- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-18
- Publication Date
- 2026-11-17
AI Technical Summary
Glass substrates are prone to cracking during reflow soldering, leading to product scrap, and existing technologies are unable to effectively solve this problem.
An improved reflow soldering process is employed, which includes steps such as preheating, isothermal control, reflow soldering, stress relief during heat preservation, and cooling zone. By gradually controlling the temperature and releasing the internal stress of the glass substrate, the risk of cracking is reduced.
It significantly reduces the defect rate of glass substrate cracks, improves the product packaging yield to 98.5%, and meets the MSL3 level test requirements.
Smart Images

Figure CN123106022A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of electronic module packaging technology, specifically to a method and reflow soldering equipment for preventing cracks in glass substrates during reflow soldering. Background Technology
[0002] The pace of product updates and replacements in today's consumer electronics is accelerating, with product designs increasingly focused on precision, miniaturization, and compactness. Many control modules utilize packaging technologies, and these packages integrate various functional blocks, employing multiple interconnecting boards. While silicon substrates are currently the mainstream material for these boards, glass substrates have gained increasing popularity in recent years due to their low dielectric loss, excellent thermal stability, chemical stability, and environmental friendliness. The thermal expansion coefficient of glass substrates is close to that of the components themselves, helping to reduce the risk of chip breakage and deformation under thermal changes. Furthermore, glass substrates possess ultra-flat properties, allowing for more precise etching and increasing circuit density per unit area.
[0003] However, glass substrates are prone to cracking during the packaging process due to improper internal stress release paths. This is a fatal quality defect that can lead to the direct scrapping of products. Temperature changes during the reflow soldering process are the main cause of cracking in glass substrates. Therefore, it is necessary to improve the current reflow soldering process to increase the yield of glass substrates. Summary of the Invention
[0004] To address the problems in the prior art, this invention provides a method and reflow soldering equipment for preventing cracks in glass substrates during reflow soldering, which can release the internal stress of the glass after heating and reduce the risk of cracks in the glass substrate.
[0005] The method for preventing cracks during reflow soldering of glass substrates according to the present invention includes the following steps: S1: The glass substrate to be soldered is sent into the preheating zone of the reflow soldering equipment, and the glass substrate is gradually preheated to the first temperature range to evaporate the solvent in the solder paste. S2: The preheated glass substrate is sent into the constant temperature zone of the reflow soldering equipment to balance the temperature of each area of the glass substrate and activate the flux. S3: After the temperature is balanced, the glass substrate is sent into the reflow soldering area to completely melt the solder paste in the area to be soldered on the glass substrate, and chemical bonding is formed between the areas to be soldered. S4: The welded glass substrate is sent into the heat preservation and stress relief zone to release the internal stress of the glass substrate and at the same time achieve the crystallization and solidification of the weld joint. S5: The glass substrate with released internal stress is sent into the cooling zone to rapidly cool down the glass substrate and solder joints and then output to the next processing step.
[0006] Furthermore, the glass substrate is sequentially fed into each zone in steps S1-S5 via a conveyor belt at a speed of 75-85 cm / min.
[0007] Furthermore, in step S1, the preheating zone includes a first temperature zone, a second temperature zone, and a third temperature zone with increasing temperature gradient. The three temperature zones are arranged side by side, and each temperature zone includes an upper temperature zone located above the conveyor belt and a lower temperature zone located below the conveyor belt.
[0008] Furthermore, the set temperatures for the first, second, and third temperature zones are 130, 150, and 170°C, respectively.
[0009] Furthermore, the constant temperature zone includes a fourth temperature zone, a fifth temperature zone, a sixth temperature zone, and a seventh temperature zone with increasing temperature gradients. The four temperature zones are arranged in parallel, and the set temperature difference between the sixth temperature zone and the seventh temperature zone is less than 5-8℃.
[0010] Furthermore, the reflow soldering zone includes an eighth, ninth, and tenth temperature zone with an increasing temperature gradient. The three temperature zones are arranged side by side, with a temperature difference of 3-6℃ between adjacent temperature zones.
