A method and system for low-carbon all-coal smelting of industrial silicon based on dynamic control

By using a dynamic, low-carbon coal smelting method, the problem of carbon imbalance in industrial silicon production has been solved. By replacing coke with washed coal, controlling electrode power and raw material impurities, in-furnace reaction balance has been achieved, improving production stability and efficiency, and reducing costs.

CN123105646APending Publication Date: 2026-11-17NINGXIA HAISHENG IND CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611499470.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-24
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In existing industrial silicon production, all-coal smelting is prone to carbon balance imbalance, leading to unstable furnace conditions, abnormal silicon water temperature, sticky furnace charge, difficulty in tapping, increased slag volume, and low smelting efficiency. In addition, the traditional coal-coke composite smelting process is costly and difficult to control carbon balance.

Method used

A dynamic control method for low-carbon industrial silicon smelting using all-coal is adopted. By establishing raw material input detection and silicon output detection, the distance between the electrode and the furnace bottom and the electrode consumption are obtained. The electrode power factor is adjusted, and multi-stage carbon balance adjustment is carried out to ensure that the silicon input and output are matched. Washed coal is used to replace coke and wood chips as a reducing agent, and the impurity content of silica, coal and wood chips is controlled to achieve reaction balance in the furnace.

Benefits of technology

It has achieved stability and efficiency in industrial silicon production, reduced production costs, avoided carbon excess or carbon deficiency, and increased silicon output and smelting efficiency, which is in line with the trend of low-carbon and green development.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

This application discloses a dynamic control-based all-coal low-carbon smelting method for industrial silicon, comprising the following steps: establishing raw material input detection and silicon output detection; acquiring the distance between the electrode and the furnace bottom, the electrode input depth, and the electrode consumption; establishing matching data for raw material input and silicon output per unit time, matching data for electrode consumption and input, and matching data for the proportion of silicon products and microsilica powder, and recording the electrode parameters acquired during this period; this application also includes a dynamic control-based all-coal low-carbon smelting system for industrial silicon, including an electrode depth monitoring module, an electrode pressure release monitoring module, an electrode power monitoring module, a current compensation acquisition module, a current acquisition module, and a voltage acquisition module. This application replaces all the coal used in smelting with washed coal, ensuring the supply of raw materials. After the raw materials are fed into the furnace, dynamic control is performed according to the furnace conditions to ensure the reaction balance and energy consumption within the furnace, while also controlling the silicon output to ensure stable production of industrial silicon.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of industrial silicon production technology, and in particular to a method and system for low-carbon coal smelting of industrial silicon based on dynamic control. Background Technology

[0002] Industrial silicon smelting is a high-temperature reduction metallurgical process. Carbonaceous reducing agents are the core raw materials that ensure the smooth progress of the reduction reaction in the furnace and maintain stable furnace conditions. Their type, ratio, fixed carbon content, and physicochemical properties directly determine smelting efficiency, unit power consumption, product quality, and production costs, making them a key control point in the entire industrial silicon production process. Currently, the mainstream production processes in China's industrial silicon industry generally adopt a composite reducing agent model of coal combined with coking coal and coke, or a pure coal-coke or pure coke smelting process.

[0003] There are currently few mature large-scale application cases of all-coal metallurgy in the industry. The reason for this is that the fixed carbon content, ash content, moisture, resistivity and other indicators of conventional coal are different from those of coke and coking coal. Directly using all-coal metallurgy can easily lead to furnace condition problems such as carbon balance imbalance, abnormal electrode insertion depth, in-furnace sparking and material sticking, furnace bottom rising, and low silicon recovery rate, resulting in insufficient process stability. However, coking coal and coke are byproducts of coking and are scarce carbonaceous reducing agents, resulting in persistently high market prices. Furthermore, their supply chains are heavily influenced by coal industry regulations, transportation costs, and market supply and demand fluctuations, significantly increasing the raw material costs for industrial silicon production. In addition, traditional coal-coke composite smelting processes involve complex reducing agent ratios and difficult carbon balance control, leading to issues of excessive or insufficient carbon in the furnace. Excessive carbon results in shallow electrode insertion, SiC hard shell accumulation, and abnormal silicon water temperature, while insufficient carbon causes sticky furnace charge, difficulty in tapping, and increased slag. This not only leads to low smelting efficiency and high unit product power consumption but also contradicts the current development trend of low-carbon, green, cost-reducing, efficiency-enhancing, and energy-saving industrial silicon. Therefore, we propose a dynamic control-based all-coal low-carbon smelting process for industrial silicon to address these problems. Summary of the Invention

[0004] This application provides a method and system for low-carbon smelting of industrial silicon using all-coal based on dynamic control, which solves the problems of carbon balance imbalance, abnormal silicon water temperature, sticky furnace charge, difficulty in tapping, increased slag volume, and low smelting efficiency that easily occur in the low-carbon smelting of industrial silicon using all-coal.

