A self-sensing, impact-resistant, ultra-high performance underwater concrete and its preparation method
By designing organic conductive elastic aggregates with core-shell structures, the problems of signal instability and insufficient abrasion resistance in traditional concrete under abrasion conditions were solved, achieving a unity of self-sensing and high toughness in concrete, and improving abrasion resistance and electrical signal stability.
Patent Information
- Application Number
- CN202511951856.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-12-23
- Publication Date
- 2026-11-17
AI Technical Summary
Traditional conductive admixtures are prone to uneven dispersion in concrete, corrosion, and significant humidity interference, resulting in poor signal stability and difficulty in achieving reliable sensing under impact and abrasion conditions. Furthermore, traditional concrete has insufficient impact and abrasion resistance.
The design incorporates an organic conductive elastic aggregate with a core-shell structure. The core is an organosilicon elastomer containing dynamic borate ester bonds, while the outer shell is a conductive network. Through heating and melting, hot pressing, oxygen plasma treatment, and surface modification, a stable conductive pathway is formed, ensuring the interfacial adhesion and conductivity of the aggregate-cement matrix.
It achieves a balance between the self-sensing ability and high toughness of concrete in underwater high-impact and abrasion environments, improves its resistance to impact and abrasion, and possesses stable mechanical load-sensitive resistor response characteristics and electrical signal stability with minimal environmental interference.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention relates to the field of ultra-high performance concrete technology, specifically to an underwater self-sensing impact-resistant ultra-high performance concrete and its preparation method. Background Technology
[0002] Hydraulic concrete structures are subjected to harsh abrasive environments such as high-speed water flow and sand-laden waves for extended periods. Critical components such as bridge piers are subjected to intense abrasion and cavitation over long periods, which can easily lead to mortar abrasion and spalling on the concrete surface, performance degradation, and even structural failure, seriously affecting the safety and durability of the project.
[0003] To improve the impact and abrasion resistance of concrete, traditional technical approaches mainly include using high-strength aggregates, incorporating ultrafine mineral admixtures such as silica fume, optimizing aggregate gradation, and introducing fiber reinforcement for toughening. Among these, ultra-high performance concrete, due to its superior mechanical and durability properties, exhibits impact and abrasion resistance more than ten times that of ordinary concrete, making it a promising candidate for the preparation of impact-resistant and abrasion-resistant cementitious materials. Recent research has found that introducing elastic components such as rubber particles into concrete can effectively dissipate impact energy and buffer stress concentration, thereby significantly improving the impact and abrasion resistance of cementitious materials.
[0004] On the other hand, the development of modern engineering structures towards intelligence and multifunctionality has created an urgent need for the "self-sensing" capabilities of materials. This means that materials must be able to sense their own stress or damage status in real time during service and output electrical signals to achieve health monitoring and early warning. Materials subjected to impact and abrasion conditions also have technical requirements for self-sensing, which is particularly important for structures in harsh environments such as impact and abrasion. However, traditional conductive admixtures are prone to uneven dispersion in concrete, corrosion, and significant humidity interference, resulting in poor signal stability and making reliable sensing difficult under impact and abrasion conditions. Therefore, there is an urgent need to develop a new type of concrete material that can synergistically improve impact and abrasion resistance while maintaining stable self-sensing functionality. Summary of the Invention
[0005] To address the shortcomings of existing technologies, this invention provides an underwater self-sensing, abrasion-resistant ultra-high performance concrete and its preparation method. This invention innovatively designs and prepares an organic conductive elastic aggregate with a core-shell structure. The organic conductive elastic aggregate uses an organosilicon elastomer containing dynamic borate ester bonds as its core to impart high elasticity and damage tolerance. Furthermore, through an internal and external composite conductive network design and surface modification, the stability of the conductive pathway and the interfacial adhesion between the aggregate and cement matrix are ensured. By using the aforementioned organic conductive elastic aggregate in the preparation of self-sensing, abrasion-resistant ultra-high performance concrete, this invention not only significantly enhances the concrete's abrasion and impact resistance through an elastic buffering mechanism, but also, thanks to its stable three-dimensional conductive network, enables the concrete to possess resistive response characteristics that are sensitive to mechanical loads and less affected by environmental interference. Thus, it successfully achieves a balance between the self-sensing capability and high toughness of concrete under underwater high-abrasion environments.
[0006] To achieve the above objectives, the specific technical solution of the present invention is as follows:
[0007] In a first aspect, the present invention provides a method for preparing an organic conductive elastic aggregate, comprising the following steps:
[0008] S1. Mix the organic elastomer powder with the pretreated conductive filler I, heat and melt, hot press and mold, crush and screen to obtain the organic conductive elastic aggregate core.
[0009] The organic elastomer powder is prepared by the following method: a cyclotrisiloxane mixed monomer is mixed with bis(dimethylborate)hexamethyldisiloxane (B2), and dehydrated at 80°C and a vacuum degree <0.1 mm Hg for 1-3 h; a catalyst is added, and the system temperature is set at 85-95°C for a ring-opening copolymerization reaction for 7-10 min; a terminator is added to terminate the reaction, and the system is naturally cooled to 58-62°C, and an end-capping agent is added to promote borate bond exchange and end-group capping; the temperature is then raised to 100-120°C and maintained for 13-18 min to decompose the residual catalyst and obtain a crude product; the crude product is purified, dried, and ground to obtain the organic elastomer powder.
[0010] S2. After the organic conductive elastic aggregate core is treated with oxygen plasma to activate the surface, it is mixed with polymerizable conductive slurry and subjected to in-situ polymerization reaction. A layer of polymerizable conductive slurry composed of polymerizable siloxane monomer and conductive filler II is coated on the surface of the organic conductive elastic core. After post-curing, purification and drying, an outer shell is formed to obtain the organic conductive elastic aggregate precursor.
[0011] The polymerizable conductive slurry is prepared by the following method: first, conductive filler II is dispersed in a solvent and ultrasonically treated to form a uniform dispersion; then, under inert gas protection, cyclotrisiloxane monomers and bis(dimethylborate)hexamethyldisiloxane (B2) are added to the uniform dispersion and mixed evenly; just before use, an initiator is added and mixed evenly to avoid premature reaction, thus obtaining the polymerizable conductive slurry;
[0012] S3. After soaking the organic conductive elastic aggregate precursor in an alkaline solution, it is cleaned and dried, and then immersed in a titanate coupling agent solution, cleaned, and dried to obtain an organic conductive elastic aggregate with a core-shell structure.
[0013] Further, in step S1, the mass ratio of the organic elastomer powder to the pretreated conductive filler I is 100:(10-40).
[0014] Further, in step S1, the cyclotrisiloxane mixed monomers include phenyltrimethylcyclotrisiloxane (P3), γ-epoxypropoxypropyltrimethylcyclotrisiloxane (E3), and methylvinylcyclotrisiloxane (V3) in a molar ratio of (50-80):(10-30):(5-20).
[0015] Further, in step S1, the amount of bis(dimethylborate)hexamethyldisiloxane used is 3%-6% of the total mass of the cyclotrisiloxane mixed monomers.
[0016] Further, in step S1, the catalyst includes at least one of tetramethylammonium hydroxide silanoate and tetramethylammonium hydroxide.
[0017] Further, in step S1, after adding the catalyst, the mixture is stirred at a speed of 400-600 r / min for 25-35 s, and then the speed is adjusted back to 200-300 r / min for reaction.
[0018] Further, in step S1, the terminating agent includes at least one of methanol, ethanol, and isopropanol.
[0019] Furthermore, in step S1, after adding a terminator to terminate the reaction, the number-average molecular weight (Mn) of the product in the system is 80,000-120,000.
[0020] Further, in step S1, the capping agent includes at least one of hexamethyldisiloxane and trimethylchlorosilane.
[0021] Further, in step S1, the purification, drying, and grinding of the crude product are performed as follows: the crude product is dissolved in a solvent, and a mixture of precipitant and water is added dropwise under vigorous stirring. The mixture is filtered, washed three times with methanol, the filter cake is collected, dried, and ground to obtain organic elastomer powder. The solvent includes at least one of tetrahydrofuran and acetone. The precipitant includes at least one of methanol and ethanol. The volume ratio of precipitant to water is (9-8):(1-2). The drying temperature is 70-100℃, and the drying time is 4-7 h.
[0022] Further, in step S1, the pretreatment operation of the conductive filler I is as follows: the conductive filler I is surface modified with a modifier to improve its compatibility and dispersibility with the organic elastic powder matrix, thereby obtaining the pretreated conductive filler I; the mass ratio of the conductive filler I to the modifier is 100:(1-5); the modifier includes at least one of 3-aminophenylboronic acid pinacol ester, tridecafluorooctyltriethoxysilane, and 3-mercaptopropyltrimethoxysilane; the conductive filler I includes at least one of carbon nanotubes, polyaniline, and ultrafine copper powder.
[0023] Furthermore, in step S1, the heating and melting temperature is 160-190℃, and the time is 10-15 min.
[0024] Further, in step S2, the mass ratio of the organic conductive elastic aggregate core to the solids in the polymerizable conductive slurry is (5-10):1.
[0025] Further, in step S2, the operation of activating the surface of the organic conductive elastic aggregate core by oxygen plasma treatment is as follows: the organic conductive elastic aggregate core is subjected to oxygen plasma treatment in a vacuum environment, and after treatment, the organic conductive elastic aggregate core is stored in a dry inert atmosphere and used for the next step of slurry coating within 8 hours to prevent the active sites from becoming ineffective; in the oxygen plasma treatment, the oxygen flow rate is 20-50 sccm, the power of the plasma generator is 100-200 W, and the treatment time is 60-180 s; the inert atmosphere includes at least one of nitrogen and argon.
[0026] Further, in step S2, the conductive filler II includes at least one of graphene, carbon nanotubes, and polyaniline.
[0027] Further, in step S2, the mass ratio of the conductive filler II to the epoxy trisilane monomer is (5%-10%):(90%-93%), and the amounts of the dynamic crosslinking agent and the initiator are 2%-2.3% and 2%-2.5% of the mass of the epoxy trisilane monomer, respectively.
