A low-lead frit and glaze for architectural glazed tiles and their applications
By adjusting the low-lead frit formula and glaze composition, and regulating the thermal expansion properties, the problem of high gloss and color consistency of glaze at low temperatures is solved, achieving the traditional effect of low-lead glazed products, which is suitable for the production of architectural glazed products.
Patent Information
- Application Number
- CN202611127763.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-28
- Publication Date
- 2026-11-17
AI Technical Summary
Existing low-lead or lead-free glass glazes are difficult to maintain high gloss and the color effect of traditional architectural glazed tiles under low-temperature firing conditions, and the glaze color tone is inconsistent, which cannot meet the process requirements of traditional glazed products.
The formula uses a low-lead frit, which contains components such as SiO2, PbO, MgO, K2O, BaO, ZnO, Al2O3, B2O3, CaO and Na2O. By adjusting the melting temperature and thermal expansion properties, the glaze surface is ensured to have high gloss and traditional ice crackle effect at low temperatures. Suzhou clay and quartz are used to adjust the thermal expansion properties of the glaze layer to match the body.
Under low-temperature firing conditions, it achieves high gloss and the continuation of traditional glass colors, reduces lead content by more than 50%, maintains the traditional glaze texture, and is suitable for the production process of traditional glass products without the need to modify kiln equipment.
Smart Images

Figure CN123105992A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of glass processing technology, and in particular to a low-lead frit and glaze for architectural glass and their applications. Background Technology
[0002] Architectural glazed tiles, with their unique artistic effect of shimmering brilliance and resplendent gold, have become a treasure of traditional Chinese architectural culture. Their craftsmanship is listed as a national intangible cultural heritage, with the official glazed tiles used in royal buildings such as the Forbidden City in Beijing being particularly representative. The bright and translucent colors of architectural glazed tiles originate from traditional high-lead glazes, with a lead oxide (PbO) content as high as 60-70%. Utilizing the high refractive index and low melting point of PbO, the glaze surface is endowed with high gloss and vibrant colors, encompassing yellow, green, blue, black, and white hues, with yellow-green being the most prevalent. Currently, architectural glazed tile restoration and cultural and creative products still use traditional high-lead glazes to preserve the original colors. However, lead is a heavy metal element, and long-term exposure to the outdoor environment, including acid rain and industrial waste gas, poses a risk of lead leaching, which can threaten human health and the environment.
[0003] To overcome the aforementioned shortcomings, those skilled in the art have proposed various low-lead or lead-free technical solutions, but none of them can meet the process and appearance requirements of traditional architectural glazed tiles. Common defects in existing technologies include: low-temperature lead-free glaze systems typically require the introduction of alkali metal or alkaline earth metal oxides to replace PbO, resulting in a significant decrease in glaze gloss and an inability to achieve the high-gloss mirror effect of traditional glazed tiles; while some lead-free glazes can achieve high gloss, their firing temperatures are generally as high as around 1200℃, far exceeding the 900℃ low-temperature firing system of traditional lead glazes, making them unsuitable for direct adaptation to existing glazed tile production processes and kiln equipment, and significantly increasing energy consumption. Furthermore, existing low-lead glaze technical solutions lack systematic formula design for the most representative main color systems of traditional architectural glazed tiles—bright yellow and emerald green—resulting in glaze tones that are generally too light, grayish, or lack sufficient color saturation, failing to achieve the continuity and uniformity of traditional official glazed tile colors. Therefore, developing an architectural glaze material that combines low lead content, high gloss, pure yellow-green color, and good adaptability to body and glaze under low-temperature firing conditions is a technical problem that urgently needs to be solved in this field. Summary of the Invention
[0004] To address the aforementioned problems in the prior art, this invention provides a low-lead frit and glaze for architectural glazed tiles and their applications.
[0005] The present invention specifically adopts the following technical solution: In a first aspect, the present invention provides a low-lead frit for architectural glazed tiles, the low-lead frit comprising a base material, a coloring flux, and an expansion regulator in a mass ratio of (65-77):(12-17):(8-18); the base material, in addition to SiO2 and PbO, also comprises MgO, K2O, BaO, and ZnO; the coloring flux is composed of Al2O3 and B2O3; the expansion regulator is composed of CaO and Na2O; and the PbO content in the low-lead frit is not higher than 30%wt.
