Multi-source solid waste alkali-activated cementitious material based on temperature-sensitive microcapsule staged controlled-release activator

By using temperature-sensitive microcapsule staged controlled-release activator technology, the problems of excessively high early alkali concentration and insufficient activation in the middle and later stages caused by the one-time release of alkali activator in alkali-activated cementitious materials for multi-source solid waste are solved, realizing the staged supply of alkali activator and the synergistic reaction of multi-source solid waste.

CN123106041APending Publication Date: 2026-11-17TSINGHUA UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611573909.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-12
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing multi-source solid waste alkali-activated cementitious materials suffer from problems such as excessively high local alkali concentrations in the early stages due to the one-time release of alkali activator, mismatch between the activator supply process and the reaction process of different solid waste components, and insufficient continuous activation in the middle and later stages.

Method used

A staged controlled-release activator using thermosensitive microcapsules is employed, including a free alkali activator and a thermosensitive microcapsule alkali activator. The free alkali activator preferentially dissolves and releases during the initial stage of water addition and mixing. The thermosensitive response structure changes the mass transfer state after the exothermic reaction and temperature rise of the gelation system, allowing the alkali activator to be further released. The target response temperature is determined based on the internal temperature rise characteristics of the multi-source solid waste gelation system.

Benefits of technology

This approach enables the phased supply of alkali activators, avoiding excessively high alkali concentrations in the early stages, adapting to the reaction requirements of different solid waste components, improving the alkaline environment in the middle and later stages, and promoting the synergistic reaction and resource utilization of multi-source solid waste.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123106041A_ABST
    Figure CN123106041A_ABST
Patent Text Reader

Abstract

This invention discloses a multi-source solid waste alkali-activated gelling material based on a staged controlled-release activator using temperature-sensitive microcapsules. The gelling material comprises a multi-source solid waste gelling component, a free alkali activator, a temperature-sensitive microcapsule alkali activator, and water. The multi-source solid waste gelling component consists of at least two of the following: slag, fly ash, desulfurized gypsum, steel slag, and decarbonized coal gangue. The temperature-sensitive microcapsule comprises an alkali activator core, a barrier layer, and a temperature-sensitive response layer. The target response temperature is determined based on the internal temperature rise characteristics of the gelling system after mixing with water from 0 to 48 hours, satisfying T... r =T0+α(T max (-T0), 0.4≤α≤0.8. During the initial mixing stage, the free alkali activator is preferentially released. After the system reaction reaches the target response temperature, the temperature-sensitive response layer alters the mass transfer channels, allowing for further release of the coated alkali activator, thus achieving staged alkali supply. This invention avoids excessively high local alkali concentrations in the early stages caused by a one-time alkali release, mismatch with the multi-source solid waste stage reaction, and insufficient activation in the middle and later stages. It improves the compressive strength of multi-source solid waste cementitious materials in the middle and later stages and is suitable for low-carbon building materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a multi-source solid waste alkaline-activated gelling material based on a staged controlled-release activator of temperature-sensitive microcapsules, belonging to the technical field of industrial solid waste resource utilization and low-carbon gelling material preparation. Background Technology

[0002] Industrial solid wastes such as slag, fly ash, desulfurization gypsum, steel slag, and coal gangue contain potentially active components such as silicon, aluminum, and calcium. These components can be activated by alkali to promote dissolution reactions and form cementitious products, making them important raw materials for preparing low-carbon cementitious materials. Due to differences in the chemical composition, mineral composition, and activity of various solid wastes, the reaction rates of different components in a multi-source solid waste system are not consistent.

[0003] Existing alkaline-activated gelling materials for multi-source solid waste typically employ a one-time activation method, adding alkaline activators such as sodium hydroxide and sodium silicate all at once. The rapid dissolution and release of these activators during the initial mixing stage can easily lead to high local alkali concentrations and excessively rapid early reactions. Meanwhile, some slower-reacting solid waste components require a continuous alkaline environment in the later stages, resulting in a mismatch between the activator supply process and the multi-source solid waste reaction process. While existing conventional slow-release microcapsules can delay activator release, their release process is primarily controlled by the fixed encapsulation structure, making it difficult to adjust the release rate according to the actual reaction state of the gelling system.

[0004] To address the aforementioned technical shortcomings, this invention aims to provide a multi-source solid waste alkali-activated gelling material based on a staged controlled-release activator using temperature-sensitive microcapsules. This addresses the problems in existing multi-source solid waste alkali-activated gelling materials, such as excessively high local alkali concentrations in the early stages due to the one-time release of the alkali activator, mismatch between the activator supply process and the staged reaction processes of different solid waste components, and insufficient continuous activation in the middle and later stages. Summary of the Invention

[0005] The purpose of this invention is to provide a multi-source solid waste alkali-activated gelling material based on a temperature-sensitive microcapsule staged controlled-release activator, so as to solve the problems of insufficient early concentrated alkali release and insufficient continuous activation in the middle and later stages caused by the one-time addition of alkali activator in existing multi-source solid waste alkali-activated gelling materials.

