A method for preparing sodium iron phosphate (Na4Fe3(PO4)2(P2O7)) cathode material for sodium-ion batteries by recycling waste lithium iron phosphate electrodes.

By combining the NMP solvent method and the sulfuric acid-hydrogen peroxide system with a carbon source reducing agent, the problems of aluminum impurity introduction and performance degradation in the lithium iron phosphate recycling process were solved, achieving efficient preparation of high-performance NFPP materials and improving resource utilization and battery performance.

CN123105586APending Publication Date: 2026-11-17MINGGUANG HENGCHUANG RUINENG NEW ENERGY TECHNOLOGY CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611377403.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-07
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In existing technologies, the recycling process of lithium iron phosphate is cumbersome and costly, and it is easy to introduce aluminum impurities, which leads to a decline in the performance of sodium-ion battery cathode materials, low resource utilization, and difficulty in achieving high-value processing.

Method used

Aluminum foil was peeled off using the NMP solvent method, and lithium was selectively leached using a sulfuric acid-hydrogen peroxide system. Subsequently, a carbon source was used as a reducing agent and a conductive coating agent to achieve iron reduction and carbon coating in one step during high-temperature sintering, thus preparing sodium iron pyrophosphate Na4Fe3(PO4)2(P2O7).

Benefits of technology

The entire composition of lithium, iron, and phosphorus elements has been utilized to prepare NFPP materials with high crystallinity and excellent conductivity. These materials exhibit excellent rate performance and long-term cycle stability, making them suitable for small-batch laboratory production and industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123105586A_ABST
    Figure CN123105586A_ABST
Patent Text Reader

Abstract

This invention belongs to the field of battery material recycling and sodium-ion battery cathode material preparation, and discloses a method for preparing sodium iron phosphate pyrophosphate (NFPP) cathode material using waste lithium iron phosphate electrode sheets. The method includes: S1, subjecting the waste electrode sheets to NMP constant-temperature immersion with assisted ultrasonic treatment, peeling off the aluminum foil, drying and grinding to obtain lithium iron phosphate electrode sheet powder; S2, selectively leaching lithium using a sulfuric acid-hydrogen peroxide system, separating the solid and liquid to obtain a lithium-containing filtrate and phospho-iron slag, washing the phospho-iron slag, supplementing with sodium, phosphorus, and carbon sources, ball milling, and drying to obtain an NFPP precursor; S3, sintering the precursor at high temperature under a high-purity nitrogen atmosphere to achieve trivalent iron reduction and in-situ carbon coating in one step, cooling and grinding to obtain the NFPP cathode material. This invention achieves a lithium leaching rate >91%, realizing high-value resource utilization of phospho-iron slag; the product has high crystallinity and few impurities, possessing excellent rate performance and cycle stability, with a short process flow, suitable for industrial production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of battery material recycling and sodium-ion battery cathode material preparation technology, specifically involving a method for preparing sodium-ion battery cathode material Na4Fe3(PO4)2(P2O7) by recycling waste lithium iron phosphate electrode sheets. Background Technology

[0002] With the rapid development of the new energy industry, lithium iron phosphate batteries have been widely used in power and energy storage fields, and a large-scale retirement wave is imminent. Currently, the mainstream process for lithium iron phosphate recycling is wet lithium extraction, which generates a large amount of phosphorus iron slag. Direct discharge of this slag not only wastes resources but also puts pressure on the environment. The high-value resource utilization of phosphorus iron slag has become an urgent problem to be solved in the industry.

[0003] Sodium-ion batteries, with their advantages of abundant resources, low cost, and excellent safety performance, have shown great promise in the field of large-scale energy storage. Sodium iron phosphate pyrophosphate (NFPP), as a polyanionic cathode material, possesses a stable three-dimensional framework structure and excellent ion conductivity, making it a highly promising cathode material for sodium-ion batteries. Using the phosphorus slag generated from the recycling of lithium iron phosphate as raw material to prepare NFPP can achieve high-value recycling of iron and phosphorus elements, combining economic and environmental benefits.

[0004] In the prior art, CN119349539A discloses a method for recycling lithium iron phosphate into sodium-ion battery cathode material. This method involves ball milling and activating waste lithium iron phosphate material with phosphorus and iron sources, followed by lithium-sodium ion conversion with a sodium source under a reducing atmosphere to obtain the target material. However, this process is cumbersome, has a long heat treatment cycle, and lithium elements are easily volatilized and lost at high temperatures, resulting in high industrial production costs. CN119370817A discloses a method for preparing waste lithium iron phosphate into sodium iron pyrophosphate, which involves wet oxidation-reduction de-powdering, solid-liquid separation, and ball milling sintering to obtain the product. However, this process easily introduces aluminum impurities when peeling off the electrode under strong acid conditions, and the high concentration of sulfate in the filtrate increases the difficulty and cost of lithium salt purification. Furthermore, after oxidation leaching, iron exists in a trivalent form; insufficient reduction during sintering can easily lead to material structural failure and decreased electrochemical performance. Additionally, residual fluorine in the binder can affect the material's crystallinity.

