A method for the combined preparation of lithium carbonate and lithium sulfide from spodumene
By continuously roasting spodumene, sulfation roasting, and sulfidation reaction, combined with the absorption of MDEA aqueous solution, a closed-loop hydrogen sulfide recycling system is constructed. This solves the problems of low production capacity, high energy consumption, and resource waste in the production of lithium carbonate and lithium sulfide by the spodumene sulfuric acid method, and realizes efficient resource utilization and green production.
Patent Information
- Application Number
- CN202611378462.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-07
- Publication Date
- 2026-11-17
AI Technical Summary
The existing lithium carbonate production process using spodumene sulfuric acid has problems such as low production capacity, high energy consumption, poor product stability, serious hydrogen sulfide tail gas pollution and resource waste, and the treatment of industrial sulfuric acid waste gas is separated from lithium salt production, resulting in low overall resource utilization and difficulty in meeting the needs of large-scale production, green and low-carbon development and resource recycling.
By employing continuous roasting of spodumene, sulfation roasting, continuous lithium carbonate preparation and sulfidation reaction, combined with MDEA aqueous solution absorption and negative pressure desorption, a closed-loop hydrogen sulfide circulation system is constructed to synergistically treat external sulfuric acid-containing waste gas, achieving continuous production and comprehensive resource utilization throughout the entire process.
It has achieved a significant increase in production capacity and quality, improved stability, reduced production costs, realized the closed-loop recycling of sulfur resources and the synergistic treatment of multiple waste gases, and meets the requirements of green chemical industry.
Abstract
Description
Technical Field
[0001] This invention relates to the fields of lithium resource deep processing and sulfur-containing tail gas resource recycling technology, specifically to a method for the joint preparation of lithium carbonate and lithium sulfide from spodumene. Background Technology
[0002] Lithium carbonate is a core raw material for lithium-ion battery cathode materials. With the rapid development of new energy vehicles and large-scale electrochemical energy storage industries globally, the market demand for high-purity battery-grade lithium carbonate continues to surge. Lithium sulfide, as a key cathode / electrolyte material for high-energy-density all-solid-state lithium batteries and lithium-sulfur batteries, has become a key research material in the next-generation energy storage battery field due to its excellent electrochemical performance, and its industrial application prospects are very broad. Spodumene, as a hard-rock lithium ore with abundant reserves and high lithium oxide content, is the mainstream raw material for the industrial production of lithium carbonate. The sulfuric acid process for lithium extraction has become the most widely used technical route in the spodumene processing field due to its high lithium leaching rate, mature process, and easy control of product purity.
[0003] Existing technologies for producing lithium carbonate using the spodumene sulfuric acid process have yielded numerous industrialized solutions. For example, Chinese invention CN103950956B discloses a process for producing lithium carbonate from spodumene concentrate using the sulfuric acid process. This process provides the core steps of the traditional sulfuric acid process: roasting, acid leaching, impurity removal, and lithium precipitation of spodumene to produce lithium carbonate. However, the entire process employs an intermittent operation mode, with each step operating independently, requiring multiple material transfers and temporary storage. This type of traditional intermittent process has several inherent shortcomings: First, the capacity of a single unit is limited, making it difficult to meet the current demand for large-scale lithium production; second, repeated heating, cooling, and transfer of materials result in high overall energy consumption and auxiliary material consumption, leading to high production costs; third, the operating parameters of the intermittent reaction are difficult to precisely standardize, easily causing differences in purity and particle size between different batches of lithium carbonate, resulting in poor product quality stability; fourth, the fragmented design of the processes makes automation upgrades difficult, requiring significant manual intervention and resulting in high production management costs.
[0004] In addition, several other patents on improved lithium extraction from spodumene (such as CN119409211A) focus on optimizing the impurity removal process and improving the purity of lithium carbonate through membrane separation and other means. However, they have not solved the capacity and energy consumption problems caused by intermittent production, nor have they integrated the downstream lithium sulfide preparation and tail gas treatment.
[0005] In the field of lithium carbonate deep processing to produce lithium sulfide, existing processes mainly involve the reaction of lithium carbonate with elemental sulfur and a reducing agent. This reaction process continuously produces hydrogen sulfide (H2S) tail gas. For example, CN119654292A provides methods for purifying hydrogen sulfide and manufacturing lithium sulfide. Currently, the industry's approach to treating this tail gas is polarized: some small and medium-sized enterprises directly discharge hydrogen sulfide tail gas at high altitudes. Hydrogen sulfide is a highly toxic and corrosive acidic gas; direct discharge not only causes air pollution and acid rain but also corrodes factory equipment. Other companies use simple alkaline absorption and other end-of-pipe treatment methods, which only achieve harmless treatment of the tail gas but cannot recover and reuse sulfur resources, resulting in a significant waste of sulfur and a substantial reduction in raw material utilization. Furthermore, most existing lithium sulfide production processes are independent units, separate from the upstream lithium carbonate production process. These two production lines are separately laid out and managed, resulting in a lengthy overall process and further increasing the consumption of land resources and public works.
