A tough, carbon-fixing, waste-utilizing, three-functional geopolymer and its preparation method

By using high-calcium fly ash, mineral powder, and steel slag combined with biochar-modified fibers, a strong and tough carbon-fixing geopolymer was prepared. This solved the problems of insufficient early strength, poor toughness, and limited carbon fixation capacity of geopolymers in deep-earth and deep-water oil well environments, and achieved efficient utilization of industrial solid waste and reduction of carbon emissions.

CN123106086APending Publication Date: 2026-11-17TONGJI UNIV
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611438116.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-16
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing geopolymers exhibit performance degradation in deep-earth and deep-water oil well environments, exhibiting problems such as insufficient early strength, poor toughness, limited carbon fixation capacity, and poor fiber-matrix adhesion. Furthermore, the low utilization rate of industrial solid waste leads to environmental pollution and high carbon emissions.

Method used

Using high-calcium fly ash, mineral powder, and steel slag as the main raw materials, combined with biochar-modified multi-sized plastic fibers and metal fibers, a strong and tough carbon-fixing and waste-utilizing polymer is prepared through alkali activators and retarders. The biochar modification process simplifies the bonding between fibers and the matrix, forming a multi-scale bridging network.

Benefits of technology

It significantly improves the early strength, toughness, and carbon fixation properties of geopolymers, enhances the utilization rate of industrial solid waste, reduces carbon emissions, achieves negative carbon production, and is suitable for deep-earth and deep-water oil well environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123106086A_ABST
    Figure CN123106086A_ABST
Patent Text Reader

Abstract

This invention relates to a strong, tough, carbon-fixing, and waste-utilizing three-functional geopolymer and its preparation method. The raw materials for the geopolymer include the following components in parts by weight: 85-115 parts of solid waste-based cementitious material, 1.1-1.3 parts of modified mixed fibers, 35-37 parts of alkali activator, 2.8-3.2 parts of retarder, and 27-31 parts of water. The modified mixed fibers include plastic fibers and metal fibers of different sizes modified with biochar, in a mass ratio of (0.1-0.3):1. The plastic fibers consist of three sizes with lengths of 5-7 mm, 8-10 mm, and 11-13 mm, in a mass ratio of (0.8-1.2):(0.8-1.2):1. The metal fibers consist of two sizes with lengths of 5-7 mm and 11-13 mm, in a mass ratio of (0.3-0.7):1. Compared with the prior art, this invention can improve the early strength, toughness, and carbon fixation performance of the geopolymer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of solid waste materials technology, and relates to a strong, tough, carbon-fixing, waste-utilizing, three-functional geopolymer and its preparation method. Background Technology

[0002] For a long time, oil well cement has been used in oil well cementing operations. However, as oil well development activities have gradually shifted to complex geological environments such as deep earth and deep water, the performance degradation of oil well cement in these environments has become increasingly apparent. For example, defects such as uncontrollable pumping time and insufficient high-temperature and corrosion resistance can lead to performance failure. Simultaneously, the production of oil well cement releases large amounts of carbon dioxide (CO2), a major contributor to global warming. It is reported that global cement production has exceeded 4 billion tons, accounting for 7-10% of global CO2 emissions. Therefore, using low-carbon cementing materials to partially replace oil well cement in cementing operations is a key approach to alleviating current technical challenges.

[0003] Geopolymer is a green, low-carbon cementitious material made primarily from silica-alumina minerals. Unlike oil well cement, geopolymer can use industrial solid waste as its raw material, and has advantages such as low carbon dioxide emissions, high early strength, high temperature resistance, and freeze-thaw resistance. However, in practical use, geopolymer has the following drawbacks: (1) The most commonly used raw material for geopolymer is low-calcium fly ash. However, with the rapid development of the power industry and the depletion of coal resources, more and more high-calcium fly ash has been generated, which urgently needs to be treated and utilized. Compared with low-calcium fly ash, high-calcium fly ash contains more free calcium oxide (CaO), which increases the risk of geopolymer cracking. Steel slag is an industrial solid waste from steel production. The global annual output of steel slag exceeds 100 million tons, but the utilization rate is less than 30%. Granulated blast furnace slag powder (referred to as slag powder) is a glassy material formed by the liquid slag formed by impurities in molten ore during the blast furnace ironmaking process, which is rapidly cooled by water or air quenching. The global annual output of slag powder exceeds 500 million tons, but only 20-30% is effectively utilized. The accumulation of industrial solid waste not only occupies land resources, but also causes serious environmental problems. (2) Although geopolymers have better early strength than oil well cement, they sometimes fail to meet the requirements of actual cementing conditions, such as the need for higher early strength, in the face of increasingly complex oil well environments. (3) Geopolymers are brittle materials with poor toughness, which limits their application in practical engineering. (4) Geopolymers are also porous materials that can adsorb carbon dioxide and react with it to form carbonates for storage. However, some scholars have pointed out that geopolymers have limited carbon dioxide adsorption capacity.

[0004] Fiber reinforcement is considered one of the most economical and effective methods to improve the toughness of geopolymers. Currently, the main types of fibers used to reinforce geopolymers include carbon fiber, basalt fiber, polyethylene fiber, polypropylene fiber, steel fiber, and natural fibers. Among them, plastic fibers, such as polyethylene or polypropylene fibers, have low elastic modulus and high elongation, which helps to delay crack propagation; while metal fibers, such as steel fibers, exhibit high strength and high elastic modulus, which can significantly improve the load-bearing capacity of materials. However, the improvement in geopolymer performance using a single type of fiber is usually limited. Furthermore, plastic fibers are hydrophobic and, similar to metal fibers, have relatively smooth surfaces, resulting in insufficient interfacial adhesion between the fiber and the geopolymer matrix, easily forming weak interfacial transition zones, thus limiting further development of matrix strength.