[0006] The present invention provides a multi-source solid waste alkali-activated gelling material based on a thermosensitive microcapsule staged controlled-release activator, comprising multi-source solid waste gelling components, free alkali activator, thermosensitive microcapsule alkali activator, and water; The multi-source solid waste cementitious component is composed of at least two of the following: slag, fly ash, desulfurized gypsum, steel slag, and decarbonized coal gangue. The thermosensitive microcapsule alkali activator includes an alkali activator core and a thermosensitive response structure encapsulating the alkali activator core; based on the total mass of the effective components of the alkali activator being 100%, the free alkali activator accounts for 20%-40%, and the alkali activator core in the thermosensitive microcapsule alkali activator accounts for 60%-80%; The free alkali activator is preferentially dissolved and released during the initial stage of water addition and mixing to provide an initial alkaline environment for initiating the reaction; the temperature-sensitive response structure is used to change the mass transfer state after the gelation system reacts exothermically and heats up to the target response temperature, so as to further release the alkali activator in the core of the alkali activator to provide supplemental alkalinity and / or soluble silicon source in the middle and later stages; the target response temperature is determined based on the internal temperature rise characteristics of the multi-source solid waste gelation system within 0-48 hours after water addition and mixing.

[0007] Taking the total mass of the multi-source solid waste cementitious components as 100%, the mass fraction of each component is as follows: The solid waste components consist of 40%-90% slag, 0-30% fly ash, 0-30% desulfurized gypsum, 0-30% steel slag, and 0-30% decarbonized coal gangue, with at least two of these solid waste components having a mass fraction greater than 0.

[0008] Preferably, the free alkali activator and the alkali activator core each independently comprise one or more of sodium hydroxide, sodium silicate, and sodium metasilicate; when a composite alkali activator composed of sodium hydroxide and sodium silicate is used, the mass ratio of sodium hydroxide to sodium silicate is 1:1 to 1:3.

[0009] Preferably, the temperature-sensitive response structure includes a barrier layer located outside the alkali activator core and a temperature-sensitive response layer located outside the barrier layer; the barrier layer is used to reduce the rate at which water directly contacts the alkali activator core during storage and initial mixing; the temperature-sensitive response layer is used to change the effective mass transfer performance of the temperature-sensitive microcapsules according to the temperature change inside the gelation system. The temperature-sensitive responsive layer includes one or more of poly(N-isopropylacrylamide), N-isopropylacrylamide copolymers, temperature-sensitive acrylic copolymers, and temperature-sensitive polyvinyl alcohol modified materials.

[0010] Preferably, the material of the thermosensitive response layer is distributed in the form of a thermosensitive microgel or a thermosensitive polymer network on the outside of the barrier layer or at the mass transfer channel location of the barrier layer; when the system temperature is lower than the target response temperature, the thermosensitive response layer is in a hydrated and expanded state and blocks at least part of the mass transfer channel; when the system temperature reaches the target response temperature, the thermosensitive response layer undergoes conformational and volume changes, thereby increasing the effective cross-sectional area of ​​the mass transfer channel; The target response temperature T r Satisfy: T r =T0+α(T max-T0), where T0 is the initial internal temperature of the gelling system after mixing with water, T max The highest internal temperature of the gelling system within 0-48 hours after adding water and mixing is α, where α is the response position coefficient and 0.4≤α≤0.8; By establishing the above relationships, the temperature-sensitive response temperature is positioned appropriately within the actual heating process of the corresponding multi-source solid waste system, rather than using a fixed response temperature uniformly for different solid waste systems. When changes in the solid waste composition lead to changes in the highest exothermic temperature or the timing of the exothermic peak, the composition and cross-linking degree of the temperature-sensitive material are adjusted accordingly to alter its actual response temperature.

[0011] In this invention, the average particle size of the thermosensitive microcapsule alkali activator is 50-200 μm, the alkali activator core accounts for 65%-85% of the total mass of the thermosensitive microcapsule alkali activator, and the thermosensitive response structure accounts for 15%-35% of the total mass of the thermosensitive microcapsule alkali activator; After adding water and mixing, the system releases 20%-40% of the total effective components of the alkali activator within 0-2 hours; 40%-70% within 2-12 hours; and 60%-90% within 24 hours.

[0012] The present invention also provides a method for preparing the multi-source solid waste alkali-activated cementitious material, comprising the following steps: S1. Select at least two types from slag, fly ash, desulfurized gypsum, steel slag and decarbonized coal gangue, and mix them according to the design ratio after drying, grinding and / or screening to obtain multi-source solid waste cementitious components. S2. Prepare the alkali activator as the alkali activator core, and form a temperature-sensitive response structure on the outside of the alkali activator core to obtain a temperature-sensitive microcapsule alkali activator; S3. Weigh the free alkali activator and the temperature-sensitive microcapsule alkali activator according to the design ratio, and mix them with the multi-source solid waste gelling components. S4. Add water and stir, shape and cure; S5. The free alkali activator is preferentially released in the initial stage of mixing, and after the internal temperature rise generated by the reaction in the multi-source solid waste coagulation system causes the temperature-sensitive response structure to reach the target response temperature, the alkali activator in the temperature-sensitive microcapsule is further released.