[0005] Therefore, developing a method for preparing NFPP cathode materials from waste lithium iron phosphate with a short process flow, low impurity content, and excellent product performance is of great significance for promoting the coordinated development of the battery recycling industry and the sodium-ion battery industry. Summary of the Invention

[0006] Therefore, it is necessary to provide a method for preparing sodium iron phosphate (Na4Fe3(PO4)2(P2O7)) cathode material for sodium-ion batteries by recycling waste lithium iron phosphate electrodes to address the above problems.

[0007] S1. After cutting the waste lithium iron phosphate electrode sheets, immerse them in NMP solution and sonicate them to completely peel off the aluminum foil. After filtration, washing and drying, grind and sieve to obtain lithium iron phosphate electrode sheet powder. S2. Take the above lithium iron phosphate electrode powder and leach it under sulfuric acid and hydrogen peroxide conditions, controlling the pH of the leaching endpoint to be 2.0~3.0. After solid-liquid separation, obtain phosphorus iron slag filter cake and lithium-containing filtrate. Wash the phosphorus iron slag to neutral and dry it. Use the phosphorus iron slag as a base to supplement sodium source, phosphorus source and carbon source. Put it into a ball mill for grinding and spray drying to obtain light gray NFPP precursor powder. S3. The NFPP precursor powder is placed in a tube furnace, an inert atmosphere is introduced, and it is sintered at a high temperature of 300~600℃. After natural cooling, it is ground and sieved to obtain sodium iron phosphate pyrophosphate cathode material powder.

[0008] Preferably, in step S1, the soaking is carried out at 50~100℃ and a solid-liquid ratio of 1:3~1:5 (g:mL) with NMP constant temperature stirring for 2~8h; the ultrasonic treatment power is 100~500W and the ultrasonic time is 10~60min; and the grinding and filtration is grinding through a 100~400 mesh sieve.

[0009] Preferably, in step S1 and step S2, the specific conditions for acid leaching are as follows: lithium iron phosphate electrode powder and water are mixed at a solid-liquid ratio of 1:2.5~3.75g:mL to form a slurry; concentrated sulfuric acid is added, with a ratio of concentrated sulfuric acid to lithium iron phosphate electrode powder of 0.175~0.25mL:1g; hydrogen peroxide is then added, with a ratio of hydrogen peroxide to lithium iron phosphate electrode powder of 1~3mL:1g; the leaching temperature is 60~100℃, and the stirring time is 2~8h.

[0010] Preferably, in step S2, sodium, phosphorus and carbon sources are added during the preparation process in a Na:Fe:P molar ratio of 4:2.96 to 3:4. The sodium source is one or more of anhydrous sodium carbonate, sodium bicarbonate, sodium hydroxide, anhydrous sodium acetate, and anhydrous sodium oxalate. The phosphorus source is one or more of the following: ammonium dihydrogen phosphate, diammonium hydrogen phosphate, ammonium phosphate, sodium dihydrogen phosphate, phosphoric acid, and ammonium pyrophosphate. The carbon source is one or more of glucose, sucrose, fructose, sorbitol, and D-mannitol.

[0011] Preferably, in step S2, the amount of carbon source added is calculated in terms of carbon elements, and the final carbon coating mass fraction in the material is 0.5%~6%.

[0012] Preferably, in step S2, the mixing ball milling involves preparing the ingredients into an aqueous suspension with a solid content of 20% to 40%, placing it in a planetary ball mill, and ball milling it at a speed of 1500 to 3000 r / min for 7 to 10 hours, with zirconia balls as the grinding media; after ball milling, spray drying or oven drying is performed, and the precursor powder is obtained after crushing.

[0013] Preferably, when using spray drying, the inlet air temperature is 150~220℃ and the outlet air temperature is 80~120℃.

[0014] Preferably, in step S3, the inert atmosphere is high-purity nitrogen gas with a flow rate of 50~200mL / min; the heating rate of the high-temperature sintering is 2~6℃ / min, and the holding time is 7~15h.

[0015] Preferably, in step S3, the grinding and sieving is performed through a standard sieve of 100-400 mesh.

[0016] Preferably, during the acid leaching process in step S2, the lithium leaching rate is >91%, and the resulting lithium-containing filtrate is used for the subsequent preparation of lithium carbonate.

[0017] 1. High resource utilization rate: The aluminum foil is stripped using the NMP solvent method, avoiding aluminum impurities introduced by strong acid stripping, and high-purity lithium iron phosphate powder is obtained; lithium is selectively leached through the sulfuric acid-hydrogen peroxide system, with a lithium leaching rate of >91%. The phosphorus iron slag after leaching is directly used to prepare NFPP cathode material, realizing the full-component resource utilization of lithium, iron and phosphorus elements and solving the problem of phosphorus iron slag treatment.

[0018] 2. Integrated reduction and coating: Using carbon source as both reducing agent and conductive coating agent, the reduction of ferric iron and carbon coating are achieved in one step during high-temperature sintering. This ensures the accuracy of the valence state of ferrous iron in the target material and forms a uniform carbon coating layer in situ to improve the conductivity of the material. No additional steps are required, and the process flow is short.

[0019] 3. Excellent product performance: By precisely controlling the proportion of ingredients and the sintering process, the obtained NFPP material has high crystallinity, pure phase, and uniform particle size. It has excellent rate performance and long cycle stability. The discharge specific capacity at 0.5C rate can reach more than 108mAh / g, and the capacity retention rate after 100 cycles is >95%.

