Preparation method and application of a composite improvement material for strongly weathered rock slopes

By regulating microbial agents and functional additives in stages, and combining compost products with water-retaining components and biomass loosening agents, the nutrient and structural problems of strongly weathered rock slopes were solved, achieving dynamic balance of the substrate and promoting vegetation growth and stable recovery.

CN123106296APending Publication Date: 2026-11-17KUNMING UNIV OF SCI & TECH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202611315816.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-27
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Strongly weathered rock slopes are difficult to restore vegetation due to their lack of nutrients and humus, dense structure, and weak water and fertilizer retention capacity. Existing technologies are unable to achieve a dynamic balance between nutrient supply, water regulation, and structural optimization, resulting in unstable restoration effects.

Method used

By synergistically regulating microbial agents and functional additives during the composting process, and combining compost products with water-retaining components and biomass loosening agents, a microporous water-storage structure and a loose skeleton are formed, thereby improving the substrate's nutrient availability, water retention capacity, and pore structure.

Benefits of technology

It significantly improves the ecological restoration effect of strongly weathered rock slopes, increases soil organic matter and available potassium content, increases matrix saturated water holding capacity and total porosity, promotes plant germination and root development, and improves vegetation coverage and long-term stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123106296A_ABST
    Figure CN123106296A_ABST
Patent Text Reader

Abstract

This invention discloses a method for preparing and applying a composite improvement material for strongly weathered rock slopes, belonging to the interdisciplinary technical field of ecological restoration in geotechnical engineering and resource utilization of solid waste. The method utilizes sludge, livestock manure, and agricultural and forestry waste such as coffee grounds for co-composting. During the primary fermentation stage, a high-temperature composting agent is inoculated, and ferrous salts are added at a ratio of 0.2%–0.5% of the total mass of the compost. The ferrous salts consist of ferrous sulfate and ferrous gluconate, with ferrous gluconate accounting for 5%–15% of the mass. During the secondary fermentation stage, solid waste from the phosphate coal industry and a conditioning and promoting agent are added. The resulting compost product is then combined with water-retaining components and a biomass loosening agent. These three components synergistically form a composite improvement material with functions of nutrient supply, water regulation, and structural optimization. When mixed into the soil of strongly weathered rock slopes, it can simultaneously improve nutrient availability, water retention capacity, and pore structure, promoting plant germination and root development. This invention achieves resource utilization of organic solid waste at a low cost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the interdisciplinary technical field of geotechnical engineering ecological restoration and solid waste resource utilization, specifically involving a preparation method and application of a composite improvement material for strongly weathered rock slopes. Background Technology

[0002] Strongly weathered rock slopes are a common type of slope in engineering activities such as highway construction and mining. Their surface rock mass is subjected to long-term natural factors such as rainfall leaching, alternating wet and dry periods, and temperature changes, resulting in a high degree of weathering and a loose structure. This typically manifests as a shallow or even completely absent soil layer, extremely low organic matter and nutrient content, high acidity, and poor water and fertilizer retention capacity. These slopes present extremely harsh site conditions, with severe water and fertilizer deficiencies and soil erosion, making vegetation restoration extremely difficult under multiple stresses. The core challenge in the ecological restoration of strongly weathered rock slopes lies in the severe lack of soil matrix and nutrients necessary for plant growth. Furthermore, the soil layer formed after rock weathering has a dense structure, poor aeration, rapid water infiltration but weak water retention capacity, and is often acidic. Plant roots struggle to extend and absorb nutrients normally in a matrix lacking a suitable water-air-heat environment. Additionally, the soil formation process under natural conditions is extremely slow, making it difficult to create a suitable environment for plant establishment and growth in the short term. If only nutrients or water are supplemented through a single approach, without ignoring the synergistic regulation of matrix structure and hydrothermal conditions, it is often difficult to achieve the expected repair effect.