[0013] Step S2 includes: placing the alkali activator core in a fluidized coating device, forming a barrier layer on the surface of the alkali activator core using a barrier layer coating liquid; preparing a temperature-sensitive microgel, mixing the temperature-sensitive microgel with a film-forming material to form a temperature-sensitive response coating liquid, spraying the temperature-sensitive response coating liquid onto the surface of particles with a barrier layer, and obtaining the temperature-sensitive microcapsule alkali activator after drying; Before determining the composition of the temperature-sensitive material, the internal temperature change curve of the corresponding multi-source solid waste coagulation system after water addition was measured from 0 to 48 hours to obtain the initial temperature T0 and the highest temperature T0. max Then according to T r =T0+α(T max -T0) Calculate the target response temperature T r Where 0.4≤α≤0.8; then, by adjusting the type of temperature-sensitive material, the proportion of comonomers, the degree of crosslinking and the coating structure, the actual response temperature of the temperature-sensitive response layer is matched with the target response temperature.

[0014] Finally, this invention also provides a staged controlled-release activation method for a multi-source solid waste alkali-activated gelling material, comprising the following steps: using the multi-source solid waste alkali-activated gelling material, after adding water and mixing, the free alkali activator preferentially dissolves and is released; the multi-source solid waste gelling system reacts exothermically, causing the internal temperature to rise; when the internal temperature reaches the target response temperature, the temperature-sensitive response structure changes the mass transfer state, causing the alkali activator in the temperature-sensitive microcapsules to be further released; wherein, after adding water and mixing, 20%-40% of the total effective components of the alkali activator are released cumulatively in 0-2 hours, 40%-70% in 2-12 hours, and 60%-90% in 24 hours.

[0015] Compared with traditional multi-source solid waste alkali activation materials that require the addition of alkali activator only once, the present invention has the following advantages: First, the present invention uses free alkali activator and temperature-sensitive microcapsule alkali activator in synergy, so that a part of the alkali activator provides the alkali environment required to start the reaction in the early stage of mixing, and another part of the alkali activator is released in the later stage, thus avoiding the concentration of all alkali activator in the early stage of mixing.

[0016] Secondly, the present invention utilizes the exothermic reaction of the gelation system itself as a trigger signal for the change in the release state of the temperature-sensitive microcapsules, without the need for additional external triggering devices.

[0017] Third, the present invention determines the target response temperature based on the actual internal temperature rise characteristics of different multi-source solid waste systems, so that the temperature-sensitive microcapsules can adapt to the differences in reaction exothermics caused by different solid waste compositions.

[0018] Fourth, this invention controls the mass transfer process of the alkali activator through the synergistic control of the barrier layer and the thermosensitive response layer, so that the temperature change of the thermosensitive response material can be converted into an adjustable alkali activator release behavior.

[0019] Fifth, this invention can provide a sustained alkaline environment in the middle and late stages for components such as fly ash, steel slag, and decarbonized coal gangue that react relatively slowly, which is beneficial to improving the synergistic reaction and resource utilization level of multi-source solid waste. Attached Figure Description

[0020] Figure 1This is a schematic diagram of the structure of the thermosensitive microcapsule alkali activator of the present invention.

[0021] Figure 2 This is a schematic diagram illustrating the working principle of the thermosensitive response structure controlling the release of the alkali activator in this invention.

[0022] Figure 3 This is a schematic diagram showing the correspondence between temperature rise, temperature-sensitive response, and staged alkali release within the multi-source solid waste coagulation system of this invention.

[0023] Figure 4 This is a flowchart illustrating the preparation process of multi-source solid waste alkali-activated cementitious material based on a staged controlled-release activator using temperature-sensitive microcapsules, as described in this invention. Detailed Implementation

[0024] Numerous specific details are set forth in the following description to provide a full understanding of the invention. However, the invention can be practiced in many other ways different from those described herein, and those skilled in the art can make similar extensions without departing from the spirit of the invention. Therefore, the invention is not limited to the specific embodiments disclosed below.

[0025] It should be understood that the terminology used in this invention is merely for describing particular embodiments and is not intended to limit the invention. Furthermore, with respect to numerical ranges in this invention, it should be understood that each intermediate value between the upper and lower limits of the range is also specifically disclosed. Every smaller range between any stated value or intermediate value within a stated range, and any other stated value or intermediate value within said range, is also included within the scope of this invention. The upper and lower limits of these smaller ranges may be included independently.

[0026] Unless otherwise stated, all technical and scientific terms used in this invention have the same meaning as commonly understood by one of ordinary skill in the art. While only preferred methods and materials have been described in this invention, any methods and materials similar to or equivalent to those described herein may be used in the practice or testing of this invention.

[0027] Various modifications and variations can be made to the specific embodiments described in this specification without departing from the scope or spirit of the invention, as will be apparent to those skilled in the art. Other embodiments derived from this specification will be obvious to those skilled in the art, and the specification and embodiments are merely exemplary.

