A cathode material precursor pellet and its dynamic continuous sintering method
By preparing cathode material precursor pellets through wet mixing and pelletizing processes, the problems of complex and high energy consumption of traditional processes are solved, and efficient and low-cost high-density material preparation is achieved. This method is suitable for continuous sintering and improves the yield and electrochemical performance of the material.
Patent Information
- Application Number
- CN202611418927.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-14
- Publication Date
- 2026-11-17
AI Technical Summary
Traditional preparation processes are complex and energy-intensive, and the low bulk density of powdered precursors makes them difficult to apply to continuous sintering equipment, resulting in low yields and limited improvement in material compaction density.
The precursor pellets of the cathode material are prepared by wet mixing, pelletizing and drying processes to form a dense pellet structure, which is suitable for continuous dynamic sintering and eliminates the high energy consumption of sand milling-spray drying process. The third carbon source is uniformly dispersed by forming a three-dimensional network using glutenin and prolysin.
Simplify the process, reduce costs, increase material yield, form cathode materials with high bulk density and high compaction density, adapt to continuous sintering equipment, reduce dust generation, and improve electronic conductivity and ionic conductivity.
Smart Images

Figure SMS_2
Abstract
Description
Technical Field
[0001] This invention relates to the field of secondary battery materials technology, and in particular to a method for preparing precursor pellets for synthesizing high-density cathode materials, and a dynamic continuous sintering method thereof. Background Technology
[0002] For secondary battery cathode materials, especially phosphate cathode materials (such as lithium iron phosphate and lithium manganese iron phosphate), the compaction density is a key indicator affecting the volumetric energy density of the battery. Traditional preparation processes typically involve wet ball milling, sand milling, and spray drying of active materials, carbon sources, and dispersants to obtain precursor powder, which is then sintered to obtain the final product. This process suffers from problems such as complex procedures, high equipment investment, high energy consumption, and limited improvement in the compaction density of the obtained material. Furthermore, the low bulk density of powdered precursors easily generates dust during subsequent sintering, leading to low yields and making it difficult to apply to more efficient continuous sintering equipment such as rotary kilns. Therefore, developing a simple precursor morphology and preparation method that can significantly improve the bulk density of the precursor and lay the foundation for subsequent high-compact-density sintering is of great significance. Summary of the Invention
[0003] The purpose of this invention is to overcome the shortcomings of the prior art and provide a method for preparing cathode material precursor pellets that is simple in process, low in cost, and can serve as the basis for preparing high-density cathode materials, as well as a dynamic continuous sintering method thereof.
[0004] The technical solution of the present invention is as follows: In a first aspect, the present invention provides a method for preparing cathode material precursor pellets, characterized in that it comprises: Step 1: The phosphate cathode material active precursor, alkali metal source, glutenin, prolysin and third carbon source are thoroughly mechanically dry-mixed in a mixing device to obtain a uniformly mixed dry powder. The third carbon source includes at least one of glucose, sucrose, starch, cellulose, fructose, cyclodextrin, conductive carbon, acetylene black, Super P, graphene, carbon nanotubes, citric acid, ascorbic acid, polyethylene glycol and polyvinylpyrrolidone. Step 2: Add deionized water to the mixed dry powder at a certain flow rate, mix and knead in the mixing equipment to obtain a mixed wet material; Step 3: The mixed wet material is pelletized using a pelletizing device to obtain mixed wet material pellets; Step 4: The mixed wet pellets are dried to obtain cathode material precursor pellets. The obtained pellets have a radius of 0.6~18cm and a bulk density ≥1.2g / cm³. 3 The mechanical strength is ≥25N / particle, and the cathode material precursor pellets are suitable for continuous dynamic sintering to prepare high-pressure real-density cathode materials.
