A Low-Temperature Crack-Resistant Asphalt Concrete and Its Preparation Method
By using a specific composite filler and wood fiber synergistic reinforcement system, the problem of asphalt concrete cracking at low temperatures in cold regions has been solved, achieving high efficiency in low-temperature crack resistance, water stability and high-temperature stability, thereby improving the structural integrity and driving safety of roads.
Patent Information
- Application Number
- CN202611371925.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-05
- Publication Date
- 2026-11-17
AI Technical Summary
Existing asphalt concrete is prone to cracking under low-temperature conditions in cold regions, and cannot simultaneously meet the requirements of water stability, low-temperature crack resistance, high-temperature stability and water impermeability, resulting in reduced pavement structural integrity and driving safety, and increased maintenance costs.
A specific composite filler and wood fiber synergistic reinforcement system is adopted. A dense skeleton is formed by three-grade basalt, modified diatomaceous earth is used to buffer low-temperature thermal stress, nano-silica is uniformly dispersed, and a second silane coupling agent is used to bridge the interface adhesion, thereby improving the low-temperature crack resistance of asphalt concrete.
It significantly improves the low-temperature crack resistance of asphalt concrete, enhances water stability and high-temperature stability, reduces the occurrence of thermal shrinkage cracks, and improves the structural integrity and driving safety of roads.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] This application relates to the technical field of asphalt concrete, and in particular to a low-temperature crack-resistant asphalt concrete and its preparation method. Background Technology
[0002] Asphalt concrete, one of the most widely used pavement materials in modern road construction, is widely applied in various transportation infrastructure projects such as highways, municipal roads, and airport runways due to its excellent adhesion and ease of construction. It plays a crucial role in ensuring smooth traffic flow and improving the service experience of road surfaces. Currently, the preparation of existing asphalt concrete mainly uses asphalt as the binder, combined with aggregates, mineral powder, and necessary modifiers. It is mixed, paved, and compacted through reasonable gradation design and specific processes. Among these, modification technology and gradation optimization are the main means to improve its road performance. For example, SBS modified asphalt is used to improve high and low temperature performance, and the density and stability of the mixture are improved by adjusting the aggregate gradation. At the same time, the promotion of asphalt pavement recycling technology has also realized the recycling of waste materials, which expands the application scenarios of asphalt concrete while saving resources and reducing energy consumption. However, existing technologies still mainly aim to meet the road requirements in conventional temperature ranges.
[0003] In cold regions and high-altitude, low-temperature areas, asphalt concrete pavements face long-term challenges from harsh environments such as freeze-thaw cycles and sudden diurnal temperature variations. Insufficient low-temperature crack resistance has become a core technical bottleneck restricting their service life. Under low-temperature conditions, the asphalt binder in existing asphalt concrete transforms from a viscoelastic state to a glassy state, restricting molecular chain movement, drastically increasing stiffness modulus while significantly decreasing toughness, and significantly weakening stress relaxation ability. When the thermal stress generated by temperature contraction exceeds the material's ultimate tensile strength, microcracks are easily initiated and rapidly propagated, forming transverse cracks, network cracks, and other defects. At the same time, existing modification technologies have limited effectiveness in improving low-temperature crack resistance, and the performance of some modified asphalt deteriorates over time. Furthermore, traditional gradation designs struggle to balance high-temperature stability and low-temperature toughness. Coupled with the damage to the internal pore structure caused by freeze-thaw cycles, this further exacerbates the risk of pavement cracking, reducing not only the structural integrity and driving safety of the pavement but also significantly increasing pavement maintenance costs, failing to meet the actual needs of long-term stable service for transportation infrastructure in cold regions.
[0004] Therefore, how to effectively solve the problem of asphalt concrete in cold regions being prone to cracking at low temperatures and failing to simultaneously balance water stability, low-temperature crack resistance, high-temperature stability, and water impermeability has become an urgent issue to be addressed. Summary of the Invention
[0005] To address the shortcomings of existing technologies, this application provides a low-temperature crack-resistant asphalt concrete and its preparation method.
[0006] In the first aspect, this application provides a low-temperature crack-resistant asphalt concrete, which adopts the following technical solution: A low-temperature crack-resistant asphalt concrete comprises the following raw materials in parts by weight: 90-115 parts of mixture, 1-10 parts of asphalt, 0.2-0.8 parts of wood fiber, and 0.5-1 parts of composite filler.
