A method for preparing high-strength, high-temperature resistant aerogel composite materials by ternary metal hybridization
By introducing ternary metal hybridization and metal adhesion promoters, a stable three-dimensional aerogel network is constructed, which solves the problems of structural collapse and reduced thermal insulation performance of traditional aerogels under high temperature environments. This enables the preparation of high-strength and high-temperature resistant aerogel composite materials suitable for high-temperature extreme environments.
Patent Information
- Application Number
- CN202610735516.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-05-26
- Publication Date
- 2026-11-17
AI Technical Summary
Traditional aerogels have low mechanical strength, high brittleness and poor high-temperature stability, making them difficult to use in extreme high-temperature environments. Existing metal doping technologies have problems such as uneven distribution of impurity phases, weak framework bonding and insufficient high-temperature stability, which cannot meet the needs of industrial high-temperature insulation and aerospace thermal protection.
By employing a ternary metal hybridization strategy, metal adhesion promoters are introduced to facilitate in-situ bonding of metal ions with the silicon-based framework, thereby constructing a continuous and dense three-dimensional aerogel network. The synergistic effect of zirconium, aluminum, and nickel ternary metal oxides is utilized to form a stable bonding network, enhancing the mechanical properties and high-temperature stability of the aerogel.
A high-strength, high-temperature resistant, and ultra-insulating aerogel composite material was prepared, which solved the problems of structural collapse and reduced thermal insulation performance of traditional aerogels under high-temperature environments. It is suitable for high-temperature extreme environments and has good prospects for industrial application.
Smart Images

Figure CN123105664A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the technical field of high-strength, high-temperature resistant SiO2 aerogel preparation methods, specifically relating to a method for preparing high-strength, high-temperature resistant aerogel composite materials by ternary metal hybridization. Background Technology
[0002] Aerogels, as nanoporous materials with ultra-high specific surface area, extremely low density, and excellent thermal insulation properties, have broad application prospects in aerospace, energy, chemical industry, and building energy conservation. However, traditional aerogels (such as silica and alumina aerogels) face two major bottlenecks in practical applications: first, they have low mechanical strength and high brittleness, making them difficult to withstand mechanical loads during processing and service; second, they have poor high-temperature stability, easily undergoing sintering, crystal transformation, or pore structure collapse under long-term high-temperature environments, leading to a sharp decline in thermal insulation performance and limiting their use in extreme high-temperature environments.
[0003] To overcome these shortcomings, researchers have attempted to introduce metal or metal oxide reinforcing phases, utilizing metal hybridization effects to improve the aerogel's skeletal structure. Current metal-doped aerogel technologies primarily employ single-metal and bimetallic modification methods. These methods not only suffer from performance defects such as uneven impurity phase distribution, weak skeletal bonding, and insufficient high-temperature stability, but also face practical challenges including high preparation costs, complex processes, and difficulties in large-scale production. Specifically, single-metal doping methods struggle to simultaneously achieve both mechanical enhancement and improved high-temperature resistance in aerogels, while the synergistic effect of bimetallic systems is relatively limited. Ultimately, this technology fails to meet the dual core requirements of high-strength and ultra-high-temperature resistant aerogels for applications such as industrial high-temperature insulation and aerospace thermal protection.
[0004] Furthermore, there is currently a lack of a preparation method that can systematically solve the above problems through a ternary metal hybridization strategy. Summary of the Invention
[0005] To address the aforementioned problems, the present invention aims to provide a method for preparing high-strength, high-temperature-resistant aerogel composite materials using ternary metal hybridization. This method employs a ternary metal synergistic hybridization strategy, introducing a metal adhesion promoter to effectively solve the problem of metal ion sedimentation and further enhance the in-situ bonding ability between metal ions and the silicon-based framework. This enables directional cross-linking, constructing a continuous, dense, and high-temperature-resistant three-dimensional aerogel network, thus solving the technical challenges of poor mechanical properties, poor high-temperature resistance, and easy pulverization and cracking of traditional aerogels. This method is simple, controllable, and low-cost, and the resulting product possesses excellent properties such as high strength, high-temperature resistance, and superior thermal insulation, facilitating large-scale production.