[0011] Furthermore, the heat preservation and stress relief zone includes an eleventh temperature zone and a twelfth temperature zone, the eleventh temperature zone and the twelfth temperature zone have the same temperature, and the temperature is lower than that of the reflow soldering temperature zone.
[0012] Furthermore, the cooling zone includes a thirteenth temperature zone and a fourteenth temperature zone, and a cooling structure is provided in the upper and lower temperature zones of the thirteenth and fourteenth temperature zones. The cooling structure is used to reduce the temperature of the glass substrate to room temperature.
[0013] The present invention also provides a reflow soldering device for preventing cracks in glass substrates, comprising a conveyor belt for transporting glass substrates, and a preheating zone, a constant temperature zone, a reflow soldering zone, a heat preservation and stress relief zone, and a cooling zone arranged sequentially along the conveyor belt transport direction. The preheating zone, constant temperature zone, reflow soldering zone, heat preservation and stress relief zone, and cooling zone are respectively provided with an upper temperature zone and a lower temperature zone, and the conveyor belt is disposed between the upper temperature zone and the lower temperature zone.
[0014] Furthermore, the outer surfaces of the preheating zone, constant temperature zone, reflow soldering zone, heat preservation and stress relief zone, and cooling zone are respectively provided with heat preservation structures to prevent heat leakage.
[0015] Compared with the prior art, the beneficial effects of the present invention are: after reflow soldering, the present invention does not enter the cooling zone for cooling, but adds a heat preservation and stress relief zone, realizing the crystallization of the solder joint and the heat preservation of the glass substrate within a certain temperature range, providing a buffer zone for the release of internal stress in the glass substrate, while not affecting the crystallization and solidification of the solder joint, reducing the internal stress of the glass substrate, greatly reducing the risk of cracks in the glass substrate, and maintaining the quality of the solder joint. Attached Figure Description
[0016] To more clearly illustrate the solutions in this invention or the prior art, the accompanying drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of this invention. For those skilled in the art, other drawings can be obtained from these drawings without creative effort.
[0017] Figure 1 This is a flowchart of the method for preventing cracks during reflow soldering of glass substrates according to the present invention; Figure 2 This is a schematic diagram of the reflow soldering equipment of the present invention. Detailed Implementation
[0018] Unless otherwise defined, all technical and scientific terms used in this invention have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains; the terminology used in this specification is for the purpose of describing particular embodiments only and is not intended to limit the invention; the terms "comprising" and "having," and any variations thereof, in the specification, claims, and foregoing drawings are intended to cover non-exclusive inclusion. The terms "first," "second," etc., in the specification, claims, or foregoing drawings are used to distinguish different objects, not to describe a particular order.
[0019] In this invention, the reference to "embodiment" means that a specific feature, structure, or characteristic described in connection with an embodiment may be included in at least one embodiment of the invention. The appearance of this phrase in various places in the specification does not necessarily refer to the same embodiment, nor is it a mutually exclusive, independent, or alternative embodiment to other embodiments. It will be explicitly and implicitly understood by those skilled in the art that the embodiments described in this invention can be combined with other embodiments.
[0020] To enable those skilled in the art to better understand the present invention, the technical solutions in the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings.
[0021] Preventing and controlling cracks in glass substrates, especially temperature changes, is the main cause of cracks in glass substrates. In the product packaging process, the temperature change occurs in the reflow soldering process. Therefore, this invention mainly addresses the technical problems by improving the reflow soldering process.
