used in the method for preparing disc-shaped ferric phosphate based on ferric phosphate slag provided in Embodiment 1 of the present invention.

[0067] Figure 4 This is a SEM image of the ground iron phosphate seed crystals used in the method for preparing disc-shaped iron phosphate based on iron phosphate slag provided in Embodiment 1 of the present invention.

[0068] Figure 5 This is a particle size distribution diagram of the ground ferric phosphate seed crystals used in the method for preparing disc-shaped ferric phosphate based on ferric phosphate slag provided in Embodiment 1 of the present invention.

[0069] Figure 6 This is a SEM image of ferric phosphate prepared by the method for preparing disc-shaped ferric phosphate based on ferric phosphate slag provided in Example 1 of the present invention.

[0070] Figure 7 This is a SEM image of ferric phosphate prepared by the method for preparing disc-shaped ferric phosphate based on ferric phosphate slag provided in Embodiment 2 of the present invention.

[0071] Figure 8 This is a SEM image of ferric phosphate prepared by the method for preparing disc-shaped ferric phosphate based on ferric phosphate slag provided in Example 3 of the present invention.

[0072] Figure 9 This is a SEM image of ferric phosphate prepared by the method for preparing disc-shaped ferric phosphate based on ferric phosphate slag provided in Example 10 of the present invention.

[0073] Figure 10 This is a SEM image of ferric phosphate prepared by the method for preparing disc-shaped ferric phosphate based on ferric phosphate slag provided in Example 11 of the present invention.

[0074] Figure 11 This is a SEM image of the seed precipitate formed in the initial stage of the reaction in the method for preparing disc-shaped iron phosphate based on iron phosphate slag provided in Comparative Example 1 of this invention.

[0075] Figure 12 This is a SEM image of the ferric phosphate prepared by the method for preparing disc-shaped ferric phosphate based on ferric phosphate slag provided in Comparative Example 1 of this invention.

[0076] Figure 13This is a SEM image of the ferric phosphate prepared by the method for preparing disc-shaped ferric phosphate based on ferric phosphate slag provided in Comparative Example 2 of the present invention.

[0077] Figure 14 This is a SEM image of the ferric phosphate seed crystals used in the method for preparing disc-shaped ferric phosphate based on ferric phosphate slag provided in Comparative Example 3 of this invention.

[0078] Figure 15 This is a SEM image of the ferric phosphate prepared by the method for preparing disc-shaped ferric phosphate based on ferric phosphate slag provided in Comparative Example 3 of this invention.

[0079] Figure 16 This is a SEM image of lithium iron phosphate material prepared from disc-shaped iron phosphate in Example 1 of the present invention.

[0080] Figure 17 This is a SEM image of the lithium iron phosphate material prepared from iron phosphate in Comparative Example 3 of this invention. Detailed Implementation

[0081] To facilitate understanding of the present invention, the following embodiments are provided. Those skilled in the art should understand that these embodiments are merely illustrative and should not be construed as limiting the scope of the invention.

[0082] As a specific embodiment of the present invention, a method for preparing disc-shaped ferric phosphate based on ferric phosphate slag is provided, the method comprising the following steps:

[0083] The pH value and element concentration of the ferrophosphorus leaching solution obtained by acid dissolution of ferrophosphorus slag are adjusted to obtain a ferrophosphorus conditioning solution. The pH value of the ferrophosphorus conditioning solution is 0.2~1.2; the aluminum content in the ferrophosphorus conditioning solution is 30~500ppm.

[0084] Hydrogen peroxide and the ferric phosphorus conditioning solution are mixed to obtain a solution containing ferric iron. Granular ferric phosphate dihydrate is then mixed with the ferric iron solution to undergo a precipitation conversion reaction, yielding a ferric phosphorus reaction slurry. The ferric phosphorus reaction slurry is subsequently subjected to solid-liquid separation, washing, and drying to obtain disc-shaped ferric phosphate. The average diameter of the primary particles of the disc-shaped ferric phosphate is 200-500 nm, and the aluminum content in the disc-shaped ferric phosphate is ≤50 ppm.

[0085] Iron phosphate slag refers to the residue remaining after the waste lithium iron phosphate batteries are crushed, sorted, and lithium extracted. It contains impurities such as aluminum and copper. When using iron phosphate slag as raw material to prepare iron phosphate using the traditional hydrothermal method, these impurities easily enter the iron phosphate product, affecting its quality. This invention, through simple acid dissolution, the addition of granular iron phosphate dihydrate seed crystals, and a precipitation conversion reaction, enables the preparation of iron phosphate from iron phosphate slag, achieving a closed-loop recycling process and high-value recycling of iron and phosphorus.

[0086] The principle behind this invention's ability to prepare uniformly dispersed, disc-shaped iron phosphate is that, as... Figure 2 As shown, the present invention controls the reaction to proceed under a high acidity and low pH environment. High acidity helps suppress the precipitation reaction of ferric phosphate and reduces supersaturation, ensuring that the system can only spontaneously generate very few or no crystal nuclei. This is achieved by adding monodisperse crystal nuclei (…). Figure 2 As shown in A1, ions in the solution continuously deposit and accumulate on the surface of the crystal nucleus, such as... Figure 2 As shown in A2-A3, the induced primary particles assemble along a specific two-dimensional direction in a directional attachment manner, gradually forming a disc-like morphology (e.g., ...). Figure 2 As shown in Figure A4. Compared to spontaneously formed nuclei, imported monodisperse nuclei have the characteristics of larger primary particle size and are less prone to agglomeration into secondary irregular aggregates. Therefore, the disc-shaped particles formed by the attachment and growth of primary particles on imported nuclei are also less likely to agglomerate. The initial nuclei spontaneously formed in the system (such as…) Figure 2 As shown in B1, their size is often only a few nanometers or tens of nanometers, their surface energy is large, and they spontaneously aggregate into irregular aggregates. Figure 2 As shown in B2), Figure 2 As shown in B3, subsequent primary particles attach and grow on irregular aggregates, resulting in severe aggregation of ferric phosphate dihydrate (e.g., Figure 2 (As shown in B4).

[0087] In a specific embodiment, the pH of the phosphorus-iron adjusting solution is 0.2 to 1.2, for example, it can be 0.2, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1, 1.1 or 1.2, etc., but is not limited to the listed values. Other unlisted values ​​within this range are also applicable.