[0005] This application provides a method for low-carbon smelting of industrial silicon from all-coal based on dynamic control, characterized by the following steps: Establish a system for detecting incoming raw materials and silicon output from the furnace; Obtain the distance between the electrode and the furnace bottom, the depth of each electrode entering the furnace, and the amount of electrode consumption; Establish matching data for raw material input and silicon output per unit time, matching data for electrode consumption and input, and matching data for the ratio of silicon products to microsilicon powder, and record the electrode parameters obtained during this period. Adjust the electrode power factor to the set value to enter the multi-stage carbon balance adjustment stage; When the recorded data of silicon input and output at multiple unit times are within the set range and the proportion of microsilicon powder is greater than the upper limit of the range of 20%-35%, the multi-stage carbon balance adjustment stage of carbon increase is entered. When the recorded data of silicon feed and output at multiple unit times are not within the set range, and the proportion of microsilicon powder is lower than the lower limit of the 20%-35% range, or the electrode insertion depth continues to decrease, or the furnace bottom distance continues to shorten, or the output is consistently low, the carbon balance adjustment stage of carbon reduction multi-stage is entered. Take a set of production data in which all indicators are in the optimal range during the period and carry out production, and save the production data for this period; When the deviations of all indicators in the raw material entry inspection data from the raw material indicators corresponding to the saved original production data are all within the preset tolerance range, the corresponding original production data can be directly retrieved for production.

[0006] Preferably, the multi-stage carbon balance adjustment stage for increasing carbon includes: In the next unit of time, the amount of washed coal fed into the furnace during the furnace stage will increase by 2%-4% of the microsilica powder production during that period, corresponding to a fixed carbon content. After running for several unit times, the data matching the silicon feed rate and output rate are within the set range. Then, the amount of washed coal corresponding to 0.5%-2% fixed carbon of microsilica powder in the silicon output rate is increased again, and this step is continued. If the data on the silicon feed rate and the output rate are not within the set range, obtain data on the distance between the electrode and the furnace bottom, the electrode insertion depth, and the electrode power. If the electrode pressure release is less than the preset value, the electrode insertion depth gradually becomes shallower or the furnace bottom rises, ending the multi-stage carbon balance adjustment stage.

[0007] Preferably, the multi-stage carbon balance adjustment stage for carbon reduction includes: In the next unit of time, the amount of silica added during the furnace feeding stage increases by 2%-4%; After running for several unit times, the data matching the amount of silicon fed into the furnace and the amount of silicon discharged from the furnace did not return to the set range value. During the feeding stage, 0.5%-2% more silicon was added, and this step was continued. When the silicon feed rate and output rate match the set range, the multi-stage carbon balance adjustment phase ends. If the data still does not recover after adding silicon four times, the adjustment is paused and the furnace condition is checked.

[0008] Preferably, the raw materials for the all-coal low-carbon smelting are silica, washed coal and wood chips, wherein wood chips account for 14%-17% of the total fixed carbon based on fixed carbon.

[0009] Preferably, the raw material entry inspection includes testing the elemental content, particle size, anti-explosion properties, and impurity content of silica, and testing the fixed carbon, ash, volatile matter, moisture, impurity content, and particle size of coal.

[0010] Preferably, the silica contains ≥99.5% silicon dioxide, ≤0.05% Fe2O3, ≤0.1% Al2O3, and has a particle size of 60-180mm, wherein the total particle size smaller than 60mm and larger than 180mm cannot exceed 5%, and its explosion resistance range is 75-85.

[0011] Preferably, the washed coal has a moisture content of ≤14%, an ash content of ≤4%, a volatile matter content of ≥32%, a fixed carbon content of ≥60%, and a particle size of 8-20 mm, wherein the total of particles smaller than 8 mm or larger than 20 mm does not exceed 5%.