[0003] For the ecological restoration of rock slopes, existing technologies mainly focus on engineering measures such as topsoil spraying, planting bags, and vegetation concrete, as well as the compounding of substrate materials. Patent CN101485282 describes the preparation of a greening substrate for rock slopes by mixing and fermenting straw, cow manure, edible mushroom residue, sludge, and organic fiber, and then compounding it with compound fertilizer, water-retaining agent, binder, attapulgite powder, and pH adjuster. Patent CN101116414A describes the preparation of a slope cultivation substrate using organic materials, peat, raw soil, rice husks, water-retaining agent, binder, and fertilizer, using slow-release nitrogen fertilizer combined with phosphorus and potassium fertilizers to supply nutrients. Patent CN120136635A discloses a method for treating acidic waste rock dump slopes. This method involves mixing residual sludge, cow dung, agricultural and forestry solid waste, and hydrothermal charcoal, adding silicate minerals and sulfur-containing minerals / waste rock, and then inoculating with a compound bacterial agent of *Bacillus mucilaginosus* and *Thiobacillus thiooxidans* for composting. This approach primarily targets the source control of acid production from the oxidation of sulfur-containing minerals and the solidification of heavy metals. It requires the addition of hydrothermal charcoal from kitchen waste and the introduction of acidophilic functional bacteria, necessitating high-level pretreatment of raw materials. For strongly weathered rock slopes, the core issue lies in the combined effect of multiple limiting factors, such as nutrient and humus scarcity, dense structure, and weak water and fertilizer retention capacity, rather than simple acidification. Overall, while the above technical solutions can achieve solid waste resource utilization, they mostly remain at the level of physical mixing of organic matter and functional materials, lacking systematic and coordinated control over the multiple limiting factors of strongly weathered rock slopes. Compost products have limited water retention and are prone to compaction. Simply adding water-retaining agents and fiber materials makes it difficult to achieve a dynamic balance between nutrient release, water regulation, and structural optimization, resulting in unstable restoration effects and difficulty in long-term vegetation survival.

[0004] To address the shortcomings of the existing technologies, this invention provides a method for preparing and applying a composite improvement material for strongly weathered rock slopes. By implementing phased and targeted regulation of microbial agents and functional additives during composting, and by combining compost products with water-retaining components and biomass loosening agents, the method achieves synergistic effects in nutrient supply, moisture regulation, and structural optimization, providing an effective technical solution for the ecological restoration of strongly weathered rock slopes. Summary of the Invention

[0005] This invention provides a method for preparing and applying a composite improvement material for strongly weathered rock slopes. The method uses sludge, livestock manure, and agricultural and forestry waste such as coffee grounds, camellia fruit shells, tobacco straw, and soybean straw as raw materials for co-composting. During the primary fermentation stage, ferrous salts are added and a high-temperature composting agent is inoculated to accelerate organic matter degradation and nutrient release, and to regulate the pH environment of the compost pile. During the post-fermentation stage, solid waste from the phosphorus coal industry and an adjusting and promoting agent are added to promote humus formation and the slow release of mineral elements. The resulting compost product is then combined with water-retaining components and a biomass loosening agent. The water-retaining components form a microporous water-storing structure in the matrix, while the fibrous materials in the biomass loosening agent form a loose skeleton. These three components complement each other, simultaneously improving the matrix's nutrient availability, water retention capacity, and pore structure. This invention provides a composite improvement material for the ecological restoration of strongly weathered rock slopes, combining nutrient supply, water regulation, and structural optimization functions.

[0006] The preparation method of the composite improvement material for strongly weathered rock slopes of the present invention specifically includes the following steps:

[0007] (1) Mix sludge, livestock manure with one or two of coffee grounds, camellia fruit shells, tobacco straw, and soybean straw for co-composting;

[0008] (2) During the main fermentation stage, ferrous salts are added to the compost pile and aerobic fermentation is carried out by inoculating with high-temperature composting bacteria.

[0009] (3) After the main fermentation is completed, the secondary fermentation stage is started, and phosphorus coal industrial solid waste and conditioning and accelerators are added to the pile for secondary fermentation.

[0010] (4) After the post-fermentation is completed, the obtained compost product is mixed with water-retaining components and biomass loosening agent in proportion to obtain the composite improvement material for strongly weathered rock slope.

