Preparation process of high-durability asphalt concrete composite materials

By modifying basalt fibers with silane coupling agents, adding fibers in stages, and combining them with anti-stripping agents, the problem of uneven fiber dispersion in asphalt mixtures was solved, resulting in improved durability of asphalt concrete and enhanced overall pavement performance.

CN123106071APending Publication Date: 2026-11-17CITIC CONSTR
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611078684.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-20
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In existing technologies, basalt fiber and polyester fiber are difficult to disperse evenly and simultaneously in asphalt mixtures, resulting in poor durability improvement of fiber-reinforced asphalt concrete and easy occurrence of pavement defects during service.

Method used

In-situ modification of basalt fibers was carried out using silane coupling agents. The fibers were added in stages and combined with anti-stripping agents. The temperature gradient was controlled by a heat transfer oil jacket. Activated mineral powder was used to enhance interfacial bonding. Vibration leveling was used to optimize fiber distribution, ultimately forming a high-durability asphalt concrete composite material.

Benefits of technology

It significantly improves the durability of asphalt concrete, enhances high-temperature stability, low-temperature crack resistance and water stability, and extends the service life of the pavement.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

This invention discloses a preparation process for a high-durability asphalt concrete composite material, relating to the field of road engineering materials technology. The invention includes: heating base asphalt and adding a silane coupling agent while stirring to obtain modified asphalt; heating the modified asphalt and adding basalt fibers while shearing to obtain fiber-modified asphalt; dry-mixing coarse aggregate, fine aggregate, and mineral powder and then adding them to the fiber-modified asphalt for wet mixing; adding polyester fibers and mixing; adding an anti-stripping agent and mixing; and finally compacting and molding. This invention improves the fiber-asphalt interface bonding and fiber dispersion uniformity by in-situ modifying basalt fibers in asphalt with a silane coupling agent, combined with the stepwise addition of dual fibers and the post-addition of an anti-stripping agent, significantly enhancing the durability of asphalt concrete. It can be used for paving heavy-duty traffic surfaces such as high-grade highways and bridge decks.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of road engineering materials technology. More specifically, this invention relates to a preparation process for a high-durability asphalt concrete composite material. Background Technology

[0002] Asphalt concrete is one of the main materials for highway pavement construction. During long-term use, asphalt concrete pavements are prone to various defects such as high-temperature rutting, low-temperature cracking, fatigue cracking, and water damage under the combined effects of vehicle loads and environmental factors, affecting driving comfort and safety and shortening the pavement's service life. To improve the road performance of asphalt concrete, researchers have explored incorporating fiber materials into asphalt or asphalt mixtures. Fibers in asphalt mixtures can act as reinforcement, adsorption, stabilization, and viscosity increase, effectively improving the overall performance of asphalt mixtures, including high-temperature stability, low-temperature crack resistance, and water stability. Basalt fiber, due to its high tensile strength and elastic modulus and good compatibility with asphalt mixtures, is considered a promising asphalt mixture reinforcement material. Polyester fiber is also a commonly used asphalt mixture reinforcement material, capable of improving the mixture's resistance to deformation and durability. Researchers have attempted to simultaneously incorporate both types of fiber into asphalt mixtures to leverage their respective reinforcing advantages. However, different fibers have different surface properties, densities, and dispersion behaviors, making it difficult to achieve good dispersion simultaneously under the same process conditions. This can easily lead to uneven dispersion or localized agglomeration, affecting the uniformity of the mixture and the stability of its road performance. These issues often result in the actual durability improvement of fiber-reinforced asphalt concrete falling short of expectations, and various road defects still appearing relatively early during service. Summary of the Invention

[0003] This invention provides a preparation process for a high-durability asphalt concrete composite material, which can improve the fiber-asphalt interface bonding and fiber dispersion uniformity, significantly enhancing the durability of asphalt concrete. It can be used for the paving of heavy-duty traffic pavements such as high-grade highways and bridge decks.

[0004] To achieve these objectives and other advantages according to the present invention, a process for preparing a high-durability asphalt concrete composite material is provided, comprising the following steps: S1 Heat the base asphalt to 160~180℃, add 0.3~1.0% of silane coupling agent by mass of the base asphalt, and stir at 300~500 rpm for 20~30 min at 160~180℃ to obtain silane coupling agent modified asphalt. S2 involves heating silane coupling agent modified asphalt to 190~210℃, adding basalt fibers accounting for 1.5~3.0% of the mass of the base asphalt, with the basalt fibers having a length of 6~12mm and a diameter of 13~25μm, and shearing at 2000~4000rpm for 20~30min at 190~210℃ to obtain fiber modified asphalt; S3. Coarse aggregate, fine aggregate and mineral powder are put into the mixer in a mass ratio of 100:(42~55):(11~16) and dry-mixed at 175~195℃ for 15~25s to obtain a dry mixture. S4 adds 6-11% fiber-modified asphalt by weight of coarse aggregate to the dry mixture and wet mixes it at 175-195℃ for 45-75 seconds to obtain asphalt mixture; S5 adds 0.15~0.5% polyester fiber by mass of coarse aggregate to asphalt mixture. The polyester fiber has a length of 3~9mm and a diameter of 15~30μm. It is mixed at 155~175℃ for 60~90s to obtain fiber reinforced mixture. S6 Add 0.015~0.06% of anti-stripping agent by weight of coarse aggregate to fiber-reinforced mixture, and mix at 155~175℃ for 30~60s to obtain composite material mixture; S7 compacts the composite material mixture at 150~170℃ to obtain a high-durability asphalt concrete composite material.

[0005] Preferably, the silane coupling agent in step S1 is γ-aminopropyltriethoxysilane.

[0006] Preferably, in step S1, before adding the silane coupling agent to the base asphalt, it is first stirred with 1-3% of the aromatic oil by mass ratio of 1:(2-4) at 20-30°C for 3-5 minutes to obtain a silane pre-dispersion, and then the silane pre-dispersion is added to the heated base asphalt.