[0005] Preferably, the alkali metal source includes at least one of a lithium source, a sodium source, and a potassium source; the lithium source is at least one of lithium carbonate, lithium bicarbonate, lithium hydroxide, lithium nitrate, lithium sulfate, lithium oxalate, lithium acetate, lithium formate, lithium chloride, lithium fluoride, lithium phosphate, lithium dihydrogen phosphate, dilithium hydrogen phosphate, lithium benzoate, lithium tert-butoxide, and lithium tetraborate; the sodium source is at least one of sodium carbonate, sodium bicarbonate, sodium hydroxide, sodium chloride, sodium phosphate, sodium dihydrogen phosphate, disodium hydrogen phosphate, sodium nitrate, sodium oxalate, sodium acetate, sodium chloride, sodium sulfate, and sodium fluoride; the potassium source is one of potassium carbonate, potassium bicarbonate, potassium phosphate, potassium dihydrogen phosphate, dipotassium hydrogen phosphate, potassium hydroxide, potassium chloride, potassium sulfate, potassium acetate, potassium nitrate, and potassium fluoride.
[0006] Preferably, the mass ratio of glutenin to prolamins is 0.65 to 1:1, and the total weight of glutenin and prolamins accounts for 5 to 25% of the total mass of the mixed dry powder; the third carbon source accounts for 1 to 10% of the total mass of the mixed dry powder.
[0007] Preferably, the molar ratio of the positive electrode material active precursor to the alkali metal source is based on the stoichiometric ratio of the positive electrode material chemical formula; the flow rate of deionized water is 0.1~100L / min; and the mass ratio of deionized water to mixed dry powder is 0.1~5:1.
[0008] Preferably, the mixing equipment includes at least one of a ball mill, a mixer, and a kneading machine; the pelletizing equipment includes at least one of a disc pelletizer, a pressure forming machine, a cylindrical pelletizer, and an extrusion rounding machine.
[0009] Preferably, the drying temperature in step 4 is 80~200℃, and the drying time is 2~12 hours.
[0010] Secondly, the present invention provides a method suitable for continuous dynamic sintering of cathode materials, comprising: Step 1: The cathode material precursor pellets prepared by any of the above methods are loaded into a continuous feeding device, and the cathode material precursor pellets are fed into the sintering device through the feeding device. Step 2: Under a protective atmosphere, the precursor pellets are moved within a dynamic sintering apparatus to complete the sintering reaction, yielding sintered clinker pellets. During the sintering process, the powder generation rate of the precursor pellets is ≤1 wt%. Step 3: The sintered clinker pellets are crushed and sieved to obtain high-density cathode material powder.
[0011] Preferably, the dynamic sintering equipment includes at least one of a rotary kiln, a vertical shaft furnace, a belt sintering machine, a chain grate machine, a fluidized bed sintering furnace, and a multi-hearth furnace.
[0012] Preferably, the sintering reaction is divided into a first-stage sintering and a second-stage sintering; the first-stage sintering temperature is 250~650℃, the sintering time is 4~12 hours, and the heating rate is 1~10℃ / min; the second-stage sintering temperature is 500~850℃, the sintering time is 6~20 hours, and the heating rate is 1~10℃ / min; the protective atmosphere is at least one of nitrogen, argon, and helium; and the oxygen content is ≤200ppm.
[0013] The beneficial effects of this invention are as follows: (1) Simplified process and reduced cost: The present invention can adhere the precursor to the carbon source and form pellets through a simple wet mixing, pelletizing and drying process. No additional dispersant is required during the mixing process, which eliminates the energy-intensive "sand milling-spray drying" process and greatly reduces equipment investment and production energy consumption.
[0014] (2) Laying the foundation for high density: The dense pellet structure formed by pelletizing promotes the growth of cathode material particles; the high packing density of the precursor and the large particle size of the cathode material create conditions for subsequent sintering to prepare cathode materials with high density.
[0015] (3) Adaptation to continuous sintering: The high-strength pellets obtained can withstand the mechanical stress in dynamic sintering equipment (such as rotary kiln), realizing the mode transformation from "static powder sintering" to "dynamic pellet sintering", which provides the possibility for achieving efficient, continuous and low-loss sintering process.