[0006] In the base material, silicon dioxide (SiO2) and PbO are essential components. SiO2 forms a silicon-oxygen tetrahedral network framework, endowing the glaze with mechanical strength and chemical stability; PbO enters the interstices of the framework in the form of network exosomes, and its high polarizability reduces the melt viscosity and surface tension, enabling the glaze to obtain a high refractive index and specular gloss under low-temperature firing conditions. In addition, magnesium oxide (MgO), potassium oxide (K2O), barium oxide (BaO), and zinc oxide (ZnO) are also introduced into the base material as auxiliary components. Among them, MgO and K2O regulate the high-temperature rheological properties during the melting process within the base material, while BaO and ZnO help maintain the refractive index of the glaze from an optical perspective.
[0007] In the coloring flux, boron trioxide (B2O3) replaces part of SiO2 as a glass network forging body to lower the melting temperature; aluminum trioxide (Al2O3) enters the network gaps as an intermediate oxide to improve the chemical stability and corrosion resistance of the glaze layer to inhibit lead ion dissolution, while constraining the high-temperature fluidity of the melt to avoid glaze flow defects.
[0008] In the expansion regulator, sodium oxide (Na2O) acts as a strong fluxing component to compensate for the decrease in fluidity caused by the reduction of PbO, while calcium oxide (CaO) works in conjunction with Na2O. The difference in their coefficients of thermal expansion regulates the overall thermal expansion behavior of the glaze layer, keeping the difference between the body and glaze expansion coefficients within a suitable range. This ensures that the density, depth, and distribution pattern of the glaze cracks after firing are essentially consistent with traditional products, preserving the unique ice-crack texture of traditional architectural glazed tiles. If the difference in the body and glaze expansion coefficients is too large, resulting in cracks that are too deep or too shallow, it will alter the glaze texture characteristics of traditional glazed tiles and cause them to lose their original artistic effect. Through the above adjustments, this invention achieves the continuation of the traditional ice-crack effect while reducing lead content, ensuring that the appearance and texture of low-lead glazed tiles are highly consistent with traditional products.
[0009] The base material provides the glass network and gloss foundation, the coloring flux enables low-temperature melting and uniform coloring of Fe2O3, and the expansion regulator ensures the thermal expansion of the body and glaze are compatible. Together, these three elements achieve the high gloss, bright yellow tone, and low-temperature firing effect of traditional architectural glazed tiles under low-lead conditions.
[0010] According to the present invention, a low-lead frit preferably comprises, by weight, 30-36 parts SiO2, 2-5 parts MgO, 3-6 parts K2O, 24-29 parts PbO, 1-3 parts BaO and 0.85-2.95 parts ZnO; the coloring flux is composed of 1-5 parts Al2O3 and 10-15 parts B2O3; and the expansion regulator is composed of 3-8 parts CaO and 5-10 parts Na2O.
[0011] According to the present invention, a low-lead frit is preferably provided in which the PbO content is 24%wt to 30%wt.
[0012] More preferably, in the low-lead frit, the content of SiO2 is 30%wt to 36%wt, the content of MgO is 2%wt to 5%wt, the content of K2O is 3%wt to 6%wt, the content of PbO is 24%wt to 29%wt, the content of BaO is 1%wt to 3%wt, the content of ZnO is 0.85%wt to 2.95%wt, the content of Al2O3 is 1%wt to 5%wt, the content of B2O3 is 10%wt to 15%wt, the content of CaO is 3%wt to 8%wt, and the content of Na2O is 5%wt to 10%wt.
[0013] In this invention, the components of the low-lead frit are calculated as oxides, and their core composition range is not limited by the form of raw material source. Those skilled in the art can select pure chemical reagents, natural mineral raw materials, or a combination of both as the source of each oxide, depending on actual production conditions. As long as the oxide composition of the final frit falls within the range defined by this invention, the same technical effect can be achieved. For example, SiO2 can be introduced from raw materials such as quartz powder, silica sol, or tetraethyl orthosilicate; Al2O3 can be introduced from aluminum-containing minerals such as industrial alumina, feldspar, and kaolin; PbO can be introduced from red lead powder, lead oxide, lead silicate, or other lead-containing compounds; Na2O, K2O, CaO, MgO, BaO, ZnO, and B2O3 can also be introduced from corresponding carbonates, nitrates, borates, or natural mineral raw materials. Regardless of the form of raw materials used, any low-lead frit prepared within the oxide composition range described in this invention falls within the protection scope of this invention.