[0028] Further, in step S2, the cyclotrisiloxane monomer includes at least one of methylvinylcyclotrisiloxane and γ-epoxypropoxypropyltrimethylcyclotrisiloxane.
[0029] Further, in step S2, the initiator includes at least one of benzoyl peroxide and azobisisobutyronitrile.
[0030] Further, in step S2, the solvent includes at least one of toluene, N-methylpyrrolidone, and tetrahydrofuran.
[0031] Furthermore, in step S2, the mixture is stirred mechanically at a speed of 250-400 r / min for a time of 30-80 min.
[0032] Furthermore, in step S2, the post-curing temperature is 100-120℃ and the time is 1-2 h.
[0033] Furthermore, in step S2, the purification solvent used for purification includes at least one of n-hexane, ethanol, and petroleum ether.
[0034] Furthermore, in step S2, the drying temperature is 50-60°C.
[0035] Further, the specific operation of step S2 is as follows: After surface activation of the organic conductive elastic aggregate core by oxygen plasma treatment, a polymerizable conductive slurry is added, and most of the solvent is removed under reduced pressure at 40-60℃, so that the polymerizable conductive slurry forms a viscous prepolymer layer on the surface of the organic conductive elastic aggregate core; the temperature is raised to 80-110℃ for 1-3 h to initiate a free radical copolymerization reaction of vinyl groups on the surface of the organic conductive elastic aggregate core and in the slurry, and then placed in an oven for post-curing at 100-120℃ for 1-2 h, and finally purified using a purification solvent, and vacuum dried at 50-60℃ to obtain the organic elastic conductive aggregate precursor.
[0036] Further, in step S3, the alkaline solution comprises a NaOH aqueous solution with a mass fraction of 5%-8%.
[0037] Furthermore, in step S3, the organic elastic conductive aggregate precursor is soaked in alkaline solution for 20-30 minutes.
[0038] Further, in step S3, the titanate coupling agent solution is a titanate coupling agent ethanol solution with a mass fraction of 1%-2.5%.
[0039] Further, in step S3, the organic elastic conductive aggregate precursor is immersed in the titanate coupling agent solution for 25-45 minutes.
[0040] Furthermore, in step S3, the cleaning is performed by rinsing with clean water.
[0041] This invention first synthesizes an organosilicon elastomer with dynamic borate ester bonds by synthesizing a mixture of cyclotrisiloxane monomers P3, E3, and V3 in the presence of dynamic crosslinking agent B2 through ring-opening copolymerization, dynamic bond formation and end-capping, and purification. Further, the obtained organosilicon elastomer powder is mixed with surface-modified conductive filler I, and then melt-blended, hot-pressed, crushed, and sieved to obtain an organic conductive elastic aggregate core. Subsequently, the organic conductive elastic aggregate core is treated with oxygen plasma to activate its surface. Then, through impregnation and in-situ polymerization, a polymerizable conductive slurry composed of polymerizable cyclotrisiloxane monomers and conductive filler II is coated onto the surface of the organic conductive elastic aggregate to form an outer shell. Finally, the outer shell is surface-modified using a titanate coupling agent solution to obtain the final product, the organic conductive elastic aggregate.
[0042] This invention synthesizes an organosilicon elastomer with high elasticity, stable conductivity, and excellent durability through the synergistic effect of cyclotrisiloxane mixed monomers P3, E3, and V3 and a dynamic crosslinking agent B2. By introducing dynamic borate ester bonds, the aggregate core acquires good stress buffering and damage tolerance capabilities. Simultaneously, it provides a foundation for constructing a robust three-dimensional conductive network and optimizing the interface, thereby endowing concrete with stable force-electric sensing function and high toughness. Replacing traditional aggregates with this organic conductive elastic aggregate can produce self-sensing, impact-resistant, ultra-high performance concrete.
[0043] Further, the phenyltrimethylcyclotrisiloxane is prepared by the following method: phenyltrichlorosilane is slowly added dropwise to an ice-water mixture, and the temperature is controlled below 10°C to carry out a hydrolysis reaction; after hydrolysis, the organic phase is extracted and collected, and then dried and concentrated to obtain phenylsilanetriol; then, the phenylsilanetriol is cyclized at 125-145°C for 3-6 h under an acidic catalyst; finally, it is vacuum distilled at 180-190°C to collect phenyltrimethylcyclotrisiloxane; the acidic catalyst includes at least one of toluenesulfonic acid and trifluoromethanesulfonic acid.
[0044] Further, the γ-epoxypropoxypropyltrimethylcyclotrisiloxane is prepared by the following method: γ-epoxypropoxypropyltrimethoxysilane is added dropwise to a mixture of water and a co-solvent, the pH is adjusted to 3.5-4.5 with acid, and a hydrolysis-condensation reaction is carried out by stirring at room temperature. The solvent is removed under reduced pressure to obtain an epoxy silanol mixture. The epoxy silanol mixture is cyclized under alkaline conditions at 150-170℃ for 4-7 h, and then purified by vacuum distillation at 180-200℃ to collect γ-epoxypropoxypropyltrimethylcyclotrisiloxane. The co-solvent includes at least one of methanol, ethanol, and isopropanol; the acid includes at least one of acetic acid and trifluoroacetic acid; the alkaline conditions include KOH solution and / or tetramethylammonium hydroxide solution with a mass concentration of 0.03%-0.06%.
[0045] Further, the bis(dimethylborate)hexamethyldisiloxane is prepared by the following method: hexamethyldisiloxane is reacted with n-butyllithium at a low temperature of -65 to -80°C to generate a bislithium salt, then trimethylborate is slowly added, and the temperature is raised to room temperature for 10-16 h; then hydrolysis is carried out in a hydrolysis solution, followed by extraction, drying, and finally purification by vacuum distillation to obtain bis(dimethylborate)hexamethyldisiloxane; the molar ratio of hexamethyldisiloxane, n-butyllithium solution, and trimethylborate is 1:(2.1-2.3):(2.0-2.1); the hydrolysis solution includes at least one of saturated ammonium chloride aqueous solution and dilute hydrochloric acid solution.
[0046] In a second aspect, the present invention provides an organic elastic conductive aggregate prepared by the aforementioned preparation method, wherein the organic conductive elastic aggregate has a particle size of 2.36-4.75 mm, an elongation of 300%-400%, and an apparent density of 1020-1200 kg / m³. 3 Volume resistivity ≤200 Ω / cm.
[0047] A third aspect of the invention provides the application of the organic elastic conductive aggregate in the preparation of self-sensing concrete.
[0048] In a fourth aspect, the present invention provides an underwater self-sensing, impact-resistant, ultra-high performance concrete, comprising the following raw materials in parts by weight: 650-850 parts cement, 100-250 parts fly ash microspheres, 50-250 parts silica fume, 50-200 parts organic conductive elastic aggregate, 800-950 parts manufactured sand, 150-240 parts copper-plated steel fiber, 15-30 parts water-reducing agent, and 170-200 parts water.
[0049] Furthermore, the cement is 52.5 ordinary Portland cement.
[0050] Furthermore, the fly ash microspheres have a loss on ignition of ≤5.3%, a water requirement ratio of ≤92%, and a spherical particle volume fraction of ≥90%.
[0051] Furthermore, the silica fume contains ≥94% SiO2 by mass and has a specific surface area ≥14400 m². 2 / kg, 28d activity index ≥98%.
[0052] Furthermore, the copper-plated steel fiber has a nominal length of 13-16 mm, a diameter of 0.2-0.3 mm, a tensile strength greater than 1400 MPa, an elastic modulus of 200-260 GPa, and a density of 6900-8000 g / m³. 3 .
[0053] Furthermore, the water-reducing agent is a polycarboxylate water-reducing agent with a water reduction rate greater than 30%.
[0054] This invention utilizes the aforementioned organic conductive elastic aggregate to prepare ultra-high performance concrete, achieving intelligent concrete design while optimizing its overall performance. The organic conductive elastic aggregate, with its highly elastic core and three-dimensional conductive network, enables the concrete to possess excellent stress buffering, impact and abrasion resistance, and stable force-electric response, achieving a balance between structural self-sensing and high toughness. The lightweight properties of the organic conductive elastic aggregate help reduce the structural weight, and its surface modification ensures a strong bond with the cement matrix. Combined with the use of mineral admixtures and high-efficiency water-reducing agents, the workability, density, and durability of the concrete are further optimized. This provides an effective solution for developing a new generation of multifunctional, high-toughness cement-based composite materials.
[0055] A fifth aspect of the present invention provides a method for preparing the self-sensing impact-resistant ultra-high performance concrete, comprising the following steps:
[0056] P1: Add manufactured sand, cement, silica fume and fly ash microspheres to a concrete mixer and premix for 1-3 minutes. Then add organic elastic conductive aggregate and mix for 1-3 minutes. Add water and water-reducing agent and continue mixing for 2-4 minutes. After the mixture in the mixer reaches a viscous state, add copper-plated steel fibers evenly and continue mixing for 1-3 minutes.
[0057] P2: The mixed material is placed in molds, vibrated, and shaped. The surface is covered with a waterproof film. The standard curing conditions specified in GB / T50081 are adopted. After 1 day, the mold is removed and standard curing is carried out. The standard curing and testing age is 28 days, which yields self-sensing impact and abrasion resistant ultra-high performance concrete.
[0058] Compared with the prior art, the advantages of the present invention are:
[0059] (1) This invention provides a novel organic conductive elastic aggregate with a core-shell structure, the core of which contains dynamic borate ester bonds, giving the aggregate excellent elasticity and toughness; through the design of an internal and external composite conductive network, the stability of the conductive performance is ensured, fundamentally improving the problem of uneven dispersion and easy failure of conductive fillers in traditional methods.
[0060] (2) The core-shell structure design and surface functionalization technology of the organic conductive elastic aggregate developed in this invention has universality. In the future, this technology can be extended to the high-value modification of bulk polymer solid wastes such as waste tire rubber and waste thermoplastic elastomers, transforming them into high-performance aggregates with similar structures and functions. This opens up a new and highly promising path for the resource utilization of solid waste, while significantly reducing dependence on natural sand and gravel aggregates, demonstrating long-term environmental protection and resource recycling benefits.