[0016] (4) Uniform carbon dispersion: The three-dimensional network formed by glutenin and prolysin can uniformly disperse the third carbon source around the active material, and can form a continuous and uniform conductive carbon network after sintering.
[0017] (5) High material yield: Due to the high strength of the precursor pellets, almost no dust is generated during the entire sintering process, and the material yield is greatly increased from 95-97% in traditional powder sintering to over 99.5%; its technical effect cannot be achieved by pellets prepared using ordinary powder or other methods. Detailed Implementation
[0018] To make the technical problems, technical solutions and technical advantages of the present invention clearer, a detailed description will be given below with reference to specific examples. However, the scope of protection of the present invention is not limited to the following specific embodiments.
[0019] Unless otherwise defined, all technical terms used herein have the same meaning as commonly understood by those skilled in the art. The technical terms used herein are for the purpose of describing particular embodiments only and are not intended to limit the scope of the invention.
[0020] Unless otherwise specified, all raw materials, reagents, instruments, and equipment used in this invention are commercially available or can be prepared using existing methods. The glutenin used in the examples and comparative examples is glutenin and prolamin.
[0021] Example 1: Lithium manganese iron phosphate (LiMn) 0.6 Fe 0.4 The active precursor (PO4), lithium carbonate, 10% gluten (glutenin and prolamin in a 1:1 mass ratio), and 2% sucrose were thoroughly mechanically dry-mixed in a ball mill to obtain a uniformly mixed dry powder. Deionized water was added to the dry powder at a flow rate of 1 L / min, with a deionized water to dry powder mass ratio of 0.5:1. The mixture was then kneaded in a mixer to obtain a wet mixed material. This wet mixed material was then pelletized using a cylindrical pelletizer to obtain wet mixed material pellets. These pellets were then dried at 100°C for 8 hours to obtain LiMn. 0.6 Fe 0.4 PO4 cathode material precursor pellets.
[0022] LiMn 0.6 Fe 0.4 PO4 cathode material precursor pellets are loaded into a continuous feeder and then fed into a rotary kiln under a nitrogen atmosphere. 0.6 Fe 0.4 PO4 cathode material precursor pellets were moved and sintered in a sintering apparatus. The first stage sintering temperature was 400℃, the sintering time was 6 hours, and the heating rate was 10℃ / min; the second stage sintering temperature was 700℃, the sintering time was 12 hours, and the heating rate was 3℃ / min. Sintered clinker pellets were obtained. These pellets were then crushed and sieved to obtain LiMn. 0.6 Fe 0.4 PO4 cathode material powder.
[0023] Example 2: Lithium manganese iron phosphate (LiMn) 0.6 Fe 0.4 The active precursor (PO4), lithium carbonate, 10% gluten (glutenin and prolamin in a 1:1 mass ratio), and 2% sucrose were thoroughly mechanically dry-mixed in a ball mill to obtain a uniformly mixed dry powder. Deionized water was added to the dry powder at a flow rate of 1 L / min, with a deionized water to dry powder mass ratio of 0.5:1. The mixture was then kneaded in a mixer to obtain a wet mixed material. This wet mixed material was then pelletized using a cylindrical pelletizer to obtain wet mixed material pellets. These pellets were then dried at 100°C for 8 hours to obtain LiMn. 0.6Fe 0.4 PO4 cathode material precursor pellets.
[0024] LiMn 0.6 Fe 0.4 PO4 cathode material precursor pellets are loaded into a continuous feeder and then fed into a rotary kiln under a nitrogen atmosphere. 0.6 Fe 0.4 PO4 cathode material precursor pellets were moved and sintered in a sintering apparatus. The first stage sintering temperature was 300℃, the sintering time was 5 hours, and the heating rate was 10℃ / min; the second stage sintering temperature was 650℃, the sintering time was 15 hours, and the heating rate was 5℃ / min. Sintered clinker pellets were obtained. These pellets were then crushed and sieved to obtain LiMn. 0.6 Fe 0.4 PO4 cathode material powder.