[0006] The objective of this invention is achieved through the following technical solution: A method for preparing high-strength, high-temperature resistant aerogel composite materials by ternary metal hybridization includes the following steps: S1. Mix the silicon source, alcohol and deionized water, add a hydrolysis aid to adjust the pH to 2-4, and hydrolyze at 40-60℃ to obtain silica sol. S2. A ternary metal hybrid agent is obtained by uniformly mixing zirconium salt, aluminum salt, nickel salt and metal adhesion promoter in a certain proportion. S3. Slowly add the ternary metal hybrid agent obtained in step S2 to the silica sol obtained in step S1, stir and mix to obtain the hybrid sol; S4. Add a catalyst to the hybrid sol obtained in step S3 to adjust the pH to 7-9, and gel to obtain a wet gel; S5. The wet gel obtained in step S4 is subjected to aging, solvent replacement and drying in sequence to obtain the final product.
[0007] Further, in step S1, the silicon source is selected from one of tetraethyl orthosilicate, methyltrimethoxysilane, dimethyldimethoxysilane, and water glass. The hydrolysis products of the above silicon sources are rich in silanol groups, which is beneficial for the subsequent polycondensation reaction to form a continuous and dense three-dimensional network structure of silica.
[0008] Further, in step S1, the hydrolysis aid is selected from acetic acid, hydrochloric acid, oxalic acid, and boric acid; the alcohol is methanol or ethanol; the mass ratio of the alcohol, deionized water, and silicon source is 1:(0.12-0.52):(3-7), and the hydrolysis time is 1-3 hours. Within the above ratio range, the silicon source can be fully hydrolyzed under acidic conditions to form a clear, transparent silica sol with suitable viscosity, laying the foundation for subsequent uniform doping of metal ions.
[0009] Further, the ternary metal hybrid agent mentioned in step S2 is obtained by mixing zirconium salt, aluminum salt, nickel salt, and metal adhesion promoter in a mass ratio of 1:(0.4-1.6):(0.3-1.2):(0.1-1.5); the total amount of the ternary metal hybrid agent added is 8%-20% of the silicon source mass; the stirring time after dropwise addition is 30-60 min. Controlling the doping amount of the ternary metal hybrid agent within the above range can significantly enhance the mechanical strength and high-temperature resistance of the aerogel framework without causing stress concentration or pore blockage due to excessive doping. Using a slow dropwise addition and thorough stirring can ensure that the ternary metal hybrid agent and silica sol are mixed evenly to form a stable hybrid sol system.
[0010] Further, in step S2, the zirconium salt is zirconium chloride or zirconium nitrate; the aluminum salt is aluminum nitrate or aluminum chloride pentahydrate; and the nickel salt is at least one of nickel nitrate, nickel chloride, or nickel acetate. By selecting zirconium, aluminum, and nickel metal salts, the synergistic high-temperature stabilizing effect of the ternary metal ions can be utilized to form a heat-resistant oxide-anchored aerogel framework at high temperatures, effectively suppressing high-temperature sintering and structural collapse.
[0011] Further, in step S2, the metal adhesion promoter is one of AP-2000 titanate coupling agent, AP-3000 aluminate coupling agent, AP-1000 general-purpose silane coupling agent, ferrocene formaldehyde, and hydrofluoroether 458. The introduction of the metal adhesion promoter effectively solves the problem of metal ion sedimentation during the gelation process, while simultaneously improving the interaction force between Zr / Al / Ni ions and the aerogel molecular chains, enabling them to form a more stable bonding network.
[0012] Furthermore, in step S4, the catalyst is selected from ammonia, ammonium fluoride, tetramethylammonium hydroxide, and ethylenediamine, and is used to promote the transformation of the sol system from acidic to alkaline, accelerate the silanol condensation reaction, and transform the hybrid sol into a wet gel; the gelation temperature is 50-60℃, and the gelation time is 20-55 min. Under these conditions, the gelation speed is moderate, which is conducive to the formation of a uniform three-dimensional network.
[0013] Furthermore, in step S4, the gelation process involves pouring the hybrid sol with the added catalyst into a mold or combining it with a reinforcing fiber matrix and then allowing it to stand to solidify; the reinforcing fiber is selected from glass fiber, ceramic fiber, and high-silica fiber. By combining the hybrid sol with the reinforcing fiber matrix, the overall mechanical properties of the aerogel composite material can be further improved, meeting the requirements of different application scenarios for material strength and toughness.