[0028] In this embodiment, the slag, fly ash, desulfurized gypsum, steel slag, and decarburized coal gangue used were all dried before use, and then ground and sieved according to their state. Unless otherwise specified, the pretreatment, mixing, molding, and curing procedures for the raw materials were kept consistent across all experimental groups.

[0029] like Figure 4As shown, the preparation process of the multi-source solid waste alkali-activated gelling material based on the phased controlled-release activator of temperature-sensitive microcapsules in this invention mainly includes the selection and pretreatment of multi-source solid waste raw materials, design of the multi-source solid waste gelling component ratio, determination of temperature-sensitive response parameters, preparation of temperature-sensitive microcapsule alkali activator, configuration of the phased alkali activation system, and mixing, molding, and curing. During the preparation process, the target response temperature is first determined based on the internal temperature rise characteristics of the multi-source solid waste gelling system, and a temperature-sensitive microcapsule alkali activator with corresponding temperature-sensitive response characteristics is prepared simultaneously. Then, the free alkali activator and the temperature-sensitive microcapsule alkali activator are mixed with the multi-source solid waste gelling components according to the designed ratio and water is added for molding. During the curing process, the free alkali activator is released first, and the exothermic reaction of the gelling system raises the internal temperature. When the target response temperature is reached, the temperature-sensitive response structure changes the mass transfer state, causing the alkali activator encapsulated in the temperature-sensitive microcapsules to be further released, thereby achieving phased alkali release.

[0030] Example 1: Optimization of the proportion of binary solid waste cementitious materials This embodiment screens the proportion of slag-desulfurized gypsum binary solid waste cementitious materials. The slag and desulfurized gypsum are dried and ground separately for later use. With the total mass of slag and desulfurized gypsum as 100%, different slag to desulfurized gypsum mass ratios are set, and the proportions of each group of raw materials are shown in Table 1.

[0031] Table 1. Proportioning of Ternary Solid Waste Cementitious Materials

[0032] After the above solid waste powders are mixed evenly, NaOH-Na2SiO3 composite alkali activator is added, with the alkali activator dosage being 2% of the mass of the cementitious material. The liquid-solid ratio is 0.5. The mixed slurry is poured into a 40 mm × 40 mm × 40 mm mold, compacted, and then cured at a temperature of 20±2℃ and a relative humidity of over 95%. The compressive strength is tested at 3 days, 7 days, and 28 days.

[0033] The compressive strength of each group of specimens was tested at 3 days, 7 days and 28 days, and the results are shown in Table 2.

[0034] Table 2 Compressive Strength of Alkali-Activated Cementitious Materials for Binary Solid Waste

[0035] As shown in Table 2, the 28-day compressive strength of group BD82 is 32.60 MPa. Therefore, the following examples use a cementing component of 80% slag and 20% desulfurized gypsum as a representative multi-source solid waste cementing system.

[0036] Example 2: Optimization of the proportion of ternary solid waste cementitious materials Based on the test results of Example 1, the 28-day compressive strength was highest when the mass ratio of slag to desulfurized gypsum was 8:2. Following this, the mass fraction of slag was fixed at 80%, and fly ash was used to replace part of the desulfurized gypsum, with the sum of the mass fractions of fly ash and desulfurized gypsum remaining at 20%. The proportions of each component are shown in Table 3 (e.g., BDF25175 represents a desulfurized gypsum mass fraction of 17.5% and a fly ash mass fraction of 2.5%).

[0037] Table 3. Proportions of Ternary Solid Waste Cementitious Materials

[0038] After the above solid waste powders are mixed evenly, NaOH-Na2SiO3 composite alkali activator is added, with the alkali activator dosage being 2% of the mass of the cementitious material. The liquid-solid ratio is 0.5. The mixed slurry is poured into a 40 mm × 40 mm × 40 mm mold, compacted, and then cured at a temperature of 20±2℃ and a relative humidity of over 95%. The compressive strength is tested at 3 days, 7 days, and 28 days.

[0039] The compressive strength of cementitious materials with different proportions was tested, and the test results are shown in Table 4.

[0040] Table 4 Compressive Strength of Alkali-Activated Cementitious Materials for Ternary Solid Waste

[0041] As shown in Table 4, the 28-day compressive strength of the BDF1010 group is 41.91 MPa. Therefore, the following examples use a cementing composition of 80% slag, 10% fly ash, and 10% desulfurized gypsum as a representative multi-source solid waste cementing system.

[0042] Example 3: Preparation of temperature-sensitive microcapsule alkali activator Weigh out sodium hydroxide and solid sodium silicate, mix them in a mass ratio of 1:2, grind them, and then sieve out particles with a particle size of 50-100 μm as the core of the alkali activator.

[0043] Weigh 100 g of alkali activator core and place it in a fluidized bed coating device. Dissolve 5 g of ethyl cellulose in 95 g of ethanol to form a barrier coating solution. Spray the solution onto the surface of the alkali activator core at a rate of 5 mL / min under 40-50℃ conditions. After coating, continue fluidized drying for 30 min to obtain the first coated particles with a barrier layer.