[0007] Preferably, before adding basalt fibers in step S2, saturated water vapor with a flow rate of 0.2~0.8L / min is introduced into the silane coupling agent modified asphalt for 1~3 minutes. During the introduction process, the mixture is stirred at a speed of 300~500rpm. After the aeration is completed, the mixture is stirred at a constant temperature of 190~210℃ for 2~5 minutes. After no obvious bubbles escape from the asphalt system, the basalt fibers are added and the shearing is started.

[0008] Preferably, the fiber-modified asphalt obtained after shearing in step S2 is stored and transported in an insulated storage tank with a heat transfer oil jacket before being transferred to the mixer and mixed with the dry mixture in step S4. The asphalt cooling rate is controlled within the range of 2~5℃ / min by circulating the heat transfer oil in the jacket. After the asphalt temperature drops to 180~190℃, it is injected into the mixer.

[0009] Preferably, the mineral powder used in step S3 is activated limestone mineral powder that has been calcined at 650~750℃ for 2~3 hours.

[0010] Preferably, the anti-stripping agent in step S6 is an amine-based anti-stripping agent.

[0011] Preferably, the anti-stripping agent added in step S6 is preloaded onto a porous limestone mineral powder carrier. The amount of anti-stripping agent added is based on the effective component of the anti-stripping agent, and the mass ratio of the anti-stripping agent to the carrier mineral powder is 1:(1~2). The loading method is to spray the anti-stripping agent into the stirred mineral powder at room temperature, and obtain the loaded anti-stripping agent after adsorption equilibrium. In step S6, the loaded anti-stripping agent is added to the fiber-reinforced mixture for mixing.

[0012] Preferably, before compaction in step S7, the composite material mixture loaded into the test mold is vibrated and leveled. The vibration frequency is 25~35Hz, the amplitude is 0.3~0.8mm, and the vibration time is 6~12s. After vibration and leveling, double-sided compaction is performed. During the compaction process, the test mold is placed in a heat-insulating sleeve preheated to 140~160℃.

[0013] Preferably, after compaction and before demolding in step S7, the specimen and the mold are placed in a constant temperature chamber at 120~140℃ for 4~6 hours for heat preservation. After curing, the specimen is taken out and allowed to cool naturally until the temperature of the specimen is below 60℃ before demolding.

[0014] The present invention has at least the following beneficial effects: First, this invention modifies basalt fibers in asphalt in situ using a silane coupling agent, eliminating the need for separate fiber pretreatment. The addition of two fibers in stages avoids mutual interference from simultaneous feeding. The anti-stripping agent is added later to prevent high-temperature degradation. All three work together to improve the overall durability of asphalt concrete.

[0015] Secondly, this invention uses a silane coupling agent that is premixed with aromatic oil at room temperature before being added to asphalt to avoid local agglomeration caused by polarity differences. Saturated water vapor is introduced before adding basalt fibers to provide hydrolysis-bound water, thereby improving coupling efficiency and strengthening the interfacial bonding strength of the fibers.

[0016] Third, this invention controls the slow cooling of fiber-modified asphalt through a heat-conducting oil jacket, avoiding damage to the interfacial chemical bonds by sudden cooling thermal stress. It also uses calcined activated mineral powder to connect to the coupling network, thereby improving the cohesive strength of the mortar and simultaneously improving high-temperature stability and water stability.

[0017] Fourth, this invention achieves slow-release and uniform distribution by loading anti-stripping agent onto porous mineral powder, optimizes the three-dimensional distribution of fibers by vibration leveling before compaction, and improves the coupling and cross-linking network by heat preservation and curing after molding, thereby enhancing the overall durability of the composite material in multiple dimensions.

[0018] Other advantages, objectives and features of the present invention will become apparent in part from the following description, and in part from those skilled in the art through study and practice of the invention. Detailed Implementation

[0019] The present invention will be further described in detail below with reference to examples, so that those skilled in the art can implement it based on the description.

[0020] It should be understood that terms such as "having," "comprising," and "including" as used herein do not exclude the presence or addition of one or more other elements or combinations thereof. It should be noted that the experimental methods described in the following embodiments, unless otherwise specified, are conventional methods, and the reagents and materials, unless otherwise specified, are commercially available and therefore should not be construed as limiting the invention.

[0021] This invention provides a preparation process for a high-durability asphalt concrete composite material, comprising the following steps: S1. The base asphalt is heated to 160~180℃. The base asphalt can be No. 70 or No. 90 road petroleum asphalt. 0.3~1.0% of silane coupling agent by mass of base asphalt is added. The general formula of silane coupling agent is Y-Si-X3, where X is a hydrolyzable alkoxy group and Y is a functional group that can react with organic polymers. Stir at 300~500 rpm for 20~30 min at 160~180℃ to fully disperse and partially hydrolyze the silane coupling agent in the asphalt. The alkoxy group in the silane coupling agent molecule is partially hydrolyzed under the action of trace moisture in the asphalt to generate silanol groups (Si-OH), thus obtaining silane coupling agent modified asphalt. S2 involves heating silane coupling agent modified asphalt to 190-210℃, adding basalt fibers (1.5-3.0% of the matrix asphalt mass), with a length of 6-12 mm and a diameter of 13-25 μm. The asphalt is then sheared at 2000-4000 rpm for 20-30 minutes at 190-210℃ to disperse the basalt fibers into monofilaments, which are then uniformly distributed in the asphalt system. The silane coupling agent dispersed in the asphalt reacts chemically with the surface of the basalt fibers; specifically, the silanol groups in the coupling agent molecules condense with the silanol groups on the fiber surface, forming Si-O-Si covalent bonds. This chemically anchors the coupling agent to the fiber surface, resulting in fiber-modified asphalt. S3 adds coarse aggregate (crushed stone or gravel with a particle size greater than 2.36 mm), fine aggregate (natural sand, artificial sand or stone chips with a particle size less than 2.36 mm), and mineral powder (alkaline stone powder with a particle size less than 0.075 mm) into a mixer at a mass ratio of 100:(42~55):(11~16) and dry-mixes it at 175~195℃ for 15~25s to uniformly mix the aggregates and mineral powder of different particle sizes and obtain a dry mixture. S4 adds 6-11% fiber-modified asphalt by weight of coarse aggregate to the dry mixture and wet mixes it at 175-195℃ for 45-75 seconds to obtain asphalt mixture; S5 involves adding 0.15-0.5% polyester fiber (by weight of coarse aggregate) to asphalt mixtures. The polyester fiber has a length of 3-9 mm and a diameter of 15-30 μm. The mixture is stirred at 155-175℃ for 60-90 seconds, allowing the polyester fiber to disperse in the gaps of the mixture skeleton under stirring. This forms a complementary reinforcement with the basalt fiber already dispersed in the asphalt mastic, resulting in a fiber-reinforced mixture. S6 adds an anti-stripping agent at a mass of 0.015~0.06% of the coarse aggregate to the fiber-reinforced mixture and mixes it at 155~175℃ for 30~60s. The anti-stripping agent contains polar groups and non-polar segments in its molecular structure. During the mixing process, the polar groups are adsorbed on the aggregate surface, and the non-polar segments are compatible with the asphalt, forming a chemical bridge at the asphalt-aggregate interface to obtain the composite material mixture. S7 uses the Marshall compaction method, where the composite material mixture is compacted at 150~170℃. The mixture is placed into a mold preheated to the molding temperature and compacted on both sides with a compaction hammer to obtain a high-durability asphalt concrete composite material.