[0061] (3) Compared with traditional functional aggregates, the organic conductive elastic aggregate of the present invention has strong adhesion to the cement matrix and good alkali resistance after surface activation and modification. When used in concrete, it can improve the material’s resistance to impact and cracking, while giving it a stable force-electric sensing function, laying the foundation for the development of intelligent and high-toughness cement-based materials. Detailed Implementation
[0062] The following further illustrates the application and preparation method of the organic conductive elastic aggregate of this application in UHPC materials with specific embodiments. This section further illustrates the content of the present invention with reference to specific embodiments, but should not be construed as limiting the present invention. Unless otherwise specified, the technical means used in the embodiments are conventional means well known to those skilled in the art. Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art. The technical solutions in the embodiments of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, and not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0063] This invention provides a method for preparing an organic conductive elastic aggregate, comprising the following steps:
[0064] S1. Preparation of organic elastomer powder: Using phenyltrimethylcyclotrisiloxane (P3), γ-epoxypropoxypropyltrimethylcyclotrisiloxane (E3), and methylvinylcyclotrisiloxane (V3) as mixed monomers, and bis(dimethylborate)hexamethyldisiloxane (B2) as a dynamic crosslinking agent, organic elastomer powder is obtained through dehydration treatment, ring-opening copolymerization reaction, dynamic bond formation and end-capping, purification, drying, and grinding.
[0065] S2. Preparation of organic conductive elastic aggregate core: Mix organic elastomer powder with pretreated conductive filler I, heat and melt, hot press molding, crush and screen to obtain organic conductive elastic aggregate core;
[0066] S3. Preparation of organic conductive elastic aggregate shell: After the organic conductive elastic aggregate core is treated with oxygen plasma to activate the surface, it is mixed with polymerizable conductive slurry and subjected to in-situ polymerization reaction. A layer of polymerizable conductive slurry composed of polymerizable siloxane monomer and conductive filler II is coated on the surface of the organic conductive elastic core. After post-curing, purification and drying, the shell is formed to obtain the organic conductive elastic aggregate precursor.
[0067] S4. Surface modification of organic conductive elastic aggregate precursor: After soaking the organic conductive elastic aggregate precursor in alkaline solution, it is cleaned and dried, and then immersed in titanate coupling agent solution, cleaned and dried to obtain organic conductive elastic aggregate with core-shell structure.
[0068] In a specific example of the present invention, the preparation method of the organic conductive elastic aggregate is as follows:
[0069] (1) Synthesis of P3: The raw materials for P3 include phenyltrichlorosilane, deionized water, and extractant. The synthesis steps are as follows: First, phenyltrichlorosilane is slowly added dropwise to an ice-water mixture (deionized water) and the temperature is controlled at <10℃ to carry out the hydrolysis reaction; after the hydrolysis is completed, the organic phase is extracted with the extractant, and then the organic phase is dried with a drying agent. The drying agent is removed by filtration, and the organic phase is removed by vacuum distillation to obtain phenylsilanetriol; then phenylsilanetriol is cyclized at 125-145℃ for 3-6 h under acidic catalyst; finally, P3 is collected by vacuum distillation at 180-190℃.
[0070] The molar ratio of the above-mentioned phenyltrichlorosilane to deionized water is 1:(13-18), and the volume ratio of the extractant to deionized water is (0.5-2):1;
[0071] The above-mentioned extractants include at least one of dichloromethane, toluene, n-hexane, and cyclohexane;
[0072] The aforementioned dryer includes at least one of anhydrous sodium sulfate and anhydrous magnesium sulfate;
[0073] The aforementioned acidic catalysts include at least one of toluenesulfonic acid and trifluoromethanesulfonic acid.
[0074] (2) Synthesis of E3: The raw materials for E3 include γ-epoxypropoxypropyltrimethoxysilane, deionized water, and co-solvent. The synthesis steps are as follows: First, γ-epoxypropoxypropyltrimethoxysilane is added dropwise to a mixture of deionized water and co-solvent. The pH is adjusted to 3.5-4.5 with acid. The hydrolysis and condensation reaction is carried out under stirring at room temperature. The solvent is removed under reduced pressure to obtain an epoxy silanol mixture. The epoxy silanol mixture is cyclized under alkaline conditions at 150-170℃ for 5-7 h. Then, it is purified by vacuum distillation at 180-200℃ to collect E3.
[0075] The molar ratio of the above-mentioned γ-epoxypropoxypropyltrimethoxysilane to deionized water is 1:(5-9), and the volume ratio of the co-solvent to γ-epoxypropoxypropyltrimethoxysilane is (2-5):1.
[0076] The co-solvents mentioned above include at least one of methanol, ethanol, and isopropanol;
[0077] The aforementioned acids include at least one of acetic acid and trifluoroacetic acid;
[0078] The alkaline conditions mentioned above include at least one of KOH solution and tetramethylammonium hydroxide solution, with a mass concentration of 0.03%-0.06%.
[0079] (3) Synthesis of B2: The raw materials for B2 include: hexamethyldisiloxane, n-butyllithium solution, and trimethylboronic acid ester. The synthesis steps are as follows: first, hexamethyldisiloxane and n-butyllithium solution are reacted at a low temperature of -65 to -80℃ to generate a dilithium salt, then trimethylboronic acid ester is slowly added, and the temperature is raised to room temperature for 10-16 h; then hydrolysis is carried out in the hydrolysis solution, and after extraction and drying, B2 is purified by vacuum distillation at 90-110℃.
[0080] The molar ratio of the above-mentioned hexamethyldisiloxane, n-butyllithium solution, and trimethylboronic acid ester is 1:(2.1-2.3):(2.0-2.1).
[0081] The above-mentioned hydrolysis solution includes at least one of saturated ammonium chloride aqueous solution and dilute hydrochloric acid solution (1-2 mol / L);
[0082] The extractant used in the above extraction includes at least one of diethyl ether and n-hexane;
[0083] The drying agent used in the above-mentioned drying process includes at least one of anhydrous sodium sulfate and anhydrous magnesium sulfate.
[0084] (4) Preparation of organic elastomer powder:
[0085] a. Dehydration treatment: Accurately weigh P3, E3, and V3 into a flask, then add B2, connect the vacuum system, and slowly heat to 80℃ at a heating rate of 1-2℃ / min. Perform dehydration treatment for 1-3 h at 80℃ and a vacuum degree <0.1 mmHg. Finally, turn off the vacuum and purge with high-purity nitrogen (99.999%) three times.
[0086] The molar ratio of P3:E3:V3 mentioned above is (50-80):(15-30):(5-20);
[0087] The amount of B2 mentioned above is 3%-6% of the total mass of P3, E3, and V3.
[0088] b. Ring-opening copolymerization reaction: The mixture obtained after dehydration is heated to 60-70℃ while maintaining a rotation speed of 200-300 r / min to dissolve it. Then, the reaction temperature is set to 85-95℃, the condenser is turned on, the catalyst is added and the ring-opening copolymerization reaction is carried out for 7-10 min. The reaction process is monitored, the reaction is terminated by adding a terminator, and then a sample is taken for testing.
[0089] The catalyst dosage mentioned above is 0.01%-0.1% of the total mass of P3, E3, and V3;
[0090] The catalysts mentioned above include at least one of tetramethylammonium hydroxide silanoate and tetramethylammonium hydroxide (TMAH);
[0091] Immediately after adding the catalyst, increase the stirring speed to 400-600 r / min and mix for 25-35 s, then adjust back to 200-300 r / min;
[0092] The amount of the terminator mentioned above is 1.1-5 times the molar amount of the catalyst;
[0093] The aforementioned terminating agents include at least one of methanol, ethanol, and isopropanol;
[0094] The number-average molecular weight (Mn) of the sampled products was 80,000-120,000.
[0095] c. Dynamic bond formation and end-capping: After the ring-opening copolymerization reaction, the system is naturally cooled to 58-62℃, an end-capping agent is added, and stirring is continued to promote the exchange of borate ester bonds and end-group capping; then the temperature is raised to 100-120℃ and maintained for 13-18 min to decompose the residual catalyst and obtain the crude product;
[0096] The aforementioned capping agents include at least one of hexamethyldisiloxane and trimethylchlorosilane;
[0097] The amount of the above-mentioned capping agent is 1-2 times the total molar amount of P3, E3, and V3.
[0098] d. Purification and post-treatment: The crude product was dissolved in a solvent and prepared into a solution. Under vigorous stirring, a mixture of precipitant and water was added dropwise, and a white precipitate gradually precipitated. Stirring was continued, and the mixture was then filtered through a Buchner funnel. The filter cake was washed three times with methanol, and then vacuum dried at 70-100℃ for 4-7 h. The filter cake was then ground to obtain organic elastomer powder.
[0099] The solvents mentioned above include at least one of tetrahydrofuran and acetone;
[0100] The precipitant mentioned above includes at least one of methanol and ethanol; the volume ratio of the precipitant to water is (9-8):(1-2).
[0101] (5) Preparation of organic conductive elastic aggregate core:
[0102] a. The conductive filler I is surface modified with a modifier to obtain pretreated conductive filler I, so as to improve its compatibility and dispersibility with organic elastic powder;
[0103] The aforementioned modifiers include at least one of the following: 3-aminophenylboronic acid pinacol ester, tridecafluorooctyltriethoxysilane, and 3-mercaptopropyltrimethoxysilane;
[0104] The conductive filler I mentioned above includes at least one of carbon nanotubes, polyaniline, and ultrafine copper powder;
[0105] The mass ratio of the conductive filler I to the modifier is 100:(1-5).
[0106] b. Mix the organic elastomer powder with the pretreated conductive filler I, add it to the mixer and melt it at 160-190℃ for 10-15 min until it is uniformly mixed;
[0107] The mass ratio of the above-mentioned organic elastomer powder to the pretreated conductive filler I is 100:(10-30).
[0108] c. Place the uniformly mixed mixture into an iron mold, place the mold into a flat vulcanizing machine, and hot-press to form a conductive composite.
