A method for preparing organic-inorganic hybrid terbium-based halides, its products and applications

Organic-inorganic hybrid terbium-based halide single crystals were prepared by seed crystal-induced directional evaporation growth process, which solved the problems of high preparation cost, toxicity risk and single crystal size limitation of deep ultraviolet photoelectric detection materials, and realized high-sensitivity non-destructive testing of multiple physical evidences and bio-anti-counterfeiting identification.

CN123106433APending Publication Date: 2026-11-17CHONGQING UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611378474.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-07
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing deep ultraviolet photoelectric detection materials suffer from high preparation costs, lead-based halides pose a risk of biotoxicity, terbium-based halides are difficult to stably prepare centimeter-scale high-quality single crystals, and detectors have limited functionality. Furthermore, they lack the ability to perform combined non-destructive testing of complex biological evidence.

Method used

An organic-inorganic hybrid terbium-based halide single crystal was prepared by dissolving organic ammonium salts and terbium salts in a volatile organic solvent, statically evaporating and crystallizing them, and epitaxially growing them layer by layer on the seed crystal surface. This was used to construct a metal-semiconductor-metal type photodetector, which was then used to detect biological evidence by combining the difference in characteristic absorption spectra in the 235 nm and 285 nm wavelength bands.

Benefits of technology

We have successfully prepared high-quality MA3TbCl6 single crystals at the centimeter scale, achieving high-sensitivity deep ultraviolet photoelectric detection. This enables non-destructive imaging detection of multiple physical evidences and biometric fingerprint anti-counterfeiting identification, breaking through the technical bottlenecks of high cost, small area, and single function of traditional processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123106433A_ABST
    Figure CN123106433A_ABST
Patent Text Reader

Abstract

This invention discloses a method for preparing organic-inorganic hybrid terbium-based halides, along with their products and applications, belonging to the fields of organic-inorganic hybrid halide crystal material preparation and deep ultraviolet photoelectric detection technology. The preparation method includes: dissolving organic ammonium salts and terbium salts in a volatile organic solvent, filtering to obtain a transparent precursor solution; sealing the precursor solution and statically evaporating to crystallize, selecting crystals as seed crystals; placing the precursor solution in a container containing the seed crystals, covering it with a perforated sealing film for slow evaporation, allowing the solute to grow epitaxially layer by layer along the exposed crystal face of the seed crystal, obtaining a centimeter-scale single crystal with the general chemical formula A3TbX6. The metal-semiconductor-metal type deep ultraviolet photodetector constructed from this single crystal exhibits high responsivity and specific detectivity, and can be used for non-destructive testing of biological evidence and biometric fingerprint anti-counterfeiting identification. This invention features a green and low-cost process, enabling the stable preparation of high-quality centimeter-scale single crystals.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of organic-inorganic hybrid halide crystal material preparation and deep ultraviolet photoelectric detection technology, specifically involving the preparation method of organic-inorganic hybrid terbium-based halides and their products, as well as their applications in deep ultraviolet photoelectric detection, biological evidence detection and biometric identification. Background Technology

[0002] Deep ultraviolet (DUV, λ < 280 nm) photodetector technology, due to its inherent solar blindness and strong photon-matter interaction capabilities, has broad application prospects in environmental monitoring, flame warning, space communication, and biomedical analysis. In recent years, wide-bandgap semiconductors, represented by GaN and AlGaN, have become a research hotspot in ultraviolet detection. However, the fabrication of these traditional semiconductor devices heavily relies on high-temperature epitaxial growth, complex vacuum processes, and expensive lattice-matching substrates (such as sapphire and SiC), resulting in extremely high costs and difficulty in large-area production. Compared to traditional semiconductors, lanthanide halides, with their unique 4f electron configuration and rich energy level structure, exhibit excellent wide bandgap, strong ultraviolet absorption, and efficient ligand-metal charge transfer (LMCT) characteristics, and are considered highly promising candidate materials for DUV detection. Current research on lanthanide halides is mostly focused on scintillators, phosphors, and X-ray imaging; their performance in DUV photodetector still needs significant improvement.