[0014] Secondly, the present invention also provides a method for preparing a low-lead frit for any of the architectural glazed tiles, comprising: melting all raw materials including the base material, the coloring flux and the expansion regulator, and cooling; the melting temperature is 1200℃~1250℃.
[0015] According to any of the low-lead frit preparation methods provided by the present invention, preferably, the cooling method includes: quenching in water to form a frit, thereby obtaining the low-lead frit.
[0016] More preferably, after quenching, the resulting low-lead frit is dried.
[0017] More preferably, the preparation method further includes: grinding the obtained low-lead frit and sieving it.
[0018] More preferably, it passes through a 140-180 mesh sieve.
[0019] Even more preferably, it is passed through a 160-mesh sieve.
[0020] Thirdly, the present invention also provides a glaze for architectural glazed tiles, wherein the raw materials of the glaze include any of the aforementioned low-lead frits, as well as mineral raw materials and coloring raw materials; the average coefficient of thermal expansion of the glaze at 100℃ to 500℃ is 5.0 × 10⁻⁶. -6 / ℃~7.0×10 -6 / ℃. In this invention, the expansion coefficient is measured using QB / T 1321-2012 "Method for Determining the Average Linear Thermal Expansion Coefficient of Ceramic Materials".
[0021] More preferably, the glaze has an average coefficient of thermal expansion of 5.8 × 10⁻⁶ at temperatures between 100°C and 500°C. -6 / ℃~6.2×10 -6 / ℃.
[0022] According to the glaze material for architectural glazed tiles provided by the present invention, preferably, the content of the low-lead frit in the raw materials of the glaze material is 80%wt to 98%wt.
[0023] More preferably, the mass ratio of the low-lead frit, the mineral raw material and the coloring raw material is (82-97):(2-13):(1.5-6).
[0024] According to the glaze for architectural glazed tiles provided by the present invention, preferably, the mineral raw materials are selected from any one or more of Suzhou clay, quartz, albite and talc.
[0025] Suzhou clay is a high-quality kaolin with extremely fine particles. When added to glaze, it effectively suspends heavier particles such as frit powder and quartz, preventing glaze slurry sedimentation. It also enhances the adhesion between the glaze layer and the body, preventing scratches or peeling of the glaze surface after drying. Furthermore, the Al2O3 introduced by Suzhou clay enters the gaps in the glass network, improving the chemical stability and mechanical strength of the glaze layer.
[0026] During the high-temperature melting process, quartz enters the glass network, forming the main skeleton structure of the glaze layer, which can improve the mechanical strength, hardness and chemical resistance of the glaze layer. At the same time, after quartz melts into glass, it can effectively reduce the thermal expansion coefficient of the glaze, which plays a key role in adjusting the difference between the expansion coefficients of the body and the glaze to a suitable range. This ensures that the density, depth and distribution of cracks on the glaze surface after firing are consistent with traditional products, thus continuing the unique ice crack texture of traditional architectural glazed tiles.
[0027] Suzhou clay and quartz complement each other in the glaze. Suzhou clay provides suspension and glaze strength, while quartz regulates the high-temperature rheological behavior and thermal expansion characteristics of the glaze layer. The two work synergistically within their respective appropriate dosage ranges, together with low-lead frit, to form a complete glaze composition.
[0028] More preferably, the mineral raw material is composed of Suzhou clay and quartz in a mass ratio of (1-5):(1-9).
[0029] More preferably, when the glaze is a yellow glaze, the mineral raw materials are composed of Suzhou clay and quartz in a mass ratio of (3-5):(5-9).
[0030] More preferably, when the glaze is a green glaze, the mineral raw materials are composed of Suzhou clay and quartz in a mass ratio of (1-4):(1-9).
[0031] According to the glaze for architectural glazed tiles provided by the present invention, preferably, the coloring raw material is selected from any one or more of Fe2O3, CuO, Cr2O3, CoO and MnO.
[0032] More preferably, when the glaze is a yellow glaze, the coloring raw material is Fe2O3.
[0033] More preferably, when the glaze is a yellow glaze, the raw materials of the glaze include 81%wt to 89%wt of the low-lead frit, 3%wt to 5%wt of Suzhou clay, 5%wt to 9%wt of quartz and 3%wt to 6%wt of Fe2O3.