[0109] d. The conductive composite is crushed by a jaw crusher and then screened to obtain organic conductive elastic aggregate cores of different particle sizes.
[0110] (6) Preparation of organic conductive elastic aggregate shell:
[0111] a. Surface activation of organic conductive elastic aggregate core: Place the organic conductive elastic aggregate core in the sample tray of the treatment chamber, evacuate to below 10 Pa, introduce oxygen, maintain the gas flow rate at 20-50 sccm, start the plasma generator, and treat for 60-180 s at a power of 100-200 W; The treated organic conductive elastic aggregate core should be stored in a dry inert atmosphere and used for the next slurry coating within 8 h to prevent the active sites from being deactivated.
[0112] The aforementioned inert gases include either nitrogen or argon.
[0113] b. Preparation of polymerizable conductive slurry: First, disperse conductive filler II in a portion of the solvent and treat it with high-power ultrasound for 30-60 min to form a uniform dispersion; under inert gas protection, add cyclotrisiloxane monomers, dynamic crosslinking agent B2 and the remaining solvent to the uniform dispersion and mix them evenly with mechanical stirring; just before use, add the initiator and stir evenly to avoid premature reaction;
[0114] The mass ratio of the conductive filler II to the epoxy trisilane monomer is (5%-10%):(90%-93%), and the amounts of dynamic crosslinking agent and initiator are 2%-2.3% and 2%-2.5% of the mass of the epoxy trisilane monomer, respectively.
[0115] The solvents mentioned above include at least one of toluene, N-methylpyrrolidone, and tetrahydrofuran;
[0116] The aforementioned cyclotrisiloxane monomers include at least one of V3 and E3;
[0117] The stirring speed mentioned above is 250-400 r / min, and the stirring time is 30-80 min;
[0118] The aforementioned initiators include at least one of benzoyl peroxide and azobisisobutyronitrile.
[0119] c. In a reactor equipped with stirring and temperature control, add the activated organic conductive elastic aggregate core, and then slowly add the prepared polymerizable conductive slurry. Under reduced pressure at 40-60℃, slowly rotate and evaporate or stir to remove most of the solvent, so that the slurry forms a viscous prepolymer layer on the surface of the core.
[0120] The mass ratio of the organic conductive elastic aggregate core to the solids in the polymerizable conductive slurry is (5-10):1; the stirring speed is 100-300 r / min, and the stirring time is 20-40 min.
[0121] d. Raise the temperature to 80-110℃ and maintain it for 1-3 h to initiate the in-situ free radical copolymerization reaction of vinyl groups on the core surface and in the slurry. Then place it in an oven at 100-120℃ for post-curing treatment for 1-2 h. After purification and drying, the organic elastic conductive aggregate precursor is obtained.
[0122] The purification solvent used in the above purification includes at least one of n-hexane, ethanol, and petroleum ether;
[0123] The drying temperature mentioned above is 50-60℃.
[0124] (7) Surface modification treatment of organic elastic conductive aggregate precursor: Wash the organic elastic conductive aggregate precursor with water, air dry it naturally, place it in a clean container, add 5%-8% NaOH aqueous solution until the aggregate surface is just wetted, seal it, and soak for 20-30 min; rinse with water 4-5 times until the pH is neutral, air dry it naturally, transfer it to a clean container, add 1%-2.5% titanate coupling agent ethanol solution until the aggregate surface is just wetted, seal it, soak for 25-45 min, rinse with water 4-5 times, air dry it, and obtain the finished organic elastic conductive aggregate;
[0125] The aforementioned organic elastic conductive aggregate has a particle size of 2.36-4.75 mm, an elongation of 300%-400%, and an apparent density of 1020-1200 kg / m³. 3 Volume resistivity ≤200 Ω / cm.
[0126] The present invention also provides an underwater self-sensing abrasion-resistant ultra-high performance concrete (UHPC) based on the aforementioned organic elastic conductive aggregate, comprising the following raw materials in parts by weight: 650-850 parts cement, 100-250 parts fly ash microspheres, 50-250 parts silica fume, 50-200 parts of the aforementioned organic conductive elastic aggregate, 800-950 parts manufactured sand, 150-240 parts copper-plated steel fiber, 15-30 parts water-reducing agent, and 170-200 parts water.
[0127] In the following specific embodiments, the fly ash microspheres have a loss on ignition ≤ 5.3%, a water requirement ratio ≤ 92%, and a spherical particle volume fraction ≥ 90%; the silica fume contains a SiO2 mass content ≥ 94% and a specific surface area ≥ 14400 m². 2 / kg, 28d activity index ≥98%.
[0128] The organic conductive elastic aggregate prepared by this invention; the water-reducing agent is a polycarboxylate water-reducing agent with a water reduction rate of more than 30%; the water is ordinary tap water that meets the requirements of the "Standard for Water Used in Concrete" JGJ63.
[0129] The phenyltrichlorosilane is an industrial grade with a purity ≥98.0%; the hexamethyldisiloxane is an industrial grade with a purity ≥99.0%; and the γ-epoxypropoxypropyltrimethoxysilane is a KH-560 type silane coupling agent with an epoxy value ≥0.40 eq / 100 g.
[0130] Example 1
[0131] A UHPC prepared using organic conductive elastic aggregate comprises the following raw materials in parts by weight: 780 parts cement, 150 parts fly ash microspheres, 200 parts silica fume, 150 parts organic conductive elastic aggregate, 850 parts manufactured sand, 195 parts copper-plated steel fiber, 25 parts water-reducing agent, and 200 parts water.
[0132] The method for preparing UHPC using organic conductive elastic aggregate is as follows:
[0133] S1: Synthesis of P3: Raw materials: The molar ratio of phenyltrichlorosilane to deionized water is 1:15, and the volume ratio of dichloromethane to deionized water is 1.5:1. Phenyltrichlorosilane was first slowly added dropwise to an ice-water mixture, and the hydrolysis reaction was carried out at a temperature controlled below 10℃. After hydrolysis, the organic phase was extracted with dichloromethane, then dried with anhydrous magnesium sulfate, filtered to remove the anhydrous magnesium sulfate, and then the extractant was removed by vacuum distillation to obtain phenylsilanetriol. Then, phenylsilanetriol was cyclized in 0.1% toluenesulfonic acid at 140℃ for 4 h, and finally, P3 was collected by vacuum distillation at 180℃.
[0134] S2: Synthesis of E3: Raw materials: The molar ratio of γ-epoxypropoxypropyltrimethoxysilane to deionized water is 1:8, and the volume ratio of methanol to γ-epoxypropoxypropyltrimethoxysilane is 4:1. First, γ-epoxypropoxypropyltrimethoxysilane is added dropwise to the water / methanol mixture, the pH is adjusted to 4 with acetic acid, and a hydrolysis-condensation reaction is carried out under stirring at room temperature. The solvent is removed under reduced pressure to obtain an epoxysilanol mixture. The epoxysilanol mixture is cyclized in a 0.05% KOH solution at 160℃ for 6 h, and then purified by vacuum distillation at 180℃ to obtain E3.
[0135] S3: Synthesis of B2: Raw materials: Hexamethyldisiloxane, n-butyllithium, and trimethylboronic acid ester in a molar ratio of 1:2.2:2. First, hexamethyldisiloxane and n-butyllithium were reacted at -78°C to generate a dilithium salt. Then, trimethylboronic acid ester was slowly added, and the mixture was heated to room temperature for 14 h. Next, hydrolysis was carried out in a saturated ammonium chloride solution, followed by extraction with n-hexane, drying with anhydrous magnesium sulfate, and finally purification by vacuum distillation at 100°C to obtain B2.
[0136] S4: Preparation of organic elastic powder:
[0137] S41: Dehydration treatment: Accurately weigh P3, E3, and V3 into a flask according to a molar ratio of 70:20:10, then add 5% of the total mass of P3, E3, and V3 in B2, connect the vacuum system, and slowly heat to 80℃ at a rate of 1.5℃ / min. Perform dehydration treatment for 2 h at 80℃ and a vacuum degree <0.1 mmHg. Finally, turn off the vacuum and purge with high-purity nitrogen (99.999%) three times.
[0138] S42: Ring-opening copolymerization reaction: The mixture obtained after dehydration is first heated to 65℃ for dissolution, then the reaction temperature is set to 90℃, the condenser is turned on, and 0.05% of tetramethylammonium hydroxide silanoate by total mass of mixed monomers is added to carry out the ring-opening copolymerization reaction. The stirring speed is first set at 500 r / min and mixed for 30 s, then the stirring speed is adjusted to 250 r / min and the reaction time is 8 min. Methanol is added to terminate the reaction, wherein the molar amount of methanol is 3 times that of tetramethylammonium hydroxide silanoate, and then samples are taken for monitoring.
[0139] S43: Dynamic bond formation and end-capping: After the ring-opening copolymerization reaction, the system was naturally cooled to 60°C, and hexamethyldisiloxane was added at 1.5 times the total molar amount of the mixed monomers. Stirring was continued to promote the exchange of borate ester bonds and end-capping. The temperature was then raised to 110°C and maintained for 15 min to decompose the residual catalyst and obtain the crude product.
[0140] S44: Purification and post-treatment: The crude product was dissolved in tetrahydrofuran and prepared into a solution. Under vigorous stirring, a mixture of methanol and water (9:1, v / v) was added dropwise, and a white precipitate gradually formed. Stirring was continued, and the mixture was filtered through a Buchner funnel. The filter cake was washed three times with methanol, dried under vacuum at 80°C for 6 h, and then ground to obtain organic elastomer powder.
[0141] S5: Preparation of organic conductive elastic aggregate core:
[0142] S51: The conductive filler (carbon nanotubes and polyaniline) is surface modified by using 3-aminophenylboronic acid pinacol ester, wherein the mass ratio of 3-aminophenylboronic acid pinacol ester, carbon nanotubes and polyaniline is 4:70:30, to obtain the pretreated conductive filler, so as to improve its compatibility and dispersibility with the organic elastic powder matrix.
[0143] S52: Mix the organic elastomer powder with the pretreated conductive filler at a mass ratio of 100:20, add the mixture to a mixer, heat and melt at 180℃ for 12 min, and mix evenly.