[0012] Preferably, the electrode power factor is 0.85-0.95.

[0013] Preferably, the unit time is at least 8 hours.

[0014] This application also includes a dynamic control-based industrial silicon all-coal low-carbon smelting system, including a data acquisition terminal: an electrode depth monitoring module, an electrode pressure release monitoring module, an electrode power monitoring module, a current acquisition module, a voltage acquisition module, and a current compensation acquisition module; Data fusion terminal: The central processing unit connected to each acquisition module, used to perform the multi-stage carbon balance adjustment and store data; Execution end: Electrode lifting control module, transformer gear adjustment module, and batching control module connected to the central processing unit; Display end: Human-computer interaction interface, used to display monitoring data and control commands in real time.

[0015] As can be seen from the above technical solutions, this application provides a method and system for low-carbon industrial silicon smelting using all-coal based on dynamic control. It should be understood that the all-coal smelting in this application does not involve replacing all raw materials with washed coal, but rather replacing coke, charcoal, etc., with washed coal. Wood chips, as an unavailable material, are still used, serving as an important component in providing volatile matter and creating a loose structure within the furnace. After meeting the above conditions, research on low-carbon industrial silicon smelting using all-coal has revealed that, during the feeding stage, after controlling the impurities in silica, coal, and wood chips, the main parameters are the silicon conversion rate and power factor. Matching the numbers is crucial. When the two sets of data reach their optimal matching values, ensuring reaction balance in the system and preventing carbon excess or deficiency guarantees stable production. However, the raw materials coal and silica have complex compositions. Simply calculating the addition amount based on the effective content of carbon and silica can lead to carbon excess or deficiency during actual operation, resulting in decreased production efficiency and yield. This application strictly controls the composition of the raw materials before they enter the furnace and calculates the addition amount based on the effective component content before smelting. To ensure furnace balance, this application uses multiple detection methods during smelting to obtain... During smelting, when the electrode power factor is between 0.85 and 0.95, the distance between the electrode and the furnace bottom, the electrode insertion depth, and the electrode consumption are monitored to ensure they are within the set range. Furthermore, this application also monitors silicon balance data. Specifically, the difference between the silicon addition amount and the sum of the industrial silicon output, the amount of microsilica powder, and the silicon content in the slag over multiple unit time periods must be within 98% to indicate normal silicon reaction and normal silicon consumption in the furnace. When the entire system is operating normally, to further increase industrial silicon output, the proportion of microsilica powder is also monitored. If any of the above values ​​fall outside the specified range... Depending on the specific circumstances, the furnace condition is dynamically controlled through a multi-stage carbon balance adjustment process over multiple time units until it is restored to the set value, and the production indicators are optimized. That is, after the carbon balance in the furnace is achieved, the power factor, industrial silicon output, and electrode consumption are all at their optimal levels. The adjustment process and related parameters are recorded, and the original data is accumulated. When the data collected before the raw materials enter the furnace are within the set range, the addition ratio can be directly adjusted to the original data value for production. Thus, dynamic control ensures the stability and efficiency of all-coal production.

[0016] Compared with the prior art, the beneficial effects of the present invention are: 1. This application replaces all raw materials such as charcoal, coke, and coking coal with refined washed coal, thereby ensuring the stability of raw material production. This not only reduces the cost of industrial silicon smelting but also eliminates furnace problems caused by the complex composition of charcoal, coke, and coking coal, and stabilizes the composition of both refined washed coal and wood chips as reducing agents. 2. By adjusting the electrode power factor, electrode position, and electrode consumption, basic adjustments are made to ensure the smelting quality and furnace temperature in the furnace before making detailed adjustments. 3. By monitoring the quality of silicon produced from the furnace within multiple time units, it is possible to check whether there is material accumulation in the furnace and make targeted adjustments to the furnace conditions; 4. By monitoring microsilica, the output of industrial silicon can also be controlled. When the microsilica level is high, the output of industrial silicon can be increased by controlling the furnace conditions.

[0017] In summary, this application replaces all coal used in smelting with washed coal, ensuring the supply of raw materials. After the raw materials are fed into the furnace, dynamic control is carried out according to the furnace conditions to ensure the balance of the reaction inside the furnace and energy consumption. At the same time, silicon production is also controlled to ensure output, thereby ensuring the stable production of industrial silicon. Detailed Implementation

[0018] To enable those skilled in the art to better understand the technical solutions in this application, the technical solutions in the embodiments of this application will be clearly and completely described below.