[0034] More preferably, when the glaze is a green glaze, the coloring raw materials are Cr2O3, CoO and Fe2O3.
[0035] More preferably, when the glaze is a green glaze, the raw materials of the glaze include 83%wt to 94%wt of the low-lead frit, 1%wt to 3.5%wt of Suzhou clay, 1%wt to 8.7%wt of quartz, 3.5%wt to 4.5%wt of CuO, 0.2%wt to 0.5%wt of Cr2O3 and 0.01%wt to 0.25%wt of Fe2O3.
[0036] Fourthly, the present invention also provides the application of any of the glazes described herein in the preparation of architectural glazed products. The architectural glazed products include, but are not limited to, tile components such as flat tiles, barrel tiles, drip tiles, and hook tiles; ridge components such as ridge beams, hip ridges, gable ridges, and antique ridges; and decorative components such as roof ornaments, animal figures, and finials. They also include glazed bricks, glazed windows, glazed railings, and other products used for wall or courtyard decoration. All of the above products can be glazed and fired using the low-lead glazes described herein.
[0037] Fifthly, the present invention also provides an architectural glazed tile, comprising a tile blank and a glaze, wherein the glaze of the architectural glazed tile is any of the glazes used in architectural glazing.
[0038] The difference in thermal expansion between the glaze and the body during firing and cooling is a key factor determining whether the glaze will crack or peel. Traditional architectural glazed products are characterized by their unique crackle-like texture, which stems from the specific difference in the coefficients of thermal expansion between the glaze and the body. When there is an appropriate difference between the coefficients of thermal expansion of the glaze and the body, the glaze shrinks slightly more during cooling than the body, causing the glaze to bear tensile stress and produce uniform and fine network cracks, forming the unique crackle texture of traditional glazed glass. The low-lead glaze provided by this invention controls the difference in the coefficients of thermal expansion between the body and the glaze within a suitable range, ensuring that the density, depth, and distribution of cracks on the glaze surface after firing are consistent with traditional products, without peeling due to excessive stress. Thus, it reduces the lead content while maintaining the unique crackle-like effect of traditional architectural glazed glass.
[0039] According to the present invention, the glazed tile for building construction preferably has an average coefficient of thermal expansion of 2.0 × 10⁻⁶ at 100℃ to 500℃. -6 / ℃~4.0×10 -6 / ℃. Within this range, the glaze provided by the present invention produces a glaze surface with fine, uniform, non-penetrating, and non-flaking ice cracks, and also has high flexural strength and thermal stability.
[0040] The present invention also provides a method for preparing the glazed tile, comprising: applying glaze to the tile blank with any of the glazes, and firing the glaze at 900℃ to 1000℃.
[0041] Preferably, the glaze is fired at 970℃ to 990℃.
[0042] More preferably, the glaze is fired at 980°C.
[0043] The present invention has the following beneficial effects: This invention achieves a significant reduction in lead content (by more than 50%) without altering the traditional glazing process, enabling traditional high-lead glazes to retain their original process adaptability while acquiring green and environmentally friendly properties. Simultaneously, the resulting low-lead glaze exhibits high consistency with traditional high-lead glaze products in terms of glaze color, gloss, and crackle effect, with a color difference ΔE < 5 and a gloss difference < 10%, achieving visual equivalence. The technical solution provided by this invention can be directly applied to traditional architectural glazed tile production processes without modifying existing kiln equipment and glazing procedures, thus preserving the original essence of ancient techniques. It is suitable for the restoration of ancient architectural glazed tile artifacts and the development of new products, providing a new technological option for the protection and inheritance of architectural glazed tile intangible cultural heritage. Attached Figure Description
[0044] To more clearly illustrate the technical solutions in this invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of this invention. For those skilled in the art, other drawings can be obtained from these drawings without creative effort.
[0045] Figure 1 These are comparative images of the finished products after firing, showing the yellow and green glazes prepared by applying the low-lead frit of Example 1 to the glazed tile blanks provided by this invention, and the yellow and green glazes prepared by conventional glazes. Detailed Implementation
[0046] To make the objectives, technical solutions, and advantages of this invention clearer, the technical solutions of this invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some, not all, of the embodiments of this invention. All other embodiments obtained by those skilled in the art based on the embodiments of this invention without creative effort are within the scope of protection of this invention.