[0006] Meanwhile, modern chemical industries such as petroleum refining, coal chemical industry, and hydrorefining generate large amounts of low-concentration sulfuric acid-containing waste gas during production processes. This type of waste gas has low hydrogen sulfide content and complex composition; conventional treatment processes can only achieve emission standards, not resource recovery. Although there are technologies for hydrogen sulfide purification and recycling in the industry, most are designed for single gas sources and cannot coordinate the treatment of low-concentration sulfur-containing waste gas discharged from industrial facilities with the tail gas produced by lithium sulfide production, indicating a significant shortcoming in comprehensive resource utilization.
[0007] A comprehensive review of current technologies reveals that the three major technological segments—lithium extraction from spodumene, lithium sulfide preparation, and hydrogen sulfide treatment—are currently independent and fragmented. This is manifested in several ways: the traditional spodumene-sulfuric acid process for lithium carbonate is primarily intermittent, with bottlenecks in capacity, energy consumption, and product stability; the hydrogen sulfide tail gas from the lithium carbonate-to-lithium sulfide process lacks an efficient closed-loop recovery system, resulting in both pollution and resource waste; and industrial sulfuric acid-containing waste gas resource recovery technologies are difficult to integrate with lithium salt production processes.
[0008] The existing segmented production model suffers from low overall resource utilization, significant environmental pressure, and high comprehensive production costs, making it difficult to simultaneously meet the multiple industrial demands of large-scale production, green and low-carbon practices, resource recycling, and the coordinated treatment of multiple waste gases. Therefore, developing a combined process that organically integrates three major units—continuous production of lithium carbonate from spodumene, high-temperature sulfidation of lithium carbonate to lithium sulfide, and integrated recovery and recycling of hydrogen sulfide from multiple gas sources—has significant industrial application value. Summary of the Invention
[0009] To address the technical problems of low intermittent production capacity, high energy and material consumption, severe hydrogen sulfide tail gas pollution, and inability to recycle sulfur resources in existing technologies, this invention provides a method for the joint preparation of lithium carbonate and lithium sulfide from spodumene. This invention achieves continuous operation of the entire process from lithium extraction from spodumene, lithium carbonate sulfidation, and hydrogen sulfide recovery, constructing a closed-loop hydrogen sulfide recycling system. Simultaneously, it can synergistically treat external industrial sulfuric acid-containing waste gas, improving overall resource utilization, reducing production costs and environmental impact, and exhibiting strong process stability and excellent product quality.
[0010] To achieve the above-mentioned objectives, the present invention adopts the following technical solution:
[0011] A method for the combined preparation of lithium carbonate and lithium sulfide from spodumene includes the following steps:
[0012] S1. Continuous roasting and transformation of spodumene: Spodumene concentrate is fed into a transformation roasting rotary kiln for continuous roasting to transform α-spodumene into β-spodumene; the obtained β-spodumene is mixed with ammonium sulfate and then fed into an acidification roasting kiln for sulfation roasting to obtain lithium sulfate clinker.
[0013] S2. Continuous preparation of lithium sulfate solution: The lithium sulfate clinker obtained in step S1 is mixed with process water and leached. After solid-liquid separation, a crude lithium sulfate solution is obtained. Sodium carbonate is added to the crude lithium sulfate solution to adjust the pH value, and aluminum, calcium and magnesium impurities are precipitated and removed. After purification, the solution is evaporated and concentrated to obtain a refined lithium sulfate solution.
[0014] S3, Continuous lithium carbonization precipitation: The refined lithium sulfate solution obtained in step S2 and the sodium carbonate solution are continuously fed into the lithium precipitation reaction device to react and generate lithium carbonate slurry. The slurry is cooled, filtered, washed and dried to obtain battery-grade lithium carbonate.
[0015] S4. Continuous sulfidation reaction of lithium carbonate: The battery-grade lithium carbonate obtained in step S3, elemental sulfur, and carbon-based reducing agent are mixed to prepare a reaction precursor. The precursor is fed into a high-temperature tube furnace and reacted under an inert protective atmosphere to produce crude lithium sulfide and produce tail gas containing hydrogen sulfide.
[0016] S5. Hydrogen sulfide recycling: Collect the hydrogen sulfide-containing tail gas produced in step S4, and sequentially process it through pressure stabilization filtration, countercurrent absorption of MDEA aqueous solution, rich liquid desorption, and dehydration purification to obtain high-purity hydrogen sulfide; return the high-purity hydrogen sulfide to the reaction system of step S4 for recycling as a reducing agent and sulfur source.
[0017] Furthermore, in step S1, the continuous roasting temperature is controlled at 1070~1100℃, the sulfation roasting temperature is controlled at 240~260℃, the spodumene concentrate is continuously fed and discharged in the conversion roasting rotary kiln, the material residence time is 1.5~3h, and the conversion rate of α-spodumene to β-spodumene is not less than 98%.
[0018] Furthermore, in step S2, the leaching, purification, and evaporation concentration processes all adopt a continuous operation mode. During the leaching process, the solid-liquid mass ratio of lithium sulfate clinker to process water is 1:(3~5). The filter residue generated after impurities are precipitated is treated by countercurrent washing, and the washing liquid is returned to the leaching process for recycling.