[0025] Example 3: Lithium manganese iron phosphate (LiMn) 0.6 Fe 0.4 The active precursor (PO4), lithium hydroxide, 7% gluten (glutenin to prolamin mass ratio of 0.8:1), and 5% glucose were thoroughly mechanically dry-mixed in a ball mill to obtain a uniformly mixed dry powder. Deionized water was added to the mixed dry powder at a flow rate of 3 L / min, with a deionized water to mixed dry powder mass ratio of 3:1. The mixture was then kneaded in a kneader to obtain a mixed wet material. The mixed wet material was then pelletized using a cylindrical pelletizer to obtain mixed wet material pellets. The mixed wet material pellets were dried at 150℃ for 6 hours to obtain LiMn. 0.6 Fe 0.4 PO4 cathode material precursor pellets.
[0026] LiMn 0.6 Fe 0.4 PO4 cathode material precursor pellets are loaded into a continuous feeder and then fed into a rotary kiln under a nitrogen atmosphere. 0.6 Fe 0.4 PO4 cathode material precursor pellets were moved and sintered in a sintering apparatus. The first stage sintering temperature was 400℃, the sintering time was 6 hours, and the heating rate was 10℃ / min; the second stage sintering temperature was 750℃, the sintering time was 12 hours, and the heating rate was 3℃ / min. Sintered clinker pellets were obtained. These pellets were then crushed and sieved to obtain LiMn. 0.6 Fe 0.4 PO4 cathode material powder.
[0027] Comparative Example 1: Lithium manganese iron phosphate (LiMn) 0.6 Fe 0.4 The active precursor (PO4), lithium carbonate, 10% gluten (glutenin and prolamin in a 1:1 mass ratio), and 2% sucrose were thoroughly mechanically dry-mixed in a ball mill to obtain a homogeneous LiMn. 0.6 Fe 0.4 PO4 cathode material precursor mixed dry powder.
[0028] LiMn 0.6 Fe 0.4 PO4 cathode material precursor mixed dry powder is ground evenly with water and then dried to obtain a mixture. The mixture is loaded into a continuous feeding device, which feeds the cathode material precursor pellets into a rotary kiln. Under a nitrogen atmosphere, LiMn... 0.6 Fe 0.4 PO4 cathode material precursor mixed dry powder was moved and sintered in a sintering apparatus. The first stage sintering temperature was 400℃, the sintering time was 6 hours, and the heating rate was 10℃ / min; the second stage sintering temperature was 700℃, the sintering time was 12 hours, and the heating rate was 3℃ / min. Sintered clinker powder was obtained. The sintered clinker powder was then crushed and sieved to obtain LiMn. 0.6 Fe 0.4 PO4 cathode material powder.
[0029] Comparative Example 2: Lithium manganese iron phosphate (LiMn) 0.6 Fe 0.4 PO4) active precursor, lithium carbonate, and 12% gluten (glutenin and prolamin in a 1:1 mass ratio) were thoroughly mechanically dry-mixed in a ball mill to obtain a uniformly mixed dry powder. Deionized water was added to the mixed dry powder at a flow rate of 1 L / min, with a deionized water to mixed dry powder mass ratio of 0.5:1. The mixture was then mixed and kneaded in a mixer to obtain a mixed wet material. The mixed wet material was then pelletized using a cylindrical pelletizer to obtain mixed wet material pellets. The mixed wet material pellets were then dried at 100℃ for 8 hours to obtain LiMn. 0.6 Fe 0.4 PO4 cathode material precursor pellets.