[0022] In the above technical solution, the silane coupling agent modifies the basalt fiber in situ in the asphalt, improving the interfacial bonding between the asphalt and the basalt fiber. The basalt fiber and polyester fiber are added stepwise and dispersed in the asphalt phase and the mixture phase at different stages. The basalt fiber forms a fiber-reinforced network in the asphalt mastic, improving the high-temperature stability and deformation resistance of the asphalt mastic. The polyester fiber forms a secondary reinforcement network in the gaps of the mixture skeleton, improving the crack resistance of the mixture. The anti-stripping agent is added after the fiber dispersion is completed, avoiding the impact of long-term high-temperature treatment on its performance, improving the interfacial adhesion between the asphalt and the aggregate, and enhancing the overall durability of the asphalt concrete.

[0023] In another technical solution, the silane coupling agent in step S1 is γ-aminopropyltriethoxysilane (KH550), which has good dispersibility and thermal stability in the asphalt system. Its amino functional group can form hydrogen bonds or undergo chemical reactions with polar groups such as carboxyl and carbonyl groups in the asphalt. The ethoxy functional group generates silanol groups (-SiOH) after hydrolysis, which can undergo condensation reactions with silanol groups on the surface of basalt fibers to form Si-O-Si covalent bonds, thereby improving the interfacial bonding strength between the fiber and the asphalt and enabling the fiber to play a more effective reinforcing role in the composite material.

[0024] In another technical solution, before adding the silane coupling agent to the base asphalt in step S1, it is first stirred with 1-3% of the aromatic oil (by mass of the base asphalt) at a mass ratio of 1:(2-4) at 20-30°C for 3-5 minutes. By utilizing the compatibility between the aromatic oil and the silane coupling agent, as well as the good compatibility between the aromatic oil and the asphalt, the silane coupling agent is in a pre-dispersed state before entering the asphalt system, resulting in a silane pre-dispersion. The silane pre-dispersion is then added to the heated base asphalt, making the coupling agent more evenly distributed in the asphalt and avoiding local agglomeration caused by polarity differences when the silane coupling agent is directly added to the hot asphalt.

[0025] In another technical solution, before adding basalt fibers in step S2, saturated steam with a flow rate of 0.2~0.8L / min is introduced into the silane coupling agent modified asphalt using an immersion steam gun for 1~3 minutes. During the introduction process, the stirring speed is maintained at 300~500rpm. The introduced saturated steam rapidly vaporizes at a high temperature of 190~210℃. The trace amount of water in the steam provides bound water for the hydrolysis reaction of the silane coupling agent before vaporization, allowing the steam to fully contact the asphalt. After the aeration is completed, the mixture is stirred at a constant temperature of 190~210℃ for 2~5 minutes. Most of the water rapidly vaporizes and escapes after providing the bound water required for hydrolysis, and will not form a stable foam phase in the asphalt. After no obvious bubbles escape from the asphalt system (i.e., no more continuous bubbles rise to the liquid surface by visual observation), the basalt fibers are added and shearing is initiated to avoid interference from residual bubbles on the subsequent fiber shearing and dispersion, thus ensuring the dispersion quality of the fibers in the asphalt.

[0026] In another technical solution, the fiber-modified asphalt obtained after shearing in step S2 is subjected to slow cooling control in an insulated storage tank with a heat-conducting oil jacket before being transferred to the mixer and mixed with the dry mixture in step S4. Specifically, the asphalt is stored and transported in an insulated storage tank with a heat-conducting oil jacket, and the cooling rate of the asphalt is controlled within the range of 2~5℃ / min by circulating the heat-conducting oil in the jacket. After the asphalt temperature drops to 180~190℃, it is injected into the mixer. Since there is a difference in the thermal expansion coefficient between basalt fiber and asphalt matrix, the slow cooling treatment makes the shrinkage process of asphalt matrix and fiber tend to be synchronized, protecting the interfacial bonding state and providing stable quality fiber-modified asphalt for subsequent mixing with aggregates.

[0027] In another technical solution, the mineral powder used in step S3 is activated limestone mineral powder that has been calcined at 650~750℃ for 2~3 hours. The adsorbed water and organic impurities on the surface are removed, the specific surface area is increased, and the surface active sites are exposed. The activated mineral powder can chemically bond with the silane coupling agent dispersed in the asphalt in the asphalt mortar, and embed itself in the coupling reinforcement network of the asphalt mortar, thereby improving the cohesive strength and deformation resistance of the asphalt mortar.

[0028] In another technical solution, the anti-stripping agent in step S6 is an amine-based anti-stripping agent, including aliphatic polyamines, alkylamines, amide compounds, etc. Amine-based anti-stripping agents contain polar amino groups, which can form strong chemical adsorption with the active sites on the surface of aggregates (especially acidic aggregates). At the same time, their non-polar segments have good compatibility with asphalt and can form a strong chemical bridge at the asphalt-aggregate interface.

