A method, electrochemical reaction device, and application of self-supporting molybdenum-copper electrode for electroreduction of nitrate nitrogen and simultaneous recovery of ammonia.
By utilizing the in-situ adsorption and catalysis of the porous layered structure of the self-supporting molybdenum-copper electrode, the problem of failure to simultaneously recover nitrate nitrogen after ammonia production in existing technologies has been solved, achieving efficient nitrate nitrogen removal and ammonia recovery, simplifying the treatment process, and improving resource utilization efficiency.
Patent Information
- Application Number
- CN202610964600.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-06-30
- Publication Date
- 2026-11-17
AI Technical Summary
Existing electrochemical reduction of nitrate nitrogen to produce ammonia technology fails to effectively separate and recover ammonia simultaneously, leading to secondary water pollution, increased subsequent treatment costs and complexity, and reduced resource utilization efficiency.
A self-supporting molybdenum-copper electrode is used to adsorb and store ammonia in situ through a porous layered structure formed by interwoven molybdenum trioxide nanoribbons. Combined with the catalytic effect of cuprous oxide, this achieves efficient reduction of nitrate nitrogen and simultaneous recovery of ammonia.
It achieves efficient removal of nitrate nitrogen, with a total inorganic nitrogen removal rate of 97.5% and an ammonia recovery rate of up to 97.3%, simplifying the treatment process and improving resource utilization efficiency.
Smart Images

Figure CN123105804A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of nitrate wastewater treatment and ammonia recovery technology, specifically relating to a method for electroreducing nitrate nitrogen and simultaneously recovering ammonia using a self-supporting molybdenum-copper electrode, an electrochemical reaction device, and its application. Background Technology
[0002] The rapid development of industry and agriculture has led to increasingly serious pollution of water bodies by nitrates, nitrites, and other nitrogenous substances, threatening the ecological environment and human health. Meanwhile, ammonia (NH3), as an important chemical raw material and clean energy carrier, suffers from high energy consumption and high carbon emissions in its traditional Haber process. Therefore, developing green and efficient technologies for the resource utilization of nitrogenous substances, converting them from wastewater into high-value ammonia, has significant environmental and economic benefits.
[0003] Electrochemical reduction technology is considered one of the most promising approaches for converting nitrate to ammonia due to its advantages such as requiring no external reducing agent, mild reaction conditions, and direct electronic control of the reaction pathway. In recent years, researchers have focused on developing efficient and highly selective non-precious metal catalytic electrodes for the electrochemical reduction of nitrate to ammonia. For example, existing technologies have reported the use of bimetallic or metal phosphide self-supporting electrodes. These electrodes, by modulating the electronic synergistic effect between metals or the doping of non-metallic elements, have significantly improved the catalytic activity and selectivity of nitrate reduction to ammonia, achieving good ammonia production performance on a laboratory scale.
[0004] However, analysis revealed a common, unresolved technical flaw in the existing electrochemical reduction of nitrate to ammonia: all studies focused solely on improving nitrate reduction efficiency and ammonia production selectivity, completely neglecting the simultaneous separation and recovery of the reaction product—ammonia. Specifically, in these technologies, the ammonia produced by electroreduction is directly released and dissolved in the treated water, leading to the following problems: First, it causes secondary pollution of water bodies. Ammonia itself is a common water pollutant, and excessive ammonia nitrogen discharge leads to eutrophication, increasing the burden on subsequent water treatment. Converting nitrate nitrogen to ammonia without removing it from the water does not truly achieve complete removal of nitrogen pollutants. Second, it requires additional high-cost post-treatment recovery units. To recover dissolved ammonia to obtain valuable ammonia products, additional unit operations such as stripping, gas membrane separation, capacitive deionization, or adsorption must be added. These post-treatment processes not only increase equipment investment and operating energy consumption but also lengthen the process flow, making the originally simple electrochemical treatment system complex and inefficient, losing the advantages of integrated treatment. Third, it reduces resource utilization efficiency. Ammonia exists in large quantities of water in the form of a dilute solution, making it difficult to utilize directly, and its potential economic value cannot be effectively recovered. At the same time, the accumulation of products at the reaction interface may inhibit reaction kinetics and affect the long-term operational stability of the electrodes.
[0005] Therefore, while existing electrochemical reduction technologies for ammonia production have made progress in achieving the half-stage goal of ammonia production, they have failed to solve the problem of how to simultaneously, efficiently, and cost-effectively separate and recover the produced ammonia from the water body—the entire process of resource utilization. This significantly reduces their practical application value and makes it difficult to meet the dual demands of advanced wastewater treatment and nitrogen resource recycling. Summary of the Invention
[0006] Aiming to solve the technical problem of how to provide a method for in-situ, synchronously and efficiently recovering the produced ammonia while electrochemically reducing nitrate nitrogen to ammonia, thereby achieving the integrated recovery of nitrate nitrogen and ammonia resources in water, this invention provides a method for electroreducing nitrate nitrogen and simultaneously recovering ammonia using a self-supporting molybdenum-copper electrode. An electrochemical reaction device is used, with a self-supporting molybdenum-copper electrode as the cathode, to electrochemically reduce wastewater containing nitrate nitrogen. While reducing nitrate nitrogen to ammonia, the ammonia is adsorbed and stored in-situ through the self-supporting molybdenum-copper electrode. The self-supporting molybdenum-copper electrode includes a conductive substrate and a molybdenum-copper composite layer loaded on the conductive substrate. The molybdenum-copper composite layer contains molybdenum trioxide and cuprous oxide. The self-supporting molybdenum-copper electrode exhibits a porous layered structure formed by interwoven molybdenum trioxide nanoribbons. The cuprous oxide is distributed in particulate form between the layers and / or on the surface of the molybdenum trioxide.