[0011] Preferably, the mass ratio of sludge to livestock manure in step (1) is 1:(0.7~1), and the livestock manure is a mixture of chicken manure and cow manure, wherein the mass of chicken manure accounts for 5%~30% of the mixture of chicken manure and cow manure; one or two of the coffee grounds, camellia fruit shells, tobacco straw, and soybean straw are added, and the amount of any one of the agricultural and forestry solid wastes added is 0.2%~1.5% of the wet weight of the sludge and manure mixture.

[0012] Preferably, the amount of ferrous salt added in step (2) is 0.2% to 0.5% of the total mass of the compost raw materials. The ferrous salt is composed of ferrous sulfate and ferrous gluconate, wherein the mass percentage of ferrous gluconate is 5% to 15% of the ferrous salt.

[0013] Preferably, the composting thermophilic agent in step (2) is composed of Bacillus licheniformis, Bacillus subtilis, Bacillus amyloliquefaciens, Aspergillus niger, Trichoderma harzianum, and Streptomyces sp., and the amount of the composting thermophilic agent added is 0.1‰ to 0.3‰ of the total mass of the compost mixture.

[0014] Preferably, the solid waste from the phosphorus coal industry mentioned in step (3) is composed of any one of phosphorus tailings and phosphogypsum, and any one of coal gangue and fly ash. When phosphorus tailings are used, the amount added is 1.2% to 2.0% of the total mass of the stockpile mixture; when phosphogypsum is used, the amount added is 0.3% to 0.5% of the total mass of the stockpile mixture; when coal gangue is used, the amount added is 1.6% to 3.0% of the total mass of the stockpile mixture; and when fly ash is used, the amount added is 0.8% to 1.5% of the total mass of the stockpile mixture.

[0015] Preferably, the adjusting and promoting agent added to the compost pile in step (3) is magnesium salt and composting agent. The magnesium salt is magnesium sulfate and magnesium oxide, and the mass ratio of the two is (2-4):1. The amount of magnesium salt added is 0.6‰ to 1.2‰ of the total mass of the main fermentation compost products.

[0016] Preferably, the composting agent is composed of Mucor sp., Pseudomonas sp., Bacillus mucilaginosus, Trichoderma viride, and Phanerochaete chrysosporium, and its inoculum amount is 0.1‰ to 0.3‰ of the total mass of the main fermentation compost products.

[0017] Preferably, the water-retaining component in step (4) is composed of polyurethane foam and sodium acrylate, wherein sodium acrylate accounts for 12% to 25% of the mass of the water-retaining component, and the amount of the water-retaining component added is 0.2% to 0.5% of the mass of the post-fermentation compost product; the biomass loosening agent is a mixture of sugarcane bagasse and corn stalks, the mass ratio of sugarcane bagasse to corn stalks is (1 to 3): 1, and the amount of the biomass loosening agent added is 0.5% to 1.0% of the mass of the post-fermentation compost product.

[0018] An application of a composite improvement material for strongly weathered rock slopes, wherein the application involves mixing the composite improvement material into the soil of strongly weathered rock slopes, and the mass ratio of the composite improvement material to the soil is 5% to 12%.

[0019] Compared with the prior art, the present invention has the following beneficial effects:

[0020] (1) Using sludge, livestock manure, and agricultural and forestry waste such as coffee grounds, camellia fruit shells, tobacco straw, and soybean straw as raw materials, multi-source organic solid waste is utilized through co-composting. The raw materials are widely available and inexpensive. The multi-source organic materials complement each other in terms of carbon and nitrogen. Ferrous salts prolong the high-temperature period to promote degradation and humification. The composting agent and magnesium salts synergistically enhance the formation of humus. The humic acid content of the compost products is significantly increased, and the water and fertilizer retention capacity is also improved, effectively improving the barren substrate.

[0021] (2) Ferrous salts are added and composting high-temperature bacteria are inoculated during the main fermentation stage. Phosphate coal industrial solid waste and adjustment promoters are added during the post-fermentation stage. Through phased bio-chemical synergistic targeted regulation, the degree of humification and nutrient availability of compost products are effectively improved, while also having the function of slow-release mineral nutrients.