[0007] Preferably, the composite filler comprises the following raw materials in parts by weight: 2-10 parts diatomaceous earth, 0.2-0.8 parts titanium source, 0.1-0.5 parts boron source, 2-6 parts tetrapropylammonium hydroxide, 0.5-1.5 parts nano silica, 10-30 parts ethanol, 0.01-0.05 parts first silane coupling agent, 0.02-0.1 parts sodium dodecyl sulfate, and 0.01-0.04 parts second silane coupling agent.
[0008] Preferably, the titanium source is tetrabutyl titanate.
[0009] Preferably, the boron source is boric acid.
[0010] Preferably, the first silane coupling agent is γ-aminopropyltriethoxysilane.
[0011] Preferably, the second silane coupling agent is γ-glycidoxypropyltrimethoxysilane.
[0012] Preferably, the preparation method of the composite filler includes the following steps: Diatomaceous earth is acidified to obtain acidified diatomaceous earth; Acidified diatomaceous earth was mixed with a titanium source to obtain mixture A; A boron source and tetrapropylammonium hydroxide were mixed to obtain mixture B; Nano-silica and ethanol were mixed, a first silane coupling agent was added and mixed, sodium dodecyl sulfate was added and mixed, filtered and dried to obtain modified nano-silica. Mixture A and mixture B are mixed, and modified nano-silica and second silane coupling agent are added and mixed. The mixture is then filtered and dried to obtain the composite filler.
[0013] Preferably, the diatomaceous earth is acidified by the following steps: the diatomaceous earth and sulfuric acid solution are mixed at a solid-liquid ratio of 1:(5-10), stirred and reacted at 60-80℃ for 2-4 hours, and dried to obtain acidified diatomaceous earth; the concentration of the sulfuric acid solution is 4-6 mol / L.
[0014] Preferably, the reaction temperature is 60-70℃ during the mixing of acidified diatomaceous earth and titanium source.
[0015] Preferably, the reaction temperature is 60-70℃ during the mixing of the boron source and tetrapropylammonium hydroxide.
[0016] Preferably, the reaction temperature is 60-70℃ during the mixing of mixture A and mixture B.
[0017] Preferably, nano-silica and ethanol are mixed, a first silane coupling agent is added and mixed, and then sodium dodecyl sulfate is added and mixed, with the reaction temperature being 50-60℃.
[0018] Preferably, the reaction temperature is 60-70℃ during the mixing process of adding modified nano-silica and the second silane coupling agent.
[0019] By adopting the above technical solution, this application modifies acidified diatomaceous earth with titanium and boron sources to generate modified diatomaceous earth, further increasing the specific surface area of diatomaceous earth. This allows it to adsorb lightweight components of asphalt and utilize the microporous structure of modified diatomaceous earth to buffer low-temperature thermal stress and delay crack initiation. Hydrophobically modified nano-silica, in conjunction with sodium dodecyl sulfate, achieves uniform dispersion, effectively improving the low-temperature deformation capacity of the matrix. A second silane coupling agent bridges the filler and asphalt, enhancing interfacial adhesion and preventing low-temperature debonding. Through the synergistic effect of these three components, the brittleness of asphalt concrete is reduced, the ultimate strain and tensile strength are improved, and thermal shrinkage cracks in cold-region roads are effectively suppressed.
[0020] This application improves the composite filler by using a multi-component synergistic physical-chemical modification to significantly enhance the low-temperature crack resistance of asphalt concrete.
[0021] Preferably, the mixture comprises the following raw materials in parts by weight: 40-50 parts of basalt with a particle size of 10-15 mm, 25-35 parts of basalt with a particle size of 5-10 mm, 10-20 parts of basalt with a particle size of 0.001-3 mm, and 5-15 parts of mineral powder with a particle size of 0.01-0.3 mm.
[0022] Preferably, the basalt with a particle size of 10-15 mm has an apparent relative density of 2.938 and a bulk relative density of 2.882.
[0023] The basalt with a grain size of 5-10 mm has an apparent relative density of 2.943 and a bulk relative density of 2.887.
[0024] The basalt with a grain size of 0.001-3 mm has an apparent relative density of 2.939 and a bulk relative density of 2.817.
[0025] The relative density of the mineral powder with a particle size of 0.01-0.3 mm is 2.691.
