A method and apparatus for the harmless treatment and recycling of lithium-containing waste liquid.
By combining chemical precipitation and ion exchange methods, the problems of high cost and secondary pollution in lithium-containing wastewater treatment have been solved, achieving efficient recovery and purity improvement of lithium resources and ensuring environmental safety.
Patent Information
- Application Number
- CN202611133872.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-29
- Publication Date
- 2026-11-17
AI Technical Summary
Existing methods for treating lithium-containing waste liquids suffer from high treatment costs, are prone to secondary pollution, and pose potential threats to the environment.
A method combining chemical precipitation and ion exchange is employed, including neutralization, precipitation, solid-liquid separation, ion exchange, and evaporation crystallization. Chemical precipitation removes impurities and reduces volume, while ion exchange deeply extracts lithium. D001 macroporous strong acid cation exchange resin is used for ion exchange, combined with pH monitoring and dilute hydrochloric acid regeneration, to achieve efficient recovery of lithium resources.
This approach enables the harmless disposal and resource utilization of lithium resources, reduces processing costs, extends resin lifespan, improves the purity and recovery rate of lithium salt products, and ensures that emissions meet environmental standards.
Smart Images

Figure CN123105879A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of lithium resource recycling technology, and particularly relates to a harmless treatment and recycling method and device for lithium-containing waste liquid. Background Technology
[0002] Currently, the main methods for treating lithium-containing wastewater include chemical precipitation and ion exchange. However, these traditional methods have many drawbacks. Chemical precipitation often introduces other impurities during the precipitation process, which not only affects the purity of the lithium product but also increases the difficulty and cost of subsequent purification. Ion exchange uses ion exchange resins with limited lifespans, requiring frequent replacement, which significantly increases treatment costs. Furthermore, both methods may generate secondary pollution, posing a potential threat to the environment.
[0003] Therefore, developing an efficient, safe, environmentally friendly, and economical lithium-containing wastewater treatment technology has extremely important practical significance and strategic value. Summary of the Invention
[0004] In view of the shortcomings of the existing technology, the technical problem to be solved by the present invention is that the existing methods for treating lithium-containing waste liquid have high treatment costs, are prone to secondary pollution, and pose potential threats to the environment. The present invention proposes a harmless treatment and recycling method and recycling device for lithium-containing waste liquid.
[0005] To solve the aforementioned technical problem, the technical solution adopted by the present invention is as follows: The present invention provides a method for the harmless disposal and recycling of lithium-containing waste liquid, including a neutralization treatment step, a precipitation step, a solid-liquid separation step, an ion exchange step, and an evaporation and crystallization step; The neutralization process includes: Hydrochloric acid solution was added to the pretreated lithium-containing waste liquid. When the pH value of the solution gradually decreased to 6-8, the addition of hydrochloric acid was stopped. The chemical reaction equation that occurred in this step is LiOH + HCl → LiCl + H2O. The precipitation step includes: Sodium carbonate is added to the neutralized solution and stirred continuously to form lithium carbonate precipitate. The chemical reaction equation for this step is 2LiCl + Na2CO3 → Li2CO3↓ + 2NaCl. The solid-liquid separation step includes: Solid-liquid separation was performed using a plate and frame filter press to obtain Li2CO3 filter residue and NaCl preliminary filtrate; The ion exchange step includes: The initial NaCl filtrate was passed through an ion exchange column packed with D001 macroporous strong acid cation exchange resin, with a resin bed volume of 1 L. During the reaction, the initial pH was controlled at 8-9, and the column space velocity was maintained at BV / h = 2. The pH value at the ion exchange column outlet was monitored in real time during adsorption. The ion adsorption process was considered to have started when the monitored pH value was lower than the initial pH value. The ion adsorption process consisted of three reaction stages: Before the injection volume reaches 1.5 BV, the reaction equation is: R - SO3H + Li + →R-SO3Li+H + At this point, a filtrate containing almost only NaCl can be collected; When the injection volume is between 1.5 BV and 2 BV, the reaction equation is: R - SO3H + Li + →R-SO3Li+H + R-SO3H+Na + →R-SO3Na+H + During this stage, a mixed filtrate containing NaCl and LiCl can be collected. After an injection volume of 2 BV, the reaction equation that occurs is: R - SO3H + Na + →R-SO3Na+H + At this point, a filtrate containing almost only LiCl can be collected. When the pH stabilizes at 8-9 and does not decrease for 3-5 minutes, the adsorption process is complete.
[0006] Preferably, in the ion exchange step, the preliminary NaCl filtrate is passed through the ion exchange column at a flow rate of 0.03-0.035 L / min.
[0007] Preferably, after the D001 macroporous strong acid cation exchange resin in the ion exchange step is saturated, 2 mol / L dilute hydrochloric acid can be added as a regenerator to regenerate the D001 macroporous strong acid cation exchange resin. When the pH of the washing solution is stable at 1-2 and does not decrease for 3-5 minutes, it indicates that the replacement is complete. The reaction equations for the regeneration process are: R-SO3Na+HCl→R-SO3H+NaCl, R-SO3Li+HCl→R-SO3H+LiCl.
[0008] Preferably, a pretreatment step is performed before the neutralization step, the pretreatment step including: The lithium-containing waste liquid is filtered through a filter screen with a pore size of 0.3-0.8 mm.