[0088] This invention controls the reaction to proceed under a strong acid and low pH environment, where a high acid environment inhibits the precipitation of ferric phosphate and aluminum phosphate. The reaction is carried out below the critical pH for AlPO4 precipitation. Ferric phosphate seed crystals are introduced to induce precipitation, allowing iron and phosphate ions to enter the precipitate, while aluminum ions remain in the mother liquor, thus achieving the preparation of low-aluminum ferric phosphate.

[0089] In some specific embodiments, the ferrophosphate slag comprises ferric phosphate and ferrous pyrophosphate, etc.

[0090] In some specific embodiments, the phosphorus-iron slag includes impurities such as aluminum, copper, and fluorine.

[0091] In some specific embodiments, the iron content in the phosphorus-iron slag is 28-36%, the phosphorus content is 17-20%, the aluminum content is 1-10%, the copper content is 0.5-10%, and the fluorine content is 0.01-3%.

[0092] In some specific embodiments, the preparation of the phosphorus iron slag acid dissolution to obtain the phosphorus iron leachate includes: acid dissolution of the phosphorus iron slag produced after lithium extraction, followed by solid-liquid separation to obtain the phosphorus iron leachate.

[0093] In some specific embodiments, the acid to be dissolved includes sulfuric acid and / or hydrochloric acid. It may also include purified ferric phosphate mother liquor obtained from the subsequent solid-liquid separation of the ferric phosphate reaction slurry after impurity removal treatment.

[0094] In some specific embodiments, the molar ratio of iron to sulfuric acid in the phosphate slag is controlled to be n(Fe):n(H2SO4) = 1:1.5 to 1:4.5, for example, it can be 1:1.5, 1:1.8, 1:2.0, 1:2.2, 1:2.3, 1:2.5, 1:2.8, 1:3.0, 1:3.2, 1:3.5, 1:3.8, 1:4.0, 1:4.2 or 1:4.5, etc., but is not limited to the listed values, and other unlisted values ​​within this range are also applicable.

[0095] In some specific embodiments, during the acid dissolution process, the solid content of the ferrophosphate slag is controlled to be 5-30 wt%, for example, it can be 5 wt%, 8 wt%, 11 wt%, 14 wt%, 17 wt%, 19 wt%, 22 wt%, 25 wt%, 28 wt%, or 30 wt%, etc., but is not limited to the listed values. Other unlisted values ​​within this range are also applicable.

[0096] In some specific embodiments, the acid dissolution temperature is 80~100℃, for example, it can be 80℃, 83℃, 85℃, 87℃, 89℃, 92℃, 94℃, 96℃, 98℃ or 100℃, etc., but is not limited to the listed values, and other unlisted values ​​within this range are also applicable.

[0097] In some specific embodiments, when the acid to be dissolved is sulfuric acid, the temperature of acid dissolution is 80~100℃; when the acid to be dissolved is hydrochloric acid, the temperature of acid dissolution is 80~90℃.

[0098] In some specific embodiments, the acid dissolution time is 0.5 to 5 hours, for example, it can be 0.5 hours, 1 hour, 1.5 hours, 2 hours, 2.5 hours, 3 hours, 3.5 hours, 4 hours, 4.5 hours or 5 hours, but is not limited to the listed values. Other unlisted values ​​within this range are also applicable.

[0099] In some specific embodiments, the pH adjuster used to adjust the pH of the ferrophosphate leaching solution obtained by acid dissolution of ferrophosphate slag includes any one or a combination of at least two of phosphoric acid, iron powder, or sulfuric acid.

[0100] When the pH of the ferrophosphate leachate is higher than 1.2, sulfuric acid or phosphoric acid is added to adjust the pH; when the pH of the ferrophosphate leachate is lower than 0.2, iron powder is added to adjust the pH.

[0101] In some specific embodiments, the concentrations of each element include iron concentration, phosphorus concentration, and titanium concentration.

[0102] In some specific implementations, the phosphorus source used to adjust the phosphorus concentration includes phosphoric acid.

[0103] In some specific embodiments, the titanium source used to adjust the titanium concentration includes any one or a combination of at least two of titanium sulfate, titanium oxysulfate, citrate chelated titanium, metatitanic acid solution, or titanic acid solution. Typical but non-limiting combinations include combinations of titanium sulfate and titanium oxysulfate, combinations of citrate chelated titanium and titanium oxysulfate, combinations of titanium sulfate and citrate chelated titanium, combinations of metatitanic acid solution and titanium oxysulfate, and combinations of metatitanic acid solution and titanic acid solution.

[0104] In some specific implementations, the iron source used to adjust the iron concentration includes ferrous sulfate.

[0105] In some specific embodiments, the molar ratio of iron to phosphorus in the phosphorus-iron conditioning solution is 1:1 to 1:1.2, for example, it can be 1:1, 1:1.02, 1:1.05, 1:1.08, 1:1.1, 1:1.11, 1:1.12, 1:1.15, 1:1.17, 1:1.18 or 1:2, etc., but is not limited to the listed values. Other unlisted values ​​within this range are also applicable.

[0106] In some specific embodiments, the molar concentration of iron in the phosphorus-iron conditioning solution is 0.1~1.2 mol / L, for example, it can be 0.1 mol / L, 0.3 mol / L, 0.4 mol / L, 0.5 mol / L, 0.6 mol / L, 0.8 mol / L, 0.9 mol / L, 1 mol / L, 1.1 mol / L or 1.2 mol / L, but is not limited to the listed values. Other unlisted values ​​within this range are also applicable.

[0107] In some specific embodiments, the molar ratio of titanium to iron in the phosphorus-iron conditioning solution is 0.0016:1 to 0.016:1, for example, it can be 0.0016:1, 0.0032:1, 0.004:1, 0.006:1, 0.008:1, 0.009:1, 0.011:1, 0.012:1, 0.014:1 or 0.016:1, etc., but is not limited to the listed values. Other unlisted values ​​within this range are also applicable.

[0108] In some specific embodiments, the aluminum content in the phosphorus-iron conditioning solution is 30~500ppm, for example, it can be 30ppm, 83ppm, 135ppm, 187ppm, 239ppm, 292ppm, 344ppm, 396ppm, 448ppm or 500ppm, but is not limited to the listed values, and other unlisted values ​​within this range are also applicable.

[0109] In some specific embodiments, the molar ratio of hydrogen peroxide to ferrous iron in the phosphorus-iron conditioning solution is (0.55~0.8):1, for example, it can be 0.55:1, 0.56:1, 0.58:1, 0.59:1, 0.6:1, 0.62:1, 0.65:1, 0.68:1, 0.7:1, 0.75:1, 0.78:1 or 0.8:1, etc., but is not limited to the listed values. Other unlisted values ​​within this range are also applicable.