[0044] Thermosensitive microgels were prepared using N-isopropylacrylamide. 10 g of N-isopropylacrylamide and 0.2 g of N,N'-methylenebisacrylamide were added to 200 mL of deionized water, and the mixture was heated to 70 °C under nitrogen protection. 0.1 g of ammonium persulfate was added to initiate polymerization, and the reaction was carried out for 4 h to obtain a thermosensitive microgel dispersion.

[0045] Thermosensitive microgels are mixed with film-forming materials to form thermosensitive response coating solutions, which are then sprayed onto the surface of the first coated particles and dried to obtain thermosensitive microcapsule alkali activators.

[0046] like Figure 1 As shown, the thermosensitive microcapsule alkali activator of the present invention comprises, from the inside out, an alkali activator core, a barrier layer, and a thermosensitive response layer. The alkali activator core stores the effective components of the alkali activator, such as NaOH and Na2SiO3; the barrier layer covers the outside of the alkali activator core to reduce the rate of direct contact between moisture and the alkali activator core during storage and the initial mixing stage; the thermosensitive response layer is disposed outside the barrier layer and undergoes volume and / or conformational changes under the influence of temperature changes within the gelation system to regulate the effective mass transfer channels of the microcapsules. The parameters of the thermosensitive microcapsules obtained in this embodiment are shown in Table 5.

[0047] Table 5. Parameters of the base activator for thermosensitive microcapsules

[0048] The thermosensitive microgel in the thermosensitive response layer is in an expanded state below the target response temperature, restricting the mass transfer channels in the coating layer. Upon reaching the target response temperature, it shrinks in volume, increasing the effective area of ​​the mass transfer channels and thus improving the rate of water ingress and alkali activator diffusion. For example... Figure 2 As shown, when the internal temperature of the gelation system is lower than the target response temperature, the thermosensitive microgel in the thermosensitive response layer is in a hydrated and swollen state, which blocks some of the mass transfer channels, thereby limiting the penetration of water into the microcapsule and the diffusion of the alkali activator outward. As the gelation system reacts exothermically and the internal temperature rises to near the target response temperature, the thermosensitive microgel gradually shrinks in volume, and the mass transfer channels begin to open. When the system temperature reaches or exceeds the target response temperature, the thermosensitive response layer further shrinks, increasing the effective cross-sectional area of ​​the mass transfer channels, promoting the entry of water into the microcapsule and the outward diffusion and release of the effective components in the core of the alkali activator.

[0049] To determine the release behavior of the alkali activator in the thermosensitive microcapsule, sodium was used as a tracer for the amount of alkali activator released.

[0050] Weigh a certain mass of the temperature-sensitive microcapsule alkali activator. Based on the mass of the alkali activator core in the microcapsule and the composition of the sodium component in the alkali activator core, determine the initial total mass of Na element corresponding to the alkali activator in the sample. .

[0051] The temperature-sensitive microcapsule alkali activator was added to a specified volume of deionized water or simulated pore liquid, and an isothermal release test was conducted under set temperature conditions. Temperature conditions were set below the target response temperature, near the target response temperature, and above the target response temperature.

[0052] Independent parallel samples were prepared at 0.5 h, 1 h, 2 h, 4 h, 8 h, 12 h, 24 h, 3 d, and 7 d. After the specified time, the corresponding samples were subjected to solid-liquid separation and filtered using a 0.45 μm filter membrane.

[0053] The concentration of Na in the filtrate was determined using inductively coupled plasma atomic emission spectrometry. .

[0054] time The mass of Na released into the external liquid phase is calculated using the following formula:

[0055] In the formula: For time The mass of Na released into the liquid phase at that time, in mg; For time The concentration of Na in the filtrate, mg / L; To release the volume of the medium, L.

[0056] time The cumulative release rate of the alkali activator is calculated according to the following formula:

[0057] In the formula: For time Cumulative release rate of alkaline activator, % The initial total mass of Na element corresponding to the alkaline activator encapsulated in the thermosensitive microcapsule, in mg.

[0058] When determining the release rate of alkali activator in actual multi-source solid waste gel slurry, a blank gel slurry without alkali activator is prepared simultaneously. The solid waste composition, water-cement ratio, and curing conditions of the blank gel slurry are the same as those of the gel slurry to be tested.

[0059] Take 20 g of the slurry to be tested at the specified age, add 200 mL of deionized water, shake for 30 min, let stand for 30 min, centrifuge and filter through a 0.45 μm filter membrane, and determine the Na element concentration in the filtrate.

[0060] Blank samples were extracted and measured using the same method.

[0061] After blank correction, time The mass of Na released by the alkaline activator is calculated according to the following formula:

[0062] In the formula: For time after blank correction The mass of Na released into the liquid phase by the alkaline activator, in mg; For time The total mass of Na element in the extract of the gel slurry to be tested, in mg; For time The total mass of Na element in the leachate of blank gel slurry, in mg.

[0063] The composition of multi-source solid waste, water-cement ratio, curing conditions and extraction conditions of the gelling paste to be tested and the blank gelling paste are consistent. No alkali activator is added to the blank gelling paste to deduct the soluble Na element brought in by the multi-source solid waste raw materials themselves.