[0014] Further, in step S5, the aging step involves aging the wet gel in an alcohol solution atmosphere at 50–60°C for 24–72 hours. This aging treatment further cross-links and strengthens the gel skeleton, improving its resistance to shrinkage and cracking during subsequent drying. The solvent replacement involves replacing the wet gel pores with an alcohol solution at 50–60°C 3–5 times, each time for 48 hours. Through multiple solvent replacements, the moisture and impurities in the wet gel pores are replaced with an alcohol solution with lower surface tension, which helps maintain the integrity of the gel skeleton during subsequent drying. The drying is supercritical CO2 drying, with a drying pressure of 12–15 MPa, a drying temperature of 50–60°C, and a drying time of 6–8 hours. Supercritical CO2 drying can eliminate capillary stress to the maximum extent, avoiding the collapse and shrinkage of the gel skeleton, thereby obtaining an aerogel composite material that maintains the original nanoporous structure.
[0015] Furthermore, in step S5, the solvent used for solvent replacement is a combination of methanol and deionized water or a combination of ethanol and deionized water.
[0016] The present invention also provides a ternary metal hybrid aerogel composite material, which is prepared by the method described in any one of the above methods, and comprises a silicon-oxygen framework and a Zr-Al-Ni ternary metal oxide network, wherein Zr, Al and Ni are uniformly dispersed in the silicon-oxygen framework in the form of metal oxides to form an ordered nanoporous structure.
[0017] Compared with the prior art, the present invention has the following beneficial effects:
[0018] (1) By introducing a metal adhesion promoter, the present invention effectively solves the problem of metal ion sedimentation during the gelation process, while improving the interaction force between Zr / Al / Ni ions and aerogel molecular chains, making them form a more stable bonding network with mechanical strength far superior to single / double metal doped aerogels.
[0019] (2) This invention utilizes the high-temperature stabilization effect of zirconium, aluminum and nickel ternary metal oxides to anchor the skeleton, suppress high-temperature sintering, and can be used for a long time at temperatures above 1000℃.
[0020] (3) The present invention has in-situ hybridization of metal ions, which is uniformly distributed. The prepared material is free from cracking, collapse and delamination, and has high strength, super heat insulation, high porosity, high temperature resistance and aging resistance, making it applicable to a wider range of scenarios. Attached Figure Description
[0021] Figure 1 This is a process flow diagram of Embodiment 1 of the present invention.
[0022] Figure 2 This is a photograph of the Zr-Al-Ni ternary hybrid high-strength high-temperature resistant aerogel block (sample 1) in Example 1 of the present invention.
[0023] Figure 3 This is a photograph demonstrating the temperature resistance of the Zr-Al-Ni ternary hybrid ceramic fiber aerogel composite material (sample 2) at 1200℃ in Example 2 of the present invention.
[0024] Figure 4 This is a graph showing the temperature resistance and hot / cold surface temperature change curves of the Zr-Al-Ni ternary hybrid ceramic fiber aerogel composite material (sample 2) at 1200℃ in Example 2 of the present invention.
[0025] Figure 5 This is a photograph of the Zr-doped aerogel block (sample 3) in Comparative Example 1 of this invention.
[0026] Figure 6 This is a photograph of the silica aerogel block (sample 4) in Comparative Example 2 of the present invention. Detailed Implementation
[0027] The following specific embodiments illustrate the implementation of the present invention. Those skilled in the art can easily understand other advantages and effects of the present invention from the content disclosed in this specification. The described embodiments are merely some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0028] Example 1: This embodiment provides a method for preparing high-strength, high-temperature resistant aerogel composite materials by ternary metal hybridization, including the following steps:
[0029] S1. Mix methanol, deionized water, and tetraethyl orthosilicate in a mass ratio of 1:0.14:4.5, add hydrochloric acid as a hydrolysis aid to adjust the pH to 3, and stir and hydrolyze at 50°C for 3 hours to obtain a transparent silica sol.
[0030] S2. Zirconium chloride, aluminum nitrate, nickel chloride, and AP-3000 aluminate coupling agent are mixed evenly in a mass ratio of 1:0.6:0.4:1 to obtain a ternary metal hybrid agent.