[0029] In another technical solution, the anti-stripping agent added in step S6 is preloaded onto a porous limestone mineral powder carrier. The porous structure of the mineral powder is used to adsorb the liquid anti-stripping agent into the pores. The amount of anti-stripping agent added is based on the effective component of the anti-stripping agent, and the mass ratio of the anti-stripping agent to the carrier mineral powder is 1:(1~2). The loading method is to spray the anti-stripping agent into the stirred mineral powder at room temperature, so that the anti-stripping agent is uniformly attached to the surface of the mineral powder particles and penetrates into the pores. After stirring until the rate of adsorption and desorption of the anti-stripping agent by the mineral powder reaches equilibrium, a loaded anti-stripping agent is obtained. In step S6, the loaded anti-stripping agent is added to the fiber-reinforced mixture for mixing. During the mixing process, the anti-stripping agent is gradually released from the pores of the mineral powder.

[0030] In another technical solution, before compaction in step S7, the composite material mixture loaded into the mold is vibrated and leveled. The mold containing the mixture is placed on a vibration platform with a vibration frequency of 25~35Hz, an amplitude of 0.3~0.8mm, and a vibration time of 6~12s. During the vibration, the mixture is evenly distributed in the mold, and the fibers form a random three-dimensional spatial distribution under the vibration. After vibration leveling, double-sided compaction is performed. During the compaction, the mold is placed in an insulation sleeve preheated to 140~160℃. The random distribution of fibers and the isotropic compaction quality help the composite material exhibit more balanced mechanical properties in different stress directions.

[0031] In another technical solution, after compaction and before demolding in step S7, the specimen and mold are placed in a constant temperature chamber at 120~140℃ for 4~6 hours for curing. During the curing process, a more complete Si-O-Si three-dimensional cross-linked network is gradually formed between the coupling agent molecules and between them and the surface of the fiber and mineral powder. After curing, the specimen is taken out and naturally cooled until the temperature of the specimen is below 60℃ before demolding. The composite material after curing has higher interfacial bonding strength, and its fatigue resistance and long-term durability are further improved.

[0032] <Example 1> The preparation process of high-durability asphalt concrete composite materials includes the following steps: S1 heats No. 70 road petroleum asphalt to 160℃, adds 0.5% of the matrix asphalt mass of silane coupling agent KH550, and stirs at 500 rpm for 30 minutes at 160℃ to obtain silane coupling agent modified asphalt. S2. The silane coupling agent modified asphalt is heated to 200℃, and basalt fibers (9mm in length and 20μm in diameter) accounting for 2% of the mass of the base asphalt are added. The asphalt is sheared at 3000rpm for 20min at 200℃ to obtain fiber modified asphalt. It is stored and transported in an insulated storage tank with a heat transfer oil jacket. The cooling rate is controlled at 3℃ / min by circulating the heat transfer oil in the jacket. After the temperature drops to 180℃, it is injected into the mixing plant to execute step S4. S3 adds coarse aggregate, fine aggregate and mineral powder into a mixer at a mass ratio of 100:50:15 and dry mixes at 180℃ for 20 seconds to obtain a dry mixture. S4 adds fiber-modified asphalt at a mass of 10% of coarse aggregate to the dry mixture and wet-mixes it at 180℃ for 60 seconds to obtain an asphalt mixture. S5 adds 0.2% polyester fiber (6mm in length and 20μm in diameter) by mass of coarse aggregate to asphalt mixture, and mixes at 160℃ for 90s to obtain fiber-reinforced mixture; S6 Add 0.05% of the coarse aggregate mass of amine anti-stripping agent PA-1 to the fiber-reinforced mixture, and mix at 160℃ for 40s to obtain the composite material mixture; S7 compacts the composite material mixture at 160°C to obtain a high-durability asphalt concrete composite material.

[0033] <Example 2> The preparation process of the high-durability asphalt concrete composite material is the same as in Example 1, except that... The mineral powder used in step S3 is activated limestone mineral powder that has been calcined at 650~750℃ for 2~3 hours.

[0034] <Example 3> The preparation process of the high-durability asphalt concrete composite material is the same as in Example 2, except that... In step S1, before adding the silane coupling agent to the base asphalt, it is first stirred with 2% aromatic oil (by mass of the base asphalt) at a mass ratio of 1:2 at 22°C for 5 minutes to obtain a silane pre-dispersion. The silane pre-dispersion is then added to the heated base asphalt. Before adding basalt fiber in step S2, saturated water vapor with a flow rate of 0.5 L / min is introduced into the silane coupling agent modified asphalt for 2 min. During the introduction process, the mixture is stirred at a speed of 500 rpm. After the aeration is completed, the mixture is stirred at a constant temperature of 200℃ for 5 min. After no obvious bubbles escape from the asphalt system, the basalt fiber is added and the shearing is started.

[0035] <Example 4> The preparation process of the high-durability asphalt concrete composite material is the same as in Example 3, except that... In step S6, the anti-stripping agent is preloaded onto a porous limestone mineral powder carrier. The amount of anti-stripping agent added is based on the effective component of the anti-stripping agent. The mass ratio of the anti-stripping agent to the carrier mineral powder is 1:1.5. The loading method is to spray the anti-stripping agent into the stirred mineral powder at room temperature. After adsorption equilibrium is reached, the loaded anti-stripping agent is obtained. In step S6, the loaded anti-stripping agent is added to the fiber-reinforced mixture and mixed. Before compaction molding in step S7, the composite material mixture loaded into the test mold is vibrated and leveled. The vibration frequency is 25~35Hz, the amplitude is 0.3~0.8mm, and the vibration time is 6~12s. After vibration and leveling, double-sided compaction is carried out. During the compaction process, the test mold is placed in a heat-insulating sleeve preheated to 140~160℃. After compaction and before demolding in step S7, place the specimen and mold together in a constant temperature chamber at 120~140℃ for 4~6 hours for curing. After curing, remove the specimen and allow it to cool naturally until the specimen temperature is below 60℃ before demolding.

[0036] <Comparative Example 1> The preparation process of the asphalt concrete composite material is the same as in Example 1, except that KH550 is not added. That is, in step S1, only No. 70 road petroleum asphalt is heated and stirred, and no silane coupling agent is added. The heated asphalt is directly heated to 200°C and basalt fiber is added for shearing.