[0007] Furthermore, the nitrate-containing wastewater is at least one of surface water, groundwater, municipal wastewater, or photovoltaic wastewater; The nitrate nitrogen is derived from nitrate and / or nitrite; the concentration of nitrate nitrogen in the nitrate nitrogen-containing wastewater is 10~300 mg / L; The nitrate-containing wastewater also contains coexisting cations, including at least one of sodium, potassium, calcium, or magnesium ions.
[0008] Furthermore, the method for preparing the self-supporting molybdenum-copper electrode includes: Electrodeposition is performed by immersing a conductive substrate in an electrodeposition solution containing copper ions and molybdate ions to form a molybdenum-copper precursor in situ on the surface of the conductive substrate, thus obtaining the precursor electrode. The precursor electrode is heat-treated to obtain the self-supporting molybdenum-copper electrode.
[0009] Furthermore, the mass ratio of copper to molybdenum in the electrodeposition solution is 1:50~250; the concentration of copper in the electrodeposition solution is 28~140 mg / L.
[0010] Furthermore, the current density during the electrodeposition process is 1~15 mA / cm². 2 The deposition time is 5~30 min; The heat treatment temperature is 300~400℃, the heating rate is 2~10℃ / min, and the holding time is 60~180min.
[0011] Furthermore, the electrochemical reduction treatment is carried out under constant voltage or constant current conditions; wherein, under constant voltage conditions, the voltage is 2~8 V, and under constant current conditions, the current density is 0.2~0.8 mA / cm². 2 The electrochemical reduction treatment lasts for 3 to 10 hours.
[0012] Furthermore, the electrochemical reaction device includes a cathode chamber and an anode chamber, which are separated by an ion exchange membrane; the self-supporting molybdenum-copper electrode is disposed in the cathode chamber, and the counter electrode is disposed in the anode chamber; the device also includes components for fixing and sealing the cathode chamber, the anode chamber, and the ion exchange membrane.
[0013] Furthermore, the cathode chamber and the anode chamber are provided with wastewater inlets and wastewater outlets, and the wastewater inlets and wastewater outlets are offset in the vertical direction.
[0014] The present invention provides an electrochemical reaction device for electrochemical reduction of nitrate nitrogen and simultaneous recovery of ammonia. The device includes a cathode chamber, an anode chamber, and an ion exchange membrane disposed between the cathode chamber and the anode chamber. The self-supporting molybdenum-copper electrode is disposed in the cathode chamber, and a counter electrode is disposed in the anode chamber.
[0015] The present invention provides an application of the electrochemical reaction device described above in ammonia recovery, comprising: using the electrochemical reaction device to treat wastewater containing ammonia nitrogen; wherein the ammonia nitrogen concentration in the wastewater is 10~300 mg / L, the operating voltage is 1~5 V, and the reaction time is 2~8 h.
[0016] Compared with the prior art, the method for electroreducing nitrate nitrogen and simultaneously recovering ammonia using a self-supporting molybdenum-copper electrode provided by the present invention has the following beneficial effects: The self-supporting molybdenum-copper electrode used in this invention has a cuprous oxide (Cu₂O) component that undergoes a copper valence state cycle (Cu₂O). + / Cu 2+ This method efficiently catalyzes the reduction of nitrate nitrogen to ammonia. Experimental data (see Examples 2 and 3) show that, under constant voltage of 5V and reaction time of 6h, the method of this invention achieves a nitrate removal rate of 77.9% and a nitrite removal rate of 66.1%; when treating actual municipal wastewater (Example 4), the total inorganic nitrogen removal rate is as high as 97.5%.
[0017] This invention achieves in-situ capture and simultaneous storage of ammonia produced by electrochemical reduction. This effect is achieved through strong hydrogen bonding between the molybdenum trioxide (MoO3) component in the electrode and ammonia molecules. Experimental data (see Examples 2-4) show that the method of this invention can achieve highly efficient recovery of ammonia produced by electrochemical reduction: the ammonia recovery rate reaches 89.2% when treating nitrate wastewater, as high as 95.8% when treating nitrite wastewater, and 97.3% when treating actual municipal wastewater. Furthermore, in the experiment of treating ammonia nitrogen wastewater alone (Example 5), the ammonia storage capacity of the electrode of this invention reached as high as 358.8 mg / g.