[0030] LiMn 0.6 Fe 0.4 PO4 cathode material precursor pellets are loaded into a continuous feeder and then fed into a rotary kiln under a nitrogen atmosphere. 0.6 Fe 0.4PO4 cathode material precursor pellets were moved and sintered in a sintering apparatus. The first stage sintering temperature was 400℃, the sintering time was 6 hours, and the heating rate was 10℃ / min; the second stage sintering temperature was 700℃, the sintering time was 12 hours, and the heating rate was 3℃ / min. Sintered clinker pellets were obtained. These pellets were then crushed and sieved to obtain LiMn. 0.6 Fe 0.4 PO4 cathode material powder.
[0031] Comparative Example 3: Lithium manganese iron phosphate (LiMn) 0.6 Fe 0.4 PO4) active precursor, lithium carbonate, and 12% sucrose by mass fraction were thoroughly mechanically dry-mixed in a ball mill to obtain a uniformly mixed dry powder. Deionized water was added to the mixed dry powder at a flow rate of 1 L / min, with a deionized water to mixed dry powder mass ratio of 0.5:1. The mixture was then mixed and kneaded in a mixing device to obtain a mixed wet material. The mixed wet material was then pelletized using a cylindrical pelletizer to obtain mixed wet material pellets. The mixed wet material pellets were then dried at 100℃ for 8 hours to obtain LiMn. 0.6 Fe 0.4 PO4 cathode material precursor pellets.
[0032] LiMn 0.6 Fe 0.4 PO4 cathode material precursor pellets are loaded into a continuous feeder and then fed into a rotary kiln under a nitrogen atmosphere. 0.6 Fe 0.4 PO4 cathode material precursor pellets were moved and sintered in a sintering apparatus. The first stage sintering temperature was 400℃, the sintering time was 6 hours, and the heating rate was 10℃ / min; the second stage sintering temperature was 700℃, the sintering time was 12 hours, and the heating rate was 3℃ / min. Sintered clinker pellets were obtained. These pellets were then crushed and sieved to obtain LiMn. 0.6 Fe 0.4 PO4 cathode material powder.
[0033] Comparative Example 4: Lithium manganese iron phosphate (LiMn) 0.6 Fe 0.4PO4) active precursor, lithium carbonate, 10% gluten (glutenin and prolamin in a 1:1 mass ratio), and 12% sucrose are thoroughly mechanically dry-mixed in a ball mill to obtain a uniformly mixed dry powder. Deionized water is added to the mixed dry powder at a flow rate of 1 L / min, with a deionized water to mixed dry powder mass ratio of 0.5:1. The mixture is then mixed and kneaded in a mixing device to obtain a mixed wet material. The mixed wet material is then pelletized using a cylindrical pelletizer to obtain mixed wet material pellets. The mixed wet material pellets are then dried at 100℃ for 8 hours to obtain LiMn. 0.6 Fe 0.4 PO4 cathode material precursor pellets.
[0034] LiMn 0.6 Fe 0.4 PO4 cathode material precursor pellets are loaded into a continuous feeder and then fed into a rotary kiln under a nitrogen atmosphere. 0.6 Fe 0.4 PO4 cathode material precursor pellets were moved and sintered in a sintering apparatus. The first stage sintering temperature was 400℃, the sintering time was 6 hours, and the heating rate was 10℃ / min; the second stage sintering temperature was 700℃, the sintering time was 12 hours, and the heating rate was 3℃ / min. Sintered clinker pellets were obtained. These pellets were then crushed and sieved to obtain LiMn. 0.6 Fe 0.4 PO4 cathode material powder.
[0035] Comparative Example 5: Lithium manganese iron phosphate (LiMn) 0.6 Fe 0.4 The active precursor (PO4), lithium carbonate, 10% gluten (glutenin and prolamin in a 1:1 mass ratio), and 2% sucrose were thoroughly mechanically dry-mixed in a ball mill to obtain a uniformly mixed dry powder. Deionized water was added to the dry powder at a flow rate of 1 L / min, with a deionized water to dry powder mass ratio of 0.5:1. The mixture was then kneaded in a mixer to obtain a wet mixed material. This wet mixed material was then pelletized using a cylindrical pelletizer to obtain wet mixed material pellets. These pellets were then dried at 100°C for 8 hours to obtain LiMn. 0.6 Fe 0.4 PO4 cathode material precursor pellets.