[0020] 4. Strong process adaptability: The overall process is simple to operate and the parameters are controllable. It is suitable for small-batch preparation in the laboratory and can also be scaled up to achieve industrial production through processes such as spray drying, and has good prospects for industrial application. Attached Figure Description

[0021] Figure 1 This is a process flow diagram for preparing NFPP cathode material from lithium iron phosphate according to the present invention.

[0022] Figure 2 The diagram shows the capacity coulomb efficiency for different number of cycles obtained in Example 1.

[0023] Figure 3 The graphs show charge-discharge test results obtained in Example 1 at different cycle numbers.

[0024] Figure 4 The magnification test chart is obtained from Example 2.

[0025] Figure 5 The above are charge-discharge test results obtained in Example 2 at different rates.

[0026] Figure 6 The graph shows the long-cycle performance obtained in Example 3.

[0027] Figure 7 The XRD results are for the sodium-ion cathode material obtained in Example 1.

[0028] Figure 8 The SEM results are for the sodium-ion cathode material obtained in Example 1.

[0029] Figure 9 The EDS test results are for the sodium-ion cathode material obtained in Example 1. Detailed Implementation

[0030] To make the above-mentioned objects, features, and advantages of the present invention more apparent and understandable, specific embodiments of the present invention are described in detail below. Many specific details are set forth in the following description to provide a thorough understanding of the present invention. However, the present invention can be practiced in many other ways different from those described herein, and those skilled in the art can make similar modifications without departing from the spirit of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.

[0031] As used herein, the terms “prepared from” and “comprising” are synonymous. The terms “comprising,” “including,” “having,” “containing,” or any other variations thereof, as used herein, are intended to cover non-exclusive inclusion. For example, a composition, step, method, article, or apparatus that includes the listed elements is not necessarily limited to those elements, but may include other elements not expressly listed or elements inherent to such composition, step, method, article, or apparatus.

[0032] When a quantity, concentration, or other value or parameter is expressed as a range, a preferred range, or a range defined by a series of upper and lower preferred values, this should be understood as specifically disclosing all ranges formed by any pair of any upper or preferred value with any lower or preferred value, regardless of whether the range is disclosed individually. For example, when the range “1 to 5” is disclosed, the described range should be interpreted as including the ranges “1 to 4”, “1 to 3”, “1 to 2”, “1 to 2 and 4 to 5”, “1 to 3 and 5”, etc. When numerical ranges are described herein, unless otherwise stated, the range is intended to include its endpoints and all integers and fractions within that range.

[0033] Furthermore, the indefinite articles “a” and “an” preceding the elements or components of this invention do not impose any limitation on the quantity requirement (i.e., the number of times) of the elements or components. Therefore, “an” or “a” should be interpreted as including one or at least one, and the singular form of an element or component also includes the plural form, unless the quantity clearly refers to the singular form.

[0034] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. The terminology used herein in the description of the invention is for the purpose of describing particular embodiments only and is not intended to be limiting of the invention. The term "and / or" as used herein includes any and all combinations of one or more of the associated listed items.

[0035] A method for preparing sodium-ion battery cathode NFPP material by recycling waste lithium iron phosphate electrode sheets includes: S1. After cutting the waste lithium iron phosphate electrode sheets, immerse them in NMP solution and sonicate them to completely peel off the aluminum foil. After filtration, washing and drying, grind and sieve to obtain lithium iron phosphate electrode sheet powder. S2. Take 8g of the above lithium iron phosphate electrode powder and leach it under sulfuric acid and hydrogen peroxide conditions. Control the pH of the leaching endpoint to be 2.0~3.0. After solid-liquid separation, obtain phosphorus iron slag filter cake and lithium-containing filtrate. Wash the phosphorus iron slag to neutral and dry it. Use the phosphorus iron slag as a base to supplement sodium source, phosphorus source and carbon source. Put it into a ball mill for grinding and spray drying to obtain light gray NFPP precursor powder. S3. The NFPP precursor powder is placed in a tube furnace, an inert atmosphere is introduced, and it is sintered at a high temperature of 300~600℃. After natural cooling, it is ground and sieved to obtain sodium iron phosphate pyrophosphate cathode material powder. The high-temperature calcination temperature is higher than the melting point of the sodium source, such as 300℃, 350℃, 400℃, 450℃, 500℃, 550℃, 600℃, etc.

[0036] Further, in step S1, the soaking is carried out at 60~100℃, for example 60℃, 70℃, 80℃, 90℃, 100℃, etc., with a solid-liquid ratio of 1:3~1:5 (g:mL), under constant temperature stirring with NMP for 2~8h; for example 2h, 3h, 4h, 5h, 6h, 7h, 8h, etc. The ultrasonic treatment power is 100~500W, the ultrasonic time is 10~60min, and the grinding and filtration is grinding through a 100~400 mesh sieve.