[0144] S53: Place the uniformly mixed mixture into an iron mold, then place the mold into a flat vulcanizing machine and hot press it to form a conductive composite.
[0145] S54: The conductive composite is crushed by a jaw crusher and then screened to finally obtain an organic conductive elastic aggregate core with a particle size of 2.36-4.75 mm.
[0146] S6: Preparation of an organic conductive elastic aggregate shell:
[0147] S61: Surface activation of organic conductive elastic aggregate core: Place the organic conductive elastic aggregate core in the sample tray of the treatment chamber, evacuate to below 10 Pa, introduce oxygen, maintain the gas flow rate at 30 sccm, start the plasma generator, and treat for 120 s at a power of 150 W; The treated organic conductive elastic aggregate core should be stored in a dry inert atmosphere and used for the next slurry coating within 8 hours to prevent the active sites from becoming ineffective.
[0148] S62: Preparation of polymerizable conductive slurry: First, disperse the conductive filler (carbon nanotubes and graphene in a mass ratio of 5:1) in a portion of toluene and treat it with high-power ultrasound for 45 min to form a uniform dispersion; under inert gas protection, add V3, B2 and the remaining toluene to the uniform dispersion, with the mass ratio of conductive filler to V3 being 8%:92% and the amount of B2 being 2.2% of the mass of V3; mix with mechanical stirring at a stirring rate of 300 r / min for 50 min; just before use, add 2.3% of the mass of V3 benzoyl peroxide and stir evenly to avoid premature reaction.
[0149] S63: In a reactor equipped with stirring and temperature control, the activated organic conductive elastic aggregate core is added, and then the prepared polymerizable conductive slurry is slowly added dropwise. The mass ratio of the organic conductive elastic aggregate core to the solids in the polymerizable conductive slurry is 8:1. The mixture is stirred at 200 r / min for 30 min under reduced pressure at 50℃ to remove most of the solvent, so that a viscous prepolymer layer is formed on the surface of the core.
[0150] S64: The temperature is raised to 90℃ and maintained for 2 h to initiate the in-situ free radical copolymerization reaction of vinyl groups on the core surface and in the slurry. Then, it is placed in an oven at 110℃ for post-curing treatment. Finally, hexane is added for purification and vacuum drying at 55℃ to obtain the organic elastic conductive aggregate precursor.
[0151] S65: Surface modification treatment of organic elastic conductive aggregate precursor: The organic elastic conductive aggregate precursor is washed with water, air-dried, and placed in a clean container. A 6% (w / w) NaOH aqueous solution is added until the aggregate surface is just wetted. The container is sealed and soaked for 25 min. The precursor is then rinsed 5 times with water until the pH is neutral. After air-drying, it is transferred to a clean container. A 2% (w / w) titanate coupling agent ethanol solution is added until the aggregate surface is just wetted. The container is sealed and soaked for 30 min. The precursor is then rinsed 5 times with water and air-dried to obtain the finished organic elastic conductive aggregate. The organic elastic conductive aggregate has a particle size of 2.36-4.75 mm, an elongation of 380%, and an apparent density of 1090 kg / m³. 3 Its volume resistivity is 30 Ω / cm.
[0152] S7: Preparation of UHPC:
[0153] S71: Add manufactured sand, cement, silica fume and fly ash microspheres to a concrete mixer and premix for 2 minutes. Then add organic elastic conductive aggregate and mix for 2 minutes. Add water and water-reducing agent and mix for 3 minutes. After the mixture in the mixing pot reaches a viscous state, add copper-plated steel fibers evenly and continue mixing for 2 minutes.
[0154] S72: After the fresh concrete leaves the mixing pot, it is molded, vibrated, and shaped. The surface is covered with a waterproof film and cured under the standard conditions specified in GB / T 50081. After 1 day, the mold is removed and standard curing is carried out. The standard curing and testing age is 28 days, which yields UHPC based on organic elastic conductive aggregate.
[0155] Example 2
[0156] A UHPC prepared using organic conductive elastic aggregate comprises the following raw materials in parts by weight: 700 parts cement, 120 parts fly ash microspheres, 180 parts silica fume, 100 parts organic conductive elastic aggregate, 900 parts manufactured sand, 210 parts copper-plated steel fiber, 25 parts water-reducing agent, and 190 parts water.
[0157] The method for preparing UHPC using organic conductive elastic aggregate is as follows:
[0158] S1: Synthesis of P3: Raw materials: The molar ratio of phenyltrichlorosilane to deionized water is 1:17, and the volume ratio of toluene to deionized water is 1:1. Phenyltrichlorosilane was first slowly added dropwise to an ice-water mixture, and the hydrolysis reaction was carried out at a temperature controlled below 10℃. After hydrolysis, the organic phase was extracted with toluene, then dried with anhydrous magnesium sulfate, filtered to remove the anhydrous magnesium sulfate, and then the extractant was removed by vacuum distillation to obtain phenylsilanetriol. Then, phenylsilanetriol was cyclized in 0.1% toluenesulfonic acid at 130℃ for 5 h, and finally, P3 was collected by vacuum distillation at 185℃.
[0159] S2: Synthesis of E3: Raw materials: The molar ratio of γ-epoxypropoxypropyltrimethoxysilane to deionized water is 1:7, and the volume ratio of methanol to γ-epoxypropoxypropyltrimethoxysilane is 3:1. First, γ-epoxypropoxypropyltrimethoxysilane is added dropwise to a water / isopropanol mixture, the pH is adjusted to 3 with acetic acid, and a hydrolysis-condensation reaction is carried out under stirring at room temperature. The solvent is removed under reduced pressure to obtain an epoxysilanol mixture. The epoxysilanol mixture is cyclized in a 0.04% KOH solution at 165℃ for 5 h, and then purified by vacuum distillation at 185℃ to obtain E3.
[0160] S3: Synthesis of B2: Raw materials: Hexamethyldisiloxane, n-butyllithium, and trimethylboronic acid ester in a molar ratio of 1:2.2:2.1. First, hexamethyldisiloxane and n-butyllithium were reacted at -70°C to generate a dilithium salt. Then, trimethylboronic acid ester was slowly added, and the mixture was heated to room temperature for 16 h. Next, hydrolysis was carried out in a saturated ammonium chloride solution, followed by extraction with n-hexane, drying with anhydrous magnesium sulfate, and finally purification by vacuum distillation at 105°C to obtain B2.
[0161] S4: Preparation of organic elastic powder:
[0162] S41: Dehydration treatment: Accurately weigh P3, E3, and V3 into a flask according to a molar ratio of 60:20:20, then add 4% B2 of the total mass of P3, E3, and V3, connect the vacuum system, and slowly heat to 80℃ at a rate of 1.5℃ / min. Perform dehydration treatment for 2 h at 80℃ and a vacuum degree <0.1 mmHg. Finally, turn off the vacuum and purge with high-purity nitrogen (99.999%) three times.
[0163] S42: Ring-opening copolymerization reaction: The mixture obtained after dehydration is first heated to 60℃ for dissolution, then the reaction temperature is set to 88℃, the condenser is turned on, and 0.07% of tetramethylammonium hydroxide silanoate by total mass of mixed monomers is added to carry out the ring-opening copolymerization reaction. The stirring speed is first set at 450 r / min and mixed for 32 s, then the stirring speed is adjusted to 270 r / min and the reaction time is 8 min. Ethanol is added to terminate the reaction, wherein the molar amount of ethanol is 4 times that of tetramethylammonium hydroxide silanoate, and then samples are taken for monitoring.
[0164] S43: Dynamic bond formation and end-capping: After the ring-opening copolymerization reaction, the system was naturally cooled to 60°C, and trimethylchlorosilane was added in a volume twice the total molar amount of the mixed monomers. Stirring was continued to promote the exchange of borate ester bonds and end-capping. The temperature was then raised to 115°C and maintained for 14 min to decompose the residual catalyst and obtain the crude product.
[0165] S44: Purification and post-treatment: The crude product was dissolved in tetrahydrofuran and prepared into a solution. Under vigorous stirring, a mixture of methanol and water (9:1, v / v) was added dropwise, and a white precipitate gradually formed. Stirring continued, and the mixture was filtered through a Buchner funnel. The filter cake was washed three times with methanol, dried under vacuum at 90°C for 5 h, and then ground to obtain organic elastomer powder.
[0166] S5: Preparation of organic conductive elastic aggregate core:
[0167] S51: Surface modification treatment of conductive fillers (carbon nanotubes and ultrafine copper powder) is carried out using 3-mercaptopropyltrimethoxysilane, wherein the mass ratio of 3-aminophenylboronic acid pinacol ester, carbon nanotubes and ultrafine copper powder is 3:65:35, to obtain pretreated conductive fillers to improve their compatibility and dispersibility with organic elastic powder matrix.
[0168] S52: Mix the organic elastomer powder with the pretreated conductive filler at a mass ratio of 100:25, add the mixture to a mixer, heat and melt at 170℃ for 13 min, and mix evenly.
[0169] S53: Place the uniformly mixed mixture into an iron mold, then place the mold into a flat vulcanizing machine and hot press it to form a conductive composite.
[0170] S54: The conductive composite is crushed by a jaw crusher and then screened to finally obtain an organic conductive elastic aggregate core with a particle size of 2.36-4.75 mm.
[0171] S6: Preparation of an organic conductive elastic aggregate shell:
[0172] S61: Surface activation of organic conductive elastic aggregate core: Place the organic conductive elastic aggregate core in the sample tray of the treatment chamber, evacuate to below 10 Pa, introduce oxygen, maintain the gas flow rate at 40 sccm, start the plasma generator, and treat for 130 s at a power of 150 W; The treated organic conductive elastic aggregate core should be stored in a dry inert atmosphere and used for the next slurry coating within 8 hours to prevent the active sites from becoming ineffective.