[0018] Another advantage of this invention is that the electrode forms a positive synergistic effect between the in-situ storage behavior of ammonia and the catalytic reaction, further improving the overall processing performance.
[0019] First, the reaction equilibrium shifts to the right. The in-situ removal of ammonia from the electrode surface continuously reduces the product concentration at the reaction interface (electrode / solution interface), breaking the reaction equilibrium limitation caused by product accumulation in traditional electroreduction processes.
[0020] Secondly, the in-situ removal of ammonia effectively suppresses the hydrogen evolution side reaction. In traditional electroreduction systems, the accumulation of ammonia on the electrode surface occupies active sites, inducing proton reduction to hydrogen and reducing the Faraday efficiency of the target product, ammonia. In this invention, ammonia is promptly adsorbed onto molybdenum trioxide sites, releasing the catalytically active sites of cuprous oxide, allowing electrons to be used more efficiently for nitrate reduction. Attached Figure Description
[0021] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on the structures shown in these drawings without creative effort.
[0022] Figure 1 This is a schematic diagram of the electrochemical reaction device in Embodiment 1 of the present invention; wherein, 1 is an plexiglass pad, 2 is a silicone pad, 3 is a self-supporting molybdenum-copper electrode, 4 is a cation exchange membrane, 5 is a silicone gasket, 6 is an anion exchange membrane, 7 is a type-stable electrode, 8 is a silicone pad, and 9 is plexiglass.
[0023] Figure 2 This is a scanning electron microscope image of the self-supporting molybdenum-copper electrode (sample 1) prepared in Example 1 of the present invention; Figure 3 The X-ray diffraction pattern of the self-supporting molybdenum-copper electrode (sample 1) prepared in Example 1 of the present invention; Figure 4 This is a diagram illustrating the effect of electrochemical reduction of nitrate and simultaneous recovery of ammonia in Example 2 of the present invention. Figure 5 This is a diagram illustrating the effect of electrochemical reduction of nitrite and simultaneous recovery of ammonia in Example 3 of the present invention. Figure 6 This is a graph showing the effect of total inorganic nitrogen removal rate and ammonia recovery rate when treating municipal wastewater in Example 4 of the present invention; Figure 7 This is a diagram illustrating the effect of electrochemical separate storage and recovery of ammonia in Example 5 of the present invention. Detailed Implementation
[0024] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only a part of the embodiments of the present invention, and not all of them. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0025] Furthermore, the technical solutions of the various embodiments of the present invention can be combined with each other, but only if they are based on the ability of those skilled in the art to implement them. When the combination of technical solutions is contradictory or cannot be implemented, it should be considered that such combination of technical solutions does not exist and is not within the scope of protection claimed by the present invention.
[0026] When numerical ranges are given in the embodiments, it should be understood that, unless otherwise stated in the present invention, both endpoints of each numerical range and any value between the two endpoints may be selected. Unless otherwise defined, all technical and scientific terms used in this invention, as well as the prior art known to those skilled in the art and the description of the invention, may be implemented using any prior art methods, devices, and materials similar to or equivalent to the methods, devices, and materials in the embodiments of the present invention.
[0027] This invention provides a method for electroreducing nitrate nitrogen and simultaneously recovering ammonia using a self-supporting molybdenum-copper electrode. The method employs an electrochemical reaction device with a self-supporting molybdenum-copper electrode as the cathode to electrochemically reduce nitrate nitrogen-containing wastewater. While reducing nitrate nitrogen to ammonia, the ammonia is adsorbed and stored in situ through the self-supporting molybdenum-copper electrode. The self-supporting molybdenum-copper electrode includes a conductive substrate and a molybdenum-copper composite layer loaded on the conductive substrate. The molybdenum-copper composite layer contains molybdenum trioxide and cuprous oxide, and the self-supporting molybdenum-copper electrode exhibits a porous layered structure formed by interwoven nanoribbons.
[0028] In some embodiments, the nitrate-containing wastewater is at least one of surface water, groundwater, municipal wastewater, or photovoltaic wastewater; The nitrate nitrogen is derived from nitrate and / or nitrite; the concentration of nitrate nitrogen in the nitrate nitrogen-containing wastewater is 10~300 mg / L; The nitrate-containing wastewater also contains coexisting cations, including at least one of sodium, potassium, calcium, or magnesium ions.
[0029] In this invention, the method for preparing the self-supporting molybdenum-copper electrode includes: S1. The conductive substrate is immersed in an electrodeposition solution containing copper ions and molybdate ions to perform electrodeposition, thereby forming a molybdenum-copper precursor in situ on the surface of the conductive substrate, thus obtaining the precursor electrode.
[0030] In some more specific embodiments, the mass ratio of copper to molybdenum in the electrodeposition solution is 1:50~250; and the concentration of copper in the electrodeposition solution is 28~140 mg / L.
[0031] For example, the mass ratio of copper to molybdenum in the electrodeposition solution can be 1:50, 1:100, 1:150, 1:200, or 1:250.