[0005] Patent CN120794450A discloses a hybrid fiber-reinforced ultra-high performance geopolymer concrete, its preparation method, and its application. It utilizes slag, metakaolin, and silica fume as precursor materials for the geopolymer concrete, employs a sodium hydroxide-water glass solution composite alkali activator, and incorporates steel fibers, polyvinyl alcohol fibers, and modified glass chopped fibers of different sizes. This significantly improves the brittleness of the geopolymer concrete and enhances its early strength and high-temperature resistance. Although this patent uses a silane coupling agent to modify the fiber surface, which can improve the interfacial bonding between the fiber and the geopolymer matrix to some extent, silane coupling agents are chemical reagents with relatively complex preparation processes and high prices. Large-scale use would increase the cost of fiber modification and concrete preparation, hindering the widespread application of this patent in large-volume projects.

[0006] Patent CN115321891A discloses a hybrid fiber-reinforced high-ductility geopolymer material and its preparation method, comprising the following raw materials in parts by weight: 30-40 parts fly ash; 50-60 parts granulated blast furnace slag; 20-30 parts steel slag powder; 7-10 parts anhydrous sodium silicate; 35-40 parts fine sand; 5-10 parts steel fiber; 1-2 parts polyethylene fiber; and 35-40 parts water. The steel slag powder has an average particle size of 10-50 μm, preferably 10.1-15.3 μm. The polyethylene fiber has a length of 15-18 mm and a diameter of 10-25 μm. The steel fiber has a length of 20-23 mm and a diameter of 0.1-0.5 mm. Although the patent combines polyethylene fiber and steel fiber to form hybrid fiber, which can improve the toughness and ductility of geopolymer materials, the patent only uses polyethylene fiber and steel fiber of a single size range, making it difficult to fully contain the different scale behaviors of the crack propagation process.

[0007] Patent CN117303810A discloses a fiber-reinforced high-temperature resistant geopolymer made from recycled sand and its preparation method. It uses mineral powder and silica fume as active raw materials, employs an alkali-activated method to obtain a cementitious material, uses recycled sand as fine aggregate, and is reinforced with multi-scale fibers to prepare the geopolymer solid. While this patent uses modified nanofibers as reinforcing materials, which can improve the mechanical properties and high-temperature resistance of the geopolymer, the sodium chloroacetate used in the fiber modification process has acute toxicity, posing a potential hazard to operator health and the aquatic ecosystem. Furthermore, the use of sodium chloroacetate increases raw material costs, making it unsuitable for large-scale application. In addition, although this patent reduces the consumption of natural resources and lowers carbon emissions by utilizing industrial byproducts or recycled resources such as mineral powder, silica fume, and recycled sand, this effect is essentially passive carbon reduction and is unlikely to achieve a shift from low-carbon production to carbon-negative production. Summary of the Invention

[0008] The purpose of this invention is to overcome at least one of the defects of the prior art and provide a strong, tough, carbon-fixing, waste-utilizing, three-functional geopolymer and its preparation method. This invention can improve the early strength, toughness, and carbon fixation performance of the geopolymer.

[0009] The objective of this invention can be achieved through the following technical solutions: One of the technical solutions of the present invention is to provide a strong, tough, carbon-fixing, waste-utilizing, three-functional geopolymer, the raw materials of which include the following components in parts by weight: The mixture contains 85-115 parts of solid waste-based cementitious material, 1.1-1.3 parts of modified mixed fiber, 35-37 parts of alkali activator, 2.8-3.2 parts of retarder, and 27-31 parts of water. The modified hybrid fiber includes plastic fibers and metal fibers of different sizes modified with biochar, wherein the mass ratio of plastic fibers to metal fibers is (0.1~0.3):1; The plastic fibers are composed of three sizes with lengths of 5-7 mm, 8-10 mm, and 11-13 mm, with a mass ratio of (0.8-1.2):(0.8-1.2):1. The metal fibers consist of two sizes: 5-7 mm and 11-13 mm in length, with a mass ratio of (0.3-0.7):1.

[0010] Furthermore, the solid waste-based cementitious material comprises 85-115 parts, including 60-70 parts of high-calcium fly ash, 20-30 parts of mineral powder, and 5-15 parts of steel slag.

[0011] Furthermore, the high-calcium fly ash has a SiO2 content of 30-44 wt%, an Al2O3 content of 15-25 wt%, and a CaO content of 10-26 wt%, and belongs to Class C fly ash; The mineral powder is selected from one or more of S95 grade mineral powder and S105 grade mineral powder, and the SiO2 content of the mineral powder is 20~32 wt%, the Al2O3 content is 10~18 wt%, and the CaO content is 30~46 wt%. The steel slag has a SiO2 content of 10-28 wt%, an Al2O3 content of 4-8 wt%, and a CaO content of 30-48 wt%, and the steel slag powder that passes through a 200-400 mesh sieve is retained.

[0012] Furthermore, the plastic fiber is selected from one or more of polyethylene fiber, polypropylene fiber, polyvinyl alcohol fiber, and polyacrylonitrile fiber, and the plastic fiber has a diameter of 18~38 μm, a tensile strength >400 MPa, and an elastic modulus >3.5 GPa; The metal fiber is selected from one or more steel fibers selected from hooked steel fibers, straight steel fibers, and milled steel fibers. The diameter of the metal fiber is 180~200 μm, the tensile strength is >1000 MPa, and the elastic modulus is >200 GPa.