[0037] <Comparative Example 2> The preparation process of the asphalt concrete composite material is the same as in Example 1, except that basalt fiber and polyester fiber are not added, i.e., S2 and S5 are not included.

[0038] <Comparative Example 3> The preparation process of the asphalt concrete composite material is the same as in Example 1, except that KH550, no fibers, and no anti-stripping agents are added. Coarse aggregate, fine aggregate, and mineral powder are added to a mixer in a mass ratio of 100:50:15 and dry-mixed at 180°C for 20 seconds to obtain a dry mixture. 10% of the mass of coarse aggregate (No. 70 road petroleum asphalt) is added to the dry mixture and wet-mixed at 180°C for 60 seconds to obtain an asphalt mixture. The asphalt mixture is then compacted at 160°C to obtain a high-durability asphalt concrete composite material.

[0039] <Comparative Example 4> The preparation process of the asphalt concrete composite material is the same as in Example 1, except that basalt fiber and polyester fiber are added simultaneously in stage S5. That is, basalt fiber is not added in step S2, but only heat-preserved to the corresponding temperature. In S5, basalt fiber accounting for 2% of the mass of the matrix asphalt and polyester fiber accounting for 0.2% of the mass of the coarse aggregate are added to the asphalt mixture.

[0040] <Rut Test> The test method was performed according to T0719—2011 in JTG E20-2011. Specimen molding followed the wheel rolling method in T0703—2011. The specimen size was 300mm×300mm×50mm. The compaction temperature of the mixture was controlled at 160℃. The wheel rolling mill was preheated to no less than 160℃. The mixtures from Examples 1-4 and Comparative Examples 1-4 were loaded into the molds and leveled. The molds were then placed under the wheel rolling mill. The mixtures were rolled back and forth twice, and then the specimen direction was reversed, and the rolling was continued for a total of 12 rounds to ensure the compaction degree of the specimens. If the requirements are met, after the specimen is formed, it should be placed at room temperature for 12 hours along with the mold. After demolding, the specimen should be placed in a constant temperature chamber at 60℃ for 6 hours to ensure uniform internal temperature. The specimen should then be placed on the test bench of the rutting tester with the ground pressure of the test wheel at 0.7 MPa. The contact surface between the test wheel and the specimen should be located in the center of the specimen, and the direction of travel should be consistent with the forming direction of the specimen. The tester should be started and the test wheel should be moved back and forth on the surface of the specimen at 60℃. The recorder should automatically record the deformation-time curve within 0 to 60 minutes. After the test, the specimen should be removed.

[0041] The dynamic stability is calculated as follows: DS = (t2 - t1) × N / (d2 - d1) In the formula, DS represents dynamic stability, in units of cycles / mm, t1 represents 45 min after the start of the test, t2 represents 60 min after the start of the test, N represents the rolling speed, 42 cycles / min, d1 represents the deformation at time t1, in units of mm, and d2 represents the deformation at time t2, in units of mm.

[0042] The linear segment of the deformation curve within the 45min~60min interval was used for calculation. Three specimens were used in each group, and the average value was taken as the test result. The test results are shown in Table 1.

[0043] Table 1 As shown in Table 1, the dynamic stability of Examples 1-4 is superior to that of Comparative Examples 1-4. The dynamic stability of Example 2 is improved compared to Example 1. This is likely because the pre-dispersion of aromatic oil ensures that KH550 is uniformly dispersed in the aromatic oil before being added to the asphalt, avoiding localized agglomeration during direct addition. Steam treatment provides bound water for the hydrolysis of KH550, improving coupling efficiency and allowing more fibers to form a complete chemical bond layer, resulting in stronger fiber anchoring at high temperatures. The dynamic stability of Example 3 is improved compared to Example 2. This is likely because slow cooling control avoids damage to chemical bonds caused by interfacial thermal stress from rapid cooling. After calcination, the active sites on the surface of the activated mineral powder are exposed, enabling it to chemically bond with KH550. It transforms from an inert filler into an active node of the coupling network, improving the high-temperature cohesive strength of the mortar. The dynamic stability of Example 4 is improved compared to Example 3. This is probably because the slow release of the mineral powder load allows the anti-stripping agent to be released uniformly, forming a uniform adsorption layer on the aggregate surface. Vibration leveling causes the fibers to form a three-dimensional random distribution. Heat preservation and curing promote the condensation and cross-linking of the coupling agent, and the interfacial network tends to be perfect. The interfacial stability and load transfer efficiency at high temperature reach the optimal level.

[0044] The dynamic stability of Example 1 is better than that of Comparative Example 1. This is probably because in Comparative Example 1, the basalt fiber and the asphalt are only physically adsorbed, and the interface is easy to debond at high temperature, so the fiber cannot effectively transfer stress. In Example 1, KH550 forms a chemical bonding layer on the fiber surface, which makes the fiber more firmly anchored at high temperature.

[0045] The dynamic stability of Example 1 is better than that of Comparative Example 2. This is probably because in Comparative Example 2, the mixture only relies on the asphalt bonding force and aggregate interlocking force to resist deformation. At high temperature, both of these resistances are greatly reduced. In Example 1, basalt fiber forms a micron-level reinforcing network in the asphalt mortar, and polyester fiber forms a millimeter-level reinforcing network in the skeleton gaps. The two types of fibers play a reinforcing and constraining role on the aggregate skeleton at different scales.

[0046] The dynamic stability of Example 1 is better than that of Comparative Example 3. This is probably because Comparative Example 3 is a common No. 70 asphalt mixture, which does not contain fibers, coupling agents and anti-stripping agents. At high temperature, the viscosity of asphalt is greatly reduced, the aggregate skeleton lacks additional constraints, and deformation accumulates rapidly. In Example 1, the fiber reinforcement, coupling agent interface modification and anti-stripping agent interface protection work together to improve the high temperature deformation resistance of the mixture.