[0047] Unless otherwise specified, the experimental methods involved in the following embodiments are conventional methods in the art. For example, you can refer to the experimental manual in the art or follow the conditions recommended in the manufacturer's instructions.
[0048] Unless otherwise specified, all experimental materials and reagents used in the following examples are commercially available.
[0049] Example 1: A method for preparing low-lead frit and glaze for architectural glazed tiles. 1. Preparation of low-lead frit (1) Formula The low-lead frit provided in this embodiment contains a base material, a coloring flux, and an expansion regulator in a mass ratio of 72:15.9:12.
[0050] By weight, the base material consists of 33.88 parts SiO2, 1.48 parts MgO, 4.62 parts K2O, 29.14 parts PbO, 1.88 parts BaO, and 1.00 parts ZnO; the coloring flux consists of 2.25 parts Al2O3 and 13.65 parts B2O3; and the expansion regulator consists of 5.16 parts CaO and 6.84 parts Na2O.
[0051] (2) Preparation method Weigh out each raw material according to the formula, mix them evenly, and then melt them in a high-temperature frit furnace at a melting temperature of 1230℃. After that, quench them in water to form a transparent frit, dry them, and then dry ball mill them using a high-speed ball mill. After passing them through a 160-mesh sieve, low-lead frit is obtained.
[0052] 2. Preparation of glaze (1) Formula By weight percentage, the yellow glaze consists of: 82.33% low-lead frit, 3.46% Suzhou clay, 8.55% quartz, and 5.66% Fe2O3.
[0053] By weight percentage, the green glaze consists of: 83.08% low-lead frit, 3.46% Suzhou clay, 8.65% quartz, 4.33% CuO, 0.26% Cr2O3, and 0.22% Fe2O3.
[0054] (2) Preparation method Weigh each raw material according to the formula, mix them evenly, and then use a high-speed ball mill for wet ball milling to obtain glaze slurry.
[0055] Example 2: A method for preparing low-lead frit and glaze for architectural glazed tiles. 1. Preparation of low-lead frit (1) Formula The low-lead frit provided in this embodiment contains a base material, a coloring flux, and an expansion regulator, with a mass ratio of 76.95:15:8.
[0056] By weight, the base material consists of 36 parts SiO2, 5 parts MgO, 6 parts K2O, 24 parts PbO, 3 parts BaO, and 2.95 parts ZnO; the coloring flux consists of 5 parts Al2O3 and 10 parts B2O3; and the expansion regulator consists of 3 parts CaO and 5 parts Na2O.
[0057] (2) Preparation method Weigh out each raw material according to the formula, mix them evenly, and then melt them in a high-temperature frit furnace at a melting temperature of 1250℃. After that, quench them in water to form a transparent frit, dry them, and then dry ball mill them using a high-speed ball mill. After passing through a 160-mesh sieve, a low-lead frit is obtained.
[0058] 2. Preparation of glaze (1) Formula By weight percentage, the yellow glaze consists of: 89% low-lead frit, 3% Suzhou clay, 5% quartz, and 3% Fe2O3.
[0059] By weight percentage, the green glaze consists of: 94% low-lead frit, 1% Suzhou clay, 1% quartz, 3.7% CuO, 0.29% Cr2O3, and 0.01% Fe2O3.
[0060] (2) Preparation method Weigh each raw material according to the formula, mix them evenly, and then use a high-speed ball mill for wet ball milling to obtain the glaze slurry.
[0061] Example 3: A method for preparing low-lead frit and glaze for architectural glazed tiles. 1. Preparation of low-lead frit (1) Formula The low-lead frit provided in this embodiment contains a base material, a coloring flux, and an expansion regulator, with a mass ratio of 65.85:16:18.0.
[0062] By weight, the base material consists of: 30 parts SiO2, 2 parts MgO, 3 parts K2O, 29 parts PbO, 1 part BaO, and 0.85 parts ZnO; the coloring flux consists of: 1 part Al2O3 and 15 parts B2O3; and the expansion regulator consists of: 8 parts CaO and 10 parts Na2O.
[0063] (2) Preparation method Weigh each raw material according to the formula, mix them evenly, and then melt them in a high-temperature frit furnace at a melting temperature of 1200℃. After that, quench them in water to form a transparent frit, dry them, and then dry ball mill them using a high-speed ball mill. After passing them through a 160-mesh sieve, low-lead frit is obtained.