[0173] S62: Preparation of polymerizable conductive slurry: First, disperse the conductive filler (carbon nanotubes and polyaniline in a mass ratio of 5:1) in a portion of toluene, and treat it with high-power ultrasound for 45 min to form a uniform dispersion; under inert gas protection, add V3, B2 and the remaining toluene to the uniform dispersion, with the mass ratio of conductive filler to V3 being 7%:91%, and the amount of B2 being 2.1% of the mass of V3; mix with mechanical stirring at a stirring rate of 350 r / min for 45 min; just before use, add 2.2% of the mass of V3 benzoyl peroxide and stir evenly to avoid premature reaction.
[0174] S63: In a reactor equipped with stirring and temperature control, the activated organic conductive elastic aggregate core is added, and then the prepared polymerizable conductive slurry is slowly added dropwise. The mass ratio of the organic conductive elastic aggregate core to the solids in the polymerizable conductive slurry is 7:1. The mixture is stirred at 250 r / min for 25 min under reduced pressure at 55℃ to remove most of the solvent, so that a viscous prepolymer layer is formed on the surface of the core.
[0175] S64: The temperature is raised to 95℃ and maintained for 1.8 h to initiate in-situ free radical copolymerization of vinyl groups on the core surface and in the slurry. Then, it is placed in an oven at 105℃ for post-curing treatment. Finally, hexane is added for purification and vacuum drying at 55℃ to obtain the organic elastic conductive aggregate precursor.
[0176] S65: Surface modification treatment of organic elastic conductive aggregate precursor: The organic elastic conductive aggregate precursor is washed with water, air-dried, and placed in a clean container. A 7% (w / w) NaOH aqueous solution is added until the aggregate surface is just wetted. The container is sealed and soaked for 22 min. The precursor is then rinsed 5 times with water until the pH is neutral. After air-drying, it is transferred to a clean container. A 1.5% (w / w) titanate coupling agent ethanol solution is added until the aggregate surface is just wetted. The container is sealed and soaked for 25 min. The precursor is then rinsed 5 times with water and air-dried to obtain the finished organic elastic conductive aggregate. The organic elastic conductive aggregate has a particle size of 2.36-4.75 mm, an elongation of 340%, and an apparent density of 1070 kg / m³. 3 Its volume resistivity is 85 Ω / cm.
[0177] S7: Preparation of UHPC:
[0178] S71: Add manufactured sand, cement, silica fume and fly ash microspheres to a concrete mixer and premix for 2 minutes. Then add organic elastic conductive aggregate and mix for 2 minutes. Add water and water-reducing agent and mix for 3 minutes. After the mixture in the mixing pot reaches a viscous state, add copper-plated steel fibers evenly and continue mixing for 2 minutes.
[0179] S72: After the fresh concrete leaves the mixing pot, it is molded, vibrated, and shaped. The surface is covered with a waterproof film and cured under the standard conditions specified in GB / T 50081. After 1 day, the mold is removed and standard curing is carried out. The standard curing and testing age is 28 days, which yields UHPC based on organic elastic conductive aggregate.
[0180] Example 3
[0181] A UHPC prepared using organic conductive elastic aggregate comprises the following raw materials in parts by weight: 850 parts cement, 100 parts fly ash microspheres, 50 parts silica fume, 200 parts organic conductive elastic aggregate, 800 parts manufactured sand, 240 parts copper-plated steel fiber, 30 parts water-reducing agent, and 200 parts water.
[0182] The method for preparing UHPC using organic conductive elastic aggregate is as follows:
[0183] S1: Synthesis of P3: Raw materials: The molar ratio of phenyltrichlorosilane to deionized water is 1:18, and the volume ratio of dichloromethane to deionized water is 2:1. Phenyltrichlorosilane was first slowly added dropwise to an ice-water mixture, and the hydrolysis reaction was carried out at a temperature controlled below 10℃. After hydrolysis, the organic phase was extracted with dichloromethane, then dried with anhydrous magnesium sulfate, filtered to remove the anhydrous magnesium sulfate, and then the extractant was removed by vacuum distillation to obtain phenylsilanetriol. Then, phenylsilanetriol was cyclized in 0.1% trifluoromethanesulfonic acid at 145℃ for 3 h, and finally, P3 was collected by vacuum distillation at 190℃.
[0184] S2: Synthesis of E3: Raw materials: The molar ratio of γ-epoxypropoxypropyltrimethoxysilane to deionized water is 1:9, and the volume ratio of ethanol to γ-epoxypropoxypropyltrimethoxysilane is 5:1. First, γ-epoxypropoxypropyltrimethoxysilane is added dropwise to the water / ethanol mixture, the pH is adjusted to 4.5 with trifluoroacetic acid, and a hydrolysis-condensation reaction is carried out under stirring at room temperature. The solvent is removed under reduced pressure to obtain an epoxysilanol mixture. The epoxysilanol mixture is cyclized in a 0.06% KOH solution at 170℃ for 5 h, and then purified by vacuum distillation at 200℃ to collect E3.
[0185] S3: Synthesis of B2: Raw materials: Hexamethyldisiloxane, n-butyllithium, and trimethylboronic acid ester in a molar ratio of 1:2.3:2.1. First, hexamethyldisiloxane and n-butyllithium were reacted at -80℃ to generate a dilithium salt. Then, trimethylboronic acid ester was slowly added, and the mixture was heated to room temperature for 16 h. Next, hydrolysis was carried out in 1.5 mol / L dilute hydrochloric acid solution, followed by extraction with n-hexane solution, drying with anhydrous magnesium sulfate, and finally purification by vacuum distillation at 110℃ to obtain B2.
[0186] S4: Preparation of organic elastic powder:
[0187] S41: Dehydration treatment: Accurately weigh P3, E3, and V3 into a flask according to a molar ratio of 80:20:10, then add 6% of the total mass of P3, E3, and V3 in B2, connect the vacuum system, and slowly heat to 80℃ at a rate of 2℃ / min. Perform dehydration treatment for 1 h at 80℃ and a vacuum degree <0.1 mmHg. Finally, turn off the vacuum and purge with high-purity nitrogen (99.999%) three times.
[0188] S42: Ring-opening copolymerization reaction: The mixture obtained after dehydration is first heated to 70℃ for dissolution, then the reaction temperature is set to 95℃, the condenser is turned on, and 0.1% of the total mass of the mixed monomers in a tetramethylammonium hydroxide aqueous solution is added to carry out the ring-opening copolymerization reaction. The stirring speed is first set at 600 r / min and mixed for 25 s, then the stirring speed is adjusted to 300 r / min and the reaction time is 8 min. Methanol is added to terminate the reaction, wherein the molar amount of methanol is 4 times that of the tetramethylammonium hydroxide aqueous solution, and then samples are taken for monitoring.
[0189] S43: Dynamic bond formation and end-capping: After the ring-opening copolymerization reaction, the system was naturally cooled to 62°C, and hexamethyldisiloxane with a total molar amount of 1 times the total amount of mixed monomers was added. Stirring was continued to promote the exchange of borate ester bonds and end-capping. The temperature was then raised to 120°C and maintained for 13 min to decompose the residual catalyst and obtain the crude product.
[0190] S44: Purification and post-treatment: The crude product was dissolved in tetrahydrofuran and prepared into a solution. Under vigorous stirring, a mixture of methanol and water (8:2, v / v) was added dropwise, and a white precipitate gradually formed. Stirring continued, and the mixture was filtered through a Buchner funnel. The filter cake was washed three times with methanol, dried under vacuum at 100°C for 4 h, and then ground to obtain organic elastomer powder.
[0191] S5: Preparation of organic conductive elastic aggregate core:
[0192] S51: The conductive filler (carbon nanotubes and polyaniline) is surface modified with tridecafluorooctyltriethoxysilane, wherein the mass ratio of 3-aminophenylboronic acid pinacol ester, carbon nanotubes and polyaniline is 4:40:60, to obtain the pretreated conductive filler, so as to improve its compatibility and dispersibility with the organic elastic powder matrix.
[0193] S52: Mix the organic elastomer powder with the pretreated conductive filler at a mass ratio of 100:30, add the mixture to a mixer, heat and melt at 190℃ for 10 min, and mix evenly.
[0194] S53: Place the uniformly mixed mixture into an iron mold, then place the mold into a flat vulcanizing machine and hot press it to form a conductive composite.
[0195] S54: The conductive composite is crushed by a jaw crusher and then screened to finally obtain an organic conductive elastic aggregate core with a particle size of 2.36-4.75 mm.
[0196] S6: Preparation of an organic conductive elastic aggregate shell:
[0197] S61: Surface activation of organic conductive elastic aggregate core: Place the organic conductive elastic aggregate core in the sample tray of the treatment chamber, evacuate to below 10 Pa, introduce oxygen, maintain the gas flow rate at 50 sccm, start the plasma generator, and treat for 60 s at a power of 200 W; The treated organic conductive elastic aggregate core should be stored in a dry inert atmosphere and used for the next slurry coating within 8 hours to prevent the active sites from becoming ineffective.
[0198] S62: Preparation of polymerizable conductive slurry: First, disperse the conductive filler (carbon nanotubes and graphene in a mass ratio of 5:1) in a portion of tetrahydrofuran, and treat it with high-power ultrasound for 60 min to form a uniform dispersion; under inert gas protection, add V3, B2 and the remaining tetrahydrofuran to the uniform dispersion, with the mass ratio of conductive filler to V3 being 10%:93%, and the amount of B2 being 2.3% of the mass of V3; mix with mechanical stirring at a stirring rate of 400 r / min for 30 min; just before use, add 2% of the mass of V3 azobisisobutyronitrile and stir evenly to avoid premature reaction.
[0199] S63: In a reactor equipped with stirring and temperature control, the activated organic conductive elastic aggregate core is added, and then the prepared polymerizable conductive slurry is slowly added dropwise. The mass ratio of the organic conductive elastic aggregate core to the solids in the polymerizable conductive slurry is 10:1. The mixture is stirred at 300 r / min for 20 min under reduced pressure at 60℃ to remove most of the solvent, so that a viscous prepolymer layer is formed on the surface of the core.
[0200] S64: The temperature is raised to 110℃ and maintained for 1 h to initiate the in-situ free radical copolymerization reaction of vinyl groups on the core surface and in the slurry. Then, it is placed in a 120℃ oven for post-curing treatment. Finally, hexane is added for purification and vacuum drying at 60℃ to obtain the organic elastic conductive aggregate precursor.