[0013] Furthermore, the alkali activator comprises a water glass solution and sodium hydroxide, wherein the water glass solution has a Na2O·nSiO2 content of 40~47 wt% and an initial modulus n of 2.0~2.6, and the modulus of the alkali activator after the addition of sodium hydroxide is 0.8~1.2.

[0014] Furthermore, the retarder is selected from one or more of 2-acrylamide-2-methylpropanesulfonic acid, sodium citrate, sodium lignosulfonate, and sucrose.

[0015] One of the technical solutions of the present invention is to provide a method for preparing the aforementioned strong, tough, carbon-fixing, waste-utilizing, three-functional geopolymer, the method comprising the following steps: S1. Biomass is heated and cooled under a protective atmosphere to obtain biochar. The biochar is ground and sieved. The biochar is mixed with water to obtain biochar slurry. The biochar slurry is coated on the surface of fibers and dried. Plastic fibers and metal fibers of different sizes are mixed to obtain modified mixed fibers. S2. Mix the components of the solid waste-based cementitious material, add alkali activator, retarder and water to obtain geopolymer wet mix, add modified mixed fiber to obtain geopolymer slurry; S3. The geopolymer slurry is poured, cured, and demolded to obtain a strong, tough, carbon-fixing, and waste-utilizing geopolymer.

[0016] Furthermore, the fibers are pretreated before step S1, and the pretreatment includes the following steps: The fibers were immersed in an alcohol solution, ultrasonically treated, rinsed, and dried. The alcohol solution is selected from one or more aqueous solutions of ethanol, methanol, isopropanol, and n-propanol, and the concentration of the alcohol solution is 70-80 vol%. The volume ratio of the fiber to the alcohol solution is 1:(2-6). The ultrasonic treatment was performed at a frequency of 35–45 kHz for a duration of 100–120 min. The drying temperature is 30~40 ℃ and the time is 120~240 min.

[0017] As a preferred technical solution, water rinsing is used, and the rinsing is performed 5 to 9 times. The drying process employs vacuum drying, with a vacuum level of 5-15 kPa.

[0018] As a preferred technical solution, the biomass is cleaned, dried and crushed before step S1.

[0019] Furthermore, in step S1, the biomass is selected from one or more of sawdust, corn cobs, rice husks, and sugarcane bagasse. The heating temperature is 300~400 ℃, the heating rate is 5~15 ℃ / min, and the holding time is 45~60 min. Retain the biochar that passes through a 200-400 mesh sieve. The mass ratio of biochar to water is 1:(4~8). The drying temperature is 25~40 ℃, and the time is 5~9 days.

[0020] As a preferred technical solution, the protective gas used as the protective atmosphere in step S1 is selected from one or more of nitrogen and helium. The biochar and water were mixed by stirring at a speed of 500-800 r / min for 120-300 s. Vacuum drying is used, with a vacuum degree of 5~15 kPa.

[0021] In step S1, the biochar has a carbon content of 60-70 wt%, an oxygen content of 10-20 wt%, and a density of 1.2-1.8 g / cm³. 3 The average pore size is 7.6~9 nm.

[0022] Further, in step S2, sodium hydroxide is added to a water glass solution and mixed, then allowed to stand to obtain an alkaline activator. The standing time is 12-36 h. Add alkali activator, retarder and water and mix at low speed. Add modified mixed fiber and mix at low speed and high speed. The low speed stirring speed is 130~150 r / min and the time is 60~120 s. The high speed stirring speed is 270~300 r / min and the time is 100~160 s.

[0023] As a preferred technical solution, in step S2, sodium hydroxide is added to the water glass solution and stirred for 300~400 r / min for 60~120 s.

[0024] As a preferred technical solution, the curing temperature in step S3 is 50~70 ℃ and the time is 12~36 h.