[0022] like Figure 1 As shown, the method for preventing cracks during reflow soldering of glass substrates according to the present invention includes the following steps: S1: The glass substrate to be soldered is sent into the preheating zone of the reflow soldering equipment, and the glass substrate is gradually preheated to the first temperature range to evaporate the solvent in the solder paste. S2: The preheated glass substrate is sent into the constant temperature zone of the reflow soldering equipment to balance the temperature of each area of the glass substrate and activate the flux. S3: After the temperature is balanced, the glass substrate is sent into the reflow soldering area to completely melt the solder paste in the area to be soldered on the glass substrate, and chemical bonding is formed between the areas to be soldered. S4: The welded glass substrate is sent into the heat preservation and stress relief zone to release the internal stress of the glass substrate and at the same time achieve the crystallization and solidification of the weld joint. S5: The glass substrate with released internal stress is sent into the cooling zone to rapidly cool down the glass substrate and solder joints and then output to the next processing step.
[0023] Preferably, the glass substrate is sequentially fed into each temperature zone in steps S1-S5 via a conveyor belt, and the speed of the conveyor belt is 75-85 cm / min.
[0024] like Figure 2 As shown, the present invention also provides a reflow soldering device for preventing cracks in glass substrates, including a conveyor belt for transporting glass substrates, and a preheating zone, a constant temperature zone, a reflow soldering zone, a heat preservation and stress relief zone, and a cooling zone arranged sequentially along the conveyor belt conveying direction. The preheating zone, constant temperature zone, reflow soldering zone, heat preservation and stress relief zone, and cooling zone are respectively provided with an upper temperature zone and a lower temperature zone, and the conveyor belt is arranged between the upper temperature zone and the lower temperature zone.
[0025] Preferably, the present invention employs a fourteen-temperature zone configuration. The preheating zone includes a first, second, and third temperature zone with an increasing temperature gradient, arranged side-by-side, with a temperature gradient of 20°C. The constant-temperature zone includes a fourth, fifth, sixth, and seventh temperature zone with an increasing temperature gradient, arranged side-by-side, with a set temperature difference of less than 5-8°C between the sixth and seventh temperature zones. The reflow soldering zone includes an eighth, ninth, and tenth temperature zone with an increasing temperature gradient, arranged side-by-side, with a temperature difference of 3-6°C between adjacent zones. In this example, the thermal insulation and stress-relieving zone includes an eleventh and twelfth temperature zone, with the same temperature, lower than the temperature of the reflow soldering zone. In this example, the cooling zone includes a thirteenth and fourteenth temperature zone, with cooling structures provided in the upper and lower temperature zones of the thirteenth and fourteenth temperature zones to reduce the temperature of the glass substrate to room temperature.
[0026] Preferably, the outer surfaces of the preheating zone, constant temperature zone, reflow soldering zone, heat preservation and stress relief zone, and cooling zone in this example are respectively provided with heat preservation structures to prevent heat leakage.
[0027] The temperature settings for each temperature zone in this example are shown in Table 1.
[0028] Table 1 Temperature settings for each zone of the reflow soldering equipment
[0029] The reflow soldering equipment of this invention is a reflow oven, and the temperature is mainly regulated by a controlled hot airflow, which can be hot air, steam, or nitrogen, etc. In this example, temperature-controlled nitrogen is preferably used to create an oxygen-free environment, effectively preventing soldering defects caused by solder oxidation.
[0030] As shown in Table 1, after the glass substrate is sent into the reflow oven, the temperature of the glass substrate gradually rises from the preheating zone to the reflow soldering zone to the highest point. If it is cooled directly from the highest temperature, it is easy to cause cracks in the glass substrate. The present invention innovatively improves the process and reflow soldering equipment. After reflow soldering, it does not enter the cooling zone for cooling, but adds a heat preservation and stress relief zone. This temperature can not only achieve solder crystallization, but also keep the glass substrate at a certain temperature range, giving the glass substrate a buffer zone for internal stress release, while not affecting the crystallization and solidification of the solder joint, reducing the internal stress of the glass substrate, greatly reducing the risk of cracks in the glass substrate, and maintaining the quality of the solder joint.
[0031] Through the optimization of this invention, the defect rate of glass substrate cracks is less than 0.5%, the yield rate of product packaging is greater than 98.5%, and the reliability of product packaging can pass the MSL3 level test.