[0036] LiMn 0.6 Fe 0.4PO4 cathode material precursor pellets are loaded into the feeding equipment, which then feeds them into a static sintering equipment, specifically a roller kiln. Under a nitrogen atmosphere, LiMn... 0.6 Fe 0.4 PO4 cathode material precursor pellets were moved and sintered in a sintering apparatus. The first stage sintering temperature was 400℃, the sintering time was 6 hours, and the heating rate was 10℃ / min; the second stage sintering temperature was 700℃, the sintering time was 12 hours, and the heating rate was 3℃ / min. Sintered clinker pellets were obtained. These pellets were then crushed and sieved to obtain LiMn. 0.6 Fe 0.4 PO4 cathode material powder.
[0037] The LiMn prepared in Examples 1-3 and Comparative Examples 1-5 were respectively 0.6 Fe 0.4 PO4, acetylene black, and PVDF are mixed in a ratio of 8:1:1 with an appropriate amount of N. Methylpyrrolidone (NMP) solution was used to adjust the slurry viscosity and mixed thoroughly at a concentration of 2 mg / cm³. 2 The loading capacity was coated on the current collector aluminum foil and dried under vacuum at 80°C for 12 hours; 12 mm circular electrode sheets were cut out and CR2025 button cells were assembled in an argon atmosphere glove box; lithium metal was used as the negative electrode, Celgard2500 microporous polypropylene membrane was used as the separator, and 1M LiPF6 (diethyl carbonate (DEC): ethylene carbonate (EC): ethyl methyl carbonate (EMC) volume ratio of 1:1:1) was used as the electrolyte; the rate performance of the batteries assembled from the positive electrode materials prepared in Examples 1-3 and Comparative Examples 1-5 was tested at different rates (1C=170mAh / g) using a Blue Battery Test System. The test data are shown in Table 1.
[0038] Table 1. Electrochemical performance and properties of lithium manganese iron phosphate cathode materials in Examples 1-3 and Comparative Examples 1-5 The LiMn prepared in Comparative Example 1 and Comparative Example 1 0.6 Fe 0.4 The discharge specific capacity of the battery assembled with PO4 cathode material at a 1C rate in Example 1 is significantly higher than that in Comparative Example 1, indicating that the LiMn obtained through wet mixing, pelletizing, and drying processes... 0.6 Fe 0.4 PO4 cathode material precursor pellets will incorporate LiMn 0.6 Fe 0.4The PO4 cathode material active precursor, along with the lithium source and third carbon source, is uniformly dispersed and adhered within the three-dimensional network framework formed by glutenin. After sintering, a continuous carbon coating layer is formed, which helps to improve the electronic and ionic conductivity of the material. Comparative Example 1 and Comparative Example 1 yielded LiMn... 0.6 Fe 0.4 The compaction density of the PO4 cathode material in Example 1 is higher than that in Comparative Example 1, indicating that in the cathode material synthesis and preparation process, compared with cathode material precursor powder, the preparation of cathode material precursor pellets helps to form a dense, physically confined precursor structure, which further improves the compaction density of the cathode material after sintering. The powder generation rate of Example 1 is lower than that of Comparative Example 1, while the yield of Example 1 is higher than that of Comparative Example 1. This indicates that compared with cathode material precursor powder, the cathode material precursor pellets obtained through wet mixing, pelletizing, and drying have better mechanical strength, are suitable for dynamic sintering equipment (such as rotary kilns), generate very little powder and dust during sintering, and the clinker after sintering can still maintain the pellet shape, resulting in less product loss and a high yield.