[0022] (3) The present invention combines compost products with water-retaining components and biomass loosening agents. The three complement each other. The water-retaining components make up for the poor water retention of compost products, and the loosening agents improve the defects of easy compaction. They synergistically enhance the effectiveness of substrate nutrients, water retention capacity and pore structure, promote plant germination and root development, and improve the ecological restoration effect and long-term stability of slopes. Attached Figure Description

[0023] Figure 1 A comparison of plant growth in a field experiment on a strongly weathered rock slope, where a represents the dry season and b represents the rainy season. Detailed Implementation

[0024] The following embodiments are used to further illustrate the present invention, but the scope of protection of the present invention is not limited to the following embodiments.

[0025] Example 1

[0026] Sludge and livestock manure (both pretreated to a moisture content of 67.2%) were mixed at a mass ratio of 1:0.8. The livestock manure was a mixture of chicken and cow manure, with chicken manure accounting for 8% of the mass. Coffee grounds were used as an auxiliary material, with an addition amount of 1.0% of the wet weight of the sludge and manure mixture. Ferrous salts were added to the compost pile and inoculated with a composting thermophilic microbial agent composed of Bacillus licheniformis, Bacillus subtilis, Bacillus amyloliquefaciens, Aspergillus niger, Trichoderma harzianum, and Streptomyces. The addition amounts of the two components were 0.3% and 0.2‰ of the total mass of the composting raw materials, respectively. The ferrous salts consisted of ferrous sulfate and ferrous gluconate, with ferrous gluconate accounting for 8% of the mass. The primary fermentation was carried out at high temperature for 16 days, and then the process entered the post-fermentation stage. Phosphorus tailings and fly ash from the phosphorus coal industry were added to the compost, along with magnesium salts as an adjustment and accelerator and a composting agent. The dosages of the four components were 1.5%, 1.0%, 0.6‰, and 0.2‰ of the mass of the primary fermentation compost product, respectively. Among them, the magnesium salt consisted of magnesium sulfate and magnesium oxide in a mass ratio of 3:1. The composting agent was composed of Mucor, Pseudomonas, Bacillus mucilaginosus, Trichoderma viride, and Protochaete chrysosporium. After 20 days of post-fermentation, the moisture content of the resulting compost product was adjusted to nearly 45%. It was then mixed and compounded with water-retaining components and biomass loosening agents in a certain proportion to obtain a composite improvement material for strongly weathered rock slopes. The water-retaining component consists of polyurethane foam and sodium acrylate, with sodium acrylate accounting for 20% of the mass of the water-retaining component. The amount of water-retaining component added is 0.4% of the mass of the compost product. The biomass loosening agent is made by mixing sugarcane bagasse with corn stalks with a length of 0.6~1.0 cm in a mass ratio of 2:1. The amount added is 0.8% of the mass of the post-fermented compost product.

[0027] The effects of the obtained composite amendment were verified by a pot experiment: using the original soil of a strongly weathered rocky slope as the control (CK), a treatment group was set up with the composite amendment added (mixed at 8% of the soil mass). Both groups were planted with edamame under the same conditions and cultivated for 50 days. Compared with the control group, the soil organic matter and available potassium content in the treatment group increased by 73.2% and 46.7%, respectively; the saturated water holding capacity of the substrate increased by 25.6%; and the total porosity increased to 38.4% (compared to 28.7% in the control group). The germination rate of edamame was 66.7% (compared to 34.2% in the control group); the plant height after 50 days was 8.6 cm (compared to 6.3 cm in the control group); and the fresh weight of the aboveground parts was 0.32 g / plant (compared to 0.14 g / plant in the control group).