[0019] A method for low-carbon industrial silicon smelting using all-coal based on dynamic control. It should be understood that the "all-coal" in this application refers to replacing all coal resources such as charcoal, coke, and coking coal with washed coal. Regarding specific parameter control, due to significant differences in parameters between different furnaces, the specific parameters in this method are for a 33000KVA industrial silicon furnace, and include the following steps: The process establishes raw material intake detection and silicon output quantity detection. Besides the effective components, impurity detection in incoming raw materials is crucial for maintaining operational balance within the industrial furnace. The specific addition ratio is calculated based on the amount of silicon and carbon reacting to form silicon and carbon monoxide, combined with relevant raw material substances, through effective fixation of carbon and silicon elements. Specific calculations can be found in existing technologies. In addition, the silicon output quantity is inspected. Since inspecting the silicon output quantity requires sampling and laboratory testing, this application defines silicon output quantity detection as the quantity measured per unit time. In this application, the unit time is at least 8 hours. This unit time effectively maintains stable circuit operation and obtains more accurate data. The distance between the electrode and the furnace bottom, the depth of each electrode into the furnace, and the electrode consumption are obtained. In the entire production process, in addition to the consumption of raw materials, the consumption of electrodes will also affect the carbon stability in the furnace and the production cost. In a stable reaction process, the electrode consumption is usually proportional to the electric furnace load (MW). At the same time, load imbalance, electrode position, carbon balance, etc. will also affect the consumption. This application controls the consumption through power factor. In this application, the distance between the electrode and the furnace bottom, as well as the depth of the electrode in the raw material, are crucial. If the electrode is too deep, electrode consumption will be high, the arc zone will shrink, and the corresponding crucible area will shrink accordingly, severely damaging the furnace bottom, greatly shortening the furnace life, reducing the working voltage, increasing reactive power loss, decreasing output, and worsening production indicators. When the electrode is too shallow, the reaction zone shifts upward, the furnace charge surface temperature is high, frequent sparking occurs, making it difficult to unload the furnace, increasing the production of microsilica powder, and reducing silicon recovery rate, which will have a significant impact on output and data acquisition. Therefore, before entering dynamic adjustment, this application requires adjusting the electrode to a height of 0.9-1M from the electrode tip to the furnace bottom, and then collecting data. In this application, the electrode position (the distance between the electrode bottom ring and the material surface) must not be less than 400mm to avoid continuous electrode pressing and releasing, and the interval between each electrode pressing and releasing must not be less than 20 minutes.