[0032] For example, the concentration of copper in the electrodeposition solution can be 20 mg / L or 40 mg / L or 50 mg / L or 60 mg / L or 70 mg / L or 80 mg / L or 90 mg / L or 100 mg / L or 110 mg / L or 120 mg / L or 130 mg / L or 140 mg / L, as well as any value between such a minimum and maximum value, or a range consisting of any two values.
[0033] In some more specific embodiments, the current density during the electrodeposition process is 1~15 mA / cm². 2 The deposition time is 5 to 30 minutes.
[0034] For example, the current density during the electrodeposition process can be 1 mA / cm². 2 2 mA / cm 2 3 mA / cm 2 4mA / cm 2 5 mA / cm 2 6 mA / cm 2 7 mA / cm 2 8 mA / cm 2 9 mA / cm 2 10 mA / cm 2 12 mA / cm 2 15 mA / cm 2And the range of every value between the minimum and maximum values, or any two values.
[0035] In some embodiments, the conductive substrate is a metal-based three-dimensional porous material, including but not limited to one or more of the following: nickel foam, copper foam, cobalt foam, iron foam, nickel mesh, copper mesh, nickel sheet, copper sheet, nickel foil, and copper foil. Preferably, the conductive substrate undergoes a cleaning treatment before use to remove surface impurities and oxide layers. The cleaning treatment includes: sequentially ultrasonically washing the conductive substrate with acetone, dilute hydrochloric acid, and deionized water for 10-30 minutes each, followed by drying in a vacuum drying oven.
[0036] In some embodiments, the electrodeposition solution comprises a copper salt, a molybdate, and a solvent, wherein the copper ions originate from the copper salt and the molybdate ions originate from the molybdate.
[0037] For example, the copper salt is selected from one or more of copper sulfate, copper chloride, and copper nitrate; the molybdate is selected from one or more of ammonium molybdate, ammonium heptamolybdate, sodium molybdate, and potassium molybdate; and the solvent can be water.
[0038] S2. The precursor electrode is heat-treated to obtain the self-supporting molybdenum-copper electrode.
[0039] In some more specific embodiments, the heat treatment temperature is 300~400℃, the heating rate is 2~10℃ / min, and the holding time is 60~180 min.
[0040] For example, the heat treatment temperature can be 300°C, 320°C, 330°C, 350°C, 370°C, 380°C, 400°C, or any value between such a minimum and maximum, or a range of any two such values. Preferably, the heat treatment temperature is 330~370°C.
[0041] It should be noted that in this invention, the self-supporting molybdenum-copper electrode serves as the cathode, and the electrochemical reaction can be carried out under constant voltage or constant current conditions.
[0042] When used for the electrochemical reduction of nitrate nitrogen and simultaneous recovery of ammonia (i.e., when nitrate nitrogen and / or nitrite are present in the wastewater), a higher voltage is required to drive the multi-electron reaction that reduces nitrate nitrogen to ammonia. Depending on the wastewater quality and reaction conditions, the cell voltage of the electrochemical reactor can be set to 2–8 V; or, the current density can be set to 0.2–0.8 mA / cm². 2 .
[0043] For example, the cell voltage for the electrochemical reduction reaction can be 2 V, 3 V, 4 V, 5 V, 6 V, 7 V, 8 V, or any value between such a minimum and maximum value, or a range of any two values. Preferably, the cell voltage is 4 to 6 V.
[0044] The current density of the electrochemical reduction reaction can be 0.2 mA / cm². 2 0.3 mA / cm 2 0.4 mA / cm 2 0.5mA / cm 2 0.6 mA / cm 2 0.7 mA / cm 2 0.8 mA / cm 2 And the range between this minimum and maximum value, or any two values. Preferably, the current density is 0.4~0.6 mA / cm². 2 .
[0045] When used for the separate storage and recovery of ammonia (i.e., when the nitrogen in the wastewater is mainly in the form of ammonia nitrogen, and no reduction reaction is required), only a relatively low voltage is needed to achieve effective ammonia capture. The cell voltage of the electrochemical reaction device can be set to 1~5 V. The method of this invention can also be directly applied to the treatment of ammonia nitrogen wastewater and the recovery of ammonia resources, and has a wide range of applications.
[0046] In some embodiments, the ammonia nitrogen concentration in the ammonia nitrogen-containing wastewater is 10~300 mg / L.
[0047] For example, the concentration of ammonia nitrogen in the ammonia nitrogen-containing wastewater can be 10 mg / L, 20 mg / L, 30 mg / L, 50 mg / L, 80 mg / L, 100 mg / L, 150 mg / L, 200 mg / L, 250 mg / L, 300 mg / L, and any value between such a minimum and maximum value, or a range of any two values.
[0048] In this invention, the electrochemical reaction device includes a cathode chamber and an anode chamber, which are separated by an ion exchange membrane; the self-supporting molybdenum-copper electrode is disposed in the cathode chamber, and the counter electrode is disposed in the anode chamber; the device also includes components for fixing and sealing the cathode chamber, the anode chamber, and the ion exchange membrane.