[0064] 2. Preparation of glaze (1) Formula By weight percentage, the yellow glaze consists of: 81% low-lead frit, 5% Suzhou clay, 8% quartz, and 6% Fe2O3.
[0065] By weight percentage, the green glaze consists of: 90.5% low-lead frit, 2% Suzhou clay, 2.5% quartz, 4.5% CuO, 0.45% Cr2O3, and 0.05% Fe2O3.
[0066] (2) Preparation method Weigh each raw material according to the formula, mix them evenly, and then use a high-speed ball mill for wet ball milling to obtain the glaze slurry.
[0067] Comparative Example 1: A method for preparing low-lead frit and glaze for architectural glazed tiles. 1. Preparation of low-lead frit (1) Formula The low-lead frit provided in this comparative example has the same frit composition as that in Example 5 of the prior art CN101851119A, namely, according to the chemical composition percentages: SiO2 41.8%, Al2O3 7.8%, TiO2 1.5%, CaO 0.8%, MgO 0.6%, K2O 2.0%, Na2O 3.0%, PbO 18.5%, BaO 6.0%, ZnO 4.5%, Li2O 1.5%, and B2O3 12.0%.
[0068] (2) Preparation method The preparation method is the same as that of the low-lead frit in Example 3.
[0069] 2. Preparation of glaze (1) Formula The formulation is the same as that of the glaze in Example 3.
[0070] (2) Preparation method The preparation method is the same as that of the glaze in Example 3.
[0071] Comparative Example 2: A method for preparing low-lead frit and glaze for architectural glazed tiles. 1. Preparation of low-lead frit (1) Formula The low-lead frit provided in this comparative example has the same frit composition as that in Example 1 of the prior art CN102276149A, namely, by mass percentage: 15.0% feldspar, 16.0% quartz, 20.2% red lead powder, 20.0% lepidolite, 4.0% borax, 3.3% boric acid, 1.5% CaCO3, 1.5% MgCO3, 11.0% BaCO3, 1.5% TiO2, 2.0% Al(OH)3 and 4.0% ZnO.
[0072] (2) Preparation method The preparation method is the same as that of the low-lead frit in Example 3.
[0073] 2. Preparation of glaze (1) Formula The formulation is the same as that of the glaze in Example 3.
[0074] (2) Preparation method The preparation method is the same as that of the glaze in Example 3.
[0075] Comparative Example 3: A method for preparing low-lead frit and glaze for architectural glazed tiles. 1. Preparation of low-lead frit (1) Formula The difference between the low-lead frit provided in this comparative example and Example 3 is only that the proportion of base material in the composition of the low-lead frit is reduced. The mass ratio of base material, coloring flux, and expansion regulator is 64.51:18.35:16.99, that is, by weight, the components of the base material are: 31.93 parts SiO2, 1.29 parts MgO, 3.23 parts K2O, 25.80 parts PbO, 1.29 parts BaO, and 0.97 parts ZnO; the components of the coloring flux are: 3.42 parts Al2O3 and 14.93 parts B2O3; and the components of the expansion regulator are: 7.06 parts CaO and 9.93 parts Na2O.
[0076] (2) Preparation method The preparation method is the same as that of the low-lead frit in Example 3.
[0077] 2. Preparation of glaze (1) Formula The formulation is the same as that of the glaze in Example 3.
[0078] (2) Preparation method The preparation method is the same as that of the glaze in Example 3.
[0079] Comparative Example 4: A method for preparing low-lead frit and glaze for architectural glazed tiles. 1. Preparation of low-lead frit (1) Formula The only difference between this comparative example and Example 3 is that the proportion of base material in the low-lead frit composition is increased. The mass ratio of base material, coloring flux, and expansion regulator is 78:13.89:8. That is, by weight, the base material consists of: 39 parts SiO2, 1.95 parts MgO, 5.07 parts K2O, 28.47 parts PbO, 1.95 parts BaO, and 1.56 parts ZnO; the coloring flux consists of: 1.4 parts Al2O3 and 12.49 parts B2O3; and the expansion regulator consists of: 3.0 parts CaO and 5 parts Na2O.
[0080] (2) Preparation method The preparation method is the same as that of the low-lead frit in Example 3.
[0081] 2. Preparation of glaze (1) Formula The formulation is the same as that of the glaze in Example 3.