[0020] This application establishes matching data between the amount of raw materials fed into the furnace and the amount of silicon discharged from the furnace per unit time. The main purpose of this application is to monitor the amount of silicon fed into and discharged from the furnace. In production, the materials discharged from the furnace per unit time are industrial silicon, silicon slag, micro silicon powder, coarse silicon powder, CO2 gas, etc. Among them, the gas part is more difficult to measure, while the rest are measurable. Therefore, this application uses Si element as the scalar for judging the material input and output balance of the electric furnace, and finally obtains the overall material balance of the electric furnace to ensure its long-term stable operation. If the total amount of material input into the furnace each day is greater than the total amount of material output for a long period of time, slag, silicon at the furnace bottom, or silicon carbide will accumulate in the furnace, resulting in the furnace bottom rising, electrode working end moving upward, severe surface scorching, furnace condition deterioration, and deterioration of production indicators. It should be understood that if an unadjustable problem occurs, the furnace needs to be shut down. The data on electrode consumption and feed amount are matched, as are the data on the ratio of silicon products to micro silicon powder. The electrode parameters obtained during this period are recorded. The electrode parameters include the distance between the electrode and the furnace bottom, the depth of each electrode entering the furnace, and the electrode consumption. By recording and comparing multiple parameters, the information inside the furnace is obtained, and the accuracy of dynamic adjustment is improved. The electrode power factor is adjusted to a set value. In this application, the electrode power factor is 0.85-0.95. Power factor = active power / apparent power, where apparent power = √(active power squared + reactive power squared). Active power is directly used to heat the furnace charge in the reaction zone for the production of industrial silicon. The active power input to the electric furnace is mainly controlled by the transformer tap position, i.e., the secondary side line voltage. Reactive power is dissipated in various components of the system and mainly depends on the electrode current. That is, for a given voltage, the deeper the electrode is in the furnace, the higher the reactive power. This application requires adjusting the electrode power factor to a range value before entering a multi-stage carbon balance adjustment stage. When the recorded data of silicon feed and discharge over multiple unit time periods are within a set range, the difference between the silicon addition amount and the sum of the industrial silicon output, microsilica powder amount, and silicon content in the slag over multiple unit time periods must be within 98%. This is because the time for the charge to remain on the surface, preheat, and participate in the reaction varies greatly. Therefore, this application requires multiple unit time periods to ensure the accuracy of the matching data. After a long reaction period, the direction of silicon can be basically determined. If the silicon feed and discharge are the same, it proves that the silicon element in the furnace has reached equilibrium. In order to ensure silicon output, the proportion of microsilica powder is monitored. When the proportion of microsilica powder is greater than the upper limit of the range of 20%-35%, it proves that silicon oxide has not been trapped by carbon elements and enters the multi-stage carbon balance adjustment stage of carbon increase. When the recorded data on the amount of silicon fed into and discharged from the furnace at multiple unit times are not within the set range, meaning that more silicon elements are entering the furnace and less are leaving, without timely adjustment, it will cause an increase in SiC at the furnace bottom, resulting in carbon deficiency. Further investigation is needed to determine if there is a carbon deficiency in the furnace. If the proportion of microsilicon powder in the furnace is below the lower limit of the range of 20%-35%, or the electrode insertion depth continues to decrease, or the distance to the furnace bottom continues to shorten, or the discharge rate continues to be low, it can be determined that there is a carbon deficiency in the furnace, and the furnace will enter the multi-stage carbon balance adjustment stage of carbon reduction. After exiting the multi-stage carbon balance adjustment stage, the raw material material, raw material ratio, electrode parameters, power supply parameters, and electrode position parameters of each adjustment stage can be obtained. A set of production data in which all indicators are in the optimal range during this period is used for production, that is, the data with the best power consumption and industrial silicon revenue. The production data of this stage is saved. When the deviations of all indicators of the raw material entry inspection data from the raw material indicators corresponding to the saved original production data are all within the preset tolerance range, when a new material is replaced, the previous data can be retrieved. When the error between the raw material data and the original data is within 0.5%, the corresponding original production data can be directly retrieved for production.

[0021] In this application, the multi-stage carbon balance adjustment stage for carbon increase includes: In the next unit time period, the amount of washed coal with a fixed carbon content is increased in the furnace feeding stage by 2%-4% of the microsilica powder output during that period. This application supplements this by increasing the amount of raw materials. When the microsilica powder output is large, during the SiO rising process, 2SiO + O2 = 2SiO2 > SiO + 2C = SiC + CO, which causes the microsilica powder content to exceed the normal value. By increasing the amount of coal, the reaction of the latter is improved. After running for several unit times, the data matching the silicon feed rate and output rate are within the set range. Then, add 0.5%-2% of the fixed carbon corresponding to the microsilica powder in the silicon output rate to the water-washed coal, and continue this step. This step can be performed multiple times to continuously control the microsilica powder within the optimal range. If the silicon feed rate and output rate do not match the set range, and the above steps are stopped immediately after the silicon feed rate and output rate deviate from the set value during the adjustment process, the distance between the electrode and the furnace bottom, the electrode feed depth, and the electrode power data are obtained. If the electrode pressure release is less than the preset value, that is, the speed of the electrode below per unit time is lower than the preset minimum value, which is determined by the electrode material and the electrode description, the electrode insertion depth gradually becomes shallower or the furnace bottom rises, indicating that there is excess carbon in the furnace, and the multi-stage carbon balance adjustment stage ends.

[0022] In this application, the multi-stage carbon balance adjustment stage of carbon reduction includes: In the next unit of time, due to the complexity of the raw materials, carbon excess mainly occurs during this period to find the optimal silicon addition ratio. At the same time, excess SiC at the bottom of the furnace is consumed. 2%-4% of silicon is added during the furnace feeding stage. The greater the matching data between the silicon feeding amount and the output amount and the preset value, the higher the amount of silicon added. In order to avoid excessive addition at one time, the maximum addition amount is controlled within 4%. After running for several unit times, the data matching the amount of silicon fed into the furnace and the amount of silicon discharged from the furnace did not return to the set range value. During the feeding stage, 0.5%-2% more silicon was added, and this step was continued. When the silicon feed rate and discharge rate match data return to the set range, i.e., after the silicon feed rate and discharge rate are within the set value, the multi-stage carbon balance adjustment stage ends. Since the silicon added in this step can also be discharged in the form of impurities and microsilicon powder, or the SiC in the furnace bottom cannot be discharged through reaction, if the data still does not recover after adding silicon 4 times, the adjustment is paused and the furnace condition is checked.