[0031] S3. Slowly pour the ternary metal hybrid agent into the sol. The total doping amount of the ternary metal hybrid agent is 12% of the mass of the silicon source. Continue stirring for 60 minutes to obtain a uniform hybrid sol.
[0032] S4. Add ammonia to the hybrid sol to adjust the pH to 8, stir rapidly for 15 minutes, pour into a mold, and let stand at 50°C for 25 minutes to form a wet gel.
[0033] S5. The wet gel was aged in a methanol solution atmosphere at 50℃ for 24 h, and then replaced with methanol three times, each time for 48 h, with the replacement temperature controlled at 50℃. After replacement, the wet gel was placed in a supercritical drying reactor, the valve was closed, and liquid carbon dioxide was slowly added to increase the pressure to 14 MPa. The reactor was then heated to 55℃ for supercritical CO2 drying for 8 h. After drying, the pressure was slowly released to atmospheric pressure to obtain a Zr-Al-Ni ternary hybrid high-strength high-temperature resistant aerogel block (sample 1).
[0034] Example 2:
[0035] This embodiment provides a method for preparing high-strength, high-temperature resistant aerogel composite materials by ternary metal hybridization, including the following steps:
[0036] S1. Mix methanol, deionized water, and tetraethyl orthosilicate in a mass ratio of 1:0.14:4.5, add hydrochloric acid as a hydrolysis aid to adjust the pH to 3, and stir and hydrolyze at 50°C for 3 hours to obtain a transparent silica sol.
[0037] S2. Zirconium chloride, aluminum nitrate, nickel chloride, and AP-3000 aluminate coupling agent are mixed evenly in a mass ratio of 1:0.6:0.4:1 to obtain a ternary metal hybrid agent.
[0038] S3. Slowly pour the ternary metal hybrid agent into the sol. The total doping amount of the ternary metal hybrid agent is 12% of the mass of the silicon source. Continue stirring for 60 minutes to obtain a uniform hybrid sol.
[0039] S4. Add ammonia to the hybrid sol to adjust the pH to 8, stir rapidly for 15 minutes, pour the hybrid sol into the ceramic fiber felt, and let it stand at 50°C for 28 minutes to form a wet gel.
[0040] S5. The wet gel was aged in a methanol solution atmosphere at 50℃ for 24 hours, and then replaced with methanol three times, each time for 48 hours, with the replacement temperature controlled at 50℃. After replacement, the wet gel was placed in a supercritical drying reactor, and liquid carbon dioxide was slowly added after the valve was closed, the pressure was increased to 14 MPa, and the temperature was heated to 55℃ for supercritical CO2 drying for 8 hours. After drying, the pressure was slowly released to atmospheric pressure to obtain a flexible high-temperature resistant ceramic fiber aerogel composite material (sample 2).
[0041] Comparative Example 1:
[0042] This comparative example provides a method for creating a single-metal salt aerogel composite material, comprising the following steps:
[0043] S1. Mix methanol, deionized water, and tetraethyl orthosilicate in a mass ratio of 1:0.14:4.5, add hydrochloric acid as a hydrolysis aid to adjust the pH to 3, and stir and hydrolyze at 50°C for 3 hours to obtain a transparent silica sol.
[0044] S2. Slowly pour 1 part of zirconium chloride into the transparent silica sol. The total doping amount of zirconium chloride is 12% of the mass of the silicon source. Continue stirring for 60 minutes to obtain a homogeneous hybrid sol.
[0045] S3. Add ammonia to the hybrid sol to adjust the pH to 8, stir rapidly for 15 minutes, pour into a mold, and let stand at 50°C for 37 minutes to form a wet gel.
[0046] S4. The wet gel was aged in a methanol solution atmosphere at 50℃ for 24 h, and then replaced with methanol three times, each time for 48 h, with the replacement temperature controlled at 50℃. After replacement, the wet gel was placed in a supercritical drying reactor, the valve was closed, and liquid carbon dioxide was slowly added to increase the pressure to 14 MPa. The reactor was then heated to 55℃ for supercritical CO2 drying for 8 h. After drying, the pressure was slowly released to atmospheric pressure to obtain Zr-doped aerogel blocks (sample 3).