[0026] By adopting the above technical solution, the mixture forms a dense skeleton with progressively filled basalt through three-graded basalt. During low-temperature shrinkage, the micro-slippage of particles effectively dissipates shrinkage stress. The reasonable combination of high-density aggregate and mineral powder thickens the asphalt coating film and enhances the adhesion of asphalt mastic. At the same time, the similar density of each grade of aggregate avoids segregation and unevenness, thus comprehensively ensuring the uniformity of low-temperature crack resistance of the pavement and significantly improving the ability of asphalt concrete to resist thermal shrinkage cracks. It is suitable for highway engineering in extremely cold regions.
[0027] Secondly, this application provides a method for preparing low-temperature crack-resistant asphalt concrete, employing the following technical solution: A method for preparing low-temperature crack-resistant asphalt concrete includes the following steps: The mixture, wood fiber, and composite filler are sheared and mixed to obtain a dry mixture; Add the dry mix to the asphalt preheated to 150-160℃, stir at 160-175℃ for 5-10 minutes, and after stirring, keep warm at 160-170℃ for 20-30 minutes to obtain asphalt concrete.
[0028] By adopting the above technical solution, this application utilizes a three-graded basalt to form a dense skeleton, effectively dissipating shrinkage stress; wood fibers construct a three-dimensional network to adsorb asphalt, inhibiting the propagation of microcracks; and composite fillers combine porous buffering and interfacial chemical bonding functions, reducing the brittleness of asphalt mastic. After shear mixing and precise temperature-controlled mixing, all components are fully integrated, significantly improving the ultimate strain of concrete, reducing the coefficient of thermal shrinkage, and effectively inhibiting thermal shrinkage cracks in cold-region roads.
[0029] The asphalt concrete prepared in this application achieves a comprehensive improvement in low-temperature crack resistance through the synergistic effects of aggregate skeleton reinforcement, fiber bridging toughening, filler interface modification, and temperature-controlled mixing process.
[0030] In summary, this application includes at least one of the following beneficial technical effects: This application discloses a low-temperature crack-resistant asphalt concrete and its preparation method. By introducing a specific compound filler and a wood fiber synergistic reinforcement system, the low-temperature crack resistance of the asphalt concrete is effectively improved. At the same time, the prepared asphalt concrete has good water stability, low-temperature crack resistance, high-temperature stability and water impermeability. Detailed Implementation
[0031] The technical solutions of this application are further illustrated by specific embodiments below. These specific embodiments do not represent a limitation on the scope of protection of this application. Any non-essential modifications and adjustments made by others based on the concept of this application still fall within the scope of protection of this application.
[0032] All raw materials involved in this application are commercially available products, among which, Asphalt, SBS modified asphalt, purchased from Nanjing Refinery Co., Ltd., with the following parameters: penetration (25℃, 100g, 5S) 54 (0.1mm), ductility (5cm / min, 5℃) 31cm, softening point (ring and ball method) 84℃, dynamic viscosity (135℃) 1.9Pa·s, elastic recovery 88%, segregation (softening point difference) 2.3℃, flash point 324℃, solubility 99.64%, mass loss -0.204%, and after RTFOT testing, penetration (25℃) 81%, ductility (5cm / min, 5℃) 17cm, and relative density at 15℃ 1.032.
[0033] Wood fiber, purchased from Changzhou Luyou Traffic Facilities Co., Ltd., with the following parameters: maximum fiber length 4.6mm, ash content 16.5%, pH value 8.1, moisture content 3.8%, oil absorption rate 7.8 times, mass loss (210℃×1h) 4.9% with no combustion, wood fiber content 93%, density 1.072g / cm³. 3 The 0.15mm aperture screen has a throughput of 68.3%.
[0034] Nano-silica, 99.8% purity, Aladdin reagent; Diatomaceous earth, purchased from Tianjin Chemical Plant No. 3 Co., Ltd. The basalt was purchased from Hubei Jiuhua Basalt Co., Ltd. Mineral powder, purchased from Nanjing Changsheng.
[0035] The present application will be further described in detail below with reference to embodiments and comparative examples.