[0023] In this application, the raw materials for low-carbon coal smelting are silica, washed coal, and wood chips. Wood chips account for 14%-17% of the total fixed carbon, and are characterized by a loose, porous structure. Upon arrival, the silica is tested for elemental content, particle size, anti-explosion properties, and impurity content. The silica surface must not have a 1mm thick layer of outer layer or bean-shaped iron particles or other inclusions larger than 5mm in diameter, and must not contain 0-5mm of powder. The coal is tested for fixed carbon and ash content. The content of volatile matter, moisture, impurities, and particle size must be specified. Coal must not contain coal gangue, stones, soil, or other impurities. The silica content must be ≥99.5% silicon dioxide, ≤0.05% Fe2O3, ≤0.1% Al2O3, with a particle size of 60-180mm, of which the total of particles smaller than 60mm and larger than 180mm must not exceed 5%. The explosion resistance must be in the range of 75-85. Silica with poor explosion resistance will break into the furnace charge before entering the main reaction zone, affecting the permeability of the material. Highly blast-resistant silica cannot break into pieces after entering the main reaction zone, increasing the energy required for the reaction. It also forms a small amount of raw material (unmelted silica), disrupting the local material balance and increasing operational difficulty. Therefore, 75-85°C is optimal. Simultaneously, aluminum and calcium form very viscous slag at the furnace bottom, requiring strict control. The washed coal should have a moisture content ≤14%, ash content ≤4%, volatile matter ≥32%, fixed carbon ≥60%, and a particle size of 8-20 mm, with particles smaller than 8 mm or larger than 20 mm totaling no more than 5%. It should be noted that the higher the fixed carbon content of the coal, the lower its activity and the smaller its porosity. The reaction process depends on the reactivity of the carbon in the coal with SiO gas, i.e., the coal's reactivity.

[0024] In some embodiments, a 33000KVA semi-enclosed, low-profile furnace with electrode capacity of 11000*3KVA is used, with a furnace power of 29500-31500kwh, primary voltage of 115KV, primary current of 160-180A, commonly used secondary voltage of 220-235V, secondary current of 75-95KA, and the washed coal contains 10% moisture, 3.3% ash, 35.37% volatile matter, and 61.33% fixed carbon. Daily output on August 26: 74.828 tons; Daily unit consumption: 10258kWh / t; Average daily output for the month: 70.742 tons / day; Cumulative output for the month: 1839.298 tons; Cumulative unit consumption for the month: 10220 kWh / t; Total power outage time this month: 21 hours and 41 minutes.

[0025] The system operates stably under the all-coal low-carbon process, with output at a normal level and power consumption that is moderate to excellent within the industry.

[0026] This application also includes a dynamic control-based industrial silicon all-coal low-carbon smelting system, comprising a data acquisition module: an electrode depth monitoring module, an electrode pressure release monitoring module, an electrode power monitoring module, a current acquisition module, a voltage acquisition module, and a current compensation acquisition module, used to monitor various data required in this application. The electrode insertion depth directly relates to the position of the electric arc and the reaction zone within the furnace. Specifically, temperature changes can be determined through direct weighing, ultrasonic positioning, or indirect methods based on thermocouple data inserted in the furnace bottom, and by considering factors such as furnace mouth gas composition, molten pool surface temperature, and acoustic characteristics of the electric arc within the furnace. The electrode working end position is determined by measuring the reactance of the molten pool, as detailed in existing technology; the electrode discharge monitoring module automatically and continuously measures the discharge amount to provide data for automatic control, and the electrode consumption rate can be inferred from the discharge amount; the electrode power monitoring module ensures the power load balance of the three-phase electrodes and improves efficiency; the current acquisition module and voltage acquisition module measure the magnitude of the current and voltage flowing through the electrodes and calculate the power factor; the current compensation acquisition module automatically determines how many compensation capacitors to connect or disconnect based on the acquired data, stabilizing the power factor within the range of 0.85-0.95 in this application.