[0110] In some specific embodiments, the particle size D50 of the ferric phosphate dihydrate is 150~300nm, for example, it can be 150nm, 180nm, 200nm, 210nm, 220nm, 230nm, 245nm, 250nm, 260nm, 270nm, 280nm or 300nm, but is not limited to the listed values. Other unlisted values ​​within this range are also applicable.

[0111] When the size of ferric phosphate dihydrate is outside the above range, the ferric phosphate dihydrate should be ground first so that the added ferric phosphate seed crystals are within the above range and have a uniform granular morphology, thereby improving the purity and performance of the obtained ferric phosphate product.

[0112] In some specific embodiments, the molar ratio of iron in the ferric phosphate dihydrate to iron in the ferric phosphate conditioning solution is 1:100 to 15:100, for example, it can be 1:100, 3:100, 5:100, 6:100, 8:100, 9:100, 11:100, 12:100, 14:100 or 15:100, but is not limited to the listed values. Other unlisted values ​​within this range are also applicable.

[0113] In some specific embodiments, the temperature of the precipitation conversion reaction is 80~100℃, for example, it can be 80℃, 83℃, 85℃, 87℃, 89℃, 92℃, 94℃, 96℃, 98℃ or 100℃, but is not limited to the listed values. Other unlisted values ​​within this range are also applicable.

[0114] In some specific embodiments, the holding time for the precipitation conversion reaction is 1 to 5 hours, for example, it can be 1 hour, 1.5 hours, 1.9 hours, 2.4 hours, 2.8 hours, 3.3 hours, 3.7 hours, 4.2 hours, 4.6 hours or 5 hours, but is not limited to the listed values. Other unlisted values ​​within this range are also applicable.

[0115] In some specific embodiments, the ferric phosphorus reaction slurry is subjected to solid-liquid separation to obtain ferric phosphorus mother liquor and a solid phase containing ferric phosphorus in the form of discs.

[0116] In some specific embodiments, the ferric phosphate mother liquor is subjected to impurity removal treatment, and the resulting purified ferric phosphate mother liquor is recycled to the acid dissolution step.

[0117] The impurity removal treatment described in this invention is a commonly used method for removing aluminum from phosphorus-containing solutions in the industry. However, the impurity removal treatment can also be adapted to the actual process.

[0118] This invention enables low-cost recycling of ferrophosphate slag, featuring recyclable conversion mother liquor, low acid consumption during ferrophosphate slag dissolution, and low alkali usage during ferrophosphate precipitation. Specifically, this invention prepares ferrophosphate in a strongly acidic, low-pH environment using a seed-induced method. This eliminates the need for pH adjusters such as ammonia or liquid alkali; furthermore, the conversion mother liquor retains its high acidity and low pH characteristics, allowing it to be reused for dissolving ferrophosphate slag. This saves on mother liquor treatment costs and reduces acid usage during ferrophosphate slag dissolution.

[0119] In some specific embodiments, the impurity removal treatment includes any one or a combination of at least two of the following: aluminum phosphate precipitation, fluoride precipitation, solvent extraction, or ion exchange. The purpose is to remove or partially remove unprecipitated aluminum ions from the ferric phosphate mother liquor, acting as an open path for impurity aluminum ions and preventing the continuous accumulation of aluminum in the ferric phosphate solution during the reuse of the mother liquor, which would affect the aluminum content of the finished ferric phosphate product.

[0120] In some specific embodiments, when the impurity removal method is aluminum phosphate precipitation, the aluminum phosphate precipitation method includes: mixing ferric phosphate mother liquor and iron powder, adjusting the pH to 1.2~1.6, raising the temperature to 85~95℃ to form AlPO4 precipitate, and then separating the solid and liquid to obtain purified ferric phosphate mother liquor.

[0121] For example, the pH is increased to 1.2-1.6, such as 1.2, 1.21, 1.22, 1.23, 1.25, 1.3, 1.35, 1.4, 1.45, 1.5, or 1.6, but not limited to the listed values; other unlisted values ​​within this range are also applicable. The temperature for forming AlPO4 precipitate by heating to 85-95°C is exemplarily 85°C, 86°C, 87°C, 88°C, 89°C, 90°C, 91°C, 92°C, 93°C, 94°C, or 95°C, but not limited to the listed values; other unlisted values ​​within this range are also applicable.

[0122] In some specific embodiments, when the impurity removal method is a fluoride precipitation method, the fluoride precipitation method includes: adding fluoride salts to the iron phosphate mother liquor to form AlF3 precipitate, and then performing solid-liquid separation to obtain purified iron phosphate mother liquor.

[0123] In some specific embodiments, the fluoride salt includes ammonium fluoride and / or potassium fluoride.

[0124] When the impurity removal process is solvent extraction, the specific principle of impurity removal is to use a specific extractant (such as P-15 extractant) to transfer aluminum ions from the aqueous phase to the organic phase, thereby achieving separation.

[0125] When the impurity removal process is ion exchange, the specific principle is to use the functional groups on the ion exchange resin to adsorb aluminum ions in the solution, thereby achieving the purpose of purifying the iron phosphate mother liquor.

[0126] As a preferred technical solution of the present invention, a method for preparing disc-shaped ferric phosphate based on ferric phosphate slag is provided, such as... Figure 1 As shown, the method includes the following steps:

[0127] S1. The phosphorus iron slag produced after lithium extraction is acid-dissolved with sulfuric acid at 80~100℃ for 0.5~5h. The solid content of the phosphorus iron slag is controlled at 5~30wt%, and the molar ratio of iron element to sulfuric acid in the phosphorus iron slag is controlled at n(Fe):n(H2SO4)=1:1.5~1:4.5. After solid-liquid separation, phosphorus iron leachate is obtained.

[0128] S2. Adjust the concentrations of phosphorus, iron, and titanium in the phosphorus-iron leachate obtained by acid dissolution of phosphorus-iron slag. Specifically, adjust the molar ratio of iron to phosphorus to 1:1~1:1.2, the molar concentration of iron to 0.1~1.2 mol / L, the molar ratio of titanium to iron to 0.0016:1~0.016:1, and adjust the pH value to 0.2~1.2 to obtain the phosphorus-iron conditioning solution.