[0082] (2) Preparation method The preparation method is the same as that of the glaze in Example 3.
[0083] Evaluation of glaze firing effect of glazed tile blanks in test example 1. Glazing and firing of glazed tile blanks The glaze slurries prepared in Examples 1-3 and Comparative Examples 1-4, respectively, were compared with the average coefficient of thermal expansion α of the same batch of glazed tile blanks (100℃-500℃). 平均 2.0×10 -6 / ℃~4.0×10 -6 After glazing at 980℃, the glaze is fired at 980℃ to obtain glazed tiles.
[0084] Traditional glazes (yellow glaze composition: SiO2 30%, PbO 62%, Al2O3 2.5%, Fe2O3 5%, other 0.5%; green glaze composition: SiO2 30%, PbO 61%, Al2O3 3.5%, CuO 5%, other 0.5%) were used as a control.
[0085] 2. Determination of the coefficient of thermal expansion of glaze Referring to the method in QB / T 1321-2012 "Method for Determination of Average Linear Thermal Expansion Coefficient of Ceramic Materials", the expansion coefficient of the glaze slurries prepared in Examples 1-3 and Comparative Examples 1-4, as well as the glaze products fired with traditional glazes, was tested using a thermal expansion meter.
[0086] 3. Appearance measurement Following the method in GB / T 4739-2015 "Determination of Colorimetric Properties of Daily-Use Ceramic Pigments", the colorimetric properties of each glazed tile after glazing and firing were measured using a colorimeter. The results are expressed in the CIE Lab color space, where L* value represents lightness (higher values indicate brighter colors), a* value represents the red-green axis (positive values for red, negative values for green), and b* value represents the yellow-blue axis (positive values for yellow, negative values for blue). These values allow for the precise calculation of the color difference (ΔE) between two colors, used to assess color consistency.
[0087] Referring to the method in GB / T 11420-2024 "Test Method for Gloss of Enamel Products and Enamel Glaze", the gloss of each glazed tile after glazing was tested using a gloss meter at an incident angle of 60°.
[0088] In addition, the cracking of the glaze surface of each glazed tile after glazing was observed and recorded.
[0089] 4. Measurement Results like Figure 1As shown, the glazed tiles prepared from the low-lead frit of Example 1 and the glaze slurry prepared with conventional glazes are basically identical in appearance after firing, including similar ice crack patterns. The glaze color and gloss are indistinguishable from those of glazed tiles prepared with conventional glazes to the naked eye. The glazed tiles prepared from the low-lead frit of Examples 2 and 3 also have similar appearances after firing.
[0090] Table 1. Glazing effect of yellow glaze and glazed tile blanks
[0091] Table 1 shows the performance of the yellow glaze and its glazed tile blanks. The glaze products prepared with low-lead frit in Examples 1-3 have expansion coefficients that are basically equivalent to those of traditional glazes. The color difference ΔE of the glazed tiles after firing is all <5, the gloss is significantly improved with a difference of <10%, and the glaze surface properties are consistent. The glaze products prepared with frit in Comparative Examples 1 and 2 have expansion coefficients that are significantly higher than those of traditional glazes. The thermal expansion of the body and glaze is unbalanced, and the cracks change from fine and fragmented to deep and long. The color difference ΔE of L* and a* is both >5, and the gloss is significantly reduced. Although the glaze surface remains transparent, the yellow color is significantly deepened. The glaze products prepared with frit in Comparative Examples 3 and 4 have expansion coefficients that are basically equivalent to those of traditional glazes, and the crack state of the glaze surface is basically consistent. However, due to the excessively high or low proportion of the base material, the color difference ΔE of the glazed tiles after firing is all >5, and the gloss is significantly reduced. The glaze surface is cloudy, and the color deviates significantly from true yellow.