[0037] Further, in step S1 and step S2, the specific conditions for acid leaching are as follows: Lithium iron phosphate electrode powder and water are mixed at a solid-liquid ratio of 1:2.5~3.75g:mL to form a slurry; concentrated sulfuric acid is added, with a ratio of concentrated sulfuric acid to lithium iron phosphate electrode powder of 0.175~0.25mL:1g; hydrogen peroxide is then added, with a ratio of hydrogen peroxide to lithium iron phosphate electrode powder of 1~3mL:1g; the leaching temperature is 60~100℃, for example, 60℃, 70℃, 80℃, 90℃, 100℃, etc.; the stirring time is 2~8h, for example, 2h, 3h, 4h, 5h, 6h, 7h, 8h, etc.

[0038] Furthermore, in step S2, sodium, phosphorus, and carbon sources are added during the preparation process according to a Na:Fe:P molar ratio of 4:2.96 to 3:4. The sodium source is one or more of anhydrous sodium carbonate, sodium bicarbonate, sodium hydroxide, anhydrous sodium acetate, and anhydrous sodium oxalate. The phosphorus source is one or more of the following: ammonium dihydrogen phosphate, diammonium hydrogen phosphate, ammonium phosphate, sodium dihydrogen phosphate, phosphoric acid, and ammonium pyrophosphate. The carbon source is one or more of glucose, sucrose, fructose, sorbitol, and D-mannitol.

[0039] Furthermore, in step S2, the amount of carbon source added is calculated in terms of carbon elements, and the final carbon coating mass fraction in the material is 0.5%~6%.

[0040] Further, in step S2, the mixing and ball milling involves preparing the ingredients into an aqueous suspension with a solid content of 20% to 40%, placing it in a planetary ball mill, and ball milling it at a speed of 1500 to 3000 r / min for 7 to 10 hours, using zirconia balls as the grinding media; after ball milling, it is spray-dried or oven-dried, and then crushed to obtain precursor powder. The speeds are, for example, 1500 r / min, 1750 r / min, 2000 r / min, 2250 r / min, 2500 r / min, 2750 r / min, 3000 r / min, etc.; the ball milling times are, for example, 7 hours, 7.5 hours, 8 hours, 8.5 hours, 9 hours, 9.5 hours, 10 hours.

[0041] Furthermore, when using spray drying, the inlet air temperature is 150~220℃ and the outlet air temperature is 80~120℃.

[0042] Further, in step S3, the inert atmosphere is high-purity nitrogen gas with a flow rate of 50~200 mL / min; the heating rate of the high-temperature sintering is 2~6℃ / min, for example, 2℃ / min, 3℃ / min, 4℃ / min, 5℃ / min, 6℃ / min, etc.; the holding time is 7~15h, for example, 7h, 8h, 9h, 10h, 11h, 12h, 13h, 14h, 15h, etc.

[0043] Furthermore, in step S3, the grinding and sieving is performed through a standard sieve of 100-400 mesh.

[0044] Furthermore, during the acid leaching process in step S2, the lithium leaching rate is >91%, and the resulting lithium-containing filtrate is used for the subsequent preparation of lithium carbonate.

[0045] The present invention also provides a sodium-ion battery, including the aforementioned sodium-ion cathode material.

[0046] To facilitate understanding of the present invention, the present invention will be described more fully and in detail below with reference to the accompanying drawings and preferred embodiments, but the scope of protection of the present invention is not limited to the following specific embodiments.

[0047] The waste lithium iron phosphate electrode sheets used in the following examples are all retired power lithium iron phosphate battery positive electrode sheets, with lithium iron phosphate as the active material, PVDF as the binder, and aluminum foil as the current collector; all chemical reagents used are commercially available analytical grade reagents. The typical basic composition of the phosphate slag after acid leaching is: iron element mass fraction 31%~33%, phosphorus element mass fraction 17%~19%, and the main phase is trivalent iron phosphate. The ingredient quantities in each example are calculated based on this composition range. Example

[0048] A method for preparing sodium-ion battery cathode NFPP material using recycled waste lithium iron phosphate electrode sheets, the process flow is as follows: Figure 1 As shown, it includes the following steps: (1) Electrode peeling: The waste lithium iron phosphate electrode sheets were cut into 2cm×2cm pieces and dried for later use. Under the conditions of 60℃ and solid-liquid ratio of 1:4, the aluminum foil was soaked in NMP at a constant temperature with stirring for 4h, and then ultrasonically vibrated for 10min to peel off completely. After filtration, the aluminum foil was washed three times with deionized water, dried under vacuum at 80℃, and ground through a 100-mesh sieve to obtain lithium iron phosphate electrode powder with a recovery rate of 94%.

[0049] (2) Acid leaching: Take 8g of the above-mentioned lithium iron phosphate powder, add 27mL of the slag washing liquid to make a slurry, slowly add 1.75mL of concentrated sulfuric acid, and then add 8.4mL of hydrogen peroxide dropwise for leaching experiment. The leaching temperature is 70℃, the stirring time is 3h, and the final pH is controlled at 2.0. After filtration, the phosphorus iron slag filter cake is obtained, washed with deionized water until neutral, dried at 80℃, and weighed about 5.2g. The iron content in this phosphorus iron slag is 31.8wt%, and the phosphorus content is 18.2wt%. The filtrate is retained for subsequent lithium salt recovery, and the lithium leaching rate is tested to be 94.2%.