[0129] S3. Mix hydrogen peroxide and the ferric phosphorus conditioning solution, wherein the molar ratio of ferrous iron in the hydrogen peroxide to ferric phosphorus conditioning solution is (0.55~0.8):1, so as to convert all the iron in the ferric phosphorus solution into ferric trivalent ions, thereby obtaining a solution containing ferric trivalent ions; then mix granular ferric dihydrate with a particle size D50 of 150~300nm and the solution containing ferric trivalent ions, wherein the molar ratio of iron in ferric dihydrate to iron in the ferric phosphorus conditioning solution is 1:100~15:100, and heat to 80~100℃ to carry out a precipitation conversion reaction for 1~5h, thereby obtaining a ferric phosphorus reaction slurry;

[0130] S4. The ferric phosphate reaction slurry is subjected to solid-liquid separation to obtain ferric phosphate mother liquor and ferric phosphate solid phase containing disc-shaped ferric phosphate. The ferric phosphate solid phase containing disc-shaped ferric phosphate is washed and dried to obtain disc-shaped ferric phosphate.

[0131] S5. The ferric phosphate mother liquor is treated to remove impurities, and the purified ferric phosphate mother liquor is recycled to the acid dissolution step in step S1.

[0132] The present invention does not impose any special restrictions on the solid-liquid separation in the above process. Any device and method known to those skilled in the art for solid-liquid separation can be used. It can also be adjusted according to the actual process. For example, it can be filtration, centrifugation or sedimentation separation, or a combination of different methods.

[0133] The present invention does not impose any special restrictions on the drying process described above. Any device and method known to those skilled in the art for drying can be used. Adjustments can also be made according to the actual process. For example, it can be air drying, vacuum drying, oven drying, or freeze drying, or a combination of different methods.

[0134] As another specific embodiment of the present invention, a circular ferric phosphate is provided, wherein the circular ferric phosphate is prepared by any of the methods described above for preparing circular ferric phosphate based on ferric phosphate slag.

[0135] The circular iron phosphate particles of the present invention are round, clearly defined, and do not stick together, making them well applicable in the subsequent preparation of lithium iron phosphate.

[0136] In some specific embodiments, the primary particles of the ferric phosphate in the form of discs are discs or ellipses.

[0137] In some specific embodiments, the average diameter of the primary particles of the disc-shaped iron phosphate is 200~500nm, for example, it can be 200nm, 234nm, 267nm, 300nm, 334nm, 367nm, 400nm, 434nm, 467nm or 500nm, but is not limited to the listed values. Other unlisted values ​​within this range are also applicable.

[0138] In some specific embodiments, the thickness of the disc-shaped iron phosphate is 1~30nm, for example, it can be 1nm, 5nm, 8nm, 11nm, 14nm, 18nm, 21nm, 24nm, 27nm or 30nm, but is not limited to the listed values. Other unlisted values ​​within this range are also applicable.

[0139] In some specific embodiments, the aluminum content in the disc-shaped ferric phosphate is ≤50ppm, for example, it can be 1ppm, 7ppm, 12ppm, 18ppm, 23ppm, 29ppm, 34ppm, 40ppm, 45ppm or 50ppm, etc., but is not limited to the listed values, and other unlisted values ​​within this range are also applicable.

[0140] In some specific embodiments, the disc-shaped iron phosphate is doped with titanium.

[0141] In some specific embodiments, the titanium content in the disc-shaped ferric phosphate is 500~3000ppm, for example, it can be 500ppm, 770ppm, 1050ppm, 1300ppm, 1600ppm, 1880ppm, 2160ppm, 2440ppm, 2720ppm or 3000ppm, but is not limited to the listed values, other unlisted values ​​within this range are also applicable.

[0142] In some specific embodiments, the iron-phosphorus molar ratio of the disc-shaped ferric phosphate is (97.0~98.0):100, for example, it can be 97.0:100, 97.2:100, 97.3:100, 97.4:100, 97.5:100, 97.6:100, 97.7:100, 97.8:100, 97.9:100 or 98.0:100, etc., but is not limited to the listed values, and other unlisted values ​​within this range are also applicable.

[0143] In some specific embodiments, the full width at half maximum (FWHM) of the main XRD peak of the disc-shaped iron phosphate is between 0.175 and 0.185, for example, it can be 0.175, 0.176, 0.177, 0.178, 0.179, 0.180, 0.181, 0.182, 0.183, 0.184 or 0.185, etc., but is not limited to the listed values. Other unlisted values ​​within this range are also applicable.

[0144] In this invention, the main peak of the circular iron phosphate in XRD refers to the position of the highest peak in the XRD spectrum, which is generally 2θ at the position of 19~22°.

[0145] As another specific embodiment of the present invention, an application of the disc-shaped iron phosphate described in the second aspect is provided in a battery.

[0146] The circular iron phosphate provided by this invention can be prepared into nano-lithium iron phosphate material with rounded particles, clear boundaries, and non-adhesion between particles by high-temperature solid-state method. The primary average particle size of the nano-lithium iron phosphate material is 50~100nm, for example, it can be 50nm, 56nm, 62nm, 67nm, 73nm, 78nm, 84nm, 89nm, 95nm or 100nm, but is not limited to the listed values. Other unlisted values ​​within this range are also applicable.

[0147] In some specific embodiments, the high-temperature solid-state method includes: mixing the above-mentioned disc-shaped iron phosphate, carbon source, lithium source and dopant source, adding water to adjust the solid content to a certain range, and then spray-drying the ground slurry to obtain lithium iron phosphate yellow material, then sintering it at high temperature to obtain lithium iron phosphate black material, and finally obtaining lithium iron phosphate after airflow crushing.

[0148] In some specific implementations, the carbon source includes glucose, carbon nanotubes, carbon black, and polyethylene glycol, among others.

[0149] In some specific implementations, the lithium source includes lithium phosphate and / or lithium carbonate, etc.

[0150] In some specific embodiments, the dopant source includes a titanium source, which includes titanium oxide.

[0151] In some specific embodiments, the solid content within a certain range is 30-40%, for example, it can be 30%, 31%, 32%, 33%, 34%, 35%, 36%, 37%, 38%, 39% or 40%, etc.

[0152] In some specific embodiments, the grinding process in the preparation of the above-mentioned lithium iron phosphate is to grind to D50=300±20nm.

[0153] In some specific embodiments, the high-temperature sintering temperature is 700~800℃, for example, it can be 700℃, 710℃, 720℃, 730℃, 740℃, 750℃, 760℃, 770℃, 780℃ or 800℃, etc.

[0154] The following detailed description uses specific examples.

