A method for preparing carbon-coated modified Si-SiO2 composite material
By using a carbon-coated modified Si-SiO2 composite material preparation method, the problems of volume expansion, low conductivity and surface instability of silicon-based materials in lithium-ion batteries have been solved, achieving high-efficiency and low-cost battery performance improvement.
Patent Information
- Application Number
- CN202610556423.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-04-24
- Publication Date
- 2026-11-17
AI Technical Summary
Silicon-based materials in lithium-ion batteries suffer from problems such as volume expansion leading to structural collapse, low conductivity, and surface instability, resulting in decreased battery performance. Existing technologies are also costly and inefficient.
The preparation method of carbon-coated modified Si-SiO2 composite material includes ultrasonic cleaning, vacuum drying, high-temperature calcination, acid washing and ball milling to form carbon-coated modified Si-SiO2 composite material.
It improves the cycle stability of silicon materials, reduces costs, simplifies the process, and enhances battery performance.
Smart Images

Figure CN123105645A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of lithium-ion battery electrode material technology, specifically, it relates to a method for preparing and applying a carbon-coated modified Si-SiO2 composite material. Background Technology
[0002] With the rapid rise of the global new energy industry, lithium-ion batteries, as core energy storage devices for portable electronic devices, electric vehicles, and large-scale energy storage systems, have seen their energy density, cycle stability, and safety become key bottlenecks restricting industrial upgrading. As a core component of lithium-ion batteries, the anode material directly determines the battery's capacity, charge / discharge efficiency, and cycle life. Improving its performance is one of the core paths to achieving high energy density in lithium-ion batteries, and the development of high-performance anode materials has become a research hotspot and key direction in the field of new energy materials. Currently, the main commercial lithium-ion battery anode material is graphite, with a theoretical specific capacity of 372 mAh·g⁻¹, which is far from meeting the demand for high-energy-density batteries. Silicon-based materials are widely recognized as the most promising next-generation high-energy-density lithium-ion battery anode materials due to their outstanding advantages such as extremely high theoretical specific capacity (up to 4200 mAh·g-1), suitable lithium intercalation potential, abundant crustal reserves, environmental friendliness, and low price. They can effectively make up for the shortcomings of insufficient energy density of graphite anode materials, significantly improve the overall performance of lithium-ion batteries, and meet the high-end application needs of the new energy industry. However, silicon-based materials face three major technological bottlenecks in practical applications, severely hindering their commercialization: First, silicon-based materials undergo dramatic volume expansion during charging and discharging (expansion rate exceeding 300%). During lithiation, each silicon atom can combine with up to 3.75 lithium ions to form Li15Si4. Repeated expansion and contraction generate enormous mechanical stress, leading to silicon particle breakage and pulverization, which in turn causes electrode structure collapse, detachment of active materials from current collectors, and ultimately rapid capacity decay. Second, silicon-based materials have low intrinsic conductivity (approximately 1×10⁻³ S / cm), far lower than graphite (approximately 10⁴ S / cm), resulting in obstructed charge transport during charging and discharging, poor battery rate performance, and the need to add additional conductive agents, further reducing electrode energy density. Third, the surface of silicon-based materials is unstable. Volume expansion during charging and discharging causes the solid electrolyte interphase (SEI) film to rupture, exposing a new silicon surface that continuously reacts with the electrolyte, irreversibly consuming electrolyte and lithium ions, reducing battery coulombic efficiency. At the same time, excessive thickness of the SEI film increases interfacial impedance, further deteriorating battery performance.
[0003] Chinese invention patent CN103236517A discloses a method for preparing a silicon-based anode material. This method involves calcining silicon suboxide at high temperature, followed by a high-energy ball mill to obtain silicon dioxide-coated nanoparticles. This material provides necessary buffer space for silicon expansion; however, the method's high raw material and energy consumption significantly increase costs.