[0050] (3) Precursor preparation: Using 5.2g of ferrophosphate slag as a base, 1.0g of ammonium dihydrogen phosphate and 2.1g of sodium carbonate were added according to the molar ratio of Na:Fe:P = 4:2.98:4, and 1.2g of glucose (6% carbon content) was added. A water suspension with a solid content of 35% was prepared and placed in a planetary ball mill at a speed of 2500r / min for 7.5h. The grinding balls were zirconium oxide. The mixture was dried in an oven at 80℃, crushed, and passed through a 200-mesh sieve to obtain light gray NFPP precursor powder.

[0051] (4) High-temperature sintering: The precursor powder was placed in a crucible and then placed in a tube furnace. High-purity nitrogen gas (flow rate 100 mL / min) was introduced. The temperature was increased to 550℃ at 2℃ / min and held for 10 h. Then the temperature was allowed to drop naturally to room temperature. The sintered product was removed, ground, and passed through a 200-mesh standard sieve to finally obtain black NFPP cathode material powder.

[0052] income Figure 2 , 3 The diagram shows the cycle capacity and coulombic efficiency of the sodium-ion battery cathode material prepared in Example 1 after it was assembled into a sodium half-cell. The sodium half-cell used metallic sodium as the counter electrode and a conventional sodium perchlorate electrolyte. Constant current charge-discharge cycle tests were conducted within a voltage range of 2.0V to 3.6V at a rate of 0.5C. Figure 2 As shown, the sodium half-cell has a discharge specific capacity of 96.8 mAh g at a 0.5C rate. -1 After 100 charge-discharge cycles, the capacity retention rate was 99.49% (the nominal specific capacity of the cathode material is 129 mAh g). -1 Furthermore, the capacity retention rate is 97.25% after 300 cycles at 1C. The discharge specific capacity of the sodium half-cell is 104.98 mAh g⁻¹ at 0.1C, 0.2C, 0.5C, 1C, 2C, 3C, 5C, and 8C rates. -1 100.68mAhg -1 96.12mAhg -1 94.62mAhg -1 94.21mAhg -1 93.45mAhg-1 91.17mAhg -1 and 90.23mAhg -1 .

[0053] Phase characterization: The XRD pattern of the obtained sodium-ion cathode material is shown below. Figure 7 As shown, the XRD pattern reveals the (022), (222), (612), (230), and (424) crystal planes of the sodium-ion cathode material NFPP. The SEM image of the obtained sodium-ion cathode material is shown below. Figure 8 As shown in the SEM image, the synthesized NFPP cathode material consists of uniformly sized primary nanoparticles, mostly with a size of 300±75 nm. The EDS image of the obtained sodium-ion cathode material is shown below. Figure 9 As shown in the EDS diagram, the elemental distribution results from the EDS test indicate that Na, Fe, P, O, and C are uniformly distributed in the NFPP cathode material. Example

[0054] This embodiment includes the following steps: A method for preparing sodium-ion battery cathode NFPP material using recycled waste lithium iron phosphate electrode sheets, the process flow is as follows: Figure 1 As shown, it includes the following steps: (1) Electrode peeling: The waste lithium iron phosphate electrode sheets were cut into 2cm×2cm pieces and dried for later use. Under the conditions of 70℃ and solid-liquid ratio of 1:3 (g:mL), NMP was used for constant temperature stirring and soaking for 5h, followed by ultrasonic vibration for 10min. The aluminum foil was completely peeled off, filtered, washed and dried, and ground through a 300-mesh sieve to obtain lithium iron phosphate electrode powder with a recovery rate of 93%.

[0055] (2) Acid leaching: Take 8g of the above-mentioned lithium iron phosphate powder, add 20mL of the slag washing liquid to make a slurry, slowly add 1.4mL of concentrated sulfuric acid, and then add 8.6mL of hydrogen peroxide dropwise for leaching experiment. The leaching temperature is 60℃, the stirring time is 4h, and the final pH is controlled at 2.2. After filtration, the phosphorus iron slag filter cake is obtained, washed with deionized water until neutral, dried at 80℃, and weighed about 5.1g. The iron content in this phosphorus iron slag is 32.1wt%, and the phosphorus content is 18.0wt%. The filtrate is retained for subsequent lithium recovery, and the lithium leaching rate is 93.5%; the filtrate is retained for subsequent lithium recovery.

[0056] (3) Precursor preparation: Using 5.1g of ferrophosphate slag as a base, 1.1g of diammonium hydrogen phosphate and 2.6g of anhydrous sodium acetate were added according to the molar ratio of Na:Fe:P = 4:2.96:4, and 0.2g of sucrose (carbon coating amount of about 1%) was added. An aqueous suspension with a solid content of 20% was prepared and placed in a planetary ball mill at a speed of 2000r / min for 7h. After ball milling, the powder was dried, crushed and sieved to obtain light gray NFPP precursor powder.

[0057] (4) High-temperature sintering: The precursor powder was placed in a crucible and then placed in a tube furnace. High-purity nitrogen gas (flow rate 150 mL / min) was introduced. The temperature was increased to 400℃ at 5℃ / min and held for 8 hours. Then the temperature was allowed to drop naturally to room temperature. The sintered product was removed, ground, and passed through a 200-mesh standard sieve to finally obtain black NFPP cathode material powder.