[0019] Furthermore, in step S3, the temperature of the lithium precipitation reaction is controlled at 80~95℃, and the lithium precipitation reaction device is a continuous stirred reactor. The entire lithium precipitation process eliminates the intermittent temporary storage of materials, realizing continuous operation of feeding, reaction and discharge, and the purity of the battery-grade lithium carbonate obtained is not less than 99.5%.
[0020] Furthermore, in step S4, the carbon-based reducing agent is one or two of glucose and activated carbon, and the mass ratio of lithium carbonate, elemental sulfur, and carbon-based reducing agent is 100:(40~60):(5~15). The sulfidation reaction temperature is controlled at 600~800℃.
[0021] Furthermore, in step S4, the inert atmosphere is nitrogen, and the high-temperature tubular furnace is kept at atmospheric pressure. The entire sulfidation reaction process adopts a continuous feeding and continuous discharging mode to achieve large-scale continuous preparation of lithium sulfide.
[0022] Furthermore, in step S5, the MDEA aqueous solution is prepared by combining N-methyldiethanolamine and water, the mass fraction of the MDEA aqueous solution is 10-40%, the operating pressure of the absorption process is 0.6-0.7 MPa, the operating temperature is 30-35℃, and the theoretical number of plates of the absorption tower is set to 4-6.
[0023] Furthermore, in step S5, the rich liquid desorption process adopts a negative pressure desorption process, the desorption tower operating pressure is 0.04~0.06MPa, the tower top temperature is 75~85℃, the tower bottom temperature is 130~140℃, the theoretical number of desorption tower plates is 28~32, and the desorption tower reboiler is heated by steam with a heat load of 55~63MW.
[0024] Furthermore, in step S5, crude hydrogen sulfide is fed into a dehydration distillation column for dehydration and purification. The operating pressure of the dehydration distillation column is 0.08~0.12MPa, the theoretical number of trays is 8~12, the purity of hydrogen sulfide produced at the top of the column is not less than 99%, and part of the wastewater generated at the bottom of the column is recycled for the entire plant's process water.
[0025] Furthermore, it also includes a co-treatment step for external sulfuric acid-containing waste gas, specifically: the external sulfuric acid-containing waste gas generated in the diesel hydrorefining section is combined with the hydrogen sulfide-containing tail gas produced in step S4 and sent together to the hydrogen sulfide recovery process. After the mixed gas is uniformly recovered and purified, the resulting high-purity hydrogen sulfide is recycled to the sulfidation reaction process.
[0026] Compared with the prior art, the present invention has the following beneficial effects:
[0027] (1) This invention achieves continuous production throughout the entire process, significantly improving both capacity and quality. This invention abandons the traditional intermittent operation mode of lithium extraction from spodumene and lithium sulfide preparation. From spodumene roasting, lithium sulfate leaching and purification, lithium carbide precipitation, to the lithium carbonate sulfide reaction, the entire process is carried out continuously, eliminating the intermittent material storage stage and effectively overcoming the limitations of single-line capacity. Simultaneously, stable continuous operation eliminates batch variations, ensuring a stable purity of ≥99.5% for battery-grade lithium carbonate, uniform quality of lithium sulfide products, and significantly improved production stability.
[0028] (2) This invention constructs a closed-loop hydrogen sulfide cycle, which is green, energy-saving, and has a high resource utilization rate. A combined process of MDEA aqueous solution absorption-negative pressure desorption-distillation dehydration is used to recover hydrogen sulfide. The purified high-purity hydrogen sulfide is directly returned to the sulfidation reaction process as a reducing agent and sulfur source for recycling, achieving an internal closed loop for sulfur resources. This completely solves the problems of hydrogen sulfide tail gas pollution and sulfur resource waste in traditional processes, reduces tail gas treatment costs and raw material consumption, and aligns with the development requirements of green chemical industry and energy conservation and emission reduction.
[0029] (3) The process parameters of this invention are highly adaptable and have low operating costs. This invention optimizes the original single-point process parameters into a reasonable range, adapting to the normal operating condition fluctuations in industrial production, and has higher process tolerance. The leaching residue washing liquid and desulfurization wastewater can be reused within the plant, and the consumption of water and auxiliary materials is significantly reduced. The MDEA absorbent can be recycled and reused, with low reagent loss, and the overall production and operating costs are effectively controlled.
[0030] (4) This invention expands the application scenarios and realizes collaborative resource utilization. This invention can collaboratively treat low-concentration sulfuric acid-containing waste gas generated by industrial equipment such as diesel hydrorefining, and combine external waste gas with self-produced hydrogen sulfide-containing tail gas for unified recycling. While producing lithium-based products, it completes the resource utilization and disposal of industrial hazardous waste. One process realizes multiple values, and the process has wider versatility and market application scope. Detailed Implementation
[0031] The present invention will be further described in detail below with reference to specific embodiments, but the scope of protection of the present invention is not limited to the following embodiments.
[0032] Example 1
[0033] This embodiment provides a method for the combined preparation of lithium carbonate and lithium sulfide from spodumene, the specific steps of which are as follows:
[0034] (1) Continuous roasting and conversion of spodumene: spodumene concentrate is fed into a conversion roasting rotary kiln, the roasting temperature is controlled at 1070℃, the material is continuously fed and discharged, and the residence time is 2h, so that α-spodumene is completely converted into β-spodumene with a conversion rate ≥98%. β-spodumene is uniformly mixed with ammonium sulfate and then fed into an acidification roasting kiln, the temperature is controlled at 250℃, and sulfation roasting is carried out to obtain lithium sulfate clinker.