[0027] Data fusion terminal: The central processing unit connected to each acquisition module receives real-time data from six major acquisition modules, including electrode depth, pressure release, power, current, voltage, and compensation. It performs preprocessing such as filtering, noise reduction, and outlier removal to ensure the quality of the input data. It is used to execute the multi-stage carbon balance adjustment logic mentioned above and stores the data to provide key data support for specific execution. It also establishes a database. When the deviation between new raw material data and historical data is within the preset tolerance range, the corresponding historical optimal parameters can be directly retrieved for production. The execution end consists of an electrode lifting control module, a transformer gear adjustment module, and a batching control module connected to the central processing unit, used to execute raw material feeding into the furnace, electrode control, and voltage and current regulation. Display end: Human-machine interface, used to display monitoring data and control commands in real time. Operators can monitor in real time and manually take over control when necessary.

[0028] As can be seen from the above technical solutions, this application, through research on low-carbon coal smelting of industrial silicon, found that in the feeding stage, after controlling the impurities of silica, coal, and wood chips, the main parameters are the matching of silicon conversion rate and power factor. When the two data reach the optimal matching value, the reaction balance in the system is guaranteed, and there will be no carbon excess or carbon deficiency, thus ensuring stable production of the system. However, the raw material composition of coal and silica is complex. The amount of addition obtained by calculating based solely on the effective content of carbon and silica will result in carbon excess or carbon deficiency during actual operation, leading to a decrease in production efficiency and yield. This application strictly controls the composition of raw materials before they enter the furnace and calculates the amount of addition based on the effective component content before smelting. In order to ensure the balance inside the furnace, this application uses multiple detection methods to obtain smelting information during smelting. When the electrode power factor is between 0.85 and 0.95, the distance between the electrode and the furnace bottom, the electrode insertion depth, and the electrode consumption are detected to monitor whether they are within the set range. This application also monitors silicon balance data. Within multiple time units, the difference between the added silicon amount and the sum of industrial silicon output, microsilica powder amount, and silicon content in the slag must be within 98% to ensure normal silicon reaction and furnace silicon consumption. When the entire system is operating normally, to further increase industrial silicon output, the proportion of microsilica powder will be positioned. When the above values ​​fall outside the range, the furnace condition will be dynamically adjusted through a multi-stage carbon balance adjustment phase within multiple time units until it returns to the set value, optimizing production indicators. Specifically, after furnace carbon balance, production will proceed under optimal conditions for power factor, industrial silicon output, and electrode consumption. This adjustment process and related parameters will be recorded, and the original data will be accumulated. When the data collected before raw materials enter the furnace is within the set range compared to the original data, the addition ratio can be directly adjusted to the original data value for production. This dynamic control ensures the stability and efficiency of all-coal production.

[0029] Other embodiments of this application will readily occur to those skilled in the art upon consideration of the specification and practice of the application disclosed herein. This application is intended to cover any variations, uses, or adaptations of this application that follow the general principles of this application and include common knowledge or customary techniques in the art not disclosed herein. The specification and examples are to be considered exemplary only, and the true scope of this application is indicated by the claims.

[0030] It should be understood that this application is not limited to the structure described above, and various modifications and changes can be made without departing from its scope. The embodiments of this application described above do not constitute a limitation on the scope of protection of this application.

Claims

1. A dynamic regulation-based industrial silicon full-coal low-carbon smelting method, characterized in that, Includes the following steps: Establish a system for detecting incoming raw materials and silicon output from the furnace; Obtain the distance between the electrode and the furnace bottom, the depth of each electrode entering the furnace, and the amount of electrode consumption; Establish matching data for raw material input and silicon output per unit time, matching data for electrode consumption and input, and matching data for the ratio of silicon products to microsilicon powder, and record the electrode parameters obtained during this period. Adjust the electrode power factor to the set value to enter the multi-stage carbon balance adjustment stage; When the recorded data of silicon input and output at multiple unit times are within the set range and the proportion of microsilicon powder is greater than the upper limit of the range of 20%-35%, the multi-stage carbon balance adjustment stage of carbon increase is entered. When the recorded data of silicon feed and output at multiple unit times are not within the set range, and the proportion of microsilicon powder is lower than the lower limit of the 20%-35% range, or the electrode insertion depth continues to decrease, or the furnace bottom distance continues to shorten, or the output is consistently low, the carbon balance adjustment stage of carbon reduction multi-stage is entered. Take a set of production data in which all indicators are in the optimal range during the period and carry out production, and save the production data for this period; When the deviations of all indicators in the raw material entry inspection data from the raw material indicators corresponding to the saved original production data are all within the preset tolerance range, the corresponding original production data can be directly retrieved for production.