[0058] income Figure 4 The sodium half-cell uses a conventional sodium perchlorate electrolyte, and the test voltage range is 2.0V to 3.6V. Figure 4 As can be seen, the sodium half-cell exhibits corresponding charge and discharge voltage plateaus at each test rate, and the charge and discharge curves show corresponding electrochemical response characteristics as the rate changes.

[0059] income Figure 4 , 5 The graphs show the cycle efficiency, capacity, and charge-discharge curves at different rates after assembling the sodium-ion battery cathode material prepared in Example 2 into a sodium half-cell. The sodium half-cell used a conventional sodium perchlorate electrolyte, and the test voltage range was 2.0V–3.6V. The electrochemical cycle data of the coin cell assembled with the cathode material obtained in Example 2 shows that its discharge specific capacity is 108.32 mAh g⁻¹ at a 0.5C rate. -1 Furthermore, the capacity retention rate reached 95.32% after 100 cycles and 93.32% after 300 cycles. Figure 4 As shown, the discharge specific capacity of the sodium half-cell is 114.34 mAh g at discharge rates of 0.1C, 0.2C, 0.5C, 1C, 2C, 3C, 5C, and 8C. -1 109.58mAhg -1 109.12mAhg -1 106.6mAhg -1 109.11mAhg -1 106.84mAhg -1 104.14mAhg -1 and 101.19mAhg -1 . Example

[0060] (1) Electrode peeling: The waste lithium iron phosphate electrode sheets were cut into 2cm×2cm pieces and dried for later use. Under the conditions of 80℃ and solid-liquid ratio of 1:5, the aluminum foil was stirred and soaked in NMP for 6h, and then ultrasonically vibrated for 10min. The aluminum foil was completely peeled off, filtered, washed and dried, and then ground through a 200-mesh sieve to obtain lithium iron phosphate electrode powder with a recovery rate of 92%.

[0061] (2) Acid leaching: Take 8g of the above-mentioned lithium iron phosphate powder, add 25mL of the slag washing liquid to make a slurry, slowly add 1.5mL of concentrated sulfuric acid, and then add 8.8mL of hydrogen peroxide dropwise for leaching experiment. The leaching temperature is 80℃, the stirring time is 5h, and the final pH is controlled at 2.4. After filtration, the phosphorus iron slag filter cake is obtained, washed with deionized water until neutral, dried at 80℃, and weighed about 5.2g. The iron content in this phosphorus iron slag is 31.7wt%, and the phosphorus content is 18.3wt%. The filtrate is retained for subsequent lithium recovery, and the lithium leaching rate is 92.8%.

[0062] (3) Precursor preparation: Using 5.2g of ferrophosphate slag as a base, sodium dihydrogen phosphate (1.2g) and anhydrous sodium oxalate (2.4g) were added according to the molar ratio of Na:Fe:P = 4:3:4, and fructose (approximately 2% carbon coating) was added. An aqueous suspension with a solid content of 25% was prepared and placed in a planetary ball mill at a speed of 1750 r / min for 9 h. After ball milling, the powder was dried, crushed, and sieved to obtain a light gray NFPP precursor powder.

[0063] (4) High-temperature sintering: The precursor powder was placed in a crucible and then placed in a tube furnace. High-purity nitrogen gas (flow rate 200 mL / min) was introduced. The temperature was increased to 600℃ at 3℃ / min and held for 10 h. Then the temperature was allowed to drop naturally to room temperature. The sintered product was removed, ground, and passed through a 300-mesh standard sieve to finally obtain black NFPP cathode material powder.

[0064] income Figure 6 The image shows the long-cycle performance of the sodium-ion battery cathode material prepared in Example 3 after being assembled into a sodium half-cell. The sodium half-cell uses metallic sodium as the counter electrode and conventional sodium perchlorate electrolyte. Constant current charge-discharge cycle tests were conducted within a voltage range of 2.0V–3.6V at 0.5C and 1C. At 0.5C, its discharge specific capacity was 108.32 mAh g⁻¹. -1 And after 100 cycles, the capacity retention rate reached 90.16%. Figure 6 As shown, the sodium half-cell retains 99.28% of its capacity after 300 charge-discharge cycles at a 1C rate. Example

[0065] A method for preparing sodium-ion battery cathode NFPP material using recycled waste lithium iron phosphate electrode sheets, the process flow is as follows: Figure 1 As shown, it includes the following steps: (1) Electrode peeling: The waste lithium iron phosphate electrode sheets were cut into 2cm×2cm pieces and dried for later use. Under the conditions of 90℃ and solid-liquid ratio of 1:3.5, the aluminum foil was soaked in NMP at a constant temperature with stirring for 8h, and then ultrasonically vibrated for 10min to peel off completely. After filtration, washing and drying, the aluminum foil was ground through a 100-mesh sieve to obtain lithium iron phosphate electrode powder with a recovery rate of 94%.