[0035] (2) Continuous preparation of lithium sulfate solution: Lithium sulfate clinker and process water are continuously mixed and leached at a solid-liquid mass ratio of 1:4. After leaching, crude lithium sulfate solution is obtained by continuous solid-liquid separation. Sodium carbonate is continuously added to the crude lithium sulfate solution to adjust the pH value. In the first stage, the pH of the system is adjusted to 7.8 to precipitate and remove iron and aluminum ions from the solution. In the second stage, sodium carbonate is added to adjust the pH to 11.8 to deeply remove calcium and magnesium impurities. The purified solution is sent to the evaporation and concentration unit for continuous concentration to obtain refined lithium sulfate solution. The filter residue generated by leaching is washed countercurrently, and all the washing liquid is returned to the leaching process for reuse.
[0036] (3) Continuous carbonization precipitation of lithium: Refined lithium sulfate solution and sodium carbonate solution are continuously fed into a continuously stirred reactor, the reaction temperature is controlled at 88°C, and there is no intermittent material storage in the reactor body to achieve a fully continuous reaction; the reaction generates lithium carbonate slurry, which is then cooled, filtered, washed and dried in sequence to obtain battery-grade lithium carbonate with a purity of 99.6%.
[0037] (4) Continuous sulfidation reaction of lithium carbonate: Glucose is selected as a carbon-based reducing agent and mixed according to the mass ratio of lithium carbonate: sulfur: glucose = 100: 50: 10 to prepare a reaction precursor. The precursor is continuously fed into a high-temperature tube furnace, and nitrogen is introduced into the furnace as an inert protective atmosphere to maintain normal pressure. The reaction temperature is 700℃, and the feed and discharge are continuous. The reaction produces crude lithium sulfide and produces tail gas containing hydrogen sulfide.
[0038] (5) Hydrogen sulfide recycling: The hydrogen sulfide-containing tail gas generated by the sulfidation reaction is collected, first sent to a buffer tank for pressure stabilization, and then filtered to remove solid particles and oil mist. A 30% MDEA aqueous solution is prepared as the absorbent. The absorption tower has 5 theoretical plates, an operating pressure of 0.65 MPa, and a temperature of 32°C. The MDEA aqueous solution is countercurrently contacted with the tail gas to absorb the hydrogen sulfide. The rich liquid after absorption is preheated to 90°C and then sent to the desorption tower. The desorption tower has an operating pressure of 0.05 MPa, a top temperature of 80°C, a bottom temperature of 135°C, and 30 theoretical plates. The reboiler is heated by steam with a heat load of 59 MW. The crude hydrogen sulfide obtained by desorption is sent to a dehydration distillation tower. The distillation tower has an operating pressure of 0.1 MPa and 10 theoretical plates. High-purity hydrogen sulfide with a purity of 99.2% is obtained at the top of the tower. All of this hydrogen sulfide is returned to the high-temperature tubular furnace for recycling, and part of the wastewater at the bottom of the tower is reused as process makeup water.
[0039] Example 2
[0040] This embodiment provides a method for the combined preparation of lithium carbonate and lithium sulfide from spodumene, the specific steps of which are as follows:
[0041] (1) Continuous roasting and conversion of spodumene: spodumene concentrate is fed into a rotary kiln for conversion roasting, and the roasting temperature is controlled at 1090℃. The material is continuously fed and discharged, and the residence time is 2.5h, so that α-spodumene is completely converted into β-spodumene with a conversion rate ≥98%. β-spodumene is uniformly mixed with ammonium sulfate and then fed into an acidification roasting kiln. The temperature is controlled at 245℃ for sulfation roasting to obtain lithium sulfate clinker.
[0042] (2) Continuous preparation of lithium sulfate solution: Lithium sulfate clinker and process water are continuously mixed and leached at a solid-liquid mass ratio of 1:3.5. After leaching, crude lithium sulfate solution is obtained by continuous solid-liquid separation. Sodium carbonate is continuously added to the crude lithium sulfate solution to adjust the pH value. In the first stage, the pH of the system is adjusted to 7.6 to precipitate and remove iron and aluminum ions from the solution. In the second stage, sodium carbonate is added to adjust the pH to 11.2 to deeply remove calcium and magnesium impurities. The purified solution is sent to the evaporation and concentration unit for continuous concentration to obtain refined lithium sulfate solution. The filter residue generated by leaching is washed countercurrently, and all washing liquid is returned to the leaching process for reuse.
[0043] (3) Continuous carbonization precipitation of lithium: Refined lithium sulfate solution and sodium carbonate solution are continuously fed into a continuously stirred reactor, the reaction temperature is controlled at 82°C, and there is no intermittent material storage in the reactor body to achieve a fully continuous reaction; the reaction generates lithium carbonate slurry, which is then cooled, filtered, washed and dried in sequence to obtain battery-grade lithium carbonate with a purity of 99.55%.