[0009] Preferably, the lithium in the lithium-containing waste liquid comes from the pure waste material remaining in the mold during the smelting and casting of lithium metal in an oxygen-free and water-free environment. This waste material is placed in pure water and reacted completely to obtain a strongly alkaline lithium hydroxide solution without obvious impurities.
[0010] Preferably, in the neutralization step, the concentration of the hydrochloric acid solution is 1.5-2.5 mol / L.
[0011] Preferably, the actual amount of sodium carbonate added in the precipitation step is calculated by the following method: m(Na2CO3) 理论 =1 / 2×c(LiOH)×V(LiOH)×105.99 m(Na2CO3) 实际 =(1~1.1)×m(Na2CO3) 理论 .
[0012] Preferably, in the solid-liquid separation step, the filtration pressure of the plate and frame filter press is 0.6 MPa.
[0013] Preferably, the evaporation and crystallization step includes: The NaCl filtrate was concentrated by vacuum evaporation, with the vacuum level controlled at -0.08 MPa and the temperature at 60-65℃, to remove water from the filtrate and obtain NaCl crystals. The Li2CO3 filter residue was washed with water, recrystallized, and dried.
[0014] In a second aspect, the present invention provides a harmless treatment and recycling device for lithium-containing waste liquid, comprising a filter, a neutralization tank, a sedimentation tank, a plate and frame filter press, a preliminary filtrate collection tank, and an ion exchange column connected in sequence. The filter is located at the inlet of the neutralization tank and is equipped with a filter screen inside to remove suspended impurities and large particles from the lithium-containing waste liquid. The neutralization tank is used to receive lithium-containing waste liquid from the filter. The neutralization tank is equipped with a stirring mechanism, and hydrochloric acid solution is introduced into the neutralization tank to carry out a neutralization reaction. The sedimentation tank is used to treat the neutralized solution. The tank is equipped with a stirring mechanism. Sodium carbonate powder is slowly added to fully dissolve it and react with lithium ions to generate lithium carbonate precipitate. The plate and frame filter press is used for solid-liquid separation of a mixture from a sedimentation tank; The preliminary filtrate collection tank is used to collect the preliminary NaCl filtrate after separation by the plate and frame filter press. The ion exchange column is used to adsorb lithium ions from the NaCl preliminary filtrate in the preliminary filtrate collection tank.
[0015] Compared with the prior art, the beneficial effects of the present invention are as follows: This invention provides a method for the harmless disposal and recycling of lithium-containing wastewater. By coupling chemical precipitation and ion exchange, the chemical precipitation process is responsible for impurity removal and volume reduction, while the ion exchange process is responsible for deep lithium extraction. This method can significantly reduce the ion exchange load and extend the resin's lifespan while achieving a process of first coarse extraction and then deep extraction of lithium resources, resulting in high practicality and cost-effectiveness. Through the integrated process of "neutralization treatment, precipitation, solid-liquid separation, ion exchange, and evaporation crystallization steps," the harmlessness and resource recovery of lithium-containing wastewater are achieved. Hydrochloric acid is used for neutralization and as a regenerator for the cation exchange resin R-SO3H, which is simple to operate and low in cost. The reaction process is judged by pH value, avoiding the introduction of insoluble impurities and improving the purity and recovery rate of the final lithium salt product. The entire process is efficient and controllable, ensuring environmental compliance while separating pure NaCl and LiCl salt solutions, effectively recovering valuable lithium resources. Attached Figure Description
[0016] Figure 1 This is a schematic diagram of the process for the harmless disposal and recycling of lithium-containing waste liquid, as shown in the embodiment. Figure 2 A simplified diagram of an apparatus for the harmless treatment and recycling of lithium-containing waste liquid. Detailed Implementation
[0017] The technical solutions in specific embodiments of the present invention will now be described in detail and completely with reference to the accompanying drawings. Obviously, the described embodiments are merely some specific implementations of the overall technical solution of the present invention, and not all implementations. Based on the overall concept of the present invention, all other embodiments obtained by those skilled in the art fall within the protection scope of the present invention.
[0018] This invention provides a method for the harmless disposal and recycling of lithium-containing waste liquid, including a neutralization treatment step, a precipitation step, a solid-liquid separation step, an ion exchange step, and an evaporation and crystallization step; The neutralization process includes: Hydrochloric acid solution was added to the pretreated lithium-containing waste liquid. When the pH value of the solution gradually decreased to 6-8, the addition of hydrochloric acid was stopped. The chemical reaction equation that occurred in this step is LiOH + HCl → LiCl + H2O. The precipitation process includes: Sodium carbonate is added to the neutralized solution and stirred continuously to form lithium carbonate precipitate. The chemical reaction equation for this step is 2LiCl + Na2CO3 → Li2CO3↓ + 2NaCl. Solid-liquid separation steps include: Solid-liquid separation was performed using a plate and frame filter press to obtain Li2CO3 filter residue and NaCl preliminary filtrate; The ion exchange process includes: The initial NaCl filtrate was passed through an ion exchange column packed with D001 macroporous strong acid cation exchange resin, with a resin bed volume of 1 L. During the reaction, the initial pH was controlled at 8-9, and the column space velocity was maintained at BV / h = 2. The pH value at the ion exchange column outlet was monitored in real time during adsorption. The ion adsorption process was considered to have started when the monitored pH value was lower than the initial pH value. The ion adsorption process consisted of three reaction stages: Before the injection volume reaches 1.5 BV, the reaction equation is: R - SO3H + Li + →R-SO3Li+H + At this point, a filtrate containing almost only NaCl can be collected; When the injection volume is between 1.5 BV and 2 BV, the reaction equation is: R - SO3H + Li + →R-SO3Li+H + R-SO3H+Na + →R-SO3Na+H + During this stage, a mixed filtrate containing NaCl and LiCl can be collected. After an injection volume of 2 BV, the reaction equation that occurs is: R - SO3H + Na + →R-SO3Na+H + At this point, a filtrate containing almost only LiCl can be collected. When the pH stabilizes at 8-9 and does not decrease for 3-5 minutes, the adsorption process is complete.