[0036] Preparation Example 1:
[0037] The composite filler includes the following raw materials: 6 kg of diatomaceous earth, 0.5 kg of titanium source (tetrabutyl titanate), 0.3 kg of boron source (boric acid), 4 kg of tetrapropylammonium hydroxide, 1 kg of nano silica, 20 kg of ethanol, 0.03 kg of the first silane coupling agent (γ-aminopropyltriethoxysilane), 0.06 kg of sodium dodecyl sulfate, and 0.025 kg of the second silane coupling agent (γ-glycidoxypropyltrimethoxysilane).
[0038] The preparation method of the composite filler is as follows: (1) Place the diatomaceous earth in a muffle furnace and calcine it at 450°C in an air atmosphere for 2 hours. Mix the calcined diatomaceous earth with a 5 mol / L sulfuric acid solution at a solid-liquid ratio of 1:8 and stir the mixture at 70°C for 3 hours. After the reaction is complete, filter the mixture, wash it with deionized water until neutral, and dry it at 90°C to constant weight to obtain acidified diatomaceous earth. (2) Disperse acidified diatomaceous earth in deionized water and stir at 65°C for 30 min to allow it to swell fully; dilute tetrabutyl titanate with an equal amount of anhydrous ethanol and add it to the acidified diatomaceous earth dispersion at 65°C. After the addition is complete, continue stirring and reacting for 45 min to form mixture A. (3) Dissolve the boron source and tetrapropylammonium hydroxide in deionized water and stir at 65°C for 1 hour to form a mixture B; (4) Add nano-silica to anhydrous ethanol and stir magnetically at room temperature for 2 hours to disperse it evenly; add the first silane coupling agent and reflux at 55°C for 1 hour; then add sodium dodecyl sulfate and stir at 55°C for 20 minutes, filter and dry to obtain modified nano-silica; (5) Mix mixture A and mixture B at 65°C for 1 hour, add modified nano-silica and second silane coupling agent, continue stirring at 65°C for 1.5 hours, filter, and dry at 80°C to constant weight to obtain composite filler.
[0039] Preparation Example 2:
[0040] The composite filler includes the following raw materials: 2 kg of diatomaceous earth, 0.2 kg of titanium source (tetrabutyl titanate), 0.1 kg of boron source (boric acid), 2 kg of tetrapropylammonium hydroxide, 0.5 kg of nano silica, 10 kg of ethanol, 0.01 kg of the first silane coupling agent (γ-aminopropyltriethoxysilane), 0.02 kg of sodium dodecyl sulfate, and 0.01 kg of the second silane coupling agent (γ-glycidoxypropyltrimethoxysilane).
[0041] The preparation method of the composite filler is as follows: (1) Place the diatomaceous earth in a muffle furnace and calcine it at 450°C in an air atmosphere for 2 hours. Mix the calcined diatomaceous earth with a 5 mol / L sulfuric acid solution at a solid-liquid ratio of 1:5 and stir the mixture at 70°C for 3 hours. After the reaction is complete, filter the mixture, wash it with deionized water until neutral, and dry it at 90°C to constant weight to obtain acidified diatomaceous earth. (2) Disperse acidified diatomaceous earth in deionized water and stir at 65°C for 30 min to allow it to swell fully; dilute tetrabutyl titanate with an equal amount of anhydrous ethanol and add it to the acidified diatomaceous earth dispersion at 65°C. After the addition is complete, continue stirring and reacting for 45 min to form mixture A. (3) Dissolve the boron source and tetrapropylammonium hydroxide in deionized water and stir at 65°C for 1 hour to form a mixture B; (4) Add nano-silica to anhydrous ethanol and stir magnetically at room temperature for 2 hours to disperse it evenly; add the first silane coupling agent and reflux at 55°C for 1 hour; then add sodium dodecyl sulfate and stir at 55°C for 20 minutes, filter and dry to obtain modified nano-silica; (5) Mix mixture A and mixture B at 65°C for 1 hour, add modified nano-silica and second silane coupling agent, continue stirring at 65°C for 1.5 hours, filter, and dry at 80°C to constant weight to obtain composite filler.
[0042] Preparation Example 3:
[0043] The composite filler includes the following raw materials: 10 kg of diatomaceous earth, 0.8 kg of titanium source (tetrabutyl titanate), 0.5 kg of boron source (boric acid), 6 kg of tetrapropylammonium hydroxide, 1.5 kg of nano silica, 30 kg of ethanol, 0.05 kg of the first silane coupling agent (γ-aminopropyltriethoxysilane), 0.1 kg of sodium dodecyl sulfate, and 0.04 kg of the second silane coupling agent (γ-glycidoxypropyltrimethoxysilane).