[0028] Example 2

[0029] Sludge and livestock manure were mixed at a mass ratio of 1:1. The livestock manure was a mixture of chicken and cow manure, with chicken manure accounting for 20% of the mass. Camellia oleifera fruit shells and tobacco straw were used as auxiliary materials (each accounting for 50%), with a total addition amount of 0.8% of the wet weight of the sludge and manure mixture. Ferrous salts were added to the composting material and a high-temperature composting agent was inoculated, with dosages of 0.5% and 0.3‰ of the total mass of the composting mixture, respectively. After thorough mixing, high-temperature aerobic fermentation was carried out. After 16 days of composting fermentation, phosphogypsum, coal gangue, magnesium salts, and composting agents were added to the composting material for secondary fermentation. The addition amounts of the four components were 0.4%, 2.0%, 0.8‰, and 0.3‰ of the mass of the primary fermentation compost product, respectively. The magnesium salts were composed of magnesium sulfate and magnesium oxide in a mass ratio of 4:1. After post-fermentation, the compost product is compounded with a water-retaining component and a biomass loosening agent. Sodium acrylate accounts for 15% of the mass of the water-retaining component, and the amount added is 0.3% of the mass of the post-fermented compost product. The biomass loosening agent is a mixture of sugarcane bagasse and corn stalks in a 1:1 mass ratio, and the amount added is 0.5% of the mass of the post-fermented compost product. All other unmentioned operating steps and process parameters are the same as in Example 1.

[0030] Using native soil from a strongly weathered rocky slope as the control (CK), a treatment group was established with composite amendment material added (mixed at 10% of soil mass). Both groups were planted with edamame under the same conditions and cultured in pots for 50 days. Compared to the control group, the soil organic matter and available potassium content in the treatment group increased by 79.1% and 49.3%, respectively; the saturated water holding capacity of the substrate increased by 28.4%; and the total porosity increased to 44.1% (compared to 29.3% in the control group). The germination rate of edamame was 68.3% (compared to 35.3% in the control group); the plant height at 50 days was 8.2 cm (compared to 5.7 cm in the control group); and the aboveground fresh weight was 0.30 g / plant (compared to 0.13 g / plant in the control group).

[0031] Example 3

[0032] Sludge and livestock manure were mixed at a mass ratio of 1:0.7. Soybean straw was added as an auxiliary material at a rate of 1.3% of the wet weight of the sludge and manure mixture. Ferrous salts were then added, and a high-temperature composting agent was inoculated. After thorough mixing, the mixture was subjected to high-temperature aerobic fermentation for 15 days. In the post-fermentation stage, phosphorus tailings, coal gangue, magnesium salts, and composting agents were added for secondary post-fermentation. The dosages of the four components were 1.2%, 1.8%, 0.7‰, and 0.15‰ of the mass of the main fermentation compost product, respectively. The magnesium salts consisted of magnesium sulfate and magnesium oxide in a mass ratio of 2:1. After post-fermentation, the moisture content of the compost product was adjusted to approximately 45%, and then compounded with a water-retaining component and a biomass loosening agent. Sodium acrylate comprised 25% of the water-retaining component by mass, and the amount added was 0.5% of the post-fermented compost product's mass. The biomass loosening agent was a mixture of sugarcane bagasse and corn stalks at a mass ratio of 1.5:1, and the amount added was 0.7% of the post-fermented compost product's mass. Other unmentioned operating steps and process parameters were the same as in Example 1.

[0033] A field experiment was conducted on a strongly weathered rock slope along a highway in a subtropical region. A control group (without composite amendments) and a treatment group (with composite amendments added at 8% of soil mass) were established. A mixture of seeds of *Sophora japonica*, *Bermudagrass*, and *Lysimachia foenum-graecum* was sown in holes. Compared to the control group, the treatment group showed increases in soil organic matter and available potassium content of 75.1% and 46.5%, respectively, a 27.3% increase in saturated water holding capacity of the substrate, and a total porosity of 41.7% (compared to 28.9% in the control group). After sowing during the dry season, there were two sporadic light rains over a period of 100 consecutive days. In the control group, the germination rate of *Bermudagrass* was 28% (based on the number of seeds per hole), while *Sophora japonica* did not germinate. In the treatment group, the germination rate of *Bermudagrass* was 48%, while *Sophora japonica* did not germinate. When the crop was sown in holes for 170 days, the frequency of rainfall in the experimental area increased. In the control group, the germination rate of Bermuda grass increased to 80%, the germination rate of Eriocaulon buergerianum was 6%, and the vegetation coverage was about 65-70%. In the treatment group, the germination rate of Bermuda grass reached 94%, the germination rate of Eriocaulon buergerianum was 14%, and the vegetation coverage was about 80-85%. Figure 1 ).