[0019] It should be noted that traditional treatment methods in existing technologies have many drawbacks. In chemical precipitation, the precipitate is often a mixture of lithium-containing salts. Taking lithium carbonate as an example, since lithium carbonate still has a certain solubility in water (approximately 1.3 g / L, 25℃), the resulting filtrate still contains a certain amount of lithium ions, making it difficult to meet the requirements for deep, large-scale processing or high recovery rates. This not only affects the purity of the lithium product, but the high-salt mother liquor also increases the difficulty and cost of subsequent purification, and direct discharge will damage the soil and aquatic ecosystems. Ion exchange can further purify the filtrate, but the ion exchange resins used in conventional ion exchange methods have a limited lifespan and require frequent replacement. The elution and regeneration processes must be carried out separately, and repeated high-salt environment operations easily corrode equipment. Furthermore, the sludge easily forms scale, clogging pipes and filtration equipment, resulting in high maintenance costs, which undoubtedly significantly increases the treatment cost.
[0020] To address the above issues, this application couples chemical precipitation with ion exchange. The chemical precipitation process removes impurities and reduces volume, while the ion exchange process extracts lithium at a deeper level. This significantly reduces the ion exchange load and extends resin lifespan while achieving a process of initial coarse extraction followed by deep extraction of lithium resources, offering high practicality and cost-effectiveness. Specifically, this application passes lithium-containing wastewater that has undergone preliminary ion precipitation through an ion exchange column filled with D001 macroporous strong acidic cation exchange resin (hydrogen form R-SO3H), thereby removing residual Li in the initial NaCl filtrate. + Separation and purification. Compared to gel resins that are prone to shrinkage and breakage under high salinity conditions, D001 has a stable structure, fast mass transfer, and trace amounts of Li... + It is not easily worn through, has a better selective separation effect for the two types of ions, and is not prone to clogging or pulverization when the throughput is large. It has a long service life and does not require frequent replacement. By monitoring the pH of the eluent in real time, the ion exchange column can be eluted and regenerated, and pure NaCl and LiCl salt solutions can be separated, effectively recovering valuable lithium resources.
[0021] In a preferred embodiment, the initial NaCl filtrate is passed through an ion exchange column at a flow rate of 0.03-0.035 L / min.
[0022] The above technical solution limits the flow rate of the initial NaCl filtrate. Specifically, if the flow rate is too slow, the production efficiency will be too low; while in the sample loading stage, if the flow rate is too fast, it will be difficult to adsorb Li. + The exchange process may not have been completed successfully. During the regeneration / elution stage, an excessively high flow rate can cause lithium ions and sodium ions to flow out together, making effective separation impossible.
[0023] In a preferred embodiment, after the D001 macroporous strong acid cation exchange resin is saturated during the ion exchange step, 2 mol / L dilute hydrochloric acid can be added as a regenerator to regenerate the D001 macroporous strong acid cation exchange resin. When the pH of the washing solution is stable at 1-2 and does not decrease for 3-5 minutes, it indicates that the replacement is complete. The reaction equations for the regeneration process are: R-SO3Na+HCl→R-SO3H+NaCl, R-SO3Li+HCl→R-SO3H+LiCl.
[0024] The above technical solution achieves efficient regeneration and recycling of D001 macroporous strong acid cation exchange resin by using 2 mol / L dilute hydrochloric acid and controlling the outlet pH, which significantly extends the resin life and reduces operation and maintenance costs.
[0025] In a preferred embodiment, a pretreatment step is performed before the neutralization step, the pretreatment step including: The lithium-containing waste liquid is filtered through a filter screen with a pore size of 0.3-0.8 mm.
[0026] The above technical solution limits the pore size of the filter screen and the flow rate of the waste liquid. This is because if the flow rate is too fast, the pressure on the filter screen is too high, and fine sediments may be directly carried through the filter pores, failing to achieve effective filtration. On the other hand, if the flow rate is too slow, the production efficiency is too low, the operation time is too long, and it is not suitable for large-scale processing.
[0027] In a preferred embodiment, the lithium in the lithium-containing waste liquid is derived from the pure waste material remaining in the mold during the smelting and casting of lithium metal in an oxygen-free and water-free environment. This waste material is placed in pure water and reacted completely to obtain a strongly alkaline lithium hydroxide solution without obvious impurities.
[0028] In a preferred embodiment, the concentration of the hydrochloric acid solution in the neutralization step is 1.5-2.5 mol / L.