[0155] Example 1

[0156] This embodiment provides a method for preparing disc-shaped ferric phosphate based on ferric phosphate slag, the method comprising the following steps:

[0157] S1. The phosphorus iron slag produced after lithium extraction is acid-dissolved with sulfuric acid at 90℃ for 3 hours. The solid content of the phosphorus iron slag is controlled at 25wt%, and the molar ratio of iron element to sulfuric acid in the phosphorus iron slag is controlled at n(Fe):n(H2SO4)=1:3.0. After filtration, phosphorus iron leachate is obtained.

[0158] S2. Adjust the concentrations of phosphorus, iron, and titanium in the phosphorus ferrophosphate leachate obtained by acid dissolution of phosphorus ferrophosphate slag. Specifically, adjust the molar ratio of iron to phosphorus to 1:1.15, the molar concentration of iron to 0.8 mol / L, the molar ratio of titanium to iron to 0.005:1, and adjust the pH value to 0.7 to obtain the phosphorus ferrophosphate conditioning solution.

[0159] S3. Mix hydrogen peroxide and the ferric phosphate conditioning solution, wherein the molar ratio of divalent iron in the hydrogen peroxide to divalent iron in the ferric phosphate conditioning solution is 0.6:1, to convert all iron in the ferric phosphate solution into ferric ions, thereby obtaining a solution containing ferric ions; then mix in granular ferric phosphate dihydrate seed crystals with a particle size D50 of 263 nm that have been ground (see...). Figures 4-5 The iron in the ferric phosphate dihydrate solution and the iron in the ferric phosphorus conditioning solution are in a molar ratio of 5:100. The mixture is heated to 95°C for 2 hours to carry out a precipitation conversion reaction to obtain a ferric phosphorus reaction slurry.

[0160] S4. The ferric phosphorus reaction slurry is filtered sequentially to obtain ferric phosphorus mother liquor and ferric phosphorus solid phase containing disc-shaped ferric phosphorus. The ferric phosphorus solid phase containing disc-shaped ferric phosphorus is washed and dried to obtain disc-shaped ferric phosphorus.

[0161] Figure 3 The iron phosphate dihydrate seed crystals used in the embodiments of the present invention before grinding. Figure 4 The SEM images of the iron phosphate dihydrate seed crystals (granular iron phosphate dihydrate seed crystals after grinding) used in the embodiments of the present invention are shown, as follows. Figure 4 As shown, the foreign seed crystals, after grinding, still retained their granular morphology and were more uniform in size, exhibiting a nano-particle morphology. The primary particles were nanoparticles with good dispersion among them. The particle size of the ground granular iron phosphate dihydrate seed crystals was measured using a laser particle size analyzer. Figure 5 The particle size distribution diagram of the granular iron phosphate dihydrate seed crystals after grinding treatment used in Example 1 of this invention is shown. Figure 5 It can be seen that the particle size D50 of the iron phosphate dihydrate seed crystals after grinding is 263 nm.

[0162] Figure 6 The following is a scanning electron microscope (SEM) image of the circular iron phosphate pellets prepared according to Example 1 of the present invention, as shown. Figure 6 As shown, the ferric phosphate dihydrate prepared in Example 1 has a disc-like morphology, and the average diameter of the disc-like primary particles is about 300 nm.

[0163] Example 2

[0164] This embodiment provides a method for preparing disc-shaped ferric phosphate based on ferric phosphate slag, the method comprising the following steps:

[0165] S1. The phosphorus iron slag produced after lithium extraction is acid-dissolved with sulfuric acid at 80℃ for 5 hours. The solid content of the phosphorus iron slag is controlled at 30wt%, and the molar ratio of iron element to sulfuric acid in the phosphorus iron slag is controlled at n(Fe):n(H2SO4)=1:1.5. After filtration, phosphorus iron leachate is obtained.

[0166] S2. Adjust the concentrations of phosphorus, iron, and titanium in the phosphorus ferrophosphate leachate obtained by acid dissolution of phosphorus ferrophosphate slag. Specifically, adjust the molar ratio of iron to phosphorus to 1:1.1, the molar concentration of iron to 0.8 mol / L, the molar ratio of titanium to iron to 0.006:1, and adjust the pH value to 0.4 to obtain the phosphorus ferrophosphate conditioning solution.

[0167] S3. Mix hydrogen peroxide and the ferric phosphorus conditioning solution, wherein the molar ratio of ferrous iron in the hydrogen peroxide to ferric phosphorus conditioning solution is 0.55:1, so as to convert all the iron in the ferric phosphorus solution into ferric trivalent ions, thereby obtaining a solution containing ferric trivalent ions; then mix granular ferric dihydrate with a particle size D50 of 150 nm that has been ground and the solution containing ferric trivalent ions, wherein the molar ratio of iron in the ferric dihydrate to the iron in the ferric phosphorus conditioning solution is 10:100, and heat to 96°C for precipitation conversion reaction for 3 hours to obtain ferric phosphorus reaction slurry;

[0168] S4. The ferric phosphorus reaction slurry is filtered sequentially to obtain ferric phosphorus mother liquor and ferric phosphorus solid phase containing disc-shaped ferric phosphorus. The ferric phosphorus solid phase containing disc-shaped ferric phosphorus is washed and dried to obtain disc-shaped ferric phosphorus.

[0169] Figure 7 The image shows a scanning electron microscope (SEM) image of the circular iron phosphate prepared in Example 2 of the present invention. As shown in the figure, the iron phosphate dihydrate prepared in Example 2 has a circular morphology.

[0170] Example 3

[0171] This embodiment provides a method for preparing disc-shaped ferric phosphate based on ferric phosphate slag, the method comprising the following steps:

[0172] S1. The phosphorus iron slag produced after lithium extraction is acid-dissolved with sulfuric acid at 100℃ for 0.5h. The solid content of the phosphorus iron slag is controlled at 5wt%, and the molar ratio of iron element to sulfuric acid in the phosphorus iron slag is controlled at n(Fe):n(H2SO4)=1:4.5. After filtration, phosphorus iron leachate is obtained.

[0173] S2. Adjust the concentrations of phosphorus, iron, and titanium in the phosphorus ferrophosphate leachate obtained by acid dissolution of phosphorus ferrophosphate slag. Specifically, adjust the molar ratio of iron to phosphorus to 1:1.2, the molar concentration of iron to 0.8 mol / L, the molar ratio of titanium to iron to 0.0016:1, and adjust the pH value to 0.2 to obtain the phosphorus ferrophosphate conditioning solution.