[0004] Chinese invention patent CN109524626A discloses a silicon-based anode material for lithium-ion batteries and its preparation method. This method utilizes high-energy ball milling to obtain a Si-SiO2 composite material. The irreversible phase generated during lithium intercalation of silicon dioxide is used to suppress the volume expansion of silicon, thereby improving the overall capacity of the material. However, this composite method exhibits low first-cycle coulombic efficiency, failing to meet the first-cycle coulombic efficiency required for industrial-scale silicon-based anode materials. Summary of the Invention
[0005] In view of the above-mentioned deficiencies of the prior art, the present invention provides a method for preparing carbon-coated modified Si-SiO2 composite material, comprising the following steps: 1) High-purity silica is ultrasonically cleaned, vacuum dried, then pressed into tablets and calcined at high temperature under inert gas protection; 2) The calcined product is acid-washed to remove non-silicon oxide impurities, yielding Si-SiO2 powder; 3) Mix Si-SiO2 powder with a carbon source, add solvent and binder, ball mill to form a uniform slurry, and dry and calcine to obtain carbon-coated modified Si-SiO2 composite material.
[0006] Furthermore, in step 1), the ultrasonic cleaning uses anhydrous ethanol, the cleaning time is 20 minutes, and the vacuum drying temperature is 80°C.
[0007] Furthermore, the carbon source mentioned in step 3) is selected from at least one of citric acid, dopamine hydrochloride, and peanut shell ash.
[0008] Furthermore, in step 3), the mass ratio of Si-SiO2 powder to carbon source is 9:1, 8:2, or 7:3.
[0009] Furthermore, in step 3), the ball milling speed is 250 r / min, the ball milling time is 3 h, the solvent is NMP, and the binder is PVDF.
[0010] The present invention also includes a carbon-coated modified Si-SiO2 composite material, which is prepared by the above-described preparation method.
[0011] The present invention also includes a lithium-ion battery anode comprising the above-mentioned carbon-coated modified Si-SiO2 composite material.
[0012] The present invention also includes a lithium-ion battery comprising the above-described lithium-ion battery negative electrode. This invention modifies silicon materials through carbon coating, which can buffer the expansion of silicon under certain conditions, thereby improving the cycle stability of silicon materials. It has advantages such as high energy efficiency, low cost, and simple process.
[0013] The following will further explain the concept, specific structure, and technical effects of the present invention in conjunction with the accompanying drawings, so as to fully understand the purpose, features, and effects of the present invention. Attached Figure Description
[0014] Figure 1 The X-ray diffraction (XRD) pattern of the high-purity silica raw material described in this invention; Figure 2 The X-ray diffraction (XRD) pattern of the mixture after magnesium thermal reduction as described in this invention; Figure 3 The X-ray diffraction (XRD) pattern of the acid-washed Si-SiO2 powder described in this invention; Figure 4 The X-ray diffraction (XRD) pattern of the carbon-coated Si-SiO2@C powder described in this invention; Figure 5 This is a scanning electron microscope (SEM) image of the Si-SiO2@C powder after carbon coating treatment according to the present invention. Detailed Implementation
[0015] The following description, with reference to the accompanying drawings, illustrates several preferred embodiments of the present invention to make its technical content clearer and easier to understand. The present invention can be embodied in many different forms, and the scope of protection of the present invention is not limited to the embodiments mentioned herein.
[0016] In the accompanying drawings, components with the same structure are indicated by the same numerical designation, and components with similar structures or functions are indicated by similar numerical designations. The dimensions and thicknesses of each component shown in the drawings are arbitrary, and the present invention does not limit the dimensions and thicknesses of each component. To make the illustrations clearer, the thickness of some components has been appropriately exaggerated in the drawings. Example
[0017] High-purity quartz sand: Ultrasonic cleaning with anhydrous ethanol for 20 min to remove surface impurities, then placed in a vacuum drying oven and dried at 80 ℃; the matrix material is dried under suitable temperature conditions, and then the dry powder is transferred to a tablet press for tableting to obtain cylindrical material; the obtained cylindrical material is transferred to a high-temperature calcination furnace under inert gas protection; the obtained block calcination product is acid washed to remove non-silicon oxide impurities; the above silicon-containing material is combined with a carbon source by ball milling, and after drying and calcination, biomass carbon modified Si-SiO2 composite material is obtained.