[0201] S65: Surface modification treatment of organic elastic conductive aggregate precursor: Wash the organic elastic conductive aggregate precursor with water, air dry it naturally, and place it in a clean container. Add an 8% (w / w) NaOH aqueous solution until the aggregate surface is just wetted, seal the container, and soak for 20 min. Rinse five times with clean water until the pH is neutral, air dry it naturally, transfer it to a clean container, add a 2.5% (w / w) titanate coupling agent ethanol solution until the aggregate surface is just wetted, seal the container, and soak for 25 min. Rinse five times with clean water, air dry, and obtain the finished organic elastic conductive aggregate. The organic elastic conductive aggregate has a particle size of 2.36-4.75 mm, an elongation of 300%, and an apparent density of 1120 kg / m³. 3 Its volume resistivity is 110 Ω / cm.
[0202] S7: Preparation of UHPC:
[0203] S71: Add manufactured sand, cement, silica fume and fly ash microspheres to a concrete mixer and premix for 2 minutes. Then add organic elastic conductive aggregate and mix for 2 minutes. Add water and water-reducing agent and mix for 3 minutes. After the mixture in the mixing pot reaches a viscous state, add copper-plated steel fibers evenly and continue mixing for 2 minutes.
[0204] S72: After the fresh concrete leaves the mixing pot, it is molded, vibrated, and shaped. The surface is covered with a waterproof film and cured under the standard conditions specified in GB / T 50081. After 1 day, the mold is removed and standard curing is carried out. The standard curing and testing age is 28 days, which yields UHPC based on organic elastic conductive aggregate.
[0205] Example 4
[0206] A UHPC prepared using organic conductive elastic aggregate comprises the following raw materials in parts by weight: 650 parts cement, 100 parts fly ash microspheres, 250 parts silica fume, 50 parts organic conductive elastic aggregate, 950 parts manufactured sand, 150 parts copper-plated steel fiber, 15 parts water-reducing agent, and 170 parts water.
[0207] The method for preparing UHPC using organic conductive elastic aggregate is as follows:
[0208] S1: Synthesis of P3: Raw materials: The molar ratio of phenyltrichlorosilane to deionized water is 1:13, and the volume ratio of toluene to deionized water is 0.5:1. Phenyltrichlorosilane was first slowly added dropwise to an ice-water mixture, and the hydrolysis reaction was carried out at a temperature <10℃. After hydrolysis, the organic phase was extracted with toluene, then dried with anhydrous magnesium sulfate, filtered to remove the anhydrous magnesium sulfate, and then the extractant was removed by vacuum distillation to obtain phenylsilanetriol. Then, phenylsilanetriol was cyclized in 0.1% trifluoromethanesulfonic acid at 125℃ for 6 h, and finally, P3 was collected by vacuum distillation at 180℃.
[0209] S2: Synthesis of E3: Raw materials: The molar ratio of γ-epoxypropoxypropyltrimethoxysilane to deionized water is 1:5, and the volume ratio of methanol to γ-epoxypropoxypropyltrimethoxysilane is 2:1. First, γ-epoxypropoxypropyltrimethoxysilane is added dropwise to a water / methanol mixture, the pH is adjusted to 3.5 with trifluoroacetic acid, and a hydrolysis-condensation reaction is carried out under stirring at room temperature. The solvent is removed under reduced pressure to obtain an epoxysilanol mixture. The epoxysilanol mixture is cyclized in a 0.03% KOH solution at 150°C for 7 h, and then purified by vacuum distillation at 180°C to obtain E3.
[0210] S3: Synthesis of B2: Raw materials: Hexamethyldisiloxane, n-butyllithium, and trimethylboronic acid ester in a molar ratio of 1:2.1:2. First, hexamethyldisiloxane and n-butyllithium were reacted at -65°C to generate a dilithium salt. Then, trimethylboronic acid ester was slowly added, and the mixture was heated to room temperature for 14 h. Next, hydrolysis was carried out in a saturated ammonium chloride solution, followed by extraction with diethyl ether, drying with anhydrous magnesium sulfate, and finally purification by vacuum distillation at 90°C to obtain B2.
[0211] S4: Preparation of organic elastic powder:
[0212] S41: Dehydration treatment: Accurately weigh P3, E3, and V3 into a flask according to a molar ratio of 50:15:5, then add 3% B2 of the total mass of P3, E3, and V3, connect the vacuum system, and slowly heat to 80℃ at a rate of 2℃ / min. Perform dehydration treatment for 1 h at 80℃ and a vacuum degree <0.1 mmHg. Finally, turn off the vacuum and purge with high-purity nitrogen (99.999%) three times.
[0213] S42: Ring-opening copolymerization reaction: The mixture obtained after dehydration is first heated to 60℃ for dissolution, then the reaction temperature is set to 85℃, the condenser is turned on, and 0.01% of the total mass of the mixed monomers in a tetramethylammonium hydroxide aqueous solution is added to carry out the ring-opening copolymerization reaction. The stirring speed is first set at 400 r / min and mixed for 35 s, then the stirring speed is adjusted to 200 r / min and the reaction time is 8 min. Methanol is added to terminate the reaction, wherein the molar amount of methanol is 4 times that of the tetramethylammonium hydroxide aqueous solution, and then a sample is taken for monitoring.
[0214] S43: Dynamic bond formation and end-capping: After the ring-opening copolymerization reaction, the system was naturally cooled to 58°C, and trimethylchlorosilane was added in a volume twice the total molar amount of the mixed monomers. Stirring was continued to promote the exchange of borate ester bonds and end-capping. The temperature was then raised to 100°C and maintained for 18 min to decompose the residual catalyst and obtain the crude product.
[0215] S44: Purification and post-treatment: The crude product was dissolved in tetrahydrofuran and prepared into a solution. Under vigorous stirring, a mixture of methanol and water (8:2, v / v) was added dropwise, and a white precipitate gradually formed. Stirring was continued, and the mixture was filtered through a Buchner funnel. The filter cake was washed three times with methanol, dried under vacuum at 70°C for 7 h, and then ground to obtain organic elastomer powder.
[0216] S5: Preparation of organic conductive elastic aggregate core:
[0217] S51: The conductive filler (carbon nanotubes and ultrafine copper powder) is surface modified by using 3-aminophenylboronic acid pinacol ester, wherein the mass ratio of 3-aminophenylboronic acid pinacol ester, carbon nanotubes and ultrafine copper powder is 2:40:60, to obtain the pretreated conductive filler, so as to improve its compatibility and dispersibility with the organic elastic powder matrix.
[0218] S52: Mix the organic elastomer powder with the pretreated conductive filler at a mass ratio of 100:10, add the mixture to a mixer, heat and melt at 160℃ for 15 min, and mix evenly.
[0219] S53: Place the uniformly mixed mixture into an iron mold, then place the mold into a flat vulcanizing machine and hot press it to form a conductive composite.
[0220] S54: The conductive composite is crushed by a jaw crusher and then screened to finally obtain an organic conductive elastic aggregate core with a particle size of 2.36-4.75 mm.
[0221] S6: Preparation of an organic conductive elastic aggregate shell:
[0222] S61: Surface activation of organic conductive elastic aggregate core: Place the organic conductive elastic aggregate core in the sample tray of the treatment chamber, evacuate to below 10 Pa, introduce oxygen, maintain the gas flow rate at 20 sccm, start the plasma generator, and treat for 180 s at a power of 100 W; The treated organic conductive elastic aggregate core should be stored in a dry inert atmosphere and used for the next slurry coating within 8 hours to prevent the active sites from becoming ineffective.
[0223] S62: Preparation of polymerizable conductive slurry: First, disperse the conductive filler (carbon nanotubes and polyaniline in a mass ratio of 5:1) in a portion of toluene, and treat it with high-power ultrasound for 45 min to form a uniform dispersion; under inert gas protection, add V3, B2 and the remaining toluene to the uniform dispersion, with the mass ratio of conductive filler to V3 being 5%:90%, and the amount of B2 being 2% of the mass of V3; mix with mechanical stirring at a stirring rate of 250 r / min for 80 min; just before use, add 2.5% of the mass of V3 in azobisisobutyronitrile and stir evenly to avoid premature reaction.
[0224] S63: In a reactor equipped with stirring and temperature control, the activated organic conductive elastic aggregate core is added, and then the prepared polymerizable conductive slurry is slowly added dropwise. The mass ratio of the organic conductive elastic aggregate core to the solids in the polymerizable conductive slurry is 5:1. The mixture is stirred at 100 r / min for 40 min under reduced pressure at 40℃ to remove most of the solvent, so that a viscous prepolymer layer is formed on the surface of the core.
[0225] S64: The temperature is raised to 100℃ and maintained for 2 h to initiate the in-situ free radical copolymerization reaction of vinyl groups on the core surface and in the slurry. Then, it is placed in a 120℃ oven for post-curing treatment. Finally, hexane is added for purification and vacuum drying at 50℃ to obtain the organic elastic conductive aggregate precursor.
[0226] S65: Surface modification treatment of organic elastic conductive aggregate precursor: Wash the organic elastic conductive aggregate precursor with water, air dry it naturally, and place it in a clean container. Add a 5% (w / w) NaOH aqueous solution until the aggregate surface is just wetted, seal the container, and soak for 30 min. Rinse five times with clean water until the pH is neutral, air dry it naturally, transfer it to a clean container, add a 1% (w / w) titanate coupling agent ethanol solution until the aggregate surface is just wetted, seal the container, and soak for 45 min. Rinse five times with clean water, air dry, and obtain the finished organic elastic conductive aggregate. The organic elastic conductive aggregate has a particle size of 2.36-4.75 mm, an elongation of 400%, and an apparent density of 1200 kg / m³. 3 Its volume resistivity is 190 Ω / cm.
[0227] S7: Preparation of UHPC:
[0228] S71: Add manufactured sand, cement, silica fume and fly ash microspheres to a concrete mixer and premix for 2 minutes. Then add organic elastic conductive aggregate and mix for 2 minutes. Add water and water-reducing agent and mix for 3 minutes. After the mixture in the mixing pot reaches a viscous state, add copper-plated steel fibers evenly and continue mixing for 2 minutes.