[0174] S3. Mix hydrogen peroxide and the ferric phosphorus conditioning solution, wherein the molar ratio of divalent iron in the hydrogen peroxide to that in the ferric phosphorus conditioning solution is 0.8:1, so as to convert all the iron in the ferric phosphorus solution into ferric trivalent ions, thereby obtaining a solution containing ferric trivalent ions; then mix granular ferric dihydrate with a particle size D50 of 300 nm that has been ground and the solution containing ferric trivalent ions, wherein the molar ratio of iron in the ferric dihydrate to that in the ferric phosphorus conditioning solution is 2:100, and heat to 93°C to carry out a precipitation conversion reaction for 4 hours to obtain a ferric phosphorus reaction slurry;

[0175] S4. The ferric phosphorus reaction slurry is filtered sequentially to obtain ferric phosphorus mother liquor and ferric phosphorus solid phase containing disc-shaped ferric phosphorus. The ferric phosphorus solid phase containing disc-shaped ferric phosphorus is washed and dried to obtain disc-shaped ferric phosphorus.

[0176] Figure 8 The image shows a scanning electron microscope (SEM) image of the disc-shaped ferric phosphate prepared in Example 3 of the present invention. As shown in the figure, the ferric phosphate dihydrate prepared in Example 3 has a disc-shaped morphology.

[0177] Example 4

[0178] This embodiment provides a method for preparing disc-shaped ferric phosphate based on ferric phosphate slag. The ferric phosphate slag in the method is the same as in Example 1, except that aluminum sulfate is added to the ferric phosphate conditioning solution to make the aluminum content in the ferric phosphate conditioning solution 100 ppm. The rest is the same as in Example 1 and will not be repeated here.

[0179] Example 5

[0180] This embodiment provides a method for preparing disc-shaped ferric phosphate based on ferric phosphate slag. Except for the ferric phosphate slag, which is the same as in Example 1, aluminum sulfate is added to the ferric phosphate conditioning solution to make the aluminum content in the ferric phosphate conditioning solution 400 ppm. The rest of the method is the same as in Example 1 and will not be repeated here.

[0181] Example 6

[0182] This embodiment provides a method for preparing disc-shaped iron phosphate based on ferrophosphate slag. The method is the same as in Example 1 except that the molar concentration of iron in the ferrophosphate conditioning solution is 1.2 mol / L, but the molar ratio of titanium and phosphorus to iron remains unchanged. Therefore, it will not be described again here.

[0183] Example 7

[0184] This embodiment provides a method for preparing disc-shaped iron phosphate based on ferrophosphate slag. The method is the same as in Example 1 except that the molar concentration of iron in the ferrophosphate conditioning solution is 0.6 mol / L, but the molar ratio of titanium and phosphorus to iron remains unchanged. It will not be described again here.

[0185] Example 8

[0186] This embodiment provides a method for preparing disc-shaped ferric phosphate based on ferric phosphate slag. The method is the same as in Example 1 except that the molar concentration of iron in the ferric phosphate conditioning solution is 0.1 mol / L, but the molar ratio of titanium and phosphorus to iron remains unchanged. It will not be described again here.

[0187] Example 9

[0188] This embodiment provides a method for preparing disc-shaped iron phosphate based on iron phosphate slag. Except that the sulfuric acid used to dissolve the iron phosphate slag is composed of the conversion mother liquor produced in Example 1 and the newly added sulfuric acid, the method is the same as that in Example 1, and will not be repeated here.

[0189] Example 10

[0190] This embodiment provides a method for preparing disc-shaped ferric phosphate based on ferric phosphate slag. Except for step S3, where the molar ratio of iron in ferric phosphate dihydrate to iron in the ferric phosphate adjusting solution is 0.5:100, the method is the same as in Example 1 and will not be repeated here.

[0191] When the amount of seed crystals added is too small, the size of the disc-shaped primary particles becomes larger (>500nm). Although the size of the disc-shaped primary particles of lithium iron phosphate can be increased by reducing the amount of seed crystals added, the excessively large particle size is not conducive to the subsequent preparation of nanoscale lithium iron phosphate materials. Figure 9 The image shows a scanning electron microscope (SEM) image of the disc-shaped iron phosphate prepared in Example 10 of this invention, as follows: Figure 9 As shown, the resulting disc-shaped iron phosphate pieces are larger than expected.

[0192] Example 11

[0193] This embodiment provides a method for preparing disc-shaped ferric phosphate based on ferric phosphate slag. Except for the molar ratio of iron in ferric phosphate dihydrate to iron in the ferric phosphate adjusting solution in step S3 being 18:100, the method is the same as in Example 1 and will not be repeated here.

[0194] When too much seed crystal is added in Example 11, the size of the disc-shaped primary particles becomes smaller (about 50 nm). Although nanoscale disc-shaped iron phosphate can be obtained by increasing the amount of seed crystal added, the excessively small particle size will make the slurry difficult to filter and wash.

[0195] As can be seen from Examples 1 and 10-11, the present invention preferably controls the amount of ferric phosphate dihydrate seed crystals added within a reasonable range, which can improve the roundness and purity of the obtained ferric phosphate product.

[0196] Comparative Example 1

[0197] This comparative example provides a method for preparing disc-shaped ferric phosphate based on ferric phosphate slag. Except that ferric phosphate dihydrate is not added as a seed crystal in step S3, and the pH of the ferric phosphate adjusting solution is adjusted to 1.6 in step S2 so that phosphorus and iron can be completely precipitated, allowing the system to spontaneously generate a large number of crystal nuclei, the rest of the method is the same as in Example 1, and will not be repeated here.

[0198] The SEM image of the seed crystals formed spontaneously by the system in this comparative example is shown below. Figure 11 As shown, from Figure 11 It can be seen that the seed crystals formed by the spontaneous reaction of the system exhibit severe particle adhesion and agglomeration.

[0199] The ferric phosphate prepared in this comparative example is as follows: Figure 12 As shown, compared with Example 1, Comparative Example 1 has a higher reaction pH (pH=1.6), higher supersaturation, smaller spontaneously formed seed crystal size, larger surface energy, and more severe agglomeration. When the particles attach and grow on the seed crystal surface, they will form a severely agglomerated aggregate morphology.

[0200] Comparative Example 2

[0201] This comparative example provides a method for preparing disc-shaped ferric phosphate based on ferric phosphate slag. Except that ferric phosphate dihydrate is not added as a seed crystal in step S3, and the pH of the ferric phosphate adjusting solution is adjusted to a pH value of 1.0 in step S2 so that phosphorus and iron can begin to precipitate, allowing the system to spontaneously generate a small number of crystal nuclei, the rest of the method is the same as in Example 1, and will not be repeated here.