[0044] (4) Continuous sulfidation reaction of lithium carbonate: Activated carbon is selected as a carbon-based reducing agent. The precursor is prepared by mixing lithium carbonate: sulfur element: activated carbon in a mass ratio of 100:45:8. The precursor is continuously fed into a high-temperature tube furnace. Nitrogen gas is introduced into the furnace as an inert protective atmosphere to maintain normal pressure. The reaction temperature is 650℃. The feed and discharge are continuous. The reaction produces crude lithium sulfide and produces tail gas containing hydrogen sulfide.
[0045] (5) Hydrogen sulfide recycling: Collect the hydrogen sulfide tail gas produced by the sulfidation reaction, and at the same time introduce the sulfuric acid-containing waste gas produced by the diesel hydrorefining section (volume composition: H2S 1.20%, CO2 0.80%, CH4 1.12%, C2H6 0.23%, C3H8 0.38%, H2 96.27%). After the two gases are combined, they are first sent to the buffer tank for pressure stabilization, and then filtered to remove solid particles and oil mist. An aqueous solution of MDEA and water at a mass ratio of 2.8:7.2 was used as the absorbent. The absorber had 4 theoretical plates, an operating pressure of 0.62 MPa, and a temperature of 33°C. The MDEA aqueous solution was countercurrently contacted with the tail gas to absorb hydrogen sulfide. The rich solution after absorption was preheated to 90°C and then sent to a desorption tower. The desorption tower operated at a pressure of 0.045 MPa, with a top temperature of 78°C and a bottom temperature of 132°C, and had 29 theoretical plates. The reboiler was heated by steam with a heat load of 57 MW. The crude hydrogen sulfide obtained from desorption was sent to a dehydration distillation tower. The distillation tower operated at a pressure of 0.09 MPa and had 9 theoretical plates. High-purity hydrogen sulfide with a purity of 99.1% was obtained at the top of the tower. All of this hydrogen sulfide was returned to the high-temperature tubular furnace for recycling, and part of the wastewater from the bottom of the tower was reused as process makeup water.
[0046] Example 3
[0047] This embodiment provides a method for the combined preparation of lithium carbonate and lithium sulfide from spodumene, the specific steps of which are as follows:
[0048] (1) Continuous roasting and conversion of spodumene: spodumene concentrate is fed into a rotary kiln for conversion roasting, and the roasting temperature is controlled at 1100℃. The material is continuously fed and discharged, and the residence time is 1.8h, so that α-spodumene is completely converted into β-spodumene with a conversion rate ≥98%. β-spodumene is uniformly mixed with ammonium sulfate and then fed into an acidification roasting kiln. The temperature is controlled at 255℃ for sulfation roasting to obtain lithium sulfate clinker.
[0049] (2) Continuous preparation of lithium sulfate solution: Lithium sulfate clinker and process water are continuously mixed and leached at a solid-liquid mass ratio of 1:4.8. After leaching, crude lithium sulfate solution is obtained by continuous solid-liquid separation. Sodium carbonate is continuously added to the crude lithium sulfate solution to adjust the pH value. In the first stage, the pH of the system is adjusted to 7.9 to precipitate and remove iron and aluminum ions from the solution. In the second stage, sodium carbonate is added to adjust the pH to 12.2 to deeply remove calcium and magnesium impurities. The purified solution is sent to the evaporation and concentration unit for continuous concentration to obtain refined lithium sulfate solution. The filter residue generated by leaching is washed countercurrently, and all washing liquid is returned to the leaching process for reuse.
[0050] (3) Continuous carbonization precipitation of lithium: Refined lithium sulfate solution and sodium carbonate solution are continuously fed into a continuously stirred reactor, the reaction temperature is controlled at 92°C, and there is no intermittent material storage in the reactor body to achieve a fully continuous reaction; the reaction generates lithium carbonate slurry, which is then cooled, filtered, washed and dried in sequence to obtain battery-grade lithium carbonate with a purity of 99.62%.
[0051] (4) Continuous sulfidation reaction of lithium carbonate: Glucose and activated carbon were selected as carbon-based reducing agents and mixed according to the mass ratio of lithium carbonate: sulfur: composite reducing agent = 100:58:12 to prepare a reaction precursor. The precursor was continuously fed into a high-temperature tube furnace, and nitrogen was introduced into the furnace as an inert protective atmosphere to maintain normal pressure. The reaction temperature was 780℃, and the feed and discharge were continuous. The reaction produced crude lithium sulfide and produced tail gas containing hydrogen sulfide.
[0052] (5) Hydrogen sulfide recycling: The hydrogen sulfide-containing tail gas generated by the sulfidation reaction is collected, first sent to a buffer tank for pressure stabilization, and then filtered to remove solid particles and oil mist. An aqueous solution of MDEA and water at a mass ratio of 3.2:6.8 is prepared as the absorbent. The absorption tower has 6 theoretical plates, an operating pressure of 0.68 MPa, and a temperature of 34°C. The MDEA aqueous solution is countercurrently contacted with the tail gas to absorb hydrogen sulfide. The rich liquid after absorption is preheated to 90°C and then sent to the desorption tower. The desorption tower has an operating pressure of 0.055 MPa, a top temperature of 82°C, a bottom temperature of 138°C, and 31 theoretical plates. The reboiler is heated by steam with a heat load of 61 MW. The crude hydrogen sulfide obtained by desorption is sent to a dehydration distillation tower. The distillation tower has an operating pressure of 0.11 MPa and 11 theoretical plates. High-purity hydrogen sulfide with a purity of 99.3% is obtained at the top of the tower. All of this hydrogen sulfide is returned to the high-temperature tubular furnace for recycling, and part of the wastewater at the bottom of the tower is reused as process makeup water.