[0029] The above technical solution limits the concentration of hydrochloric acid solution because if the concentration of hydrochloric acid is too low, the neutralization reaction efficiency is low and the reaction time is long, while if the concentration of hydrochloric acid is too high, the volatility is high, the corrosion is strong, and the pH is difficult to control.
[0030] In a preferred embodiment, the actual amount of sodium carbonate added during the precipitation step is calculated by the following method: m(Na2CO3) 理论 =1 / 2×c(LiOH)×V(LiOH)×105.99 m(Na2CO3) 实际 =(1~1.1)×m(Na2CO3) 理论 In a preferred embodiment, the filtration pressure of the plate and frame filter press is 0.6 MPa in the solid-liquid separation step.
[0031] In a preferred embodiment, the evaporation crystallization step includes: The NaCl filtrate was concentrated by vacuum evaporation, with the vacuum level controlled at -0.08 MPa and the temperature at 60-65℃, to remove water from the filtrate and obtain NaCl crystals. The Li2CO3 filter residue was washed with water, recrystallized, and dried.
[0032] Another aspect of the present invention provides a harmless treatment and recycling device for lithium-containing waste liquid, comprising a filter, a neutralization tank, a sedimentation tank, a plate and frame filter press, a preliminary filtrate collection tank, and an ion exchange column connected in sequence. The filter is located at the inlet of the neutralization tank and is equipped with a filter screen inside to remove suspended impurities and large particles from the lithium-containing waste liquid. The neutralization tank is used to receive lithium-containing waste liquid from the filter. The neutralization tank is equipped with a stirring mechanism and hydrochloric acid solution is introduced into the neutralization tank to carry out the neutralization reaction. The sedimentation tank is used to treat the neutralized solution. The tank is equipped with a stirring mechanism. Sodium carbonate powder is slowly added to fully dissolve it and react with lithium ions to form lithium carbonate precipitate. Plate and frame filter presses are used for solid-liquid separation of mixtures from sedimentation tanks; The preliminary filtrate collection tank is used to collect the preliminary NaCl filtrate after separation by the plate and frame filter press; Ion exchange columns are used to adsorb lithium ions from the NaCl preliminary filtrate in the preliminary filtrate collection tank.
[0033] To provide a clearer and more detailed description of the harmless treatment and recycling method and device for lithium-containing waste liquid provided in the embodiments of the present invention, the following description will be based on specific embodiments.
[0034] In the following examples and comparative examples, the D001 macroporous strong acid cation exchange resin used was purchased from Anhui Wandong Chemical Co., Ltd. It is a hydrogen-form strong acid cation exchange resin with a sulfonic acid group (R-SO3H) as its functional group; its working exchange capacity (Li) + (BV / h=2) ≥1000 mmol / L; uniformity coefficient ≤1.6; transformation expansion rate (Na + →H + ≤10%.
[0035] Example 1: A method for the harmless treatment and recycling of lithium-containing waste liquid Neutralization process steps: At room temperature, 100 L of LiOH waste liquid with a molar concentration of 5.3 mol / L was neutralized. Specifically, the waste liquid was first filtered through a 0.8 mm pore size filter at a flow rate of 20 L / min. Then, 2 mol / L hydrochloric acid solution was added to the filtered lithium-containing waste liquid. During the addition of hydrochloric acid, the mixture was continuously stirred at 150 r / min, and the reaction temperature was controlled at 25℃. When the pH of the solution gradually decreased to 7, the addition of hydrochloric acid was stopped, at which point the neutralization reaction was complete.
[0036] Precipitation steps: 28 kg of sodium carbonate was added to the neutralized solution, and the mixture was stirred continuously at 200 r / min to form lithium carbonate precipitate and NaCl preliminary filtrate.
[0037] Solid-liquid separation steps: Solid-liquid separation was performed using a plate and frame filter press at a pressure of 0.6 MPa. The separated Li2CO3 filter residue and NaCl preliminary filtrate were collected and the pH of the NaCl preliminary filtrate was measured and recorded as 8.
[0038] Ion exchange steps: At room temperature, the initial NaCl filtrate was passed through an ion exchange column packed with strongly acidic cation exchange resin R-SO3H. The resin bed volume of a single ion exchange column was 1 L, and the ion exchange column space velocity was maintained at BV / h = 2. During adsorption, the initial NaCl filtrate was passed through the ion exchange column at a flow rate of 0.033 L / min. The pH value at the ion exchange column outlet was monitored in real time. The ion adsorption process was considered to have begun when the pH value was less than 8. The reaction process was determined by recording the effluent volume of a single ion exchange column. When the effluent volume was less than 1.5 L, a filtrate containing almost only NaCl could be collected; when the effluent volume was greater than 1.5 L but less than 2 L, a mixed filtrate containing both LiCl and NaCl could be collected; when the effluent volume was greater than 2 L, a filtrate containing almost only LiCl could be collected. The pH value at the ion exchange column outlet was monitored in real time. The adsorption process was considered complete when the pH of the eluent slowly rose until it stabilized at 8 and did not decrease for 3-5 minutes.
[0039] During regeneration, 2 mol / L dilute hydrochloric acid was added as a regenerant at a flow rate of 0.033 L / min. Initially, the outlet pH was 8, and as the Li on the column... + And Na + As the solution is washed out, the pH gradually decreases. The pH of the effluent eventually stabilizes at 1 for 5 consecutive minutes and does not decrease further, indicating that regeneration is complete.