[0025] Compared with the prior art, the present invention has the following beneficial effects: (1) This invention addresses the rational utilization of high-calcium fly ash, mineral powder, and steel slag, as well as the problem of insufficient early strength of geopolymers. High-calcium fly ash is selected as the main raw material, and soluble calcium ions (Ca) can be introduced by incorporating mineral powder and steel slag. 2+ This process promotes the formation of additional CSH gel, with the gel phase serving as nucleation sites to accelerate the polymerization reaction, generate more reaction products, and fill pores. The incorporation of mineral powder consumes free water, refines capillary pores, and improves the transition zone between the slurry and fiber, increasing matrix density and effectively addressing the issues of slow reaction at room temperature and excessively long setting time. Simultaneously, the incorporation of steel slag effectively disperses the originally agglomerated fly ash particles, increasing their specific surface area and making the accumulated soluble silica (SiO2), calcium oxide (CaO), and alumina (Al2O3) more easily soluble, further accelerating the polymerization reaction and improving the early strength of the geopolymer. By synergistically utilizing high-calcium fly ash, mineral powder, and steel slag, not only are the mechanical properties of the geopolymer significantly improved, but the utilization rate of industrial solid waste is also increased, and carbon emissions are reduced. (2) This invention addresses the problems of high brittleness, insufficient carbon fixation performance, and poor adhesion between fibers and the matrix in geopolymers. It utilizes biochar obtained from heated biomass as a modifying material, achieving resource utilization of biochar solid waste. This method offers advantages such as wide availability of raw materials and low cost. Compared to existing chemical modification methods that require large amounts of chemical reagents, have high modification costs, and complex processes, the modification process of this invention only requires biochar and water, simplifying the process, increasing operational safety, and significantly reducing modification costs. Furthermore, the presence of hydrophilic groups on the surface of biochar allows it to absorb mixing water, reducing capillary pores formed during the hardening process of the geopolymer slurry due to free water evaporation, and improving matrix density. In addition, biochar… The coating transforms the originally hydrophobic fiber surface into a hydrophilic one, improving the adhesion between the fiber and the matrix. Furthermore, the biochar coating roughens the fiber surface, thereby enhancing the fiber's anchoring to the matrix and further improving the adhesion between the fiber and the matrix, thus increasing the toughness of the geopolymer. Biochar also has excellent carbon dioxide (CO2) adsorption capacity, which can promote the reaction of free calcium oxide in high-calcium fly ash with carbon dioxide to form calcium carbonate (CaCO3). This not only consumes free calcium oxide and reduces the risk of geopolymer cracking, but also improves the carbon fixation performance of the geopolymer. Moreover, the generated calcium carbonate can fill the interfacial transition zone, making the originally weak interfacial transition zone denser. (3) This invention addresses the problem of high brittleness in geopolymers by selecting plastic fibers and metal fibers of different sizes as reinforcing materials. Compared with single-size fibers, multi-size fibers can inhibit crack propagation at different scales. For plastic fibers, shorter fibers can disperse local stress within the matrix, shortening the effective propagation path of cracks in the matrix. Medium-length fibers can overlap with shorter fibers to form a multi-scale network reinforcement structure, while longer fibers can cross wider cracks and play a bridging role, thereby improving the early crack resistance and deformation coordination of the matrix. For metal fibers, shorter fibers can... The combination of high-strength, high-modulus metal fibers with low-modulus, high-elongation plastic fibers can achieve a multi-scale, multi-stage synergistic toughening mechanism. The smaller plastic fibers can prevent the propagation of microcracks in the early stages of crack development and consume the energy required for crack propagation during fiber breakage. The load is gradually transferred to the metal fibers with higher strength and modulus, further limiting crack propagation and significantly enhancing the toughness of the geopolymer. Attached Figure Description

[0026] Figure 1 This is a schematic flowchart illustrating the preparation method of the strong, tough, carbon-fixing, waste-utilizing, three-functional geopolymer in an embodiment of the present invention. Detailed Implementation

[0027] The present invention will now be described in detail with reference to specific embodiments. These embodiments are based on the technical solution of the present invention and provide detailed implementation methods and specific operating procedures. However, the scope of protection of the present invention is not limited to the following embodiments.

[0028] Unless otherwise specified, the equipment used in the following embodiments is conventional equipment in the art; unless otherwise specified, the reagents used are commercially available products or prepared by conventional methods in the art. In the following embodiments, unless otherwise described in detail, conventional experimental methods in the art can be used.

[0029] Unless otherwise specified, the following procedures are generally performed at room temperature and atmospheric pressure.

[0030] Example 1: A tough, carbon-fixing, waste-utilizing, three-functional geopolymer and its preparation method, such as Figure 1 As shown, the specific steps are as follows: S1. Weigh out polypropylene fibers and steel fibers of different sizes according to the proportions. The polypropylene fiber has a diameter of 25 μm, a tensile strength of 500 MPa, and an elastic modulus of 7.5 GPa. It is composed of three sizes with lengths of 6 mm, 9 mm, and 12 mm, with a mass ratio of 1:1:1. The steel fibers are end-hooked steel fibers with a diameter of 185 μm, a tensile strength of 1100 MPa, and an elastic modulus of 210 GPa. They are composed of two sizes with lengths of 6 mm and 12 mm, with a mass ratio of 0.5:1. The fiber pretreatment process involves the following steps: S11. Pour a 75 vol% ethanol aqueous solution into an ultrasonic cleaner, and immerse the fiber in the ethanol solution at a volume ratio of 1:4. S12. The fiber is ultrasonically treated at 40 kHz for 110 min, and then rinsed with distilled water 7 times. S13. Place the fiber in a vacuum drying oven at 35 ℃ and 10 kPa for 200 min and dry it for later use. S2. Modify the fibers using biochar to obtain modified mixed fibers. The specific steps are as follows: S21. The recycled waste wood chips are washed, dried and crushed, placed in a tubular furnace reactor, heated to 350 ℃ at 10 ℃ / min under a nitrogen protective atmosphere, and held for 55 min. Then cooled to room temperature to obtain biochar for later use. The biochar has a carbon content of 65.65 wt%, an oxygen content of 15.32 wt%, and a density of 1.54 g / cm³. 3 The average pore size is 8.29 nm; S22. Grind the biochar and keep the biochar that passes through a 300-mesh sieve; S23. Using a magnetic stirrer, the biochar and water are thoroughly mixed at 600 r / min for 200 s according to a mass ratio of 1:6 to 1:6 to obtain a biochar slurry. S24. The biochar slurry is sprayed onto the surface of the fiber and then dried in a vacuum drying oven at 30 ℃ and 10 kPa for 7 days. S25. Mix polypropylene fibers and steel fibers of different sizes evenly according to the proportion to obtain modified mixed fibers; S3. Weigh out the components of the solid waste-based cementitious material according to the proportions: high-calcium fly ash, mineral powder, and steel slag, as well as alkali activator, retarder, and water. Among them, the high-calcium fly ash has a SiO2 content of 37.16 wt%, an Al2O3 content of 20.13 wt%, and a CaO content of 17.72 wt%, and belongs to Class C fly ash; The mineral powder used is S95 grade, with a SiO2 content of 25.95 wt%, an Al2O3 content of 13.77 wt%, and a CaO content of 38.40 wt%. The steel slag has a SiO2 content of 19.40 wt%, an Al2O3 content of 6.37 wt%, and a CaO content of 38.72 wt%. Steel slag powder that passes through a 300-mesh sieve is collected. The alkaline activator includes water glass solution and sodium hydroxide. The water glass solution has a Na2O·nSiO2 content of 43.5 wt% and an initial modulus n of 2.3. After the addition of sodium hydroxide, the modulus of the alkaline activator is 1. The retarder selected is 2-acrylamide-2-methylpropanesulfonic acid; The components of the solid waste-based cementitious material are mixed, then an alkali activator, a retarder, and water are added and mixed. Next, modified mixed fibers are added and mixed to obtain a geopolymer slurry. The specific steps are as follows: S31. Add the components of the solid waste-based cementitious material to the mortar mixer and dry mix them evenly. S32. Sodium hydroxide is slowly added to the water glass solution and stirred thoroughly at 350 r / min for 100 s using a magnetic stirrer. After standing for 24 h, the alkaline activator is obtained. S33. Add alkali activator, retarder and water to mortar mixer and mix at low speed to obtain geopolymer wet mix. Then, uniformly disperse the modified mixed fiber into mortar mixer and mix at low speed and high speed in sequence to obtain geopolymer slurry. The low-speed stirring speed is 140 r / min and the stirring time is 90 s; the high-speed stirring speed is 285 r / min and the stirring time is 130 s. S4. The geopolymer slurry is poured, cured, and demolded to obtain a strong, tough, carbon-fixing, waste-utilizing, three-functional geopolymer. The casting mold was a 50.8 mm × 50.8 mm × 50.8 mm cubic mold, in accordance with the requirements of the national standard GB / T 10238-2015 "Oil Well Cement". The curing temperature was 60 ℃ and the curing time was 24 h.