[0053] Example 4
[0054] This embodiment provides a method for the combined preparation of lithium carbonate and lithium sulfide from spodumene, the specific steps of which are as follows:
[0055] (1) Continuous roasting and conversion of spodumene: spodumene concentrate is fed into a rotary kiln for conversion roasting, and the roasting temperature is controlled at 1070℃. The material is continuously fed and discharged, and the residence time is 1.5h, so that α-spodumene is completely converted into β-spodumene with a conversion rate ≥98%. β-spodumene is uniformly mixed with ammonium sulfate and then fed into an acidification roasting kiln. The temperature is controlled at 240℃ for sulfation roasting to obtain lithium sulfate clinker.
[0056] (2) Continuous preparation of lithium sulfate solution: Lithium sulfate clinker and process water are continuously mixed and leached at a solid-liquid mass ratio of 1:5. After leaching, crude lithium sulfate solution is obtained by continuous solid-liquid separation. Sodium carbonate is continuously added to the crude lithium sulfate solution to adjust the pH value. In the first stage, the pH of the system is adjusted to 7.5 to precipitate and remove iron and aluminum ions from the solution. In the second stage, sodium carbonate is added to adjust the pH to 12.5 to deeply remove calcium and magnesium impurities. The purified solution is sent to the evaporation and concentration unit for continuous concentration to obtain refined lithium sulfate solution. The filter residue generated by leaching is washed countercurrently, and all the washing liquid is returned to the leaching process for reuse.
[0057] (3) Continuous carbonization precipitation of lithium: Refined lithium sulfate solution and sodium carbonate solution are continuously fed into a continuous stirred reactor, the reaction temperature is controlled at 80°C, and there is no intermittent material storage in the reactor body to achieve a fully continuous reaction; the reaction generates lithium carbonate slurry, which is then cooled, filtered, washed and dried in sequence to obtain battery-grade lithium carbonate with a purity of 99.51%.
[0058] (4) Continuous sulfidation reaction of lithium carbonate: Glucose is selected as a carbon-based reducing agent and mixed according to the mass ratio of lithium carbonate: sulfur: glucose = 100:40:5 to prepare a reaction precursor. The precursor is continuously fed into a high-temperature tube furnace, and nitrogen is introduced into the furnace as an inert protective atmosphere to maintain normal pressure. The reaction temperature is 600℃, and the feed and discharge are continuous. The reaction produces crude lithium sulfide and produces tail gas containing hydrogen sulfide.
[0059] (5) Hydrogen sulfide recycling: The hydrogen sulfide-containing tail gas generated by the sulfidation reaction is collected, first sent to a buffer tank for pressure stabilization, and then filtered to remove solid particles and oil mist. An aqueous solution of MDEA and water at a mass ratio of 2.5:7.5 is prepared as the absorbent. The absorption tower has 6 theoretical plates, an operating pressure of 0.7 MPa, and a temperature of 35°C. The MDEA aqueous solution is countercurrently contacted with the tail gas to absorb hydrogen sulfide. The rich liquid after absorption is preheated to 90°C and then sent to the desorption tower. The desorption tower has an operating pressure of 0.06 MPa, a top temperature of 85°C, a bottom temperature of 140°C, and 32 theoretical plates. The reboiler is heated by steam with a heat load of 63 MW. The crude hydrogen sulfide obtained by desorption is sent to a dehydration distillation tower. The distillation tower has an operating pressure of 0.12 MPa and 12 theoretical plates. High-purity hydrogen sulfide with a purity of 99.0% is obtained at the top of the tower. All of this hydrogen sulfide is returned to the high-temperature tubular furnace for recycling, and part of the wastewater at the bottom of the tower is reused as process makeup water.
[0060] Example 5
[0061] This embodiment provides a method for the combined preparation of lithium carbonate and lithium sulfide from spodumene, the specific steps of which are as follows:
[0062] (1) Continuous roasting and conversion of spodumene: spodumene concentrate is fed into a rotary kiln for conversion roasting, and the roasting temperature is controlled at 1080℃. The material is continuously fed and discharged, and the residence time is 2.2h, so that α-spodumene is completely converted into β-spodumene with a conversion rate ≥98%. β-spodumene is uniformly mixed with ammonium sulfate and then fed into an acidification roasting kiln. The temperature is controlled at 250℃ for sulfation roasting to obtain lithium sulfate clinker.