[0047] The dynamic stability of Example 1 is better than that of Comparative Example 4. This is probably because the two fibers in Comparative Example 4 are intertwined and agglomerated when added at the same time due to differences in surface properties and density, making it difficult to disperse them fully. In Example 1, the basalt fiber is first dispersed by high-speed shearing in the asphalt phase, and the polyester fiber is then dispersed by mixing in the mixture phase. The two fibers obtain the optimal dispersion conditions at different stages, avoiding mutual interference.

[0048] Low-Temperature Bending Test The test method was performed in accordance with T0715—2011 of JTG E20-2011. The specimen was cut into 250mm×30mm×35mm prism beams from the plate-shaped specimen formed by the rutting test. The beam specimens were placed in an environmental chamber at -10℃ for 6 hours. The specimens were then removed from the environmental chamber and placed on a three-point bending fixture with a span of 200mm. A load was applied uniformly at a loading rate of 50mm / min until the specimen failed. The failure load P (N) and the mid-span deflection d (mm) were recorded.

[0049] The maximum flexural strain is calculated as follows: ε B = 6 × h × d × 10 6 / L 2 In the formula, ε B The maximum bending tensile strain is expressed in με, h represents the specimen height in mm, d represents the mid-span deflection in mm, and L represents the span, which is 200 mm.

[0050] Five specimens were tested in each group, and the average value was taken as the test result. The test results are shown in Table 2.

[0051] Table 2 As shown in Table 2, the maximum flexural tensile strain of Examples 1-4 is superior to that of Comparative Examples 1-4. Example 2 shows an improvement over Example 1, likely because the pre-dispersion of aromatic oil ensures that KH550 is uniformly dispersed in the aromatic oil before being added to the asphalt, avoiding localized agglomeration during direct addition. Steam treatment provides bound water for the hydrolysis of KH550, improving coupling efficiency and allowing more fibers to form a complete chemical bond layer. This results in higher interfacial bonding strength and greater fiber pull-out resistance at low temperatures, with the failure mode shifting from interfacial brittle debonding to energy-consuming fiber pull-out, leading to increased fracture work. Example 3 shows an improvement over Example 2, likely because slow cooling control avoids interfacial thermal stress microcracks caused by rapid cooling, reducing initial defect points for crack initiation. After calcination, the surface active sites of the mineral powder are exposed, enabling it to chemically bond with KH550 and connect to the coupling network. This optimizes the cohesive toughness of the asphalt mortar and delays the initiation and propagation of microcracks within the mortar. Example 4 shows improvement compared to Example 3, likely because vibration leveling breaks the directional arrangement of fibers, forming a three-dimensional randomly distributed fiber network. During crack propagation, the fiber needs to be constantly bypassed, causing path deflection, which significantly increases crack propagation resistance and fracture energy consumption. Thermal insulation promotes the condensation and crosslinking of the silane coupling agent, further improving the interfacial chemical bonding network and reducing initial interfacial defects. The main function of the mineral powder-loaded anti-stripping agent is to improve the adhesion and water stability of the asphalt-aggregate interface, with limited direct contribution to low-temperature bending strain.

[0052] The maximum flexural strain of Example 1 is better than that of Comparative Example 1. This is probably because in Comparative Example 1, the basalt fiber and the asphalt are only physically adsorbed, the interface is brittle at low temperature, and the crack is prone to debonding when it extends to the interface. The fiber pull-out resistance is small, the energy consumption is low, and the crack prevention efficiency is poor. In Example 1, KH550 forms a chemical bonding layer on the fiber surface, which significantly improves the low-temperature anchoring strength of the fiber.

[0053] The maximum flexural strain of Example 1 is better than that of Comparative Example 2. This is probably because Comparative Example 2 is a silane-modified asphalt mixture without fibers. At low temperatures, the asphalt mortar is significantly brittle. After crack initiation, it propagates rapidly in a linear manner without any additional energy dissipation mechanism, exhibiting typical brittle fracture. In Example 1, basalt fibers form a micron-level reinforcing network in the asphalt mortar, which slows down the propagation of microcracks inside the mortar. Polyester fibers form a millimeter-level reinforcing network in the skeleton gaps, bridging macroscopic cracks. The two levels of fibers jointly consume fracture energy, effectively slowing down the crack penetration rate.

[0054] The maximum flexural strain of Example 1 is better than that of Comparative Example 3. This is probably because Comparative Example 3 is a regular No. 70 asphalt mixture that does not contain fibers, coupling agents, or anti-stripping agents. Asphalt itself is brittle at low temperatures, and the mixture lacks any reinforcement or toughening mechanism. After crack initiation, it quickly penetrates the specimen, resulting in extremely poor deformation capacity. In Example 1, the synergistic effect of dual-fiber phase separation reinforcement and silane interface modification improves the resistance from multiple stages of crack initiation and propagation, achieving a leapfrog improvement in low-temperature deformation capacity.

[0055] The maximum flexural strain in Example 1 is better than that in Comparative Example 4. This is probably because, in Comparative Example 4, the two types of fibers, due to differences in surface properties and density, become entangled and agglomerated when added simultaneously. These agglomerates become stress concentration sources at low temperatures, causing cracks to preferentially initiate at the agglomeration sites, thus reducing the fracture strain. In Example 1, the stepwise addition allows the basalt fibers to first be rapidly sheared and dispersed in the asphalt phase, followed by the polyester fibers being mixed and dispersed in the mixture phase. After the two types of fibers are fully dispersed, they each play a bridging and crack-preventing role, avoiding mutual interference and stress concentration caused by agglomerates.

[0056] <Marshall Immersion Test> The test method was performed according to T 0709—2011 in JTG E20-2011. The specimens were formed by the compaction method according to T0702—2011, and were standard Marshall specimens with a diameter of 101.6 mm and a height of 63.5 mm. They were compacted on both sides 75 times. There were 8 specimens in each group of Examples 1-4, Comparative Examples 1 and 3. The specimens were divided into two groups of 4 specimens each. Group 1 (not immersed in water): the specimens were placed in a 60℃ water bath for 30 min and the Marshall stability MS1 was measured immediately after removal. Group 2 (immersed in water): the specimens were placed in a 60℃ water bath for 48 h and the Marshall stability MS2 was measured immediately after removal. The loading rate was maintained at 50 mm / min and the failure load was recorded.