[0064] After blank correction, the cumulative release rate of the alkali activator in the gelling system at time t is calculated according to the following formula:

[0065] In the formula: For time Cumulative release rate of alkaline activator, % For time after blank correction The mass of Na released into the liquid phase by the alkaline activator, in mg; w represents the initial total mass of Na element corresponding to the alkaline activator in the test sample, in mg.

[0066] in, The amount of Na component added is calculated based on the actual amount added to the free alkali activator and the thermosensitive microcapsule alkali activator in the test sample; when only the release behavior of the alkali activator coated in the thermosensitive microcapsule is measured. The initial total mass of Na element corresponding to the alkali activator core in the thermosensitive microcapsule.

[0067] The cumulative release rate of alkali activator in the gelling system is:

[0068] The cumulative release rate of the alkali activator under different temperatures and ages was determined using the above method.

[0069] Example 4: Determination of the target response temperature of the temperature-sensitive microcapsule Using the BDF1010 group from Example 2 as the reference gelling system, the mixture was stirred at 20 °C. A temperature sensor was placed in the center of the specimen, and the internal temperature change was continuously recorded for 48 h from the start of water addition and stirring.

[0070] The target response temperature of the temperature-sensitive layer is determined by the following formula:

[0071] in: The target response temperature; The initial internal temperature of the gelling system after adding water and mixing; The highest internal temperature of the gelling system within 0-48 h after adding water and mixing; The response position coefficient, and 0.4 ≤ ≤0.8.

[0072] In this embodiment, the following settings are provided: The temperature is 20.0℃. The temperature was 41.0℃. If we take 0.6, then:

[0073] Accordingly, the response temperature of the temperature-sensitive microcapsules in Example 2 was controlled within the range of 32-34 °C. Figure 3 As shown, after water is added to the multi-source solid waste coagulation system, the free alkali activator first dissolves and releases, initiating the reaction of the solid waste components. The internal temperature of the system gradually increases as the reaction exothermically. When the internal temperature of the system reaches the target response temperature... At this time, the temperature-sensitive response layer transforms from an expanded, blocked state to a contracted, open state, and the encapsulated alkali activator in the temperature-sensitive microcapsules begins to be released at an accelerated rate. As the temperature-sensitive response structure further changes, the encapsulated alkali activator continues to be released into the gelation system. Thus, the supply process of the alkali activator sequentially forms three stages: initial free alkali-initiated release, temperature-sensitive response-triggered release, and mid-to-late-stage continuous release, thereby making the alkali activator release process correspond to the internal temperature rise and staged reaction process of the multi-source solid waste gelation system.

[0074] Example 5: Multi-source solid waste alkali-activated gelling material using temperature-sensitive microcapsule staged controlled-release activator. Based on a total cementitious material mass of 1000 g, weigh out 800 g of slag, 100 g of fly ash, and 100 g of desulfurized gypsum. Use a NaOH-Na2SiO3 composite alkali activator, ensuring consistent total effective component amounts across all alkali activators. Set the mass ratio of free alkali activator to the alkali activator core in the temperature-sensitive microcapsules at 20:80, 30:70, and 40:60, respectively.

[0075] The multi-source solid waste gelling components, free alkali activator and the temperature-sensitive microcapsule alkali activator prepared in Example 2 were mixed evenly, water was added and stirred, and then the mixture was put into a 40 mm × 40 mm × 40 mm mold. After being compacted, it was cured at 20±2 ℃ and relative humidity not less than 95%.

[0076] The compressive strength was tested at 3 days, 7 days, 14 days and 28 days, and the test results are shown in Table 6.

[0077] Table 6 Compressive strength of cementitious materials with different ratios of free alkali to coated alkali

[0078] As shown in Table 4, the optimal compressive strength of group T2 at 28 days is 45.76 MPa.

[0079] Example 6: Preparation of Alkali-Activated Cementitious Material from Multi-Source Solid Waste Containing Steel Slag Weigh out 700 g of slag, 100 g of steel slag, 100 g of fly ash, and 100 g of desulfurized gypsum, based on a total cementitious material mass of 1000 g.

[0080] The thermosensitive microcapsule alkali activator prepared in Example 2 was used, and the free alkali activator and the alkali activator core in the thermosensitive microcapsule were added at an effective component mass ratio of 30:70.

[0081] The remaining preparation, molding and curing methods are the same as in Example 4.

[0082] The test results are shown in Table 7.

[0083] Table 7 Compressive Strength of Steel Slag Composite Multi-Source Solid Waste Cementitious Material

[0084] Example 7: Preparation of Alkali-Activated Cementitious Material from Multi-Source Solid Waste Containing Decarbonized Coal Gangue Weigh out 700 g of slag, 100 g of decarbonized coal gangue, 100 g of fly ash, and 100 g of desulfurized gypsum, based on a total mass of 1000 g of cementitious materials.

[0085] The thermosensitive microcapsule alkali activator prepared in Example 2 was used, and the free alkali activator and the alkali activator core in the thermosensitive microcapsule were added at an effective component mass ratio of 30:70.