[0066] (2) Acid leaching: Take 8g of the above-mentioned lithium iron phosphate powder, add 29mL of the slag washing liquid to make a slurry, slowly add 1.9mL of concentrated sulfuric acid, and then add 8.8mL of hydrogen peroxide dropwise for leaching experiment. The leaching temperature is 90℃, the stirring time is 6h, and the final pH is controlled at 2.6. After filtration, the phosphorus iron slag filter cake is obtained, washed with deionized water until neutral, dried at 80℃, and weighed about 5.1g. The iron content in this phosphorus iron slag is 32.0wt%, and the phosphorus content is 18.1wt%. The filtrate is retained for subsequent lithium recovery, and the lithium leaching rate is 94.0%.

[0067] (3) Precursor preparation: Using 5.1g of ferrophosphate slag as a base, ammonium phosphate (0.95g) and anhydrous sodium acetate (2.55g) were added at a molar ratio of Na:Fe:P = 4:2.99:4, along with 0.6g of glucose (approximately 3% carbon coating). An aqueous suspension with a solid content of 30% was prepared and placed in a planetary ball mill at 3000 r / min for 9 hours. Zirconia balls were used for milling. After ball milling, the powder was dried, crushed, and sieved to obtain a light gray NFPP precursor powder.

[0068] (4) High-temperature sintering: The precursor powder was placed in a crucible and then placed in a tube furnace. High-purity nitrogen gas (flow rate 150 mL / min) was introduced. The temperature was increased to 450℃ at 3℃ / min and held for 7 hours. Then the temperature was allowed to drop naturally to room temperature. The sintered product was removed, ground, and passed through a 400-mesh standard sieve to finally obtain black NFPP cathode material powder.

[0069] The obtained cathode material was assembled into a coin cell using the battery assembly method described in Example 1, and its electrochemical performance was tested. A coin cell assembled using the NFPP material obtained in Example 4 was also tested electrochemically. At a 0.5C rate, its discharge specific capacity was 89.26 mAh g⁻¹. -1 Furthermore, the capacity retention rate reached 92.17% after 100 cycles. At a higher 1C rate, the capacity retention rate still reached 91.23% after 300 cycles. Example

[0070] A method for preparing sodium-ion battery cathode NFPP material using recycled waste lithium iron phosphate electrode sheets, the process flow is as follows: Figure 1 As shown, it includes the following steps: (1) Electrode peeling: The waste lithium iron phosphate electrode sheets were cut into 2cm×2cm pieces and dried for later use. Under the conditions of 95℃ and solid-liquid ratio of 1:4.5, the aluminum foil was stirred and soaked in NMP for 7h, and then ultrasonically vibrated for 10min to peel off completely. After filtration, washing and drying, the aluminum foil was ground through a 150-mesh sieve to obtain lithium iron phosphate electrode powder with a recovery rate of 93%.

[0071] (2) Acid leaching: Take 8g of the above-mentioned lithium iron phosphate powder, add 28mL of the slag washing liquid to make a slurry, slowly add 1.95mL of concentrated sulfuric acid, and then add 8mL of hydrogen peroxide dropwise for leaching experiment. The leaching temperature is 50℃, the stirring time is 8h, and the final pH is controlled at 2.8. After filtration, the phosphorus iron slag filter cake is obtained, washed with deionized water until neutral, dried at 80℃, and weighed about 5.2g. The iron content in this phosphorus iron slag is 31.9wt%, and the phosphorus content is 18.2wt%. The filtrate is retained for subsequent lithium recovery, and the lithium leaching rate is 91.5%.

[0072] (3) Precursor preparation: Using 5.2g of ferrophosphate slag as a base, 0.85g of ammonium pyrophosphate and 2.05g of anhydrous sodium carbonate were added according to the molar ratio of Na:Fe:P = 4:2.97:4, and 1.2g of glucose (carbon coating amount of about 6%) was added. A water suspension with a solid content of 35% was prepared and placed in a planetary ball mill at a speed of 3000r / min for 8.5h. After ball milling, the powder was dried, crushed and sieved to obtain light gray NFPP precursor powder.

[0073] (4) High-temperature sintering: The precursor powder was placed in a crucible and then placed in a tube furnace. High-purity nitrogen gas (flow rate 100 mL / min) was introduced. The temperature was increased to 550℃ at 2℃ / min and held for 10 h. Then the temperature was allowed to drop naturally to room temperature. The sintered product was removed, ground, and passed through a 300-mesh standard sieve to finally obtain black NFPP cathode material powder.

[0074] The obtained cathode material was assembled into a coin cell using the battery assembly method described in Example 1, and its electrochemical performance was tested. The coin cell assembled from the NFPP material obtained in Example 5 exhibited a discharge specific capacity of 90.19 mAh g⁻¹ at a 0.5C rate. -1 Furthermore, the capacity retention rate reached 93.01% after 100 cycles. At a 1C rate, the capacity retention rate reached 92.36% after 300 cycles.

[0075] The various technical features described in the above embodiments can be combined arbitrarily. For the sake of brevity, not all possible combinations of the various technical features in the above embodiments are described. However, as long as the combination of these technical features does not contradict each other, it should be considered to be within the scope of this specification.

[0076] The embodiments described above are merely illustrative of several implementations of the present invention, and while the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the invention patent. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of the present invention, and these all fall within the protection scope of the present invention. Therefore, the protection scope of this invention patent should be determined by the appended claims.