[0032] The specific embodiments described above are preferred embodiments of the present invention and are not intended to limit the specific scope of the present invention. The scope of the present invention includes, but is not limited to, these specific embodiments. All equivalent changes made in accordance with the present invention are within the protection scope of the present invention.
Claims
1. A method of preventing cracks in a glass substrate reflow soldering, characterized by It includes the following steps: S1: The glass substrate to be soldered is sent into the preheating zone of the reflow soldering equipment, and the glass substrate is gradually preheated to the first temperature range to evaporate the solvent in the solder paste. S2: The preheated glass substrate is sent into the constant temperature zone of the reflow soldering equipment to balance the temperature of each area of the glass substrate and activate the flux. S3: After the temperature is balanced, the glass substrate is sent into the reflow soldering area to completely melt the solder paste in the area to be soldered on the glass substrate, and chemical bonding is formed between the areas to be soldered. S4: The welded glass substrate is sent into the heat preservation and stress relief zone to release the internal stress of the glass substrate and at the same time achieve the crystallization and solidification of the weld joint. S5: The glass substrate with released internal stress is sent into the cooling zone to rapidly cool down the glass substrate and solder joints and then output to the next processing step.
2. The method of preventing cracks in reflow soldering of glass substrates of claim 1, wherein: The glass substrate is sequentially fed into each zone in steps S1-S5 via a conveyor belt at a speed of 75-85 cm / min.
3. The method of preventing cracks in reflow soldering of glass substrates of claim 2, wherein: In step S1, the preheating zone includes a first temperature zone, a second temperature zone, and a third temperature zone with increasing temperature gradient. The three temperature zones are arranged side by side, and each temperature zone includes an upper temperature zone located above the conveyor belt and a lower temperature zone located below the conveyor belt.
4. The method of preventing cracks in reflow soldering of glass substrates of claim 3, wherein: The set temperatures for the first, second, and third temperature zones are 130, 150, and 170°C, respectively.
5. The method of preventing cracks in reflow soldering of glass substrates of claim 2, wherein: The constant temperature zone includes a fourth, fifth, sixth, and seventh temperature zone with increasing temperature gradients. The four temperature zones are set in parallel, and the set temperature difference between the sixth and seventh temperature zones is less than 5-8℃.
6. The method of preventing cracks in reflow soldering of glass substrates of claim 2, wherein: The reflow soldering zone includes an eighth, ninth, and tenth temperature zone with an increasing temperature gradient. The three temperature zones are arranged side by side, with a temperature difference of 3-6℃ between adjacent temperature zones.
7. The method of preventing cracks in reflow soldering of glass substrates of claim 2, wherein: The heat preservation and stress relief zone includes an eleventh temperature zone and a twelfth temperature zone. The eleventh temperature zone and the twelfth temperature zone have the same temperature, which is lower than the temperature of the reflow soldering temperature zone.
8. The method of preventing cracks in reflow soldering of glass substrates of claim 2, wherein: The cooling zone includes a thirteenth temperature zone and a fourteenth temperature zone. Cooling structures are provided in the upper and lower temperature zones of the thirteenth and fourteenth temperature zones. The cooling structures are used to reduce the temperature of the glass substrate to room temperature.
9. A reflow soldering apparatus for preventing cracks in a glass substrate for implementing the method for preventing cracks in a glass substrate reflow soldering according to any one of claims 1 to 8, characterized by, The device includes a conveyor belt for transporting glass substrates, and a preheating zone, a constant temperature zone, a reflow soldering zone, a heat preservation and stress relief zone, and a cooling zone arranged sequentially along the conveyor belt's transport direction. The preheating zone, constant temperature zone, reflow soldering zone, heat preservation and stress relief zone, and cooling zone are each provided with an upper temperature zone and a lower temperature zone, and the conveyor belt is disposed between the upper temperature zone and the lower temperature zone.
10. The reflow soldering equipment according to claim 9, characterized in that: The outer surfaces of the preheating zone, constant temperature zone, reflow welding zone, heat preservation and stress relief zone, and cooling zone are respectively provided with heat preservation structures to prevent heat leakage.