[0044] The preparation method of the composite filler is as follows: (1) Place the diatomaceous earth in a muffle furnace and calcine it at 450°C in an air atmosphere for 2 hours. Mix the calcined diatomaceous earth with a 5 mol / L sulfuric acid solution at a solid-liquid ratio of 1:10 and stir the mixture at 70°C for 3 hours. After the reaction is complete, filter the mixture, wash it with deionized water until neutral, and dry it at 90°C to constant weight to obtain acidified diatomaceous earth. (2) Disperse acidified diatomaceous earth in deionized water and stir at 65°C for 30 min to allow it to swell fully; dilute tetrabutyl titanate with an equal amount of anhydrous ethanol and add it to the acidified diatomaceous earth dispersion at 65°C. After the addition is complete, continue stirring and reacting for 45 min to form mixture A. (3) Dissolve the boron source and tetrapropylammonium hydroxide in deionized water and stir at 65°C for 1 hour to form a mixture B; (4) Add nano-silica to anhydrous ethanol and stir magnetically at room temperature for 2 hours to disperse it evenly; add the first silane coupling agent and reflux at 55°C for 1 hour; then add sodium dodecyl sulfate and stir at 55°C for 20 minutes, filter and dry to obtain modified nano-silica; (5) Mix mixture A and mixture B at 65°C for 1 hour, add modified nano-silica and second silane coupling agent, continue stirring at 65°C for 1.5 hours, filter, and dry at 80°C to constant weight to obtain composite filler.
[0045] Example:
[0046] Before constructing a high-temperature resistant and rutting-resistant asphalt pavement, prepare the mixture and asphalt according to its raw material parameters; Aggregates: The basalt with a grain size of 10-15 mm has an apparent relative density of 2.938 and a bulk relative density of 2.882. The basalt with a grain size of 5-10 mm has an apparent relative density of 2.943 and a bulk relative density of 2.887. The basalt with a grain size of 0.001-3 mm has an apparent relative density of 2.939 and a bulk relative density of 2.817. In this embodiment, the gradation used is SMA-13, and the raw material gradation is shown in Table 1; Table 1 Target mix design for synthetic gradation
[0047] Mineral powder: The mineral powder (limestone) has a particle size of 0.01-0.3 mm and a relative density of 2.691.
[0048] In this embodiment, the gradation used is SMA-13, and the mineral powder gradation is shown in Table 2; Table 2 Mineral Powder Grading Standards
[0049] Example 1:
[0050] A low-temperature crack-resistant asphalt concrete comprises the following raw materials: 100 kg of mixture, 6 kg of asphalt, 0.5 kg of wood fiber, and 0.8 kg of composite filler.
[0051] The mixture comprises the following raw materials: 46 kg of basalt with a particle size of 10-15 mm, 30 kg of basalt with a particle size of 5-10 mm, 15 kg of basalt with a particle size of 0.001-3 mm, and 9 kg of mineral powder with a particle size of 0.01-0.3 mm.
[0052] The composite filler was prepared according to Preparation Example 1.
[0053] A method for preparing low-temperature crack-resistant asphalt concrete includes the following steps: Weigh out each ingredient according to the formula: Basalt with a particle size of 10-15 mm, basalt with a particle size of 5-10 mm, basalt with a particle size of 0.001-3 mm, and mineral powder with a particle size of 0.01-0.3 mm are mixed and heated to 190℃ for 30 minutes to obtain a mixture. The mixture, wood fiber, and composite filler were sheared and stirred at 400 r / min for 10 minutes at 170℃ to obtain a dry mixture. Add the dry mix to the asphalt preheated to 160℃, stir at 700r / min for 8 minutes at 170℃, and after stirring, let it stand at 170℃ for 25 minutes to obtain asphalt concrete.
[0054] Example 2:
[0055] A low-temperature crack-resistant asphalt concrete comprises the following raw materials: 90 kg of mixture, 4 kg of asphalt, 0.2 kg of wood fiber, and 0.5 kg of composite filler.
[0056] The mixture comprises the following raw materials: 40 kg of basalt with a particle size of 10-15 mm, 25 kg of basalt with a particle size of 5-10 mm, 10 kg of basalt with a particle size of 0.001-3 mm, and 5 kg of mineral powder with a particle size of 0.01-0.3 mm.