[0047] Comparative Example 2:
[0048] This comparative example provides a method for producing conventional aerogel composite materials, including the following steps:
[0049] S1. Mix methanol, deionized water, and tetraethyl orthosilicate in a mass ratio of 1:0.14:4.5, add hydrochloric acid as a hydrolysis aid to adjust the pH to 3, and stir and hydrolyze at 50°C for 3 hours to obtain a transparent silica sol.
[0050] S2. Add ammonia to the silica sol to adjust the pH to 8, stir rapidly for 15 minutes, pour into a mold, and let stand at 50°C for 14 minutes to form a wet gel.
[0051] S3. The wet gel was aged in a methanol solution atmosphere at 50℃ for 24 hours, and then replaced with methanol three times, each time for 48 hours, with the replacement temperature controlled at 50℃. After replacement, the wet gel was placed in a supercritical drying reactor, the valve was closed, and liquid carbon dioxide was slowly added to increase the pressure to 14 MPa. The reactor was then heated to 55℃ for supercritical CO2 drying for 8 hours. After drying, the pressure was slowly released to atmospheric pressure to obtain silica aerogel blocks (sample 4).
[0052] Performance testing
[0053] The samples obtained in Examples 1-2 and Comparative Examples 1-2 were subjected to performance tests. The test items included: sample size and specifications, density, thermal conductivity at 25℃, thermal conductivity at 1000℃, and the appearance of the samples after supercritical drying. The test results are shown in Table 1.
[0054] Table 1. Performance Comparison of Various Examples and Comparative Samples
[0055] The data in Table 1 shows that:
[0056] (1) In Examples 1 and 2 of this invention, the Zr-Al-Ni ternary metal hybridization technique was used, and the resulting samples remained intact and undamaged after supercritical drying. In contrast, the single-metal Zr-doped aerogel in Comparative Example 1 cracked after drying, and the pure SiO2 aerogel in Comparative Example 2 cracked and broke after drying. This indicates that the method of this invention, through ternary metal hybridization and the introduction of metal adhesion promoters, effectively improves the strength and structural uniformity of the gel skeleton and significantly improves the crack resistance during the drying process.
[0057] (2) In terms of room temperature thermal insulation performance, the thermal conductivity of Examples 1 to 2 at 25℃ is 0.019 to 0.021 W / (m·K), which is comparable to 0.023 W / (m·K) of Comparative Example 1 and 0.018 W / (m·K) of Comparative Example 2, indicating that the ternary metal hybridization modification did not have an adverse effect on the room temperature thermal insulation performance of the aerogel.
[0058] (3) Regarding high-temperature thermal insulation performance, the thermal conductivity at 1000℃ of Examples 1 and 2 is 0.076–0.081 W / (m·K), which is much lower than that of Comparative Example 1 (0.11 W / (m·K)) and Comparative Example 2 (0.44 W / (m·K). This indicates that the Zr-Al-Ni ternary metal ions introduced in this invention can form a heat-resistant oxide-anchored aerogel skeleton at high temperatures, effectively suppressing high-temperature sintering and structural collapse, and significantly improving the high-temperature thermal insulation performance of the material, enabling it to be used for a long time in extreme high-temperature environments above 1000℃.
[0059] In summary, this invention successfully prepared an aerogel composite material with high strength, high temperature resistance, and superior thermal insulation properties through ternary metal hybridization and the introduction of a metal adhesion promoter. This method is simple and controllable, uses inexpensive raw materials, and produces a product with excellent overall performance, demonstrating promising prospects for industrial application.
[0060] Other aspects of this invention that are not detailed herein are all conventional techniques known to those skilled in the art.
[0061] It should be noted that the terms “comprising,” “including,” or any other variations are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such process, method, article, or apparatus.
[0062] The scope of protection of this invention is not limited to the technical solutions disclosed in the specific embodiments. Any modifications, equivalent substitutions, improvements, etc., made to the above embodiments based on the technical essence of this invention shall fall within the scope of protection of this invention.