[0040] Evaporation and crystallization steps: NaCl crystals were obtained by vacuum evaporation, with the vacuum level controlled at -0.08 MPa and the temperature at 65℃. The Li₂CO₃ filter residue was washed with water, recrystallized, and dried to obtain lithium carbonate product. For washing, deionized water was used at a solid-liquid ratio of 1:3, and the washing was performed twice. For recrystallization, the filter residue was dissolved in an appropriate amount of hot water, and then slowly cooled to crystallize, further improving the purity of the lithium salt. During drying, the drying temperature was set at 105℃ and the drying time was 8 hours, yielding 19267.5 g of dried pure lithium carbonate product, with a reaction yield of 98.4%.
[0041] Example 2: A method for the harmless treatment and recycling of lithium-containing waste liquid Neutralization process steps: At room temperature, 100 L of LiOH waste liquid with a molar concentration of 5.3 mol / L was neutralized. Specifically, the waste liquid was first filtered through a 0.8 mm pore size filter at a flow rate of 20 L / min. Then, 2 mol / L hydrochloric acid solution was added to the filtered lithium-containing waste liquid. During the addition of hydrochloric acid, stirring was continuously performed at 150 r / min, and the reaction temperature was controlled at 25℃. When the pH of the solution gradually decreased to 7, the addition of hydrochloric acid was stopped, at which point the neutralization reaction was complete.
[0042] Precipitation steps: Add 30 kg of sodium carbonate to the neutralized solution and stir continuously at 200 r / min to form lithium carbonate precipitate and NaCl preliminary filtrate.
[0043] Solid-liquid separation steps: Solid-liquid separation was performed using a plate and frame filter press at a pressure of 0.6 MPa. The separated Li2CO3 filter residue and NaCl preliminary filtrate were collected, and the pH of the coarse filtrate was measured and recorded as 9.
[0044] Ion exchange steps: At room temperature, the initial NaCl filtrate was passed through an ion exchange column packed with strongly acidic cation exchange resin R-SO3H. The resin bed volume of a single ion exchange column was 1 L, and the ion exchange column space velocity was maintained at BV / h = 2. During adsorption, the initial NaCl filtrate was passed through the ion exchange column at a flow rate of 0.033 L / min. The pH value at the ion exchange column outlet was monitored in real time. The ion adsorption process was considered to have begun when the pH value was less than 9. The reaction process was determined by recording the effluent volume of a single ion exchange column. When the effluent volume was less than 1.5 L, a filtrate containing almost only NaCl could be collected; when the effluent volume was greater than 1.5 L but less than 2 L, a mixed filtrate containing both LiCl and NaCl could be collected; when the effluent volume was greater than 2 L, a filtrate containing almost only LiCl could be collected. The pH value at the ion exchange column outlet was monitored in real time. The adsorption process was considered complete when the pH of the eluent slowly rose until it stabilized at 9 and did not decrease for 3-5 minutes.
[0045] During regeneration, 2 mol / L dilute hydrochloric acid was added as a regenerant at a flow rate of 0.033 L / min. Initially, the outlet pH was 9, and as the Li on the column... + And Na + As the solution is washed out, the pH gradually decreases. The pH of the effluent eventually stabilizes at 1 for 5 consecutive minutes and does not decrease further, indicating that regeneration is complete.
[0046] Evaporation and crystallization steps: NaCl crystals were obtained by vacuum evaporation, with the vacuum level controlled at -0.08 MPa and the temperature at 65℃. The Li₂CO₃ filter residue was washed with water, recrystallized, and dried to obtain lithium carbonate product. For washing, deionized water was used at a solid-liquid ratio of 1:3, and the washing was performed twice. For recrystallization, the filter residue was dissolved in an appropriate amount of hot water, and then slowly cooled to crystallize, further improving the purity of the lithium salt. During drying, the drying temperature was set at 105℃ and the drying time was 8 hours, yielding 18582.2 g of dried lithium carbonate product, with a reaction yield of 94.9%.
[0047] Example 3: A method for the harmless treatment and recycling of lithium-containing waste liquid Neutralization process steps: At room temperature, 100 L of collected LiOH waste liquid with a molar concentration of 5.3 mol / L was neutralized. Specifically, the waste liquid was first filtered through a 0.3 mm pore size filter. The flow rate of the waste liquid was approximately 1 / 5 of that when the filter pore size was 0.8 mm, i.e., 4 L / min. Correspondingly, the filtration time was significantly extended to 5 times that of Example 1. Then, 2 mol / L hydrochloric acid solution was added to the filtered lithium-containing waste liquid. During the addition of hydrochloric acid, stirring was continuously performed at 150 r / min, and the reaction temperature was controlled at 25°C. When the pH of the solution gradually decreased to 7, the addition of hydrochloric acid was stopped, at which point the neutralization reaction was complete.
[0048] Precipitation steps: 28 kg of sodium carbonate was added to the neutralized solution, and the mixture was stirred continuously at 200 r / min to form lithium carbonate precipitate and NaCl preliminary filtrate.
[0049] Solid-liquid separation steps: Solid-liquid separation was performed using a plate and frame filter press at a pressure of 0.6 MPa. The separated Li2CO3 filter residue and NaCl preliminary filtrate were collected and the pH of the NaCl preliminary filtrate was measured and recorded as 8.