[0057] The residual stability is calculated as follows: MS0 = MS2 / MS1 × 100% In the formula, MS0 represents the residual stability (%), MS1 represents the average Marshall stability of the unimmersed specimen (in kN), and MS2 represents the average Marshall stability of the specimen immersed in water for 48 hours (in kN).

[0058] Four specimens were tested in each group, and the average value was taken as the test result. The test results are shown in Table 3.

[0059] Table 3 As shown in Table 3, the residual stability of Examples 1-4 is superior to that of Comparative Examples 1 and 3. Example 2 shows an improvement over Example 1, likely because the pre-dispersion of aromatic oil ensures that KH550 is uniformly dispersed in the aromatic oil before being added to the asphalt, avoiding localized agglomeration during direct addition. Steam treatment provides bound water for the hydrolysis of KH550, improving coupling efficiency and allowing more fibers to form a complete chemical bond layer. This coupling layer forms a hydrophobic barrier on the fiber surface, hindering water penetration along the fiber-asphalt interface. Example 3 shows an improvement over Example 2, likely because slow cooling control avoids interfacial thermal stress microcracks caused by rapid cooling, reducing the channels for water intrusion. The activated mineral powder's surface active sites are exposed after calcination, enabling it to interact with... KH550 undergoes chemical bonding, transforming from an inert filler into an active node in the coupling network, making it more difficult for moisture to penetrate along the mineral powder-asphalt interface. Example 4 shows an improvement over Example 3, likely because the slow-release loading of mineral powder allows the anti-stripping agent to be gradually released from the pores of the mineral powder, avoiding the uneven distribution caused by local agglomeration when the liquid anti-stripping agent is directly added. The anti-stripping agent forms a uniform and dense hydrophobic adsorption layer on the aggregate surface, effectively resisting the erosion of the asphalt-aggregate interface by moisture. Vibration leveling causes the fibers to form a three-dimensional random distribution, and heat preservation and curing promote the condensation and cross-linking of the coupling agent, making the interface network more perfect and further reducing the risk of moisture penetration along the interface.

[0060] The residual stability of Example 1 is better than that of Comparative Example 1. This is probably because in Comparative Example 1, the basalt fiber and the asphalt are only physically adsorbed, and water can easily penetrate along the fiber-asphalt interface and destroy the bond. In Example 1, KH550 forms a chemical bond layer on the fiber surface, which effectively prevents water from penetrating along the interface. Both have amine anti-stripping agents to protect the asphalt-aggregate interface.

[0061] The residual stability of Example 1 is better than that of Comparative Example 3. This is probably because Comparative Example 3 is a common No. 70 asphalt mixture, which does not contain coupling agents, fibers and anti-stripping agents. The asphalt and aggregate are only physically adhered, and water can easily penetrate along the interface and weaken the adhesion. In Example 1, the interface chemical modification of KH550 and the interface protection of amine anti-stripping agents work together to significantly improve the interface's resistance to water stripping.

[0062] <Freeze-thaw splitting test> The test method was performed according to T 0729—2011 in JTG E20-2011. Specimens were formed using the compaction method according to T0702—2011, resulting in standard Marshall specimens with a diameter of 101.6 mm and a height of 63.5 mm. Each side was compacted 75 times. Eight specimens were prepared for each group in Examples 1-4, Comparative Examples 1 and 3, and divided into two groups of four. The first group (no freeze-thaw): specimens were placed in a 25℃ water bath for 2 hours, and immediately after removal, a splitting tensile test was performed to determine the splitting strength R1. The second group (freeze-thaw)... The specimen was saturated with water for 15 minutes under a vacuum of 98.5 kPa. After returning to normal pressure, it was soaked for another 0.5 hours. The saturated specimen was then placed in a plastic bag with 10 mL of water, sealed, and frozen in a -18°C freezer for 16 hours. The specimen was then removed and immediately placed in a 60°C water bath to thaw for 24 hours. The specimen was then placed in a 25°C water bath to keep warm for 2 hours. Immediately after removal, a splitting test was performed to determine the splitting strength R2. The splitting test loading rate was 50 mm / min, and the failure load was recorded.

[0063] The freeze-thaw splitting strength ratio is calculated as follows: TSR = R2 / R1 × 100% In the formula, TSR represents the freeze-thaw splitting strength ratio, in %; R1 represents the average splitting strength of the unfrozen specimen, in MPa; and R2 represents the average splitting strength of the freeze-thaw specimen, in MPa.

[0064] Four specimens were tested in each group, and the average value was taken as the test result. The test results are shown in Table 4.

[0065] Table 4 As shown in Table 4, the TSR of Examples 1-4 is superior to that of Comparative Examples 1 and 3. Example 2 shows an improvement over Example 1, likely because the pre-dispersion of aromatic oil ensures that KH550 is uniformly dispersed in the aromatic oil before being added to the asphalt, avoiding local agglomeration during direct addition. Steam treatment provides bound water for the hydrolysis of KH550, improving coupling efficiency and allowing more fiber surfaces to form complete chemically bonded layers. During freeze-thaw cycles, the expansion of water upon freezing generates frost heave force, and the complete coupling layer effectively prevents water penetration along the fiber-asphalt interface. Example 3 shows an improvement over Example 2, likely because slow cooling control avoids interfacial thermal stress microcracks caused by sudden cooling, reducing the points of application of frost heave force. Activated mineral powder is embedded in the coupling network through chemical bonds, and the chemically bonded mineral powder-asphalt interface has higher resistance to frost heave during freeze-thaw cycles, while the physical interface between ordinary mineral powder and asphalt is easily cracked by ice crystals. Example 4 shows an improvement over Example 3, likely because the slow release of mineral powder loading makes the anti-stripping agent more evenly distributed, vibration leveling makes the fibers three-dimensionally randomly distributed, avoiding local stress concentration caused by anisotropy, and heat preservation allows the coupling agent condensation and cross-linking reaction to proceed fully, making the Si-O-Si three-dimensional network more complete and exhibiting higher structural stability during freeze-thaw cycles.