[0031] The raw material mass ratio of the strong, tough, carbon-fixing, waste-utilizing, and three-functional geopolymer in this embodiment is shown in Table 1.

[0032] Table 1. Raw material mass ratios of geopolymers in the examples and comparative examples. Example 2: A tough, carbon-fixing, waste-utilizing, three-functional geopolymer and its preparation method are basically the same as in Example 1, except that the proportion of mineral powder decreases, the proportion of steel slag increases, the proportion of fiber increases, and the proportion of polypropylene fiber increases. The raw material mass ratio of the tough, carbon-fixing, waste-utilizing, three-functional geopolymer in this example is shown in Table 1.

[0033] Example 3: A tough, carbon-fixing, waste-utilizing, three-functional geopolymer and its preparation method are basically the same as in Example 1, except that the proportion of mineral powder increases, the proportion of steel slag decreases, the proportion of fiber decreases, and the proportion of polypropylene fiber decreases. The raw material mass ratio of the tough, carbon-fixing, waste-utilizing, three-functional geopolymer in this example is shown in Table 1.

[0034] Example 4: A geopolymer and its preparation method are basically the same as in Example 1, except that polypropylene fibers are replaced with polyethylene fibers. The mass ratio of raw materials of the geopolymer in this comparative example is shown in Table 1.

[0035] Comparative Example 1: A geopolymer and its preparation method are basically the same as those in Example 1, except that no fiber is added. The mass ratio of the raw materials of the geopolymer in this comparative example is shown in Table 1.

[0036] Comparative Example 2: A geopolymer and its preparation method are basically the same as those in Example 1, except that the mineral powder and steel slag are all replaced with fly ash. The raw material mass ratio of the geopolymer in this comparative example is shown in Table 1.

[0037] Comparative Example 3: A geopolymer and its preparation method are basically the same as in Example 1, except that the fiber length is only 6 mm. The raw material mass ratio of the geopolymer in this comparative example is shown in Table 1.

[0038] Comparative Example 4: A geopolymer and its preparation method are basically the same as in Example 1, except that the ratio of polypropylene fiber to steel fiber is reversed. The raw material mass ratio of the geopolymer in this comparative example is shown in Table 1.

[0039] Comparative Example 5: A geopolymer and its preparation method are basically the same as those in Example 1, except that all steel fibers are replaced with polypropylene fibers. The mass ratio of raw materials of the geopolymer in this comparative example is shown in Table 1.

[0040] Comparative Example 6: A geopolymer and its preparation method are basically the same as in Example 1, except that all polypropylene fibers are replaced with steel fibers. The mass ratio of raw materials of the geopolymer in this comparative example is shown in Table 1.

[0041] Comparative Example 7: A geopolymer and its preparation method are basically the same as in Example 1, except that the fibers are not modified. The mass ratio of the raw materials of the geopolymer in this comparative example is shown in Table 1.

[0042] Comparative Example 8: A geopolymer and its preparation method are basically the same as in Example 1, except that the fiber length is only 12 mm. The raw material mass ratio of the geopolymer in this comparative example is shown in Table 1.

[0043] The above-mentioned geopolymers were subjected to the following tests or examinations, and the results were then analyzed.

[0044] Experimental example: The mechanical properties and carbon fixation properties of the above-mentioned geopolymers were tested, and the specific steps are as follows: The geopolymer was placed in a carbonization vessel and carbonized at a temperature of 60 °C and a carbon dioxide (CO2) pressure of 8 MPa to simulate the high-temperature and high-pressure oil well environment; the carbonization time was set to 8 h, 3 d and 7 d respectively. The compressive strength of geopolymer at 8 h, 3 d, and 7 d was tested using a universal mechanical testing machine according to GB / T 10238-2015 "Oil Well Cement"; the flexural strength of geopolymer at 8 h, 3 d, and 7 d was tested using a universal mechanical testing machine according to GB / T 50081-2019 "Standard for Test Methods of Physical and Mechanical Properties of Concrete"; the carbon fixation content of geopolymer was tested by chemical analysis; the test results are shown in Table 2.