[0039] Comparing the data of Example 1 and Comparative Example 2, the LiMn prepared in Comparative Example 2... 0.6 Fe 0.4 The battery assembled with PO4 cathode material exhibited similar discharge specific capacity at 1C rate, as well as similar powder generation and yield to that in Example 1, but with a lower compaction density. This is mainly because, for the same carbon content, glutenin and prolysin have higher residual carbon content after sintering, affecting the porosity between cathode material powders and hindering the improvement of compaction density. The third carbon source, however, has a lower residual carbon content after sintering. Combining it with glutenin and prolysin helps ensure that the residual carbon content of the cathode material after sintering remains within a controllable range, thus contributing to improved compaction density.
[0040] Comparing the data of Example 1 and Comparative Example 3, the LiMn prepared in Comparative Example 3... 0.6 Fe 0.4 The battery assembled with PO4 cathode material exhibited a significantly lower discharge specific capacity at 1C rate than that of Example 1. Its cathode material showed low compaction density, low yield, and high powder generation rate. The main reason is that the first and third carbon sources failed to form a three-dimensional network framework after mixing, resulting in uneven carbon source dispersion. This led to component segregation between the active precursor and the lithium source in the cathode material, affecting the prepared LiMn. 0.6 Fe 0.4 PO4 cathode materials have poor electronic and ionic conductivity, which reduces electrochemical capacity. Secondly, the third carbon source has low viscosity, and the precursor pellets of the cathode material prepared after pelletizing have weak mechanical strength. When matched with dynamic sintering equipment, they are very easy to break during sintering, generating a large amount of dust, which in turn reduces the yield.
[0041] Comparing the data of Example 1 and Comparative Example 4, the LiMn prepared in Comparative Example 4...0.6 Fe 0.4 The battery assembled with PO4 cathode material exhibited a slightly lower discharge specific capacity at 1C rate than that of Example 1, and its cathode material compaction density was also lower than that of Example 1. However, the powder generation rate and yield were similar to those of Example 1. The main reason for this is that increasing the amount of the second carbon source beyond the preferred range leads to an increase in residual carbon in the cathode material, affecting the uniformity and thickness of the carbon coating layer and thus impacting electrochemical performance. Secondly, the increased residual carbon content affects the porosity and specific surface area of the cathode material, which is detrimental to improving the compaction density.
[0042] Comparing the data of Example 1 and Comparative Example 5, the LiMn prepared in Comparative Example 5... 0.6 Fe 0.4 The battery assembled with PO4 cathode material exhibited a discharge specific capacity close to that of Example 1 at a 1C rate, and its cathode material compaction density, powder generation rate, and yield were similar to those of Example 1. This indicates that cathode material precursor pellets are suitable not only for dynamic sintering equipment but also for static sintering equipment. In static sintering equipment, cathode material precursor pellets are placed in sintering saggers for static sintering. Due to the absence of mechanical movement, the powder generation rate is low, but the yield is high. However, dynamic sintering equipment is less expensive; for example, rotary kilns are more suitable for pellet sintering and can enhance the mass and heat transfer process. Static sintering equipment, such as roller kilns, is very expensive and can only use saggers for sintering, which are prone to peeling and slagging, affecting sintering consistency. Therefore, using dynamic sintering equipment while achieving similar powder generation and yield rates as static equipment is one of the important technical effects of this invention.
Claims
1. A method for preparing cathode material precursor pellets, characterized in that, include: Step 1: The phosphate cathode material active precursor, alkali metal source, glutenin, prolysin and third carbon source are thoroughly mechanically dry-mixed in a mixing device to obtain a uniformly mixed dry powder. The third carbon source includes at least one of glucose, sucrose, starch, cellulose, fructose, cyclodextrin, conductive carbon, acetylene black, Super P, graphene, carbon nanotubes, citric acid, ascorbic acid, polyethylene glycol and polyvinylpyrrolidone. Step 2: Add deionized water to the mixed dry powder at a certain flow rate, mix and knead in the mixing equipment to obtain a mixed wet material; Step 3: The mixed wet material is pelletized using a pelletizing device to obtain mixed wet material pellets; Step 4: The mixed wet pellets are dried to obtain cathode material precursor pellets. The obtained pellets have a radius of 0.6~18cm and a bulk density ≥1.2g / cm³. 3 The mechanical strength is ≥25N / particle, and the cathode material precursor pellets are suitable for continuous dynamic sintering equipment to prepare high-pressure solid density cathode materials.