[0229] S72: After the fresh concrete leaves the mixing pot, it is molded, vibrated, and shaped. The surface is covered with a waterproof film and cured under the standard conditions specified in GB / T 50081. After 1 day, the mold is removed and standard curing is carried out. The standard curing and testing age is 28 days, which yields UHPC based on organic elastic conductive aggregate.
[0230] Comparative Example 1
[0231] This comparative example is basically the same as Example 1, except that an equal amount of manufactured sand is used instead of organic conductive elastic aggregate.
[0232] Comparative Example 2
[0233] This comparative example is basically the same as Example 1, except that an equal amount of rubber particles are used to replace the organic conductive elastic aggregate.
[0234] Comparative Example 3
[0235] This comparative example is basically the same as Example 1, except that in the preparation process of the organic conductive elastic aggregate core, the mass ratio of organic elastomer powder to pretreated conductive filler is 100:40.
[0236] Comparative Example 4
[0237] This comparative example is basically the same as Example 1, except that in the preparation process of the organic conductive elastic aggregate core, an equal amount of rubber is used to replace the organic elastomer powder.
[0238] The UHPCs prepared in Examples 1-4 and Comparative Examples 1-4 were subjected to performance tests, and the results are shown in Table 1.
[0239] Table 1: Performance test results of UHPCs prepared in Examples 1-4 and Comparative Examples 1-4
[0240]
[0241] As can be seen from Table 1, compared with Comparative Examples 1-4, the underwater self-sensing impact-resistant ultra-high performance concrete material obtained by the present invention can reach the strength standard of ultra-high performance concrete (≥120 MPa), and its impact resistance is higher than that of traditional ultra-high performance concrete. Its volume resistivity is also significantly lower than that of traditional ultra-high performance concrete, laying the foundation for generating stable and sensitive resistance change signals under load or impact. Comparative Example 1 shows a decrease in impact resistance and a significant increase in volume resistivity compared to Example 1. This is because the manufactured sand aggregate in traditional ultra-high performance concrete lacks elasticity and cannot dissipate energy through deformation under impact loads, easily leading to stress concentration and brittle spalling, thus reducing impact resistance. The significant increase in resistivity is due to the increased amount of manufactured sand acting as an insulator, which completely destroys the three-dimensional conductive pathway constructed by conductive aggregate and steel fibers in Example 1, resulting in an increase in the volume resistivity of the concrete. Compared to Example 1, Comparative Example 2 showed a significant decrease in compressive strength and a significant increase in volume resistivity. This is because the rubber particles, acting as insulators, have poor adhesion to the cement paste, forming a noticeable weak interface in the concrete. Under impact, the particles are easily pulled out, leading to varying degrees of decrease in compressive and impact resistance, and an increase in resistivity. Comparative Example 3 showed a significant decrease in both impact resistance and compressive strength compared to Example 1, while maintaining a similar volume resistivity. This is because the excessive amount of conductive filler in the organic conductive elastic aggregate caused the aggregate to lose its high elasticity and fail to effectively dissipate impact energy. Once the amount of conductive filler reached the percolation threshold, the increase in conductivity with further filler addition became very limited. Comparative Example 4 showed a higher resistivity than Example 1. This is because the rubber has poor compatibility with the high specific surface area and highly polar carbon-based fillers CNTs and polyaniline, resulting in severe interfacial energy mismatch. This causes the fillers to easily agglomerate in the rubber, making it difficult to disperse them into a uniform percolation network. The volume resistivity of Comparative Examples 1, 2, and 4 is significantly higher than that of Example 1. This is mainly because the internal conductive network of traditional ultra-high performance concrete (UHPC) is incomplete. The internal manufactured sand and rubber particles are insulators, hindering the effective bonding of internal steel fibers. This results in a lack of channels for electron migration in the UHPC system, making it difficult to form an effective conductive pathway. In contrast, the organic conductive elastic aggregate added in Example 1 uses a highly efficient composite conductive filler system of carbon nanotubes and polyaniline. Carbon nanotubes, with their ultra-high aspect ratio, construct an electron transport framework with a low permeation threshold, while polyaniline provides a supplementary ion-electron hybrid conduction mechanism. The synergistic effect of these two components significantly improves the intrinsic conductivity of the aggregate itself. The dense polymer shell on the aggregate surface, rich in conductive filler, optimizes the interfacial contact between adjacent aggregates and between the aggregate and steel fibers, effectively reducing contact resistance. Its addition completes the conductive network within the cement-based material, forming an effective conductive pathway, thereby leading to a significant decrease in volume resistivity.
[0242] In summary, this invention first prepares an organic conductive elastic aggregate with a core-shell structure, and then prepares underwater self-sensing impact-resistant ultra-high performance concrete. The organic conductive elastic aggregate uses an organosilicon elastomer containing dynamic borate ester bonds as its core, and further ensures the stability of the conductive pathway and the interfacial adhesion between the aggregate and cement matrix through an internal and external composite conductive network design and surface modification. The self-sensing impact-resistant ultra-high performance concrete prepared based on the organic conductive elastic aggregate of this invention not only possesses significantly enhanced impact and abrasion resistance, but also exhibits resistive response characteristics that are sensitive to mechanical loads and less affected by environmental interference, showing broad application prospects.
[0243] The above detailed embodiments describe the implementation of the present invention; however, the present invention is not limited to the specific details described in the above embodiments. Within the scope of the claims and technical concept of the present invention, various simple modifications and changes can be made to the technical solution of the present invention, and these simple modifications all fall within the protection scope of the present invention.
Claims
1. A method for preparing an organic conductive elastic aggregate, characterized in that, Includes the following steps: S1. Mix the organic elastomer powder with the pretreated conductive filler I, heat and melt, hot press and mold, crush and screen to obtain the organic conductive elastic aggregate core. The organic elastomer powder is prepared by the following method: a mixture of cyclotrisiloxane monomers and bis(dimethylborate)hexamethyldisiloxane is mixed and dehydrated; a catalyst is added, and a ring-opening copolymerization reaction is carried out at 85-95℃; after terminating the reaction with a terminator, the temperature is lowered to 58-62℃, and an end-capping agent is added to promote borate bond exchange and end-group capping; the temperature is then raised to 100-120℃ to decompose the residual catalyst and obtain a crude product; the crude product is purified, dried, and ground to obtain the organic elastomer powder. S2. After treating the organic conductive elastic aggregate core with oxygen plasma, it is mixed with polymerizable conductive slurry and subjected to in-situ polymerization reaction. After post-curing, purification and drying, an outer shell is formed to obtain the organic conductive elastic aggregate precursor. The polymerizable conductive slurry is prepared by the following method: first, the conductive filler II is dispersed in a solvent to form a uniform dispersion; then, cyclotrisiloxane monomers and bis(dimethylborate)hexamethyldisiloxane are added to the uniform dispersion and mixed evenly; just before use, an initiator is added and mixed evenly to obtain the polymerizable conductive slurry. S3. After soaking the organic conductive elastic aggregate precursor in an alkaline solution, it is cleaned and dried, and then immersed in a titanate coupling agent solution, cleaned, and dried to obtain an organic conductive elastic aggregate with a core-shell structure.
2. The method for preparing an organic conductive elastic aggregate according to claim 1, characterized in that, In step S1, the cyclotrisiloxane mixed monomers include phenyltrimethylcyclotrisiloxane, γ-epoxypropoxypropyltrimethylcyclotrisiloxane and methylvinylcyclotrisiloxane in a molar ratio of (50-80):(10-30):(5-20).
3. The method for preparing an organic conductive elastic aggregate according to claim 1, characterized in that, In step S1, the mass ratio of the organic elastomer powder to the pretreated conductive filler I is 100:(10-40).
4. The method for preparing an organic conductive elastic aggregate according to claim 3, characterized in that, In step S1, the pretreatment operation of the conductive filler I is as follows: the conductive filler I is surface modified with a modifier to obtain the pretreated conductive filler I; the modifier includes at least one of 3-aminophenylboronic acid pinacol ester, tridecafluorooctyltriethoxysilane, and 3-mercaptopropyltrimethoxysilane.
5. The method for preparing an organic conductive elastic aggregate according to claim 1, characterized in that, In step S2, the mass ratio of the organic conductive elastic aggregate core to the solids in the polymerizable conductive slurry is (5-10):
1.
6. The method for preparing an organic conductive elastic aggregate according to claim 1, characterized in that, In step S2, the cyclotrisiloxane monomer includes at least one of methylvinylcyclotrisiloxane and γ-epoxypropoxypropyltrimethylcyclotrisiloxane.
7. The organic elastic conductive aggregate prepared by the preparation method according to any one of claims 1-6, characterized in that, The organic conductive elastic aggregate has a particle size of 2.36-4.75 mm, an elongation of 300%-400%, and an apparent density of 1020-1200 kg / m³. 3 Volume resistivity ≤200 Ω / cm.
8. The application of the organic elastic conductive aggregate of claim 7 in the preparation of self-sensing concrete.
9. An underwater self-sensing, impact-resistant, ultra-high performance concrete, characterized in that, The raw materials include the following parts by weight: 650-850 parts cement, 100-250 parts fly ash microspheres, 50-250 parts silica fume, 50-200 parts organic conductive elastic aggregate as described in claim 7, 800-950 parts manufactured sand, 150-240 parts copper-plated steel fiber, 15-30 parts water-reducing agent, and 170-200 parts water.
10. The method for preparing self-sensing impact-resistant ultra-high performance concrete according to claim 9, characterized in that, Includes the following steps: P1: Add manufactured sand, cement, silica fume and fly ash microspheres to a concrete mixer and premix for 1-3 minutes. Then add organic elastic conductive aggregate and mix for 1-3 minutes. Add water and water-reducing agent and continue mixing for 2-4 minutes. After the mixture in the mixer reaches a viscous state, add copper-plated steel fibers evenly and continue mixing for 1-3 minutes. P2: The mixed material is then molded, vibrated, shaped, and cured to obtain self-sensing impact-resistant ultra-high performance concrete.