[0049] In some embodiments, the ion exchange membrane includes a cation exchange membrane and an anion exchange membrane. The self-supporting molybdenum-copper electrode, the ion exchange membrane, and the counter electrode are arranged in sequence at intervals to form a wastewater flow channel that flows sequentially through the cathode chamber, the ion exchange membrane, and the anode chamber.
[0050] In some embodiments, a spacer is provided between the cation exchange membrane and the anion exchange membrane to maintain a predetermined distance and form an intermediate compartment.
[0051] In some more specific embodiments, the spacer is a silicone gasket with a thickness of 0.2 to 1 cm. The sealing gasket is a silicone gasket with a thickness of 0.1 to 0.5 cm.
[0052] In some embodiments, the components for fixing and sealing include a first pad, a second pad, and a sealing gasket disposed between the first pad and the cathode chamber, and between the second pad and the anode chamber. The first pad and the second pad are used to press and fix the cathode chamber, the anode chamber, and the ion exchange membrane.
[0053] In some more specific embodiments, the first and second pads may be plexiglass sheets.
[0054] In some embodiments, the counter electrode can be a shape-stable anode (such as a ruthenium dioxide electrode). The self-supporting molybdenum-copper electrode is the cathode. The cation exchange membrane and the anion exchange membrane are separated by a silicone gasket. The self-supporting molybdenum-copper electrode, the cation exchange membrane, the silicone gasket, the anion exchange membrane, and the shape-stable anode are arranged in sequence and sealed and fixed by plexiglass gaskets and silicone pads on both sides.
[0055] In some embodiments, the cathode chamber and / or the anode chamber are provided with a wastewater inlet and a wastewater outlet, and the wastewater inlet and the wastewater outlet are offset in the vertical direction.
[0056] In some more specific embodiments, the wastewater inlet is located at the bottom of the cathode chamber and / or the anode chamber, and the wastewater outlet is located at the top of the cathode chamber and / or the anode chamber.
[0057] For example, such as Figure 1 As shown, the electrochemical reaction device may include an anode chamber and a cathode chamber; wherein the anode chamber is provided with a shape-stable electrode as a counter electrode 7, the anode chamber and the cathode chamber are separated by anion exchange membrane 6 and a cation exchange membrane 4, and the cathode chamber is provided with the self-supporting molybdenum-copper electrode 3; further, the self-supporting molybdenum-copper electrode 3, the cation exchange membrane 4, the anion exchange membrane 6, and the shape-stable anode 7 are arranged sequentially at intervals, wherein the cation exchange membrane 4 and the anion exchange membrane 6 are separated by a silicone gasket 5, the thickness of which is 0.2~1cm. On the molybdenum-copper electrode, nitrate nitrogen can be selectively converted into ammonia through the cyclic conversion of copper and molybdenum valence states at the electrode interface, and the generated ammonia can be selectively stored by forming hydrogen bonds with molybdenum trioxide (the coexisting cations include one or more of sodium ions, potassium ions, calcium ions, and magnesium ions).
[0058] To facilitate the reaction, the electrochemical reaction device is provided with plexiglass pads 1 on both sides to fix the cathode, anode, and ion exchange membrane. The plexiglass pads 1 are separated from the anode and the molybdenum-copper electrode by silicone gaskets 2 to prevent water leakage. The thickness of the silicone gaskets is 0.1~0.5 cm.
[0059] This invention provides a self-supporting molybdenum-copper electrode for electrochemical reduction of nitrate and simultaneous recovery of ammonia. The self-supporting molybdenum-copper electrode includes a conductive substrate and a molybdenum-copper composite layer loaded on the conductive substrate. The molybdenum-copper composite layer contains molybdenum trioxide and cuprous oxide, and the self-supporting molybdenum-copper electrode exhibits a porous layered structure formed by interwoven nanoribbons.
[0060] The present invention provides an electrochemical reaction device for electrochemical reduction of nitrate nitrogen and simultaneous recovery of ammonia. The device includes a cathode chamber, an anode chamber, and an ion exchange membrane disposed between the cathode chamber and the anode chamber. A self-supporting molybdenum-copper electrode as described above is disposed in the cathode chamber, and a counter electrode is disposed in the anode chamber.
[0061] The present invention also provides an application of the electrochemical reaction device described above in ammonia recovery, comprising: using the electrochemical reaction device to treat wastewater containing ammonia nitrogen; wherein the ammonia nitrogen concentration in the wastewater is 10~300 mg / L, the operating voltage is 1~5 V, and the reaction time is 2~8 h.
[0062] It should be noted that the ammonia resources recovered in this invention are recovered in the form of salt, containing no other impurities, and have high commercial value. For example, the recovered ammonia resources are selectively stored by forming hydrogen bonds with molybdenum trioxide, such as in the form of Mo=O…H.