[0045] Downhole environments are typically located more than 800 m underground, where temperatures and pressures generally exceed the critical point of carbon dioxide (CNC), specifically the critical temperature Tc of 31.1 ℃ and the critical pressure Pc of 7.38 MPa, causing CNC to exist primarily in a supercritical state. Therefore, the 60 ℃ and 8 MPa conditions set in this experimental example allow CNC to exist in a supercritical state, more closely resembling the actual phase state, dissolution mass transfer, and mineralization reaction environment of CNC in deep reservoirs. This enhances the representativeness and engineering reference value of the experimental results for in-situ CNC geological sequestration conditions.

[0046] Thermogravimetric analysis, Fourier transform infrared spectroscopy, and X-ray diffraction are commonly used to evaluate the carbon fixation performance of geopolymers. However, compared with chemical analysis methods, these methods generally suffer from drawbacks such as complex sample pretreatment procedures, long testing cycles, and high costs, making it difficult to meet the need for rapid quantitative evaluation of carbon fixation performance. This experimental example uses chemical analysis to evaluate the carbon fixation performance of geopolymers. A 15 wt% hydrochloric acid (HCl) aqueous solution was used. First, the beaker, graduated cylinder, and glass stir bar were washed and dried to constant weight. The mass of the empty beaker was measured using an electronic balance and recorded as _____. m a The geopolymer sample, before or after carbonization, is dried, ground, and mixed evenly. A certain mass of the powder sample is weighed and placed in a beaker. The mass of the powder sample is recorded as follows: m b Separately weigh the total mass of the empty graduated cylinder and the stirring rod, and record it as follows: m c Add sufficient hydrochloric acid solution of known concentration to the vector cylinder, weigh the hydrochloric acid solution, and record the mass as . m d The hydrochloric acid solution was then slowly added to the beaker containing the powdered sample, and the mixture was continuously stirred with a stir bar to ensure that the carbon-containing components that release carbon dioxide reacted fully until no obvious bubbles were produced. During the reaction, splashing of the solution, sample adhesion loss, and prolonged exposure to prevent moisture evaporation should be avoided. After the reaction was complete, the beaker containing the reacted sample, the used graduated cylinder, and the stir bar were weighed together on a balance. The total mass was recorded as follows: m e ; The calculation formula is as follows: In the formula m C % represents the mass of carbon dioxide released per unit of acid-hydrolyzable carbon-containing component in the polymer; m a It refers to the mass of the beaker; m b It is the mass of the geopolymer; m c It is the total mass of the graduated cylinder and the stirring rod; m d It is the mass of the hydrochloric acid solution; m e It is the total mass of the beaker, graduated cylinder, stirring rod, and the mixture after the reaction. S C It is the amount of carbon sequestration; m C1 % represents the mass of carbon dioxide released per unit unit of acid-hydrolyzable carbon-containing component in the polymer after carbonization; m C2 % represents the mass of carbon dioxide released per unit of acid-hydrolyzable carbon-containing component in the polymer before carbonization.