[0202] The ferric phosphate prepared in this comparative example is as follows: Figure 13 As shown, compared to Example 1, due to the lack of external seed crystals to induce precipitation, the spontaneous precipitation driving force of ferric phosphate was insufficient under the lower pH condition (pH=1.0), making it difficult for iron and phosphorus elements to precipitate completely. Therefore, the iron yield was low (21 g / L of iron ions in the mother liquor did not precipitate), and the SEM image of ferric phosphate showed the presence of some underdeveloped particles.

[0203] Comparative Example 3

[0204] This comparative example provides a method for preparing disc-shaped iron phosphate based on iron phosphate slag. Except for the disc-shaped iron phosphate dihydrate seed crystals in step S3, the method is the same as that in Example 1, and will not be repeated here.

[0205] The SEM image of the iron phosphate dihydrate crystal used in this comparative example is shown below. Figure 14 As shown, the seed crystal has a disc-like morphology. Figure 15 The SEM image of the iron phosphate obtained in Comparative Example 3 is shown. When the disc-shaped iron phosphate is used as a seed crystal for heterogeneous nucleation, iron phosphate molecules will aggregate and grow on the disc-shaped particles, eventually forming spherical particles. Therefore, the SEM image of the prepared iron phosphate shows both disc-shaped and spherical primary particles, making it difficult to obtain iron phosphate of the desired shape.

[0206] Comparative Example 4

[0207] This comparative example provides a method for preparing disc-shaped ferric phosphate based on ferric phosphate slag. Except for adjusting the pH of the ferric phosphate conditioning solution to 1.3, the method is the same as in Example 1 and will not be repeated here.

[0208] Comparative Example 5

[0209] This comparative example provides a method for preparing disc-shaped ferric phosphate. The method is the same as that of Comparative Example 1, except that the ferric phosphate conditioning solution is replaced with a ferric phosphate solution with the same concentrations of phosphorus, iron and titanium and the same pH. It will not be described again here.

[0210] Test method: The iron, phosphorus and aluminum contents of the disc-shaped iron phosphate were obtained by ICP test, and the iron-phosphorus mass ratio was calculated.

[0211] The test results of the above embodiments and comparative examples are shown in Table 1.

[0212] Table 1

[0213]

[0214] As can be seen from Table 1:

[0215] (1) Based on the experimental results of Example 1, Comparative Example 1 and Comparative Example 2, it is shown that without the use of seed crystals for induced precipitation (Comparative Example 1 and Comparative Example 2), the iron phosphate formed at low pH is not fully developed and the iron yield is low; at high pH, ​​the spontaneously formed iron phosphate crystal nuclei are severely agglomerated, and the final iron phosphate has poor dispersion and the primary particles are not disc-shaped.

[0216] (2) Based on the experimental results of Example 1 and Comparative Example 3, it is shown that when seed crystals are introduced for induced precipitation, the morphology and size of the seed crystals have a significant impact on the final dispersion of iron phosphate. When the seed crystals are not ground, they will result in the final morphology agglomeration.

[0217] (3) The ferric phosphate prepared in Comparative Example 4 of this invention is similar to that in Example 1, also exhibiting a disc-like morphology. However, since the precipitation reaction in Comparative Example 4 was carried out at a higher pH, aluminum elements also entered the ferric phosphate precipitate. Compared with the low aluminum content (Al=16ppm) in Example 1, the aluminum content in Comparative Example 4 is at a higher level (Al=152ppm). Combining the experimental results of Examples 1-3 and Comparative Example 4, it is shown that under the induction effect of the grinding treatment seed crystals, monodisperse disc-like ferric phosphate can be prepared regardless of the reaction pH. However, when the reaction pH is too high (Comparative Example 4, pH=1.3), the Al content in the ferric phosphate will exceed the standard.

[0218] (4) As can be seen from Examples 1, 4, and 5, the method for preparing disc-shaped ferric phosphate based on ferric phosphate slag provided by the present invention can produce ferric phosphate with low aluminum content for ferric phosphate conditioning solutions with different aluminum contents, below the theoretical critical pH for aluminum phosphate precipitation, by using a seed-induced precipitation method. The technical solution provided by the present invention is applicable to ferric phosphate liquid raw materials with different impurity contents.

[0219] (5) As can be seen from the comprehensive examples 1 and 6-8, the method for preparing ferric phosphate in round pieces from ferric phosphate slag provided by the present invention can prepare ferric phosphate in round pieces with low aluminum content for ferric phosphate conditioning solutions with different phosphorus and iron contents.

[0220] (6) As can be seen from the combined examples 1 and 9, the iron phosphate mother liquor in the method for preparing ferric phosphate flakes provided by the present invention can be recycled and does not affect the quality of the prepared iron phosphate product.

[0221] In summary, the method for preparing disc-shaped iron phosphate based on iron phosphate slag provided by this invention can utilize iron phosphate slag to prepare high-quality, low-cost battery-grade iron phosphate precursors, achieving a closed-loop recycling process and high-value recycling of iron and phosphorus.

[0222] Taking the iron phosphate obtained in Example 1 and Comparative Example 3 as examples, lithium iron phosphate material was prepared by solid-state sintering. The methods and equipment used in the preparation of lithium iron phosphate are consistent with those commonly used in the industry. The specific preparation process of this invention is as follows: 3 kg of iron phosphate, 168 g of glucose, 240 g of polyethylene glycol (molecular weight 2000), 753 g of lithium carbonate, and 15 g of nano-titanium dioxide were weighed, and water was added to adjust the solid content to 35%. The mixture was then ground to a slurry with a D50 of 300 ± 20 nm. The slurry was spray-dried to obtain lithium iron phosphate yellow material, which was then sintered at 770°C to obtain lithium iron phosphate black material. Finally, lithium iron phosphate was obtained by airflow crushing.

[0223] Figure 16 The image shows a SEM image of lithium iron phosphate prepared from the disc-shaped iron phosphate in Example 1 of this invention. Figure 16 As shown, the prepared lithium iron phosphate particles are dispersed in one stage without obvious adhesion or agglomeration. When the above lithium iron phosphate is made into a button cell, the disc-shaped lithium iron phosphate prepared in Example 1 exhibits extremely high rate performance, with a 0.1C discharge capacity of 161.34 mAh / g, a 1C discharge capacity of 156.42 mAh / g, and a 5C discharge capacity of 146.15 mAh / g.