[0057] The composite filler was prepared in Preparation Example 2.
[0058] A method for preparing low-temperature crack-resistant asphalt concrete includes the following steps: Weigh out each ingredient according to the formula: Basalt with a particle size of 10-15 mm, basalt with a particle size of 5-10 mm, basalt with a particle size of 0.001-3 mm, and mineral powder with a particle size of 0.01-0.3 mm are mixed and heated to 190℃ for 30 minutes to obtain a mixture. The mixture, wood fiber, and composite filler were sheared and stirred at 400 r / min for 10 minutes at 170℃ to obtain a dry mixture. Add the dry mix to the asphalt preheated to 160℃, stir at 700r / min for 8 minutes at 170℃, and after stirring, let it stand at 170℃ for 25 minutes to obtain asphalt concrete.
[0059] Example 3:
[0060] A low-temperature crack-resistant asphalt concrete comprises the following raw materials: 115 kg of mixture, 10 kg of asphalt, 0.8 kg of wood fiber, and 1 kg of composite filler.
[0061] The mixture comprises the following raw materials: 50 kg of basalt with a particle size of 10-15 mm, 35 kg of basalt with a particle size of 5-10 mm, 20 kg of basalt with a particle size of 0.001-3 mm, and 15 kg of mineral powder with a particle size of 0.01-0.3 mm.
[0062] The composite filler was prepared in Preparation Example 3.
[0063] A method for preparing low-temperature crack-resistant asphalt concrete includes the following steps: Weigh out each ingredient according to the formula: Basalt with a particle size of 10-15 mm, basalt with a particle size of 5-10 mm, basalt with a particle size of 0.001-3 mm, and mineral powder with a particle size of 0.01-0.3 mm are mixed and heated to 190℃ for 30 minutes to obtain a mixture. The mixture, wood fiber, and composite filler were sheared and stirred at 400 r / min for 10 minutes at 170℃ to obtain a dry mixture. Add the dry mix to the asphalt preheated to 160℃, stir at 700r / min for 8 minutes at 170℃, and after stirring, let it stand at 170℃ for 25 minutes to obtain asphalt concrete.
[0064] Example 4:
[0065] The difference from Example 1 is that the composite filler was prepared by Preparation Example 2.
[0066] Example 5:
[0067] The difference from Example 1 is that the composite filler was prepared by Preparation Example 3.
[0068] Comparative Example 1:
[0069] The difference from Example 1 is that no composite filler is added.
[0070] Comparative Example 2:
[0071] The difference from Example 1 is that the composite filler is replaced with an equal weight of a composite filler composed of the following formulation.
[0072] The composite filler is a mixture of 6 kg of diatomaceous earth and 1 kg of nano-silica.
[0073] Comparative Example 3:
[0074] The difference from Example 1 is that the composite filler is replaced with an equal weight of composite filler prepared by the following method.
[0075] The composite filler includes the following raw materials: 6 kg of diatomaceous earth, 1 kg of nano silica, 20 kg of ethanol, 0.03 kg of the first silane coupling agent (γ-aminopropyltriethoxysilane), 0.06 kg of sodium dodecyl sulfate, and 0.025 kg of the second silane coupling agent (γ-glycidoxypropyltrimethoxysilane).
[0076] The preparation method of the composite filler is as follows: (1) Place the diatomaceous earth in a muffle furnace and calcine it at 450°C in an air atmosphere for 2 hours. Mix the calcined diatomaceous earth with a 5 mol / L sulfuric acid solution at a solid-liquid ratio of 1:8 and stir the mixture at 70°C for 3 hours. After the reaction is complete, filter the mixture, wash it with deionized water until neutral, and dry it at 90°C to constant weight to obtain acidified diatomaceous earth. (2) Disperse acidified diatomaceous earth in deionized water and stir at 65°C for 30 min to allow it to fully swell, thereby obtaining an acidified diatomaceous earth dispersion; (3) Add nano-silica to anhydrous ethanol and stir magnetically at room temperature for 2 hours to disperse it evenly; add the first silane coupling agent and reflux at 55°C for 1 hour; then add sodium dodecyl sulfate and stir at 55°C for 20 minutes, filter and dry to obtain modified nano-silica; (4) The acidified diatomaceous earth dispersion was mixed with modified nano-silica and second silane coupling agent, and the mixture was stirred and reacted at 65°C for 1.5 h. After filtration, the mixture was dried at 80°C to constant weight to obtain the composite filler.