Claims

1. A method for preparing a composite improvement material for strongly weathered rock slopes, characterized in that, Includes the following steps: (1) Use sludge, livestock manure, coffee grounds, camellia fruit shells, tobacco straw, and soybean straw as raw materials for co-composting; (2) During the main fermentation stage, ferrous salts are added to the compost pile and fermentation is carried out by inoculating with high-temperature composting bacteria. (3) In the post-fermentation stage, phosphorus coal industrial solid waste and conditioning and accelerators are added to the pile for secondary fermentation; (4) The obtained compost product is combined with water-retaining components and biomass loosening agent to obtain the composite improvement material for strongly weathered rock slope.

2. The preparation method according to claim 1, characterized in that, The mass ratio of sludge to livestock manure in step (1) is 1:(0.7~1), and the livestock manure is a mixture of chicken manure and cow manure, wherein the mass of chicken manure accounts for 5%~30% of the mixture of chicken manure and cow manure; one or two of the coffee grounds, camellia fruit shells, tobacco straw, and soybean straw are added, and the amount of any one of the agricultural and forestry solid wastes added is 0.2%~1.5% of the wet weight of the sludge and livestock manure compost mixture.

3. The preparation method according to claim 1, characterized in that, The amount of ferrous salt added in step (2) is 0.2% to 0.5% of the total mass of compost raw materials. The ferrous salt is composed of ferrous sulfate and ferrous gluconate, wherein the mass percentage of ferrous gluconate is 5% to 15% of the ferrous salt.

4. The preparation method according to claim 1, characterized in that, The composting thermophilic agent mentioned in step (2) is composed of Bacillus licheniformis, Bacillus subtilis, Bacillus amyloliquefaciens, Aspergillus niger, Trichoderma harzianum and Streptomyces sp. The amount of the composting thermophilic agent added is 0.1‰ to 0.3‰ of the total mass of the compost mixture.

5. The preparation method according to claim 1, characterized in that, The solid waste from the phosphorus coal industry mentioned in step (3) is composed of any one of phosphorus tailings and phosphogypsum, and any one of coal gangue and fly ash. When phosphorus tailings are used, the amount added is 1.2% to 2.0% of the total mass of the stockpile mixture; when phosphogypsum is used, the amount added is 0.3% to 0.5% of the total mass of the stockpile mixture; when coal gangue is used, the amount added is 1.6% to 3.0% of the total mass of the stockpile mixture; and when fly ash is used, the amount added is 0.8% to 1.5% of the total mass of the stockpile mixture.

6. The preparation method according to claim 1, characterized in that, The adjustment and promotion agent added to the compost pile in step (3) is magnesium salt and composting agent. The magnesium salt is magnesium sulfate and magnesium oxide, and the mass ratio of the two is (2-4):

1. The amount of magnesium salt added is 0.6‰ to 1.2‰ of the total mass of the main fermentation compost products.

7. The preparation method according to claim 6, characterized in that, The composting agent is composed of Mucor sp., Pseudomonas sp., Bacillus mucilaginosus, Trichoderma viride, and Phanerochaete chrysosporium, and its inoculum amount is 0.1‰ to 0.3‰ of the total mass of the main fermentation compost products.

8. The preparation method according to claim 1, characterized in that, The water-retaining component in step (4) is composed of polyurethane foam and sodium acrylate, wherein sodium acrylate accounts for 12% to 25% of the mass of the water-retaining component, and the amount of water-retaining component added is 0.2% to 0.5% of the mass of the post-fermentation compost product.

9. The preparation method according to claim 1, characterized in that, The biomass loosening agent mentioned in step (4) is made by mixing sugarcane bagasse and corn stalks. The mass ratio of sugarcane bagasse to corn stalks is (1~3):

1. The amount of biomass loosening agent added is 0.5% to 1.0% of the mass of the post-fermentation compost product.

10. The application of the composite improvement material for strongly weathered rock slopes prepared by the method according to any one of claims 1 to 9, characterized in that, The composite modified material is mixed into the soil of a strongly weathered rock slope, and the mass ratio of the composite modified material to the soil is 5% to 12%.

Citation Information

Patent Citations

  • Rock slope zoology green-recovery planting stroma

    CN101116414A