[0063] To facilitate a further understanding of the present invention by those skilled in the art, the following examples are provided: Example 1 Preparation of an electrochemical reduction device: The electrochemical device prepared in this embodiment is as follows: Figure 1 As shown, it includes: an acrylic glass pad 1, a silicone gasket 2, a self-supporting molybdenum-copper electrode 3, a cation exchange membrane 4, a silicone gasket 5, an anion exchange membrane 6, a shape-stabilized electrode 7, a silicone gasket 8, and an acrylic glass plate 9 arranged horizontally in sequence. All components are sealed and connected by fasteners.
[0064] The silicone pad 2 is used to separate the self-supporting molybdenum copper electrode from the plexiglass pad 1 and to prevent leakage; the silicone pad 8 is used to separate the shape-stabilized electrode 7 from the plexiglass plate 9 and to prevent leakage.
[0065] The bottom of the silicone pad 2 and the plexiglass plate 1 has small holes to allow wastewater to enter; the top of the silicone pad 8 and the plexiglass plate 9 has small holes to allow treated water to exit.
[0066] Both the cation exchange membrane 4 and the self-supporting molybdenum-copper electrode 3 have small holes at their bottoms to allow wastewater to flow through; the anion exchange membrane 6 and the shape-stabilized electrode 7 have small holes at their tops to allow wastewater to flow through. This design extends the contact time between the wastewater and the electrode plates and also provides a certain stirring effect.
[0067] The fabrication steps of the self-supporting molybdenum-copper electrode 3 used in this embodiment are as follows: S1. Cut a certain area of foamed nickel (6×6×2cm), clean its surface impurities and oxides with acetone and dilute hydrochloric acid, and then dry it in a vacuum drying oven; 125 mg of copper sulfate and 12.124 g of ammonium heptamolybdate were dissolved in 1 L of ultrapure water to obtain a mixed solution with a copper-molybdenum mass ratio of 1:140. Nickel foam was fixed using a platinum electrode clamp and immersed in a copper-molybdenum mixed solution at 8 mA / cm². 2 Electrodeposition reaction was carried out at a current density of 10 min. The resulting nickel foam was washed with ultrapure water and then vacuum dried to obtain a material with a blue-black surface.
[0068] S2. The blue-black nickel foam was heated to 350℃ in a tube furnace with nitrogen as the protective atmosphere (gas flow rate of 10 mL / min) at a heating rate of 5℃ / min, held for 120 min, and then cooled to room temperature to obtain a self-supporting molybdenum-copper electrode 3, denoted as sample one.
[0069] like Figure 2 As shown, the self-supporting molybdenum-copper electrode is a nanoribbon with a width of ~10 nm.
[0070] like Figure 3 As shown, in the self-supported molybdenum-copper electrode, copper and molybdenum exist as cuprous oxide and molybdenum trioxide, respectively.
[0071] Example 2 Electrochemical reduction of nitrate nitrogen to produce ammonia and simultaneous storage and recovery of ammonia: The wastewater was treated with 100 mL of a mixed solution of 50 mM sodium sulfate and 140 mg N / L nitrate. The electrochemical reduction apparatus prepared in Example 1 was used, with ruthenium dioxide (6×6×0.2 cm) as the anode and a self-supporting molybdenum-copper electrode 7, which was a layered molybdenum trioxide and cuprous oxide composite electrode (6×6×2 cm) deposited in situ with nickel foam. A constant voltage of 5V was applied to the cell using a DC power supply. Under these conditions, experiments were conducted on the electrochemical reduction of nitrate to ammonia and the simultaneous storage and recovery of ammonia.
[0072] Experimental results are as follows Figure 4 As shown, after 6 hours of electrolysis, the nitrate degradation rate was 77.9% and the ammonia recovery rate was 89.2%.
[0073] Example 3 Electrochemical reduction of nitrate nitrogen to produce ammonia and simultaneous storage and recovery of ammonia: The wastewater was treated with 100 mL of a mixed solution of 50 mM sodium sulfate and 140 mg N / L nitrite. The electrochemical reduction apparatus prepared in Example 1 was used, with ruthenium dioxide (6×6×0.2 cm) as the anode and a self-supporting molybdenum-copper electrode 7, which was a layered molybdenum trioxide and cuprous oxide composite electrode (6×6×2 cm) deposited in situ with nickel foam. A constant voltage of 5 V was applied to the cell using a DC power supply. Under these conditions, experiments were conducted on the electrochemical reduction of nitrate to ammonia and the simultaneous storage and recovery of ammonia.
[0074] Experimental results are as follows Figure 5 As shown, after 6 hours of electrolysis, the nitrite degradation rate was 66.1% and the ammonia recovery rate was 95.8%.
[0075] Example 4 Electrochemical reduction of nitrate nitrogen to produce ammonia and simultaneous storage and recovery of ammonia: The actual wastewater source was municipal wastewater with an ammonia nitrogen concentration of 25 mg / L and nitrate concentration of 25 mg N / L. The wastewater volume was 100 mL. The electrochemical reduction device prepared in Example 1 was used. The anode was ruthenium dioxide (6×6×0.2 cm), and the cathode was a self-supporting molybdenum-copper electrode 7, which was a layered molybdenum trioxide and cuprous oxide composite electrode deposited in situ with nickel foam (6×6×2 cm). A constant voltage of 5 V was applied to the cell using a DC power supply. Under these conditions, experiments were carried out on the electrochemical reduction of nitrate to ammonia and the simultaneous storage and recovery of ammonia.