[0077] Performance testing: The following performance tests were conducted in accordance with the specifications in the "Technical Specification for Construction of Highway Asphalt Pavement" (JTG F40-2004) and the "Test Procedures for Asphalt and Asphalt Mixtures in Highway Engineering" (JTG E20-2011).
[0078] 1. Immersion Marshall stability, freeze-thaw splitting strength (TSR), and high-temperature stability (dynamic stability). Water immersion Marshall stability: Indoor tests were conducted to simulate mixing in a mixing plant and construction site conditions. Asphalt concrete was prepared using the methods described in the above embodiments and comparative examples. The prepared asphalt concrete was then subjected to Marshall compaction molding.
[0079] The tests were conducted according to the T0709 test method in the "Test Procedures for Asphalt and Asphalt Mixtures in Highway Engineering".
[0080] Freeze-thaw splitting strength: Tested according to the test method T0729 in the "Test Procedures for Asphalt and Asphalt Mixtures in Highway Engineering".
[0081] High-temperature stability test: A rutting test was conducted at 60℃ and 0.7MPa to verify high-temperature stability.
[0082] Table 3 Experimental Results
[0083] As shown in Table 3, the low-temperature crack-resistant asphalt concrete prepared by the method of this application achieves optimal dispersion of nano-silica and the strongest chemical bonding at the filler-asphalt interface by using a moderate ratio of composite filler and synergistic modification with coupling agent, thereby further improving the water immersion Marshall stability, freeze-thaw splitting strength and high-temperature stability of asphalt concrete.
[0084] Based on the test results of Example 1, Comparative Example 1, Comparative Example 2, and Comparative Example 3, it can be seen that the test results of Example 1 are better than those of Comparative Example 1, Comparative Example 2, and Comparative Example 3, indicating that the added composite filler further improves the water immersion Marshall stability, freeze-thaw splitting strength, and high-temperature stability of asphalt concrete.
[0085] 2. Low-temperature bending test According to the test method T0715 in the "Test Procedures for Asphalt and Asphalt Mixtures in Highway Engineering", the asphalt mixture rutting slab specimens were cooled and cut into small beam specimens of 250mm×30mm×35mm. After being kept in a constant temperature chamber at -10℃ for at least 1 hour, a mid-span concentrated loading bending test was carried out under the condition of a simply supported beam with a span of 200mm at a loading rate of 50mm / min until the specimen failed. The maximum load and mid-span deflection were recorded, and the flexural tensile strength, stiffness modulus and failure strain were calculated accordingly.
[0086] Table 4. Test Results
[0087] As can be seen from the test results in Table 4, the low-temperature crack-resistant asphalt concrete prepared by the method of this application further improves the low-temperature deformation capacity of asphalt concrete by using a moderate proportion of composite filler and through the synergistic effect between the composite filler and other components.
[0088] Based on the test results of Example 1, Comparative Example 1, Comparative Example 2, and Comparative Example 3, it can be seen that the test results of Example 1 are better than those of Comparative Example 1, Comparative Example 2, and Comparative Example 3, indicating that the added composite filler effectively improves the low-temperature deformation capacity of asphalt concrete.
[0089] 3. Permeability coefficient testing and structural depth testing According to the T0730 pavement permeability meter method and the T0961 manual sand spreading method in the "Test Procedures for Asphalt and Asphalt Mixtures in Highway Engineering", the permeability coefficient and texture depth of the molded rut slab specimens were determined respectively.
[0090] Table 5. Test Results
[0091] As can be seen from the test results in Table 5, the low-temperature crack-resistant asphalt concrete prepared by the method of this application, through the use of a moderately proportioned composite filler, and through the synergistic effect of the composite filler and other components, forms a moderately uniform macroscopic texture on the surface of the mixture during the compaction process, and further improves the water resistance of the asphalt concrete.
[0092] Based on the test results of Example 1, Comparative Example 1, Comparative Example 2, and Comparative Example 3, it can be seen that the test results of Example 1 are better than those of Comparative Example 1, Comparative Example 2, and Comparative Example 3. This indicates that the addition of composite filler enables the mixture to form a moderately uniform macroscopic texture on the surface during compaction, while further improving the water resistance of asphalt concrete.