[0047] Table 2. Performance of geopolymers in the Examples and Comparative Examples As shown in Table 2, comparing the geopolymers with different amounts of mineral powder, steel slag, and fiber in Examples 1 to 3, it can be found that the geopolymer in Example 1 has the highest compressive strength, flexural strength, and carbon fixation at all curing ages. Taking the 7-day performance as an example, the compressive strength of the geopolymer in Example 1 is 6.27% and 11.21% higher than that in Examples 2 and 3, respectively; the flexural strength is 9.15% and 16.78% higher, respectively; and the carbon fixation is 16.65% and 4.79% higher, respectively. This indicates that the optimal combination of mineral powder, steel slag, and fiber in Example 1 achieves a balance. Comparing the geopolymers using different plastic fibers in Examples 1 and 4 reveals that the geopolymer in Example 1 still exhibits higher compressive strength, flexural strength, and carbon fixation at most curing ages. Taking the 7-day performance as an example, the compressive strength, flexural strength, and carbon fixation of the geopolymer in Example 1 are increased by 6.60%, 12.95%, and 11.81% respectively compared to Example 4. This indicates that under the raw material composition and modification conditions of the present invention, the combination of polypropylene fiber and steel fiber in Example 1 has better interfacial compatibility and synergistic reinforcement effect. According to the national standard GB / T10238-2015 "Oil Well Cement", the compressive strength of Grade G oil well cement at 8 hours should not be less than 10.30 MPa. The geopolymer in this invention not only meets this standard requirement at 8 hours, but in particular, the measured compressive strength of the geopolymer in Example 1 is close to four times the standard limit, showing a significant early strength advantage. Comparing the geopolymers of Example 1 and Comparative Example 1 with and without added fibers, it can be found that the compressive strength of the geopolymer in Comparative Example 1 is not much different from that of Example 1, indicating that the addition of fibers has a relatively limited effect on compressive strength; however, the flexural strength of the geopolymer in Comparative Example 1 is significantly different from that of Example 1. This is because the hybrid fibers in this invention can form a bridging structure inside the matrix, inhibiting the initiation and propagation of microcracks, thereby significantly improving the flexural strength of the geopolymer. Comparing the geopolymer in Example 1 with Comparative Example 2, which uses only fly ash as a solid waste-based cementitious material, reveals that the compressive strength, flexural strength, and carbon sequestration of the geopolymer in Comparative Example 2 are significantly reduced at all curing ages. This is because the calcium content in the pure fly ash system of Comparative Example 2 is low, resulting in slower dissolution of fly ash particles and a slower geopolymerization reaction, leading to a limited amount of gel formed in the early stages. In this invention, the addition of mineral powder and steel slag provides soluble calcium ions (Ca). 2+ The active silica-alumina components promote the formation of calcium-rich gels such as C-(A)-SH, and improve the matrix density through nucleation and micro-aggregate filling. At the same time, the calcium-rich components can also react with the captured carbon dioxide to form stable calcium carbonate, thus achieving higher early strength and carbon fixation. Comparing the geopolymer in Example 1 with Comparative Examples 3 and 8, which use a single fiber length, reveals that the geopolymers in Comparative Examples 3 and 8 exhibit lower compressive strength, flexural strength, and carbon fixation at various curing ages. This is because the use of a single fiber length in Comparative Examples 3 and 8 makes it difficult to simultaneously control cracks of different scales, and fibers of the same length are more prone to entanglement and local aggregation, resulting in pores or weak interfaces. In this invention, fibers of different lengths have complementary crack control effects. Short fibers can inhibit the initiation and early propagation of microcracks, while long fibers can cross larger cracks and bear the tensile stress during crack opening. Comparing the proportions of geopolymer and exchange fiber in Example 1 with Comparative Example 4, it can be found that the compressive strength, flexural strength and carbon fixation of geopolymer in Comparative Example 4 are significantly reduced at each curing age. This is because the elastic modulus of plastic fiber is relatively low. The excessively high volume ratio of plastic fiber in Comparative Example 4 is prone to fiber entanglement and uneven dispersion. At the same time, the number of metal fibers is insufficient, making it difficult to form an effective high-stiffness load-bearing and crack bridging network. Comparing Example 1 with Comparative Examples 5 and 6, which contain only single-material fibers, it can be found that the compressive strength, flexural strength, and carbon fixation of the geopolymers in Comparative Examples 5 and 6 are all low at various curing ages. This is because although the single plastic fiber in Comparative Example 5 can suppress microcracks, its elastic modulus is low and its load-bearing capacity is limited; although the single steel fiber in Comparative Example 6 has high tensile strength and elastic modulus, its dispersion and control effect on early microcracks is insufficient. In this invention, the two fibers, when mixed, can act on cracks of different scales respectively, forming a multi-scale bridging and stepwise crack-blocking mechanism, thereby obtaining comprehensive performance superior to that of a single-fiber system. Comparing the geopolymers of Example 1 and Comparative Example 7 with and without fiber modification, it can be found that the compressive strength and flexural strength of the geopolymer in Comparative Example 7 are similar to those of Example 1, but the carbon fixation amount is significantly different. This is because the porous structure and surface active sites of the biochar-modified layer in this invention can enrich carbon dioxide and provide an adhesion interface for the nucleation and deposition of calcium carbonate, which is the main reason for the significant increase in carbon fixation amount. At the same time, the carbon fixation amount of the geopolymer in Comparative Example 7 is basically the same as that of Comparative Example 1 without fiber, indicating that the unmodified fiber mainly plays a physical bridging and reinforcing role, and its contribution to the increase in carbon fixation amount is not significant. In summary, the high-calcium fly ash, mineral powder, and steel slag in this invention undergo dissolution, condensation, and calcium-rich gel formation reactions under alkaline activation conditions, providing a dense supporting matrix and mineralizable calcium components for the geopolymer. Plastic and metal fibers of different lengths and moduli form a multi-scale bridging network, enabling hierarchical control of micro and macro cracks. The biochar-modified layer on the fiber surface further achieves carbon dioxide enrichment and carbonate-induced nucleation. Only under the combined effects of specific solid waste-based cementitious material ratios, fiber dosage, mixing ratios, size combinations, and modification conditions can excellent compressive strength, good flexural strength, and significant carbon sequestration be simultaneously achieved, demonstrating a clear synergistic effect.

[0048] This invention, through the synergistic effect of solid waste-based cementitious materials and modified mixed fibers, enhances the early strength and toughness of geopolymers while simultaneously improving their carbon fixation capacity. This allows the material to simultaneously absorb and fix carbon during the toughening and strengthening process, thus achieving a synergistic improvement in both strength, toughness, and carbon fixation performance. Furthermore, this invention not only realizes the high-value and large-scale utilization of industrial solid waste but also significantly reduces carbon emissions in the cement industry, achieving the goal of carbon-negative production. It possesses significant environmental and economic benefits and is suitable for widespread application.

[0049] The above description of the embodiments is provided to enable those skilled in the art to understand and use the invention. It will be apparent to those skilled in the art that various modifications can be made to these embodiments, and the general principles described herein can be applied to other embodiments without inventive effort. Therefore, the present invention is not limited to the above embodiments, and any improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the invention should be within the protection scope of the present invention.