[0050] Ion exchange steps: At room temperature, the initial NaCl filtrate was passed through an ion exchange column packed with strongly acidic cation exchange resin R-SO3H. The resin bed volume of a single ion exchange column was 1 L, and the ion exchange column space velocity was maintained at BV / h = 2. During adsorption, the initial NaCl filtrate was passed through the ion exchange column at a flow rate of 0.033 L / min. The pH value at the ion exchange column outlet was monitored in real time. The ion adsorption process was considered to have begun when the pH value was less than 8. The reaction process was determined by recording the effluent volume of a single ion exchange column. When the effluent volume was less than 1.5 L, a filtrate containing almost only NaCl could be collected; when the effluent volume was greater than 1.5 L but less than 2 L, a mixed filtrate containing both LiCl and NaCl could be collected; when the effluent volume was greater than 2 L, a filtrate containing almost only LiCl could be collected. The pH value at the ion exchange column outlet was monitored in real time. The adsorption process was considered complete when the pH of the eluent slowly rose until it stabilized at 8 and did not decrease for 3-5 minutes.
[0051] During regeneration, 2 mol / L dilute hydrochloric acid was added as a regenerant at a flow rate of 0.033 L / min. Initially, the outlet pH was 8, and as the Li on the column... + And Na + As the solution is washed out, the pH gradually decreases. The pH of the effluent eventually stabilizes at 1 for 5 consecutive minutes and does not decrease further, indicating that regeneration is complete.
[0052] Evaporation and crystallization steps: NaCl crystals were obtained by vacuum evaporation, with the vacuum level controlled at -0.08 MPa and the temperature at 65℃. The Li₂CO₃ filter residue was washed with water, recrystallized, and dried to obtain lithium carbonate product. For washing, deionized water was used at a solid-liquid ratio of 1:3, and the washing was performed twice. For recrystallization, the filter residue was dissolved in an appropriate amount of hot water, and then slowly cooled to crystallize, further improving the purity of the lithium salt. During drying, the drying temperature was set at 105℃ and the drying time was 8 hours, yielding 18856.3 g of dried lithium carbonate product, with a reaction yield of 96.3%.
[0053] Comparative Example 1: Single Chemical Precipitation Method Neutralization process steps: At room temperature, 100 L of LiOH waste liquid with a molar concentration of 5.3 mol / L was neutralized. Specifically, the waste liquid was first filtered through a 0.8 mm pore size filter at a flow rate of 20 L / min. Then, 2 mol / L hydrochloric acid solution was added to the filtered lithium-containing waste liquid. During the addition of hydrochloric acid, the mixture was continuously stirred at 150 r / min, and the reaction temperature was controlled at 25℃. When the pH of the solution gradually decreased to 7, the addition of hydrochloric acid was stopped, at which point the neutralization reaction was complete.
[0054] Precipitation steps: 28 kg of sodium carbonate was added to the neutralized solution, and the mixture was stirred continuously at 200 r / min to form lithium carbonate precipitate and NaCl preliminary filtrate.
[0055] Solid-liquid separation steps: Solid-liquid separation was performed using a plate and frame filter press at a pressure of 0.6 MPa. The separated Li2CO3 filter residue and NaCl preliminary filtrate were collected and the pH of the NaCl preliminary filtrate was measured and recorded as 8.
[0056] Evaporation and crystallization steps: The Li2CO3 filter residue was washed with water, recrystallized, and dried to obtain lithium carbonate product. During washing, deionized water was used at a solid-liquid ratio of 1:3, and the washing was performed twice. For recrystallization, the filter residue was dissolved in an appropriate amount of hot water and then slowly cooled to crystallize, further improving the purity of the lithium salt. During drying, the drying temperature was set at 105℃ and the drying time was 8 hours, yielding 19110.9g of dried lithium carbonate product. The reaction yield was basically consistent with Example 1, at 97.6%. However, the large amount of lithium ions remaining in the initial NaCl filtrate cannot be recycled, and direct discharge would pollute the soil and groundwater, posing a significant ecological and environmental hazard.
[0057] Comparative Example 2 Neutralization process steps: At room temperature, 100 L of LiOH waste liquid with a molar concentration of 5.3 mol / L was filtered through a 0.8 mm pore size filter at a flow rate of 20 L / min. A 2 mol / L hydrochloric acid solution was then added uniformly to the filtered waste liquid, with stirring at 150 r / min and a reaction temperature of 25℃. Acid addition was stopped when the pH of the solution dropped to 7, indicating the neutralization reaction was complete.
[0058] Precipitation steps: Add 28 kg of sodium carbonate to the neutralized solution and stir continuously at 200 r / min to allow it to react fully and form lithium carbonate precipitate and NaCl coarse filtrate.
[0059] Solid-liquid separation steps: Solid-liquid separation was performed using a plate and frame filter press at a pressure of 0.6 MPa, yielding Li2CO3 filter residue and a preliminary NaCl filtrate with pH=8.