[0076] The results are as follows Figure 6 As shown, after 6 hours of electrolysis, the removal rate of total inorganic nitrogen in the water was 97.5%, and the ammonia recovery rate was 97.3%.
[0077] Example 5 Electrochemical storage and recovery of ammonia: The experimental study on the separate storage of ammonia used 100 mL of 10 mM ammonium sulfate solution as the research object. The anode was ruthenium dioxide (6×6×0.2 cm), and the cathode was a self-supporting molybdenum-copper electrode 7, which was a layered molybdenum trioxide and cuprous oxide composite electrode deposited in situ with nickel foam (6×6×2 cm). A constant voltage of 5 V was applied to the cell using a DC power supply. Under these conditions, experiments were carried out on the electrochemical reduction of nitrate to produce ammonia and the simultaneous storage and recovery of ammonia.
[0078] The results are as follows Figure 7As shown, after 6 hours of electrolysis, the ammonia recovery rate was 98.7%, and the storage capacity was as high as 358.8 mg / g.
[0079] Therefore, the method for electrochemical reduction of nitrate nitrogen to ammonia and simultaneous recovery using a self-supporting molybdenum-copper electrode provided by the present invention can simultaneously achieve the dual goals of purifying nitrate nitrogen wastewater and recovering ammonia.
[0080] Comparative Example 1 Self-supporting electrode containing only cuprous oxide (Cu2O) (molybdenum-free).
[0081] The fabrication steps of the self-supporting cuprous oxide electrode used in this comparative example are as follows: S1. Cut a certain area of foamed nickel (6×6×2 cm), clean its surface impurities and oxides with acetone and dilute hydrochloric acid in sequence, and then dry it in a vacuum drying oven; 125 mg of copper sulfate (excluding ammonium heptamolybdate) was dissolved in 1 L of ultrapure water to obtain an electrodeposition solution containing only copper ions; The nickel foam was fixed with a platinum electrode clamp and deposited in the electrodeposition solution at 8 mA / cm². 2 Electrodeposition reaction was carried out at a current density of 10 min. The resulting nickel foam was washed with ultrapure water and then vacuum dried to obtain a material with a reddish-brown surface.
[0082] S2. The reddish-brown nickel foam was heated to 350°C in a tube furnace under a protective atmosphere of nitrogen (gas flow rate 10 mL / min) at a heating rate of 5°C / min, held at that temperature for 120 min, and then cooled to room temperature to obtain a self-supporting cuprous oxide electrode, denoted as the electrode of Comparative Example 1.
[0083] Application test (same conditions as in Example 2): Using Comparative Example 1 electrode as cathode and ruthenium dioxide electrode as anode, 100 mL of a mixed solution containing 50 mM sodium sulfate and 140 mg N / L nitrate was treated at a constant voltage of 5 V for 6 h.
[0084] Results: The nitrate removal rate was 67.9%, while the ammonia recovery rate was only 48.1%. This indicates that although the electrode without molybdenum trioxide has a certain catalytic ammonia production capacity, it has almost no function of simultaneous storage and recovery of ammonia.
[0085] Comparative Example 2 Self-supporting electrode containing only molybdenum trioxide (MoO3) (copper-free) The preparation steps of the self-supporting molybdenum trioxide electrode used in this comparative example are as follows: S1. Cut a certain area of foamed nickel (6×6×2 cm), clean its surface impurities and oxides with acetone and dilute hydrochloric acid in sequence, and then dry it in a vacuum drying oven; 12.124 g of ammonium heptamolybdate (without copper sulfate) was dissolved in 1 L of ultrapure water to obtain an electrodeposition solution containing only molybdate ions; The nickel foam was fixed with a platinum electrode clamp and deposited in the electrodeposition solution at 8 mA / cm². 2 Electrodeposition reaction was carried out at a current density of 10 min. The resulting nickel foam was washed with ultrapure water and then vacuum dried to obtain a material with a blue-green surface.
[0086] S2. Blue-green nickel foam was heated to 350°C in a tube furnace with nitrogen as the protective atmosphere (gas flow rate 10 mL / min) at a heating rate of 5°C / min, held at that temperature for 120 min, and then cooled to room temperature to obtain a self-supporting molybdenum trioxide electrode, denoted as Comparative Example 2 electrode.
[0087] Application test: Using Comparative Example 2 electrode as cathode and ruthenium dioxide electrode as anode, 100 mL of a mixed solution containing 50 mM sodium sulfate and 140 mg N / L nitrate was treated at a constant voltage of 5 V for 6 h.
[0088] Results: The nitrate removal rate was only 20.2%, and the ammonia recovery rate was 80.1%. This indicates that although the electrode without cuprous oxide has a certain adsorption capacity for ammonia, it cannot efficiently catalyze the reduction of nitrate and nitrogen.