[0092] Table 2. Glazing effect of green glaze and glazed tile blanks
[0093] Table 2 shows the performance of the green glaze and its glazed tile blanks. The glaze products prepared by the low-lead frit in Examples 1 to 3 have a coefficient of thermal expansion that is basically the same as that of traditional glazes. The color difference ΔE of the glazed tiles after firing is all <5, and the gloss is basically the same (difference <10%), with consistent glaze properties. The glaze product prepared by the frit in Comparative Example 1 has a significantly higher coefficient of thermal expansion than traditional glazes, with deep and long cracks. At the same time, the color and gloss are significantly reduced, and the glaze surface is obviously cloudy. The glaze product prepared by the frit in Comparative Example 2 has a significantly higher coefficient of thermal expansion than traditional glazes, with deeper cracks, and significantly reduced color and gloss, with the gloss even decreasing by 25.89%. The glaze surface is no longer transparent. The glaze products prepared by the frit in Comparative Examples 3 and 4 have a coefficient of thermal expansion that is basically the same as that of traditional glazes, and the crack state of the glaze surface is basically the same. However, due to the excessively high or low proportion of the base material, the color-developing environment of CuO, Cr2O3, and Fe2O3 is destroyed, resulting in a significantly lighter color.
[0094] Based on the above test results, the low-lead frits of Examples 1 to 3 of this invention have achieved the reproduction of the traditional glaze firing effect for both yellow and green glazes. However, the frits of Comparative Examples 1 to 4 have failed to stably reproduce the traditional glaze firing effect for both yellow and green glazes. Under visual observation, the fired glazed tiles show significant differences in color, gloss, and cracks compared to glazed tiles fired with traditional glazes.
[0095] The above results show that the low-lead frits of Examples 1 to 3 of the present invention achieve a good balance between glaze color, gloss, transparency and body-glaze adaptability, meet the comprehensive requirements of glazed tiles for glaze appearance and sintering performance, and can directly reproduce the firing effect of traditional glazes under traditional firing processes.
[0096] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them; although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A low-lead frit for architectural glazed tiles, characterized in that, The low-lead frit contains a base material, a coloring flux, and an expansion regulator in a mass ratio of (65-77):(12-17):(8-18); In addition to SiO2 and PbO, the base material also contains MgO, K2O, BaO and ZnO; The coloring flux is composed of Al2O3 and B2O3; The swelling regulator is composed of CaO and Na2O; The PbO content in the low-lead frit is no higher than 30%wt.
2. The low-lead frit according to claim 1, characterized in that, By weight, the base material comprises 30 to 36 parts SiO2, 2 to 5 parts MgO, 3 to 6 parts K2O, 24 to 29 parts PbO, 1 to 3 parts BaO and 0.85 to 2.95 parts ZnO; The coloring flux is composed of 1 to 5 parts of Al2O3 and 10 to 15 parts of B2O3; The swelling regulator is composed of 3 to 8 parts CaO and 5 to 10 parts Na2O.
3. The low-lead frit according to claim 1 or 2, characterized in that, The low-lead frit contains 24%wt to 30%wt of PbO.
4. A method for preparing a low-lead frit as described in any one of claims 1 to 3, characterized in that, include: All raw materials, including the base material, the coloring flux, and the expansion regulator, are melted and then cooled. The melting temperature is 1200℃~1250℃.
5. A glaze for architectural glazed tiles, characterized in that, The raw materials for the glaze include the low-lead frit as described in any one of claims 1 to 3, as well as mineral raw materials and coloring raw materials; The average coefficient of thermal expansion of the glaze at temperatures ranging from 100℃ to 500℃ is 5.0 × 10⁻⁶. -6 / ℃~7.0×10 -6 / ℃.
6. The glaze according to claim 5, characterized in that, The content of the low-lead frit in the raw materials of the glaze is 80%wt to 98%wt.
7. The glaze according to claim 6, characterized in that, The mass ratio of the low-lead frit, the mineral raw material, and the coloring raw material is (82-97):(2-13):(1.5-6). Preferably, the mineral raw material is selected from any one or more of Suzhou clay, quartz, albite, and talc; Preferably, the coloring material is selected from any one or more of Fe2O3, CuO, Cr2O3, CoO and MnO.
8. The use of the glaze according to any one of claims 5 to 7 in the preparation of architectural glazed products.
9. A type of glazed tile for building construction, comprising a tile blank and a glaze, characterized in that, The glaze used for the glazed tiles is the glaze described in any one of claims 5 to 7.
10. The glazed tile for building construction according to claim 9, characterized in that, The average coefficient of thermal expansion of the tile blank at temperatures ranging from 100℃ to 500℃ is 2.0 × 10⁻⁶. -6 / ℃~4.0×10 -6 / ℃.
Citation Information
Patent Citations
Glazing resintering technology of unglazed ancient colored glaze components
CN101851119A
A method for preparing an antique-style glass frit glaze
CN102276149A