[0018] A fixed mass of 1 g of silicon was used to mix different types and proportions of carbon-containing raw materials, including citric acid. Three mass ratios were set for each raw material (silicon:carbon = 9:1, 8:2, 7:3), resulting in a total of 9 experimental groups. According to the experimental protocol, elemental silicon, carbon-containing raw materials, and PVDF were accurately weighed using an electronic balance and placed in the grinding jar of a planetary ball mill. An appropriate amount of NMP solvent was added to ensure thorough wetting of the raw materials. The ball mill speed was set to 250 r / min, and grinding was carried out for 3 hours to ensure uniform mixing of silicon and carbon raw materials and complete dissolution of PVDF, forming a homogeneous slurry. Example
[0019] First, silicon-containing powder was prepared using the exact same method as in Example 1 above.
[0020] A fixed mass of 1 g of silicon was used to mix different types and proportions of carbon-containing raw materials. The carbon-containing raw material was dopamine hydrochloride. Three mass ratios were set for each raw material (silicon:carbon = 9:1, 8:2, 7:3), resulting in a total of 9 experimental groups. According to the experimental protocol, elemental silicon, carbon-containing raw materials, and PVDF were accurately weighed using an electronic balance and placed in the grinding jar of a planetary ball mill. An appropriate amount of NMP solvent was added to ensure thorough wetting of the raw materials. The ball mill speed was set to 250 r / min, and grinding was carried out for 3 hours to ensure uniform mixing of silicon and carbon raw materials and complete dissolution of PVDF, forming a homogeneous slurry. Example
[0021] First, silicon-containing powder was prepared using the exact same method as in Example 1 above.
[0022] A fixed mass of 1 g of silicon was used to mix with different types and proportions of carbon-containing raw materials, including peanut shell ash. Three mass ratios were set for each raw material (silicon:carbon = 9:1, 8:2, 7:3), resulting in a total of 9 experimental groups. According to the experimental protocol, elemental silicon, carbon-containing raw materials, and PVDF were accurately weighed using an electronic balance and placed in the grinding jar of a planetary ball mill. An appropriate amount of NMP solvent was added to ensure thorough wetting of the raw materials. The ball mill speed was set to 250 r / min, and grinding was carried out for 3 hours to ensure uniform mixing of silicon and carbon raw materials and complete dissolution of PVDF, forming a homogeneous slurry.
[0023] The preferred embodiments of the present invention have been described in detail above. It should be understood that those skilled in the art can make numerous modifications and variations based on the concept of the present invention without creative effort. Therefore, all technical solutions that can be obtained by those skilled in the art based on the concept of the present invention through logical analysis, reasoning, or limited experimentation on the basis of existing technology should be within the scope of protection defined by the claims.
Claims
1. A method for preparing carbon-coated modified Si-SiO2 composite material, characterized in that, Includes the following steps: 1) High-purity silica is ultrasonically cleaned, vacuum dried, then pressed into tablets and calcined at high temperature under inert gas protection; 2) The calcined product is acid-washed to remove non-silicon oxide impurities, yielding Si-SiO2 powder; 3) Mix Si-SiO2 powder with a carbon source, add solvent and binder, ball mill to form a uniform slurry, and dry and calcine to obtain carbon-coated modified Si-SiO2 composite material.
2. The preparation method according to claim 1, characterized in that, In step 1), anhydrous ethanol is used for ultrasonic cleaning, the cleaning time is 20 minutes, and the vacuum drying temperature is 80℃.
3. The preparation method according to claim 1, characterized in that, The carbon source mentioned in step 3) is selected from at least one of citric acid, dopamine hydrochloride, and peanut shell ash.
4. The preparation method according to claim 1, characterized in that, In step 3), the mass ratio of Si-SiO2 powder to carbon source is 9:1, 8:2, or 7:
3.
5. The preparation method according to claim 1, characterized in that, In step 3), the ball milling speed is 250 r / min, the ball milling time is 3 h, the solvent is NMP, and the binder is PVDF.
6. A carbon-coated modified Si-SiO2 composite material, characterized in that, It is prepared by the preparation method according to any one of claims 1-5.
7. A lithium-ion battery negative electrode, characterized in that, It includes the carbon-coated modified Si-SiO2 composite material as described in claim 6.
8. A lithium-ion battery, characterized in that, It includes the lithium-ion battery negative electrode as described in claim 7.
Citation Information
Patent Citations
Lithium ion battery silicon-based negative material and preparation method thereof
CN103236517A
Silicon-based negative electrode material for lithium ion battery and preparation method of silicon-based negative electrode material
CN109524626A