Claims
1. A low-temperature crack-resistant asphalt concrete, characterized in that: The raw materials include the following parts by weight: 90-115 parts of mixture, 1-10 parts of asphalt, 0.2-0.8 parts of wood fiber, and 0.5-1 parts of composite filler.
2. The low-temperature crack-resistant asphalt concrete according to claim 1, characterized in that: The composite filler comprises the following raw materials in parts by weight: 2-10 parts diatomaceous earth, 0.2-0.8 parts titanium source, 0.1-0.5 parts boron source, 2-6 parts tetrapropylammonium hydroxide, 0.5-1.5 parts nano silica, 10-30 parts ethanol, 0.01-0.05 parts first silane coupling agent, 0.02-0.1 parts sodium dodecyl sulfate, and 0.01-0.04 parts second silane coupling agent.
3. The low-temperature crack-resistant asphalt concrete according to claim 2, characterized in that: The titanium source is tetrabutyl titanate; the boron source is boric acid.
4. The low-temperature crack-resistant asphalt concrete according to claim 2, characterized in that: The first silane coupling agent is γ-aminopropyltriethoxysilane; the second silane coupling agent is γ-glycidoxypropyltrimethoxysilane.
5. The low-temperature crack-resistant asphalt concrete according to claim 2, characterized in that: The preparation method of the composite filler includes the following steps: Diatomaceous earth is acidified to obtain acidified diatomaceous earth; Acidified diatomaceous earth was mixed with a titanium source to obtain mixture A; A boron source and tetrapropylammonium hydroxide were mixed to obtain mixture B; Nano-silica and ethanol were mixed, a first silane coupling agent was added and mixed, sodium dodecyl sulfate was added and mixed, filtered and dried to obtain modified nano-silica. Mixture A and mixture B are mixed, and modified nano-silica and second silane coupling agent are added and mixed. The mixture is then filtered and dried to obtain the composite filler.
6. The low-temperature crack-resistant asphalt concrete according to claim 5, characterized in that: The acidification treatment of diatomaceous earth is carried out by the following steps: diatomaceous earth and sulfuric acid solution are mixed at a solid-liquid ratio of 1:(5-10), stirred and reacted at 60-80℃ for 2-4 hours, and dried to obtain acidified diatomaceous earth; the concentration of sulfuric acid solution is 4-6 mol / L.
7. The low-temperature crack-resistant asphalt concrete according to claim 5, characterized in that: During the mixing of acidified diatomaceous earth and titanium source, the reaction temperature is 60-70℃. During the mixing of the boron source and tetrapropylammonium hydroxide, the reaction temperature is 60-70℃; During the mixing process with sodium dodecyl sulfate, the reaction temperature is 50-60℃; During the mixing of mixture A and mixture B, the reaction temperature is 60-70℃; During the mixing process of adding modified nano-silica and the second silane coupling agent, the reaction temperature is 60-70℃.
8. The low-temperature crack-resistant asphalt concrete according to claim 1, characterized in that: The mixture comprises the following raw materials in parts by weight: 40-50 parts of basalt with a particle size of 10-15 mm, 25-35 parts of basalt with a particle size of 5-10 mm, 10-20 parts of basalt with a particle size of 0.001-3 mm, and 5-15 parts of mineral powder with a particle size of 0.01-0.3 mm.
9. The low-temperature crack-resistant asphalt concrete according to claim 8, characterized in that: The basalt with a grain size of 10-15 mm has an apparent relative density of 2.938 and a bulk relative density of 2.
882. The basalt with a grain size of 5-10 mm has an apparent relative density of 2.943 and a bulk relative density of 2.
887. The basalt with a grain size of 0.001-3 mm has an apparent relative density of 2.939 and a bulk relative density of 2.
817. The relative density of the mineral powder with a particle size of 0.01-0.3 mm is 2.
691.
10. A method for preparing the low-temperature crack-resistant asphalt concrete according to any one of claims 1-9, characterized in that: Includes the following steps: The mixture, wood fiber, and composite filler are sheared and mixed to obtain a dry mixture; Add the dry mix to the asphalt preheated to 150-160℃, stir at 160-175℃ for 5-10 minutes, and after stirring, keep warm at 160-170℃ for 20-30 minutes to obtain asphalt concrete.