[0060] Ion exchange steps: At room temperature, the initial NaCl filtrate was passed through an ion exchange column packed with strongly acidic cation exchange resin R-SO3H. The resin bed volume of a single ion exchange column was 1 L, the space velocity (BV / h) was controlled at 1, and the feed flow rate was 0.0167 L / min. The outlet pH was monitored; adsorption was considered to have started when pH < 8. The reaction process was assessed by recording the effluent volume of a single ion exchange column. When the effluent volume was less than 1.5 L, a filtrate containing almost only NaCl could be collected; when the effluent volume was greater than 1.5 L but less than 2 L, a mixed filtrate containing both LiCl and NaCl could be collected; when the effluent volume was greater than 2 L, a filtrate containing almost only LiCl could be collected. The pH value at the ion exchange column outlet was monitored in real time. The adsorption process was considered complete when the pH of the eluent slowly rose until it stabilized at 8 and did not decrease for 3-5 minutes. During regeneration, 2 mol / L dilute hydrochloric acid was added as a regenerator at a flow rate of 0.033 L / min. Initially during regeneration, the outlet pH was 8, and as the Li on the column... + And Na + As the solution is washed out, the pH gradually decreases. The pH of the effluent eventually stabilizes at 1 for 5 consecutive minutes and does not decrease further, indicating that regeneration is complete.
[0061] Evaporation and crystallization: The Li2CO3 filter residue was washed with water, recrystallized, and dried to obtain lithium carbonate product. During water washing, deionized water was used, and the washing was carried out at a solid-liquid ratio of 1:3, with two washing cycles. During recrystallization, the filter residue was dissolved in an appropriate amount of hot water, and then slowly cooled to crystallize, further improving the purity of the lithium salt. During the drying process, the drying temperature was set at 105℃ and the drying time was 8 hours to obtain the lithium carbonate product, with a reaction yield of 92%.
[0062] Using a flow rate of BV / h=1 is too slow, resulting in an excessively long residence time of the feed solution within the column, which reduces the adsorbed Li... + Partial desorption, displacement, and elongated tailing can occur, disrupting the originally clearly defined three effluent segments, resulting in a reduction in the amount of LiCl recovered and ultimately a decrease in lithium yield.
[0063] Comparative Example 3 Neutralization process steps: At room temperature, 100 L of LiOH waste liquid with a molar concentration of 5.3 mol / L was filtered through a 0.8 mm pore size filter at a flow rate of 20 L / min. A 2 mol / L hydrochloric acid solution was then added uniformly to the filtered waste liquid, with stirring at 150 r / min and a reaction temperature of 25℃. Acid addition was stopped when the pH of the solution dropped to 7, indicating the neutralization reaction was complete.
[0064] Precipitation steps: Add 28 kg of sodium carbonate to the neutralized solution and stir continuously at 200 r / min to allow it to react fully and form lithium carbonate precipitate and NaCl coarse filtrate.
[0065] Solid-liquid separation steps: Solid-liquid separation was performed using a plate and frame filter press at a pressure of 0.6 MPa, yielding Li2CO3 filter residue and a preliminary NaCl filtrate with pH=8.
[0066] Ion exchange steps: At room temperature, the initial NaCl filtrate was passed through an ion exchange column packed with strongly acidic cation exchange resin R-SO3H. The resin bed volume of a single ion exchange column was 1 L, with a space velocity (BV / h) of 3 and a feed flow rate of 0.05 L / min. The outlet pH was monitored; adsorption was considered to have started when pH < 8. The reaction process was assessed by recording the effluent volume of a single ion exchange column. When the effluent volume was less than 1.5 L, a filtrate containing almost only NaCl was collected; when the effluent volume was greater than 1.5 L but less than 2 L, a mixed filtrate containing both LiCl and NaCl was collected; and when the effluent volume was greater than 2 L, a filtrate containing almost only LiCl was collected. The pH value at the ion exchange column outlet was monitored in real time. The adsorption process was considered complete when the pH of the eluent slowly increased until it stabilized at 8 and did not decrease for 3-5 minutes. During regeneration, 2 mol / L dilute hydrochloric acid was added as a regenerator at a flow rate of 0.033 L / min. Initially during regeneration, the outlet pH was 8, and as the Li on the column... + And Na + As the solution is washed out, the pH gradually decreases. The pH of the effluent eventually stabilizes at 1 for 5 consecutive minutes and does not decrease further, indicating that regeneration is complete.
[0067] Evaporation and crystallization: The Li2CO3 filter residue was washed with water, recrystallized, and dried to obtain lithium carbonate product. During water washing, deionized water was used, and the washing was carried out at a solid-liquid ratio of 1:3, with two washing cycles. During recrystallization, the filter residue was dissolved in an appropriate amount of hot water, and then slowly cooled to crystallize, further improving the purity of the lithium salt. During the drying process, the drying temperature was set at 105℃ and the drying time was 8 hours to obtain the lithium carbonate product, with a reaction yield of 90%.
[0068] Using a BV / h=3, the flow rate is too fast, and the residence time of the liquid in the resin column is too short. + Not yet with H on the resin + Sufficient exchange leads to being washed away, with a large amount of Li + If it gets mixed into the NaCl filtrate, it will be carried away and cannot be recovered, resulting in a decrease in the final lithium yield.