[0066] The TSR of Example 1 is better than that of Comparative Example 1. This is probably because in Comparative Example 1, the basalt fiber and the asphalt are only physically adsorbed. During the freeze-thaw cycle, water seeps in along the fiber-asphalt interface. The frost heave force generated by the expansion of ice causes the microcracks at the interface to gradually expand, and the fiber anchoring fails. In Example 1, the Si-O-Si chemical bond layer formed by KH550 on the fiber surface has extremely high hydrolytic stability and can effectively resist the penetration of water along the interface and the damage caused by the frost heave force.

[0067] The TSR of Example 1 is better than that of Comparative Example 3. This is probably because Comparative Example 3 is a common No. 70 asphalt mixture, which does not contain coupling agents, fibers and anti-stripping agents. During the freeze-thaw cycle, water penetrates along the asphalt-aggregate interface, and the expansion of ice causes the interface to gradually debond, resulting in a significant decrease in strength.

[0068] The number of devices and processing scale described herein are for the purpose of simplifying the description of the invention. Applications, modifications, and variations of the invention will be readily apparent to those skilled in the art.

[0069] Although embodiments of the present invention have been disclosed above, they are not limited to the applications listed in the specification and embodiments. They can be applied to various fields suitable for the present invention. For those skilled in the art, other modifications can be easily made. Therefore, without departing from the general concept defined by the claims and their equivalents, the present invention is not limited to the specific details and examples shown and described herein.

Claims

1. A preparation process for high-durability asphalt concrete composite materials, characterized in that, Includes the following steps: S1 Heat the base asphalt to 160~180℃, add 0.3~1.0% of silane coupling agent by mass of the base asphalt, and stir at 300~500 rpm for 20~30 min at 160~180℃ to obtain silane coupling agent modified asphalt. S2 involves heating silane coupling agent modified asphalt to 190~210℃, adding basalt fibers accounting for 1.5~3.0% of the mass of the base asphalt, with the basalt fibers having a length of 6~12mm and a diameter of 13~25μm, and shearing at 2000~4000rpm for 20~30min at 190~210℃ to obtain fiber modified asphalt; S3. Coarse aggregate, fine aggregate and mineral powder are put into the mixer in a mass ratio of 100:(42~55):(11~16) and dry-mixed at 175~195℃ for 15~25s to obtain a dry mixture. S4 adds 6-11% fiber-modified asphalt by weight of coarse aggregate to the dry mixture and wet mixes it at 175-195℃ for 45-75 seconds to obtain asphalt mixture; S5 adds 0.15~0.5% polyester fiber by mass of coarse aggregate to asphalt mixture. The polyester fiber has a length of 3~9mm and a diameter of 15~30μm. It is mixed at 155~175℃ for 60~90s to obtain fiber reinforced mixture. S6 Add 0.015~0.06% of anti-stripping agent by weight of coarse aggregate to fiber-reinforced mixture, and mix at 155~175℃ for 30~60s to obtain composite material mixture; S7 compacts the composite material mixture at 150~170℃ to obtain a high-durability asphalt concrete composite material.

2. The preparation process of the high-durability asphalt concrete composite material according to claim 1, characterized in that, In step S1, the silane coupling agent is γ-aminopropyltriethoxysilane.

3. The preparation process of the high-durability asphalt concrete composite material according to claim 1, characterized in that, In step S1, before adding the silane coupling agent to the base asphalt, it is first stirred with 1-3% of the aromatic oil by mass ratio of 1:(2-4) at 20-30℃ for 3-5 minutes to obtain a silane pre-dispersion. Then, the silane pre-dispersion is added to the heated base asphalt.

4. The preparation process of the high-durability asphalt concrete composite material according to claim 1, characterized in that, Before adding basalt fibers in step S2, saturated water vapor with a flow rate of 0.2~0.8L / min is introduced into the silane coupling agent modified asphalt for 1~3 minutes. During the introduction process, the stirring speed is maintained at 300~500rpm. After the aeration is completed, the mixture is stirred at a constant temperature of 190~210℃ for 2~5 minutes. After no obvious bubbles escape from the asphalt system, the basalt fibers are added and the shearing is started.

5. The preparation process of the high-durability asphalt concrete composite material according to claim 1, characterized in that, The fiber-modified asphalt obtained after shearing in step S2 is stored and transported in an insulated storage tank with a heat transfer oil jacket before being transferred to the mixer and mixed with the dry mixture in step S4. The asphalt cooling rate is controlled within the range of 2~5℃ / min by circulating the heat transfer oil in the jacket. After the asphalt temperature drops to 180~190℃, it is injected into the mixer.

6. The preparation process of the high-durability asphalt concrete composite material according to claim 1, characterized in that, The mineral powder used in step S3 is activated limestone mineral powder that has been calcined at 650~750℃ for 2~3 hours.

7. The preparation process of the high-durability asphalt concrete composite material according to claim 1, characterized in that, In step S6, the anti-stripping agent is an amine-based anti-stripping agent.

8. The preparation process of the high-durability asphalt concrete composite material according to claim 1, characterized in that, In step S6, the anti-stripping agent is preloaded onto a porous limestone mineral powder carrier. The amount of anti-stripping agent added is based on the effective component of the anti-stripping agent. The mass ratio of the anti-stripping agent to the carrier mineral powder is 1:(1~2). The loading method is to spray the anti-stripping agent onto the stirred mineral powder at room temperature. After adsorption equilibrium is reached, the loaded anti-stripping agent is obtained. In step S6, the loaded anti-stripping agent is added to the fiber-reinforced mixture for mixing.

9. The preparation process of the high-durability asphalt concrete composite material according to claim 1, characterized in that, Before compaction molding in step S7, the composite material mixture loaded into the test mold is vibrated and leveled. The vibration frequency is 25~35Hz, the amplitude is 0.3~0.8mm, and the vibration time is 6~12s. After vibration and leveling, double-sided compaction is carried out. During the compaction process, the test mold is placed in a heat-insulating sleeve preheated to 140~160℃.

10. The preparation process of the high-durability asphalt concrete composite material according to claim 1, characterized in that, After compaction and before demolding in step S7, place the specimen and mold together in a constant temperature chamber at 120~140℃ for 4~6 hours for curing. After curing, remove the specimen and allow it to cool naturally until the specimen temperature is below 60℃ before demolding.