[0063] (2) Continuous preparation of lithium sulfate solution: Lithium sulfate clinker and process water are continuously mixed and leached at a solid-liquid mass ratio of 1:4.2. After leaching, crude lithium sulfate solution is obtained by continuous solid-liquid separation. Sodium carbonate is continuously added to the crude lithium sulfate solution to adjust the pH value. In the first stage, the pH of the system is adjusted to 7.7 to precipitate and remove iron and aluminum ions from the solution. In the second stage, sodium carbonate is added to adjust the pH to 11.5 to deeply remove calcium and magnesium impurities. The purified solution is sent to the evaporation and concentration unit for continuous concentration to obtain refined lithium sulfate solution. The filter residue generated by leaching is washed countercurrently, and all washing liquid is returned to the leaching process for reuse.
[0064] (3) Continuous carbonization precipitation of lithium: Refined lithium sulfate solution and sodium carbonate solution are continuously fed into a continuously stirred reactor, the reaction temperature is controlled at 85°C, and there is no intermittent material storage in the reactor body to achieve a fully continuous reaction; the reaction generates lithium carbonate slurry, which is then cooled, filtered, washed and dried in sequence to obtain battery-grade lithium carbonate with a purity of 99.58%.
[0065] (4) Continuous sulfidation reaction of lithium carbonate: Activated carbon is selected as a carbon-based reducing agent. The precursor is prepared by mixing lithium carbonate: sulfur element: activated carbon in a mass ratio of 100:55:13. The precursor is continuously fed into a high-temperature tube furnace. Nitrogen gas is introduced into the furnace as an inert protective atmosphere to maintain normal pressure. The reaction temperature is 750℃. The feed and discharge are continuous. The reaction produces crude lithium sulfide and produces tail gas containing hydrogen sulfide.
[0066] (5) Hydrogen sulfide recycling: Collect the hydrogen sulfide tail gas produced by the sulfidation reaction, and at the same time introduce the sulfuric acid-containing waste gas produced by the diesel hydrorefining section (volume composition: H2S 1.20%, CO2 0.80%, CH4 1.12%, C2H6 0.23%, C3H8 0.38%, H2 96.27%). After the two gases are combined, they are first sent to the buffer tank for pressure stabilization, and then filtered to remove solid particles and oil mist. An aqueous solution of MDEA and water at a mass ratio of 3.0:7.0 was used as the absorbent. The absorber had 5 theoretical plates, an operating pressure of 0.65 MPa, and a temperature of 32°C. The MDEA aqueous solution was countercurrently contacted with the tail gas to absorb hydrogen sulfide. The rich solution after absorption was preheated to 90°C and then sent to a desorption tower. The desorption tower operated at 0.05 MPa, with a top temperature of 80°C and a bottom temperature of 135°C, and had 30 theoretical plates. The reboiler was heated by steam with a heat load of 59 MW. The crude hydrogen sulfide obtained from desorption was sent to a dehydration distillation tower. The distillation tower operated at 0.1 MPa and had 10 theoretical plates. High-purity hydrogen sulfide with a purity of 99.2% was obtained at the top of the tower. All of this hydrogen sulfide was returned to the high-temperature tubular furnace for recycling, and part of the wastewater from the bottom of the tower was reused as process makeup water.
[0067] The principle is explained as follows:
[0068] The principle of spodumene roasting and conversion: Natural α-spodumene has a dense structure and low chemical activity. At a high temperature of 1070~1100℃, it undergoes a crystal transformation to generate β-spodumene, which has a loose structure and high reactivity. β-spodumene reacts with ammonium sulfate at 240~260℃ to undergo a sulfation reaction, and lithium element is converted into water-soluble lithium sulfate to obtain lithium sulfate clinker.
[0069] Leaching, purification and lithium precipitation principle: After leaching lithium sulfate clinker in water, soluble lithium sulfate enters the liquid phase; sodium carbonate is added to adjust the pH, so that impurity ions such as aluminum, calcium, and magnesium ions are removed by forming hydroxide / carbonate precipitates. The refined lithium sulfate solution undergoes a metathesis reaction with sodium carbonate at 80~95℃ to generate solid lithium carbonate precipitate, which is then post-processed to obtain high-purity battery-grade lithium carbonate.
[0070] The principle of sulfidation reaction: Under the inert atmosphere of nitrogen, at a high temperature of 600~800℃ and with the action of a carbon-based reducing agent, lithium carbonate reacts with elemental sulfur to form lithium sulfide. The reaction process is accompanied by the generation of hydrogen sulfide gas.
[0071] Hydrogen sulfide recovery and recycling principle: Utilizing the selective absorption characteristics of MDEA aqueous solution for hydrogen sulfide, hydrogen sulfide in the tail gas is absorbed under normal temperature and medium pressure conditions. The rich solution is then desorbed by negative pressure heating to release crude hydrogen sulfide. High-purity hydrogen sulfide is then obtained through distillation and dehydration, and reintroduced into the sulfidation reaction unit as a sulfur source and reducing agent, achieving a closed loop of sulfur resources. Simultaneously, this process can co-treat external sulfuric acid-containing waste gas, further improving the comprehensive utilization rate of resources.