[0089] The above technical solutions of the present invention are merely preferred embodiments of the present invention and do not limit the patent scope of the present invention. All equivalent structural transformations made under the technical concept of the present invention using the contents of the present invention specification and drawings, or direct / indirect applications in other related technical fields, are included in the patent protection scope of the present invention.
Claims
1. A method for electroreducing nitrate nitrogen and simultaneously recovering ammonia using a self-supporting molybdenum-copper electrode, characterized in that, An electrochemical reaction device is used, with a self-supporting molybdenum-copper electrode as the cathode, to electrochemically reduce wastewater containing nitrate nitrogen. While reducing nitrate nitrogen to ammonia, the ammonia is adsorbed and stored in situ through the self-supporting molybdenum-copper electrode. The self-supporting molybdenum-copper electrode includes a conductive substrate and a molybdenum-copper composite layer loaded on the conductive substrate. The molybdenum-copper composite layer contains molybdenum trioxide and cuprous oxide. The self-supporting molybdenum-copper electrode exhibits a porous layered structure formed by interwoven molybdenum trioxide nanoribbons. The cuprous oxide is distributed in particulate form between the layers and / or on the surface of the molybdenum trioxide.
2. The method for electroreducing nitrate nitrogen and simultaneously recovering ammonia using a self-supporting molybdenum-copper electrode according to claim 1, characterized in that, The nitrate-containing wastewater is at least one of surface water, groundwater, municipal wastewater, or photovoltaic wastewater; The nitrate nitrogen is derived from nitrate and / or nitrite; the concentration of nitrate nitrogen in the nitrate nitrogen-containing wastewater is 10~300 mg / L; The nitrate-containing wastewater also contains coexisting cations, including at least one of sodium, potassium, calcium, or magnesium ions.
3. The method for electroreducing nitrate nitrogen and simultaneously recovering ammonia using a self-supporting molybdenum-copper electrode according to claim 1, characterized in that, The method for preparing the self-supporting molybdenum-copper electrode includes: Electrodeposition is performed by immersing a conductive substrate in an electrodeposition solution containing copper ions and molybdate ions to form a molybdenum-copper precursor in situ on the surface of the conductive substrate, thus obtaining the precursor electrode. The precursor electrode is heat-treated to obtain the self-supporting molybdenum-copper electrode.
4. The method for electroreducing nitrate nitrogen and simultaneously recovering ammonia using a self-supporting molybdenum-copper electrode according to claim 1, characterized in that, The mass ratio of copper to molybdenum in the electrodeposition solution is 1:50~250; the concentration of copper in the electrodeposition solution is 28~140 mg / L.
5. The method for electroreducing nitrate nitrogen and simultaneously recovering ammonia using a self-supporting molybdenum-copper electrode according to claim 1, characterized in that, The current density during the electrodeposition process is 1~15 mA / cm². 2 The deposition time is 5~30 min; The heat treatment temperature is 300~400℃, the heating rate is 2~10℃ / min, and the holding time is 60~180 min.
6. The method for electroreducing nitrate nitrogen and simultaneously recovering ammonia using a self-supporting molybdenum-copper electrode according to claim 1, characterized in that, The electrochemical reduction treatment is carried out under constant voltage or constant current conditions; wherein, under constant voltage conditions, the voltage is 2~8 V, and under constant current conditions, the current density is 0.2~0.8 mA / cm². 2 The electrochemical reduction treatment lasts for 3 to 10 hours.
7. The method for electroreducing nitrate nitrogen and simultaneously recovering ammonia using a self-supporting molybdenum-copper electrode according to claim 1, characterized in that, The electrochemical reaction device includes a cathode chamber and an anode chamber, which are separated by an ion exchange membrane; the self-supporting molybdenum-copper electrode is disposed in the cathode chamber, and the counter electrode is disposed in the anode chamber; the device also includes components for fixing and sealing the cathode chamber, the anode chamber, and the ion exchange membrane.
8. The method for electroreducing nitrate nitrogen and simultaneously recovering ammonia using a self-supporting molybdenum-copper electrode according to claim 7, characterized in that, The cathode chamber and the anode chamber are provided with wastewater inlets and wastewater outlets, and the wastewater inlets and wastewater outlets are offset in the vertical direction.
9. An electrochemical reaction device for electrochemical reduction of nitrate nitrogen and simultaneous recovery of ammonia, characterized in that, The device includes a cathode chamber, an anode chamber, and an ion exchange membrane disposed between the cathode chamber and the anode chamber; a self-supporting molybdenum-copper electrode as described in claim 1 is disposed in the cathode chamber, and a counter electrode is disposed in the anode chamber.
10. The application of the electrochemical reaction device according to claim 9 in ammonia recovery, characterized in that, include: The electrochemical reaction device is used to treat wastewater containing ammonia nitrogen; wherein the concentration of ammonia nitrogen in the wastewater is 10~300 mg / L, the operating voltage is 1~5 V, and the reaction time is 2~8 h.