Claims

1. A strong, tough, carbon-fixing, waste-utilizing, three-functional geopolymer, characterized in that, The raw materials for this polymer include the following components in parts by weight: The mixture contains 85-115 parts of solid waste-based cementitious material, 1.1-1.3 parts of modified mixed fiber, 35-37 parts of alkali activator, 2.8-3.2 parts of retarder, and 27-31 parts of water. The modified hybrid fiber includes plastic fibers and metal fibers of different sizes modified with biochar, wherein the mass ratio of plastic fibers to metal fibers is (0.1~0.3):1; The plastic fibers are composed of three sizes with lengths of 5-7 mm, 8-10 mm, and 11-13 mm, with a mass ratio of (0.8-1.2):(0.8-1.2):

1. The metal fibers consist of two sizes: 5-7 mm and 11-13 mm in length, with a mass ratio of (0.3-0.7):

1.

2. The strong, tough, carbon-fixing, waste-utilizing, three-functional geopolymer according to claim 1, characterized in that, The solid waste-based cementitious material comprises 85-115 parts, including 60-70 parts of high-calcium fly ash, 20-30 parts of mineral powder, and 5-15 parts of steel slag.

3. The strong, tough, carbon-fixing, waste-utilizing, three-functional geopolymer according to claim 2, characterized in that, The high-calcium fly ash has a SiO2 content of 30-44 wt%, an Al2O3 content of 15-25 wt%, and a CaO content of 10-26 wt%, and belongs to Class C fly ash. The mineral powder is selected from one or more of S95 grade mineral powder and S105 grade mineral powder, and the SiO2 content of the mineral powder is 20~32 wt%, the Al2O3 content is 10~18 wt%, and the CaO content is 30~46 wt%. The steel slag has a SiO2 content of 10-28 wt%, an Al2O3 content of 4-8 wt%, and a CaO content of 30-48 wt%, and the steel slag powder that passes through a 200-400 mesh sieve is retained.

4. The strong, tough, carbon-fixing, waste-utilizing, three-functional geopolymer according to claim 1, characterized in that, The plastic fiber is selected from one or more of polyethylene fiber, polypropylene fiber, polyvinyl alcohol fiber, and polyacrylonitrile fiber. The diameter of the plastic fiber is 18~38 μm, the tensile strength is >400 MPa, and the elastic modulus is >3.5 GPa. The metal fiber is selected from one or more steel fibers selected from hooked steel fibers, straight steel fibers, and milled steel fibers. The diameter of the metal fiber is 180~200 μm, the tensile strength is >1000 MPa, and the elastic modulus is >200 GPa.

5. The strong, tough, carbon-fixing, waste-utilizing, three-functional geopolymer according to claim 1, characterized in that, The alkaline activator comprises a water glass solution and sodium hydroxide. The water glass solution has a Na2O·nSiO2 content of 40~47 wt% and an initial modulus n of 2.0~2.

6. After the addition of sodium hydroxide, the modulus of the alkaline activator is 0.8~1.

2.

6. The strong, tough, carbon-fixing, waste-utilizing, three-functional geopolymer according to claim 1, characterized in that, The retarder is selected from one or more of 2-acrylamide-2-methylpropanesulfonic acid, sodium citrate, sodium lignin sulfonate, and sucrose.

7. A method for preparing a strong, tough, carbon-fixing, waste-utilizing, three-functional geopolymer as described in any one of claims 1 to 6, characterized in that, The method includes the following steps: S1. Biomass is heated and cooled under a protective atmosphere to obtain biochar. The biochar is ground and sieved. The biochar is mixed with water to obtain biochar slurry. The biochar slurry is coated on the surface of fibers and dried. Plastic fibers and metal fibers of different sizes are mixed to obtain modified mixed fibers. S2. Mix the components of the solid waste-based cementitious material, add alkali activator, retarder and water to obtain geopolymer wet mix, add modified mixed fiber to obtain geopolymer slurry; S3. The geopolymer slurry is poured, cured, and demolded to obtain a strong, tough, carbon-fixing, and waste-utilizing geopolymer.

8. The preparation method of a strong, tough, carbon-fixing, waste-utilizing, three-functional geopolymer according to claim 7, characterized in that, Before step S1, the fibers are pretreated, which includes the following steps: The fibers were immersed in an alcohol solution, ultrasonically treated, rinsed, and dried. The alcohol solution is selected from one or more aqueous solutions of ethanol, methanol, isopropanol, and n-propanol, and the concentration of the alcohol solution is 70-80 vol%. The volume ratio of the fiber to the alcohol solution is 1:(2-6). The ultrasonic treatment was performed at a frequency of 35–45 kHz for a duration of 100–120 min. The drying temperature is 30~40 ℃ and the time is 120~240 min.

9. The preparation method of a strong, tough, carbon-fixing, waste-utilizing, three-functional geopolymer according to claim 7, characterized in that, In step S1, the biomass is selected from one or more of sawdust, corn cobs, rice husks, and sugarcane bagasse. The heating temperature is 300~400 ℃, the heating rate is 5~15 ℃ / min, and the holding time is 45~60 min. Retain the biochar that passes through a 200-400 mesh sieve. The mass ratio of biochar to water is 1:(4~8). The drying temperature is 25~40 ℃, and the time is 5~9 days.

10. The method for preparing a strong, tough, carbon-fixing, waste-utilizing, three-functional geopolymer according to claim 7, characterized in that, In step S2, sodium hydroxide is added to the water glass solution and mixed, then allowed to stand to obtain the alkali activator. The standing time is 12-36 hours. Add alkali activator, retarder and water and mix at low speed. Add modified mixed fiber and mix at low speed and high speed. The speed of low speed mixing is 130~150 r / min and the time is 60~120 s. The speed of high speed mixing is 270~300 r / min and the time is 100~160 s.

Citation Information

Patent Citations

  • Hybrid fiber reinforced ultrahigh-performance geopolymer concrete as well as preparation method and application thereof