Claims
1. A method for the harmless disposal and recycling of lithium-containing waste liquid, characterized in that, It includes neutralization, precipitation, solid-liquid separation, ion exchange, and evaporation crystallization steps; The neutralization process includes: Hydrochloric acid solution was added to the pretreated lithium-containing waste liquid. When the pH value of the solution gradually decreased to 6-8, the addition of hydrochloric acid was stopped. The chemical reaction equation that occurred in this step is LiOH + HCl → LiCl + H2O. The precipitation step includes: Sodium carbonate is added to the neutralized solution and stirred continuously to form lithium carbonate precipitate. The chemical reaction equation for this step is 2LiCl + Na2CO3 → Li2CO3↓ + 2NaCl. The solid-liquid separation step includes: Solid-liquid separation was performed using a plate and frame filter press to obtain Li2CO3 filter residue and NaCl preliminary filtrate; The ion exchange step includes: The initial NaCl filtrate was passed through an ion exchange column packed with D001 macroporous strong acid cation exchange resin, with a resin bed volume of 1 L. During the reaction, the initial pH was controlled at 8-9, and the column space velocity was maintained at BV / h = 2. The pH value at the ion exchange column outlet was monitored in real time during adsorption. The ion adsorption process was considered to have started when the monitored pH value was lower than the initial pH value. The ion adsorption process consisted of three reaction stages: Before the injection volume reaches 1.5 BV, the reaction equation is: R - SO3H + Li + →R-SO3Li+H + At this point, a filtrate containing almost only NaCl can be collected; When the injection volume is between 1.5 BV and 2 BV, the reaction equation is: R - SO3H + Li + →R-SO3Li+H + R-SO3H+Na + →R-SO3Na+H + During this stage, a mixed filtrate containing NaCl and LiCl can be collected. After an injection volume of 2 BV, the reaction equation that occurs is: R - SO3H + Na + →R-SO3Na+H + At this point, a filtrate containing almost only LiCl can be collected. When the pH stabilizes at 8-9 and does not decrease for 3-5 minutes, the adsorption process is complete.
2. The method for harmless disposal and recycling according to claim 1, characterized in that, In the ion exchange step, the preliminary NaCl filtrate is passed through the ion exchange column at a flow rate of 0.03-0.035 L / min.
3. The harmless disposal and recycling method according to claim 1, characterized in that, When the D001 macroporous strong acid cation exchange resin in the ion exchange step is saturated, 2 mol / L dilute hydrochloric acid can be added as a regenerator to regenerate the D001 macroporous strong acid cation exchange resin. When the pH of the washing solution is stable at 1-2 and does not decrease for 3-5 minutes, it indicates that the replacement is complete. The reaction equations for the regeneration process are: R-SO3Na+HCl→R-SO3H+NaCl, R-SO3Li+HCl→R-SO3H+LiCl.
4. The method for harmless disposal and recycling according to claim 1, characterized in that, A pretreatment step is performed before the neutralization step, the pretreatment step including: The lithium-containing waste liquid is filtered through a filter screen with a pore size of 0.3-0.8 mm.
5. The method for harmless disposal and recycling according to claim 1, characterized in that, The lithium in the lithium-containing waste liquid comes from the pure waste material remaining in the mold during the smelting and casting of lithium metal in an oxygen-free and water-free environment. This waste material is placed in pure water and reacted completely to obtain a strongly alkaline lithium hydroxide solution without obvious impurities.
6. The method for harmless disposal and recycling according to claim 1, characterized in that, In the neutralization step, the concentration of the hydrochloric acid solution is 1.5-2.5 mol / L.
7. The method for harmless disposal and recycling according to claim 1, characterized in that, In the precipitation step, the actual amount of sodium carbonate added is calculated using the following method: m(Na2CO3) 理论 =1 / 2×c(LiOH)×V(LiOH)×105.99 m(Na2CO3) 实际 =(1~1.1)×m(Na2CO3) 理论 。 8. The method for harmless disposal and recycling according to claim 1, characterized in that, In the solid-liquid separation step, the filtration pressure of the plate and frame filter press is 0.6 MPa.
9. The method for harmless disposal and recycling according to claim 1, characterized in that, The evaporation and crystallization step includes: The NaCl filtrate was concentrated by vacuum evaporation, with the vacuum level controlled at -0.08 MPa and the temperature at 60-65℃, to remove water from the filtrate and obtain NaCl crystals. The Li2CO3 filter residue was washed with water, recrystallized, and dried.
10. A harmless treatment and recycling device for lithium-containing waste liquid, characterized in that, It includes a filter, a neutralization tank, a sedimentation tank, a plate and frame filter press, a preliminary filtrate collection tank, and an ion exchange column connected in sequence; The filter is located at the inlet of the neutralization tank and is equipped with a filter screen inside to remove suspended impurities and large particles from the lithium-containing waste liquid. The neutralization tank is used to receive lithium-containing waste liquid from the filter. The neutralization tank is equipped with a stirring mechanism, and hydrochloric acid solution is introduced into the neutralization tank to carry out a neutralization reaction. The sedimentation tank is used to treat the neutralized solution. The tank is equipped with a stirring mechanism. Sodium carbonate powder is slowly added to fully dissolve it and react with lithium ions to generate lithium carbonate precipitate. The plate and frame filter press is used for solid-liquid separation of a mixture from a sedimentation tank; The preliminary filtrate collection tank is used to collect the preliminary NaCl filtrate after separation by the plate and frame filter press. The ion exchange column is used to adsorb lithium ions from the NaCl preliminary filtrate in the preliminary filtrate collection tank.