Claims
1. A method for preparing high-strength high-temperature-resistant aerogel composites by ternary metal hybridization, characterized in that, Includes the following steps: S1. Mix the silicon source, alcohol and deionized water, add a hydrolysis aid to adjust the pH to 2-4, and hydrolyze at 40-60℃ to obtain silica sol; S2. A ternary metal hybrid agent is obtained by uniformly mixing zirconium salt, aluminum salt, nickel salt and metal adhesion promoter in a certain proportion; S3. Slowly add the ternary metal hybrid agent obtained in step S2 to the silica sol obtained in step S1, stir and mix to obtain the hybrid sol; S4. Add a catalyst to the hybrid sol obtained in step S3 to adjust the pH to 7-9, and gel to obtain a wet gel; S5. The wet gel obtained in step S4 is subjected to aging, solvent replacement and drying in sequence to obtain the final product.
2. The method of claim 1, wherein the ternary metal hybrid is used to prepare high-strength, high-temperature resistant aerogel composites. In step S1, the silicon source is selected from one of tetraethyl orthosilicate, methyltrimethoxysilane, dimethyldimethoxysilane, and water glass.
3. The method of claim 1, wherein the ternary metal hybrid is prepared to form the high-strength, high-temperature resistant aerogel composite material. In step S1, the hydrolysis aid is selected from one of acetic acid, hydrochloric acid, oxalic acid, and boric acid; the alcohol is methanol or ethanol; the mass ratio of the alcohol, deionized water, and silicon source is 1:(0.12-0.52):(3-7), and the hydrolysis time is 1-3 hours.
4. The method of claim 1 for the preparation of high-strength, high-temperature resistant aerogel composites by ternary metal hybridization, characterized by: The ternary metal hybrid agent mentioned in step S2 is obtained by mixing zirconium salt, aluminum salt, nickel salt and metal adhesion promoter in a mass ratio of 1:(0.4~1.6):(0.3~1.2):(0.1-1.5); the total amount of ternary metal hybrid agent added is 8%~20% of the mass of silicon source; the stirring time after drop addition is 30~60min.
5. The method of claim 1 for the preparation of high-strength, high-temperature resistant aerogel composites by ternary metal hybridization, characterized by: In step S2, the zirconium salt is zirconium chloride or zirconium nitrate; the aluminum salt is aluminum nitrate or aluminum chloride pentahydrate; and the nickel salt is at least one of nickel nitrate, nickel chloride, or nickel acetate.
6. The method of claim 1 for the preparation of high-strength, high-temperature resistant aerogel composites by ternary metal hybridization, characterized by: In step S2, the metal adhesion promoter is one of AP-2000 titanate coupling agent, AP-3000 aluminate coupling agent, AP-1000 general silane coupling agent, ferrocene formaldehyde, and hydrofluoroether 458.
7. The method of claim 1, wherein the ternary metal hybrid is used to prepare high-strength, high-temperature resistant aerogel composites. In step S4, the catalyst is selected from ammonia, ammonium fluoride, tetramethylammonium hydroxide, and ethylenediamine; the gelation temperature is 50-60℃, and the gelation time is 20-55 min.
8. The method of claim 1, wherein the ternary metal hybrid is used to prepare high-strength, high-temperature resistant aerogel composites. In step S4, the gelation process involves pouring the hybrid sol with the added catalyst into a mold or combining it with the reinforcing fiber matrix and then allowing it to stand to form a solid shape; the reinforcing fiber is selected from one of glass fiber, ceramic fiber, and high silica fiber.
9. The method of claim 1, wherein the ternary metal hybrid is used to prepare high-strength, high-temperature resistant aerogel composites. In step S5, the aging step involves aging the wet gel in an alcohol solution atmosphere at 50-60°C for 24-72 hours; the solvent replacement involves replacing the solvent 3-5 times with an alcohol solution at 50-60°C, each time for 48 hours; the drying is supercritical CO2 drying, with a drying pressure of 12-15 MPa, a drying temperature of 50-60°C, and a drying time of 6-8 hours.
10. The ternary metal hybrid aerogel composite prepared according to the method of any one of claims 1 to 8, characterized by: Prepared by any one of claims 1 to 9, it comprises a silicon-oxygen framework and a Zr-Al-Ni ternary metal oxide network, wherein Zr, Al, and Ni are uniformly dispersed in the silicon-oxygen framework in the form of metal oxides to form an ordered nanoporous structure.