2. The method for preparing cathode material precursor pellets as described in claim 1, characterized in that, The alkali metal source includes at least one of lithium, sodium, and potassium sources; the lithium source is at least one of lithium carbonate, lithium bicarbonate, lithium hydroxide, lithium nitrate, lithium sulfate, lithium oxalate, lithium acetate, lithium formate, lithium chloride, lithium fluoride, lithium phosphate, lithium dihydrogen phosphate, dilithium hydrogen phosphate, lithium benzoate, lithium tert-butoxide, and lithium tetraborate; the sodium source is at least one of sodium carbonate, sodium bicarbonate, sodium hydroxide, sodium chloride, sodium phosphate, sodium dihydrogen phosphate, disodium hydrogen phosphate, sodium nitrate, sodium oxalate, sodium acetate, sodium chloride, sodium sulfate, and sodium fluoride; the potassium source is one of potassium carbonate, potassium bicarbonate, potassium phosphate, potassium dihydrogen phosphate, dipotassium hydrogen phosphate, potassium hydroxide, potassium chloride, potassium sulfate, potassium acetate, potassium nitrate, and potassium fluoride.
3. The method for preparing cathode material precursor pellets as described in claim 1, characterized in that, The mass ratio of glutenin to prolamins is 0.65 to 1:1, and the total weight of glutenin and prolamins accounts for 5 to 25% of the total mass of the mixed dry powder; the third carbon source accounts for 1 to 10% of the total mass of the mixed dry powder.
4. The method for preparing cathode material precursor pellets as described in claim 1, characterized in that, The molar ratio of the positive electrode material active precursor to the alkali metal source is based on the stoichiometric ratio of the positive electrode material chemical formula; the flow rate of deionized water is 0.1~100L / min; and the mass ratio of deionized water to mixed dry powder is 0.1~5:
1.
5. The method for preparing cathode material precursor pellets as described in claim 1, characterized in that, The mixing equipment includes at least one of a ball mill, a mixer, and a kneading machine; the pelletizing equipment includes at least one of a disc pelletizer, a pressure forming machine, a cylindrical pelletizer, and an extrusion rounding machine.
6. The method for preparing cathode material precursor pellets as described in claim 1, characterized in that, The drying temperature in step 4 is 80~200℃, and the drying time is 2~12 hours.
7. A method for continuous dynamic sintering of cathode materials, characterized in that, include: Step 1: The cathode material precursor pellets prepared by any one of claims 1-6 are loaded into a continuous feeding device and fed into a sintering device through the feeding device. Step 2: Under a protective atmosphere, the precursor pellets are moved within a dynamic sintering apparatus to complete the sintering reaction, yielding sintered clinker pellets. During the sintering process, the powder generation rate of the precursor pellets is ≤1 wt%. Step 3: The sintered clinker pellets are crushed and sieved to obtain high-density cathode material powder.
8. The method as described in claim 7, characterized in that, The dynamic sintering equipment includes at least one of the following: rotary kiln, vertical shaft furnace, belt sintering machine, chain grate machine, fluidized bed sintering furnace, and multi-hearth furnace.
9. The method as described in claim 7, characterized in that, The sintering reaction is divided into a first-stage sintering and a second-stage sintering; the first-stage sintering temperature is 250~650℃, the sintering time is 4~12 hours, and the heating rate is 1~10℃ / min; the second-stage sintering temperature is 500~850℃, the sintering time is 6~20 hours, and the heating rate is 1~10℃ / min; the protective atmosphere is at least one of nitrogen, argon, and helium; the oxygen content is ≤200ppm.