[0086] The remaining preparation, molding and curing methods are the same as in Example 5.

[0087] The test results are shown in Table 8.

[0088] Table 8 Compressive Strength of Decarbonized Coal Gangue Composite Multi-Source Solid Waste Cementitious Material

[0089] Comparative Example 1 This comparative example uses the same cementitious materials as Example 5, namely 800 g of slag, 100 g of fly ash and 100 g of desulfurized gypsum.

[0090] Instead of using a temperature-sensitive microcapsule structure, all alkali activators were added at once as free alkali activators. The total amount of effective alkali activator components, water-to-binder ratio, molding, and curing methods were the same as in Example 4.

[0091] The test results are shown in Table 9.

[0092] Table 9 Compressive strength of Comparative Example 1

[0093] Comparative Example 2 This comparative example uses the same cementitious material composition and total amount of effective alkali activator components as Example 5.

[0094] The free alkali activator and the alkali activator encapsulated in ordinary non-thermosensitive microcapsules were added at an effective component mass ratio of 30:70. The ordinary non-thermosensitive microcapsules have the same barrier layer as in Example 3, but without a thermosensitive response layer.

[0095] The remaining preparation, molding and curing methods are the same as in Example 5.

[0096] The test results are shown in Table 10.

[0097] Table 10 Comparative Example 2 Compressive Strength

[0098] Example 8: Testing the release behavior of alkaline activators with different activator addition methods Comparative Example 1, Comparative Example 2, and Group T2 from Example 5 were used as test subjects, and the release rate of the alkali activator was measured according to the above-described test method.

[0099] Among them, Comparative Example 1 is a system in which all alkali activators are added at once; Comparative Example 2 is a non-thermosensitive sustained-release microcapsule system; and the T2 group in Example 5 is a staged controlled-release system in which free alkali activators and thermosensitive microcapsule alkali activators are added at a ratio of 30:70.

[0100] The cumulative release rate of the alkali activator was measured at 0.5 h, 2 h, 4 h, 8 h, 12 h and 24 h, respectively, and the results are shown in Table 11.

[0101] Table 11 Cumulative alkaline activator release rate under different activation methods

[0102] As shown in Table 11, the alkali activator in Comparative Example 1 was released rapidly in the initial stage of mixing; Comparative Example 2 maintained a relatively slow release process throughout the entire test stage; Example 4-T2 maintained a low release rate in the initial stage of mixing and showed a faster cumulative release growth in the subsequent stage.

[0103] As can be seen from the above embodiments and comparative examples, this invention sets the alkali activator into two parts: a free alkali activator and a temperature-sensitive microcapsule alkali activator. The temperature-sensitive response temperature is determined based on the early reaction exothermic characteristics of the multi-source solid waste gelling system. This allows the free alkali activator to be released preferentially in the initial mixing stage, while the alkali activator in the temperature-sensitive microcapsules is further released after the system temperature reaches the target response condition, thus achieving a phased supply of the alkali activator. Compared with the one-time addition of the alkali activator and the conventional non-temperature-sensitive microcapsule slow-release method, this invention can regulate the release process of the alkali activator at different reaction stages and improve the compressive strength of the multi-source solid waste gelling material in the later stages. The method is applicable to multi-source solid waste gelling systems composed of at least two of the following: slag, fly ash, desulfurized gypsum, steel slag, and decarburized coal gangue. The temperature-sensitive response parameters and the alkali activator distribution ratio can be adjusted according to the reaction exothermic characteristics of different solid waste compositions.

[0104] The above description is only a preferred embodiment of the present invention and is not intended to limit the scope of protection of the present invention; any equivalent substitutions, simple transformations or improvements made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.

Claims

1. A multi-source solid waste alkali-activated gelling material based on a thermosensitive microcapsule staged controlled-release activator, comprising multi-source solid waste gelling components, free alkali activator, thermosensitive microcapsule alkali activator, and water; The multi-source solid waste cementitious component is composed of at least two of the following: slag, fly ash, desulfurized gypsum, steel slag, and decarbonized coal gangue. The thermosensitive microcapsule alkali activator includes an alkali activator core and a thermosensitive response structure covering the outside of the alkali activator core; based on the total mass of the effective components of the alkali activator being 100%, the free alkali activator accounts for 20%-40%, and the alkali activator core in the thermosensitive microcapsule alkali activator accounts for 60%-80%.

2. The multi-source solid waste alkali-activated cementitious material according to claim 1, characterized in that: Taking the total mass of the multi-source solid waste cementitious components as 100%, the mass fraction of each component is as follows: The solid waste components consist of 40%-90% slag, 0-30% fly ash, 0-30% desulfurized gypsum, 0-30% steel slag, and 0-30% decarbonized coal gangue, with at least two of these solid waste components having a mass fraction greater than 0.

3. The multi-source solid waste alkali-activated cementitious material according to claim 1 or 2, characterized in that: The free alkali activator and the alkali activator core each independently include one or more of sodium hydroxide, sodium silicate, and sodium metasilicate; when a composite alkali activator composed of sodium hydroxide and sodium silicate is used, the mass ratio of sodium hydroxide to sodium silicate is 1:1 to 1:

3.