Claims
1. A method for the combined production of lithium carbonate and lithium sulfide from spodumene, characterized in that, Includes the following steps: S1. Continuous roasting and transformation of spodumene: Spodumene concentrate is fed into a transformation roasting rotary kiln for continuous roasting to transform α-spodumene into β-spodumene. The β-spodumene is then mixed with ammonium sulfate and fed into an acidification roasting kiln for sulfation roasting to obtain lithium sulfate clinker. S2. Continuous preparation of lithium sulfate solution: The lithium sulfate clinker obtained in step S1 is mixed with process water and leached. After solid-liquid separation, a crude lithium sulfate solution is obtained. Sodium carbonate is added to the crude lithium sulfate solution to adjust the pH value, and aluminum, calcium and magnesium impurities are precipitated and removed. After purification, the solution is evaporated and concentrated to obtain a refined lithium sulfate solution. S3, Continuous lithium carbonization precipitation: The refined lithium sulfate solution obtained in step S2 and the sodium carbonate solution are continuously fed into the lithium precipitation reaction device to react and generate lithium carbonate slurry. The slurry is cooled, filtered, washed and dried to obtain battery-grade lithium carbonate. S4. Continuous sulfidation reaction of lithium carbonate: The battery-grade lithium carbonate obtained in step S3, elemental sulfur, and carbon-based reducing agent are mixed to prepare a reaction precursor. The precursor is fed into a high-temperature tube furnace and reacted under an inert protective atmosphere to produce crude lithium sulfide and produce tail gas containing hydrogen sulfide. S5. Hydrogen sulfide recycling: Collect the hydrogen sulfide-containing tail gas produced in step S4, and sequentially process it through pressure stabilization filtration, countercurrent absorption of MDEA aqueous solution, rich liquid desorption, and dehydration purification to obtain high-purity hydrogen sulfide. Return the high-purity hydrogen sulfide to the reaction system of step S4 and use it as a reducing agent and sulfur source for recycling.
2. The process of claim 1, wherein, In step S1, the continuous roasting temperature is controlled at 1070~1100℃, the sulfation roasting temperature is controlled at 240~260℃, the spodumene concentrate is continuously fed and discharged in the conversion roasting rotary kiln, the material residence time is 1.5~3h, and the conversion rate of α-spodumene to β-spodumene is not less than 98%.
3. The process of claim 1, wherein, In step S2, the leaching, purification, and evaporation concentration processes all adopt a continuous operation mode. During the leaching process, the solid-liquid mass ratio of lithium sulfate clinker to process water is 1:(3~5). The filter residue generated after impurities are precipitated is treated by countercurrent washing, and the washing liquid is returned to the leaching process for recycling.
4. The method of claim 1, wherein, In step S3, the temperature of the lithium precipitation reaction is controlled at 80~95℃. The lithium precipitation reaction device is a continuous stirred reactor. The entire lithium precipitation process eliminates the intermittent temporary storage of materials, realizing continuous operation of feeding, reaction and discharge. The purity of the battery-grade lithium carbonate obtained is not less than 99.5%.
5. The method of claim 1, wherein, In step S4, the carbon-based reducing agent is one or two of glucose and activated carbon used in combination, and the mass ratio of lithium carbonate, elemental sulfur and carbon-based reducing agent is 100:(40~60):(5~15); the sulfidation reaction temperature is controlled at 600~800℃.
6. The method according to claim 1, characterized in that, In step S4, the inert atmosphere is nitrogen, and the high-temperature tubular furnace is kept at atmospheric pressure. The entire sulfidation reaction process adopts a continuous feeding and continuous discharging mode to realize the large-scale continuous preparation of lithium sulfide.
7. The method according to claim 1, characterized in that, In step S5, the MDEA aqueous solution is a mixture of N-methyldiethanolamine and water, with a mass fraction of 10-40%. The operating pressure of the absorption process is 0.6-0.7 MPa, the operating temperature is 30-35℃, and the theoretical number of plates in the absorption tower is set to 4-6.
8. The method according to claim 1, characterized in that, In step S5, the rich liquid desorption process adopts a negative pressure desorption process. The desorption tower operating pressure is 0.04~0.06MPa, the tower top temperature is 75~85℃, the tower bottom temperature is 130~140℃, the theoretical number of tower plates is 28~32, and the desorption tower reboiler is heated by steam with a heat load of 55~63MW.
9. The method according to claim 1, characterized in that, In step S5, crude hydrogen sulfide is fed into a dehydration distillation column for dehydration and purification. The operating pressure of the dehydration distillation column is 0.08~0.12MPa, the theoretical number of trays is 8~12, the purity of hydrogen sulfide produced at the top of the column is not less than 99%, and part of the wastewater generated at the bottom of the column is recycled for the entire plant's process water.
10. The method according to claim 1, characterized in that, It also includes a co-treatment step for external sulfuric acid-containing waste gas, specifically: the external sulfuric acid-containing waste gas generated in the diesel hydrorefining section is combined with the hydrogen sulfide-containing tail gas produced in step S4 and sent together to the hydrogen sulfide recovery process. After unified recovery and purification, the high-purity hydrogen sulfide obtained is recycled to the sulfidation reaction process.
Citation Information
Patent Citations
A process for producing lithium carbonate from spodumene concentrate using the sulfuric acid process
CN103950956B
Method for extracting lithium carbonate from spodumene in pegmatite
CN119409211A