Claims

1. A method for preparing sodium-ion battery cathode NFPP material by recycling waste lithium iron phosphate electrode sheets, characterized in that, include: S1. After cutting the waste lithium iron phosphate electrode sheets, immerse them in NMP solution and sonicate them to completely peel off the aluminum foil. After filtration, washing and drying, grind and sieve to obtain lithium iron phosphate electrode sheet powder. S2. Take the above lithium iron phosphate electrode powder and leach it under sulfuric acid and hydrogen peroxide conditions, controlling the pH of the leaching endpoint to be 2.0~3.

0. After solid-liquid separation, obtain phosphorus iron slag filter cake and lithium-containing filtrate. Wash the phosphorus iron slag to neutral and dry it. Use the phosphorus iron slag as a base to supplement sodium source, phosphorus source and carbon source. Put it into a ball mill for grinding and spray drying to obtain light gray NFPP precursor powder. S3. The NFPP precursor powder is placed in a tube furnace, an inert atmosphere is introduced, and it is sintered at a high temperature of 300~600℃. After natural cooling, it is ground and sieved to obtain sodium iron phosphate pyrophosphate cathode material powder.

2. The method for preparing sodium-ion battery cathode NFPP material by recycling waste lithium iron phosphate electrode sheets according to claim 1, characterized in that, In step S1, the soaking is carried out at 50~100℃ and a solid-liquid ratio of 1:3~1:5 (g:mL) with NMP constant temperature stirring for 2~8h; the ultrasonic treatment power is 100~500W and the ultrasonic time is 10~60min; the grinding and filtration is grinding through a 100~400 mesh sieve.

3. The method for preparing sodium-ion battery cathode NFPP material by recycling waste lithium iron phosphate electrode sheets according to claim 1, characterized in that, In step S1 and step S2, the specific conditions for acid leaching are as follows: Lithium iron phosphate electrode powder and water are mixed at a solid-liquid ratio of 1:2.5~3.75g:mL to form a slurry; concentrated sulfuric acid is added, with a ratio of concentrated sulfuric acid to lithium iron phosphate electrode powder of 0.175~0.25mL:1g; hydrogen peroxide is then added, with a ratio of hydrogen peroxide to lithium iron phosphate electrode powder of 1~3mL:1g; the leaching temperature is 60~100℃, and the stirring time is 2~8h.

4. The method for preparing sodium-ion battery cathode NFPP material by recycling waste lithium iron phosphate electrode sheets according to claim 1, characterized in that, In step S2, sodium, phosphorus and carbon sources are added during the preparation process according to a Na:Fe:P molar ratio of 4:2.96 to 3:

4. The sodium source is one or more of anhydrous sodium carbonate, sodium bicarbonate, sodium hydroxide, anhydrous sodium acetate, and anhydrous sodium oxalate. The phosphorus source is one or more of the following: ammonium dihydrogen phosphate, diammonium hydrogen phosphate, ammonium phosphate, sodium dihydrogen phosphate, phosphoric acid, and ammonium pyrophosphate. The carbon source is one or more of glucose, sucrose, fructose, sorbitol, and D-mannitol.

5. The method for preparing sodium-ion battery cathode NFPP material by recycling waste lithium iron phosphate electrode sheets according to claim 1, characterized in that, In step S2, the amount of carbon source added is calculated in terms of carbon elements, and the final carbon coating mass fraction in the material is 0.5%~6%.

6. The method for preparing sodium-ion battery cathode NFPP material by recycling waste lithium iron phosphate electrode sheets according to claim 1, characterized in that, In step S2, the mixing ball milling involves preparing the ingredients into an aqueous suspension with a solid content of 20% to 40%, placing it in a planetary ball mill, and ball milling it at a speed of 1500 to 3000 r / min for 7 to 10 hours. The grinding media is zirconia balls. After ball milling, the precursor powder is obtained by spray drying or oven drying and crushing.

7. The method for preparing sodium-ion battery cathode NFPP material by recycling waste lithium iron phosphate electrode sheets according to claim 6, characterized in that, When using spray drying, the inlet air temperature is 150~220℃ and the outlet air temperature is 80~120℃.

8. The method for preparing sodium-ion battery cathode NFPP material by recycling waste lithium iron phosphate electrode sheets according to claim 1, characterized in that, In step S3, the inert atmosphere is high-purity nitrogen gas with a flow rate of 50~200mL / min; the heating rate of the high-temperature sintering is 2~6℃ / min, and the holding time is 7~15h.

9. The method for preparing sodium-ion battery cathode NFPP material by recycling waste lithium iron phosphate electrode sheets according to claim 1, characterized in that, In step S3, the grinding and sieving process involves passing the material through a standard sieve of 100-400 mesh.

10. The method for preparing sodium-ion battery cathode NFPP material by recycling waste lithium iron phosphate electrode sheets according to claim 1, characterized in that, During the acid leaching process in step S2, the lithium leaching rate is >91%, and the resulting lithium-containing filtrate is used for the subsequent preparation of lithium carbonate.

Citation Information

Patent Citations

  • Preparation method for regenerating waste lithium iron phosphate into ferric sodium pyrophosphate

    CN119370817A