[0224] Figure 17 The SEM images of lithium iron phosphate prepared from the iron phosphate in Comparative Example 3 of this invention are shown. Because the iron phosphate prepared in Comparative Example 3 contains both spherical and flake-shaped iron phosphate particles, the flake-shaped iron phosphate particles are dispersed, resulting in highly dispersed lithium iron phosphate particles. The spherical iron phosphate particles agglomerate, resulting in larger lithium iron phosphate particles with poor separation between primary particles. Therefore, the corresponding SEM images of lithium iron phosphate simultaneously show dispersed nanoscale lithium iron phosphate particles, lithium iron phosphate agglomerates with multiple particles adhering together, and larger lithium iron phosphate particles.

[0225] The present invention has been illustrated with the above embodiments to illustrate its detailed features, but the present invention is not limited to the above detailed features, that is, it does not mean that the present invention must rely on the above detailed features to be implemented. Those skilled in the art should understand that any improvements to the present invention, equivalent substitutions for the selected technical features, additions of auxiliary technical features, and selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A method for preparing disc-shaped ferric phosphate based on ferric phosphate slag, characterized in that, The method includes the following steps: The pH value and element concentration of the ferrophosphate leaching solution obtained by acid dissolution of ferrophosphate slag are adjusted to obtain a ferrophosphate conditioning solution; the pH value of the ferrophosphate conditioning solution is 0.2~1.2; the ferrophosphate slag contains aluminum; Hydrogen peroxide and the ferric phosphorus conditioning solution are mixed to obtain a solution containing ferric iron; then granular ferric phosphate dihydrate and the solution containing ferric iron are mixed to carry out a precipitation conversion reaction to obtain a ferric phosphorus reaction slurry; The ferric phosphate reaction slurry is subjected to solid-liquid separation, washing and drying in sequence to obtain spherical ferric phosphate. The average diameter of the primary particles of the spherical ferric phosphate is 200~500nm, and the aluminum content in the spherical ferric phosphate is ≤50ppm.

2. The method according to claim 1, characterized in that, The preparation of the phosphorus iron slag acid dissolution solution obtained by the phosphorus iron slag includes: acid dissolution of the phosphorus iron slag produced after lithium extraction, followed by solid-liquid separation to obtain the phosphorus iron leaching solution; The acid that is acid-soluble includes sulfuric acid and / or hydrochloric acid; The molar ratio of iron to sulfuric acid in the phosphorus-iron slag is controlled to be n(Fe):n(H2SO4) = 1:1.5~1:4.5; During the acid dissolution process, the solid content of the ferrophosphate slag is controlled at 5-30 wt%. The acid dissolution temperature is 80~100℃; The acid dissolution time is 0.5~5h.

3. The method according to claim 1 or 2, characterized in that, The pH adjuster used to adjust the pH of the ferrophosphate leaching solution obtained by acid dissolution of ferrophosphate slag includes any one or a combination of at least two of phosphoric acid, iron powder, or sulfuric acid.

4. The method according to claim 1, characterized in that, The concentrations of each element include iron concentration, phosphorus concentration, and titanium concentration; Phosphorus sources used to adjust phosphorus concentration include phosphoric acid; The titanium source used to adjust the titanium concentration includes any one or a combination of at least two of titanium sulfate, titanium oxysulfate, citrate chelated titanium, metatitanic acid solution or titanic acid solution. The iron source used to adjust the iron concentration includes ferrous sulfate.

5. The method according to claim 1, characterized in that, The phosphorus-iron conditioning solution satisfies at least one of the following conditions: A1. The molar ratio of iron to phosphorus in the phosphorus-iron conditioning solution is 1:1 to 1:1.2; A2. The molar concentration of iron in the phosphorus-iron conditioning solution is 0.1~1.2 mol / L; A3. The molar ratio of titanium to iron in the phosphorus-iron conditioning solution is 0.0016:1 to 0.016:1; A4. The aluminum content in the phosphorus-iron conditioning solution is 30~500ppm.

6. The method according to claim 1, characterized in that, The method satisfies at least one of the following conditions: B1. The molar ratio of hydrogen peroxide to ferrous iron in the phosphorus-iron conditioning solution is (0.55~0.8):1; B2. The particle size D50 of the ferric phosphate dihydrate is 150~300nm; B3. The molar ratio of iron in the iron dihydrate to iron in the iron phosphate conditioning solution is 1:100 to 15:

100. B4. The temperature of the precipitation conversion reaction is 80~100℃; B5. The holding time for the precipitation conversion reaction is 1~5h.

7. The method according to claim 1, characterized in that, The ferric phosphate reaction slurry was subjected to solid-liquid separation to obtain ferric phosphate mother liquor and a solid phase containing ferric phosphate in the form of discs; The ferric phosphate mother liquor is treated to remove impurities, and the resulting purified ferric phosphate mother liquor is recycled to the acid dissolution step. The impurity removal process includes any one or a combination of at least two of the following: aluminum phosphate precipitation, fluoride precipitation, solvent extraction, or ion exchange. When the impurity removal method is aluminum phosphate precipitation, the aluminum phosphate precipitation method includes: mixing iron phosphate mother liquor and iron powder, adjusting the pH to 1.2~1.6, raising the temperature to 85~95℃ to form AlPO4 precipitate, and then separating the solid and liquid to obtain purified iron phosphate mother liquor. Alternatively, when the impurity removal method is a fluoride precipitation method, the fluoride precipitation method includes: adding fluoride salts to the iron phosphate mother liquor to form AlF3 precipitate, and then performing solid-liquid separation to obtain purified iron phosphate mother liquor; wherein the fluoride salts include ammonium fluoride and / or potassium fluoride.

8. A type of circular flake-shaped iron phosphate, characterized in that, The disc-shaped ferric phosphate is prepared by the method for preparing disc-shaped ferric phosphate based on ferric phosphate slag as described in any one of claims 1 to 7.

9. The disc-shaped ferric phosphate according to claim 8, characterized in that, The disc-shaped iron phosphate must satisfy at least one of the following conditions: C1. The primary particles of the circular iron phosphate are circular or elliptical in shape; C2. The average diameter of the primary particles of the circular iron phosphate is 200~500nm; C3. The thickness of the disc-shaped iron phosphate is 1~30nm; C4. The aluminum content in the disc-shaped ferric phosphate is ≤50ppm; C5. The disc-shaped iron phosphate is doped with titanium. C6. The titanium content in the disc-shaped iron phosphate is 500~3000 ppm; C7. The iron-phosphorus molar ratio of the circular iron phosphate is (97.0~98.0):

100.

10. The use of the disc-shaped iron phosphate as described in claim 8 or 9 in a battery.