4. The multi-source solid waste alkali-activated cementitious material according to any one of claims 1-3, characterized in that: The temperature-sensitive response structure includes a barrier layer located outside the alkali activator core and a temperature-sensitive response layer located outside the barrier layer; the barrier layer is used to reduce the rate at which water directly contacts the alkali activator core during storage and initial mixing; the temperature-sensitive response layer is used to change the effective mass transfer performance of the temperature-sensitive microcapsules according to the temperature change inside the gelation system. The temperature-sensitive responsive layer includes one or more of poly(N-isopropylacrylamide), N-isopropylacrylamide copolymers, temperature-sensitive acrylic copolymers, and temperature-sensitive polyvinyl alcohol modified materials.

5. The multi-source solid waste alkali-activated cementitious material according to claim 4, characterized in that: The material of the thermo-responsive layer is distributed in the form of thermo-sensitive microgel or thermo-sensitive polymer network on the outside of the barrier layer or at the mass transfer channel of the barrier layer; when the system temperature is lower than the target response temperature, the thermo-responsive layer is in a hydrated and expanded state and blocks at least part of the mass transfer channel; when the system temperature reaches the target response temperature, the thermo-responsive layer undergoes conformational and volume changes, thereby increasing the effective cross-sectional area of ​​the mass transfer channel. The target response temperature T r Satisfy: T r =T0+α(T max -T0), where T0 is the initial internal temperature of the gelling system after mixing with water, T max The highest internal temperature of the gelling system within 0-48 hours after water is added and mixed is α, where α is the response position coefficient and 0.4≤α≤0.

8.

6. The multi-source solid waste alkali-activated cementitious material according to any one of claims 1-5, characterized in that: The average particle size of the thermosensitive microcapsule alkali activator is 50-200 μm, the alkali activator core accounts for 65%-85% of the total mass of the thermosensitive microcapsule alkali activator, and the thermosensitive response structure accounts for 15%-35% of the total mass of the thermosensitive microcapsule alkali activator; After adding water and mixing, the system releases 20%-40% of the total effective components of the alkali activator within 0-2 hours; 40%-70% within 2-12 hours; and 60%-90% within 24 hours.

7. A method for preparing the multi-source solid waste alkali-activated cementitious material according to any one of claims 1-6, comprising the following steps: S1. Select at least two types from slag, fly ash, desulfurized gypsum, steel slag and decarbonized coal gangue, and mix them according to the design ratio after drying, grinding and / or screening to obtain multi-source solid waste cementitious components. S2. Prepare the alkali activator as the alkali activator core, and form a temperature-sensitive response structure on the outside of the alkali activator core to obtain a temperature-sensitive microcapsule alkali activator; S3. Weigh the free alkali activator and the temperature-sensitive microcapsule alkali activator according to the design ratio, and mix them with the multi-source solid waste gelling components. S4. Add water and stir, shape and cure; S5. The free alkali activator is preferentially released in the initial stage of mixing, and after the internal temperature rise generated by the reaction in the multi-source solid waste coagulation system causes the temperature-sensitive response structure to reach the target response temperature, the alkali activator in the temperature-sensitive microcapsule is further released.

8. The preparation method according to claim 7, characterized in that: Step S2 includes: placing the alkali activator core in a fluidized coating device, forming a barrier layer on the surface of the alkali activator core using a barrier layer coating liquid; preparing a temperature-sensitive microgel, mixing the temperature-sensitive microgel with a film-forming material to form a temperature-sensitive response coating liquid, spraying the temperature-sensitive response coating liquid onto the surface of particles with a barrier layer, and obtaining the temperature-sensitive microcapsule alkali activator after drying; Before determining the composition of the temperature-sensitive material, the internal temperature change curve of the corresponding multi-source solid waste coagulation system after water addition was measured from 0 to 48 hours to obtain the initial temperature T0 and the highest temperature T0. max Then according to T r =T0+α(T max -T0) Calculate the target response temperature T r Where 0.4≤α≤0.8; then, by adjusting the type of temperature-sensitive material, the proportion of comonomers, the degree of crosslinking and the coating structure, the actual response temperature of the temperature-sensitive response layer is matched with the target response temperature.

9. A staged controlled-release activation method for a multi-source solid waste alkali-activated gelling material, comprising the following steps: using the multi-source solid waste alkali-activated gelling material according to any one of claims 1-6, adding water and mixing, the free alkali activator preferentially dissolves and is released; the multi-source solid waste gelling system reacts exothermically, causing the internal temperature to rise; when the internal temperature reaches the target response temperature, the temperature-sensitive response structure changes the mass transfer state, causing the alkali activator in the temperature-sensitive microcapsules to be further released; wherein... After mixing with water, 20%-40% of the total effective components of the alkali activator are released cumulatively in 0-2 hours, 40%-70% in 2-12 hours, and 60%-90% in 24 hours.

10. The application of the multi-source solid waste alkali-activated cementitious material according to any one of claims 1-6 in industrial solid waste resource utilization, low-carbon cementitious materials or building materials.