2. The method for low-carbon industrial silicon smelting using all-coal based on dynamic control according to claim 1, characterized in that, The multi-stage carbon balance adjustment phase of carbon increase includes: In the next unit of time, the amount of washed coal fed into the furnace during the furnace stage will increase by 2%-4% of the microsilica powder production during that period, corresponding to a fixed carbon content. After running for several unit times, the data matching the silicon feed rate and output rate are within the set range. Then, the amount of washed coal corresponding to 0.5%-2% fixed carbon of microsilica powder in the silicon output rate is increased again, and this step is continued. If the data on the silicon feed rate and the output rate are not within the set range, obtain data on the distance between the electrode and the furnace bottom, the electrode insertion depth, and the electrode power. If the electrode pressure release is less than the preset value, the electrode insertion depth gradually becomes shallower or the furnace bottom rises, ending the multi-stage carbon balance adjustment stage.

3. The method for low-carbon industrial silicon smelting using all-coal based on dynamic control according to claim 2, characterized in that, The multi-stage carbon balance adjustment phase of carbon reduction includes: In the next unit of time, the amount of silica added during the furnace feeding stage increases by 2%-4%; After running for several unit times, the data matching the amount of silicon fed into the furnace and the amount of silicon discharged from the furnace did not return to the set range value. During the feeding stage, 0.5%-2% more silicon was added, and this step was continued. When the silicon feed rate and output rate match the set range, the multi-stage carbon balance adjustment phase ends. If the data still does not recover after adding silicon four times, the adjustment is paused and the furnace condition is checked.

4. The method for low-carbon industrial silicon smelting using all-coal based on dynamic control according to claim 3, characterized in that, The raw materials for the all-coal low-carbon smelting are silica, washed coal and wood chips, of which wood chips account for 14%-17% of the total fixed carbon.

5. The method for low-carbon industrial silicon smelting using all-coal based on dynamic control according to claim 4, characterized in that, The raw material entry inspection includes testing the elemental content, particle size, anti-explosion properties, and impurity content of silica, and testing the fixed carbon, ash content, volatile matter, moisture content, impurity content, and particle size of coal.

6. The method for low-carbon industrial silicon smelting using all-coal based on dynamic control according to claim 5, characterized in that, The silica contains ≥99.5% silicon dioxide, ≤0.05% Fe2O3, ≤0.1% Al2O3, and has a particle size of 60-180mm, of which the total particle size smaller than 60mm and larger than 180mm cannot exceed 5%, and its explosion resistance range is 75-85.

7. The method for low-carbon industrial silicon smelting using all-coal based on dynamic control according to claim 5, characterized in that, The washed coal has a moisture content of ≤14%, ash content of ≤4%, volatile matter of ≥32%, fixed carbon of ≥60%, and a particle size of 8-20 mm, of which the total of particles smaller than 8 mm and larger than 20 mm does not exceed 5%.

8. The method for low-carbon industrial silicon smelting using all-coal based on dynamic control according to claim 3, characterized in that, The electrode power factor is 0.85-0.

95.

9. A method for low-carbon industrial silicon smelting using all-coal based on dynamic control according to claim 3, characterized in that, The unit of time is at least 8 hours.

10. The method for low-carbon smelting of industrial silicon using all-coal based on dynamic control as described in claims 1-9 further includes a system for low-carbon smelting of industrial silicon using all-coal based on dynamic control, characterized in that: Includes data acquisition modules: electrode depth monitoring module, electrode pressure discharge monitoring module, electrode power monitoring module, current acquisition module, voltage acquisition module, and current compensation acquisition module; Data fusion terminal: a central processing unit connected to each acquisition module, used to execute the multi-stage carbon balance adjustment logic as described in any one of claims 1-9, and to store data; Execution end: Electrode lifting control module, transformer gear adjustment module, and batching control module connected to the central processing unit; Display end: Human-computer interaction interface, used to display monitoring data and control commands in real time.