[0003] Currently, deep ultraviolet photodetectors are mainly based on wide-bandgap semiconductors and metal halides. Wide-bandgap semiconductors (such as AlGaN and β-Ga2O3) are typically fabricated using high-temperature epitaxial processes such as metal-organic chemical vapor deposition (MOCVD) or molecular beam epitaxy (MBE), with growth temperatures generally reaching 800–1200 °C. This process is characterized by high complexity, large equipment investment, and high manufacturing costs. In recent years, metal halide materials have shown advantages in terms of simpler processes and lower costs due to their ability to be prepared using low-temperature solution methods from room temperature to 100 °C. Currently, high-performance metal halide systems are still primarily based on lead (Pb). However, their biotoxicity and environmental pollution risks limit their application in biomedical and public safety fields. Furthermore, these materials generally suffer from bottlenecks such as insufficient environmental stability, difficulty in fabricating large-size, high-quality single crystals, and poor device uniformity. In addition, although terbium (Tb)-based halides can be obtained by low-temperature solution method or recrystallization method, existing research is mostly focused on scintillation detection applications of doped systems or microcrystalline materials. It is still difficult to stably prepare large-size single crystals that meet the requirements of photodetectors, and systematic research on them in the field of deep ultraviolet photodetection is still relatively scarce.

[0004] Based on the existing deep ultraviolet photoelectric detection materials and fabrication processes, the following technical problems mainly exist: Wide bandgap semiconductors rely on high-temperature epitaxial processes, which are costly to equipment and have complex fabrication processes, making it difficult to achieve low-cost, large-scale applications. High-performance metal halide detection materials are mostly lead-based systems, which have unavoidable biological toxicity and environmental risks, seriously restricting their promotion in high-safety-level biological monitoring and public safety fields. Existing terbium-related materials are mainly in trace doping systems or microcrystalline powder form, and the preparation process is difficult to stably grow centimeter-scale high-quality single crystals that meet the assembly requirements of optoelectronic devices; Current deep ultraviolet detectors are mostly designed for single targets or single scenarios, and generally lack the function of joint non-destructive testing for complex biological evidence. There is also a significant technological gap in bio-anti-counterfeiting identification based on the spectral characteristics of endogenous substances. Summary of the Invention

[0005] This invention addresses the technical problems in existing technologies, such as the high cost of wide-bandgap semiconductor fabrication, the toxicity risks of lead-based halides, the difficulty in stably preparing centimeter-scale high-quality single crystals of terbium-based halides, and the limited functionality of existing deep ultraviolet detectors. It provides a green, low-cost method for preparing centimeter-scale organic-inorganic hybrid terbium-based halide single crystals, along with its products and applications. This method aims to obtain high-quality single crystals, improve deep ultraviolet photoelectric detection performance, achieve highly sensitive non-destructive joint detection of complex biological evidence, and expand its applications in fields such as biometric fingerprint anti-counterfeiting identification.

[0006] To achieve the above objectives, the present invention adopts the following technical solution: A method for preparing organic-inorganic hybrid terbium-based halide single crystals includes the following steps: S1: Dissolve the organic ammonium salt and terbium salt in a volatile organic solvent, filter after dissolution to obtain a transparent precursor solution; S2: After sealing the precursor solution with a perforated sealing film, statically evaporate and crystallize it, and select crystals with smooth surface, regular morphology and no cracks as seed crystals; S3: The filtered precursor solution is placed in a container containing the seed crystal, covered with a perforated sealing film, and slowly evaporated, so that the solute is arranged in an orderly manner on the surface of the seed crystal and grows epitaxially layer by layer along the exposed crystal face of the seed crystal to obtain an organic-inorganic hybrid terbium-based halide single crystal; the general chemical formula of the organic-inorganic hybrid terbium-based halide single crystal is A3TbX6, where A is an organic ammonium ion and X is a halide ion.

[0007] Further, the organic ammonium ion A is selected from at least one of methylammonium ion, ethylammonium ion, and propanemonium ion, and the halide ion X is selected from Cl... - ,Br - and I - At least one of the following; the molar ratio of the organic ammonium salt to the terbium salt is 3:1.

[0008] Furthermore, the volume ratio of the seed crystal to the precursor solution in S3 is 1:50 to 1:2000.

[0009] Furthermore, the volatile organic solvent is anhydrous ethanol; the dissolution in S1 is achieved by stirring at 40 °C for half an hour until completely dissolved, and the filtration is achieved by filtering through a 0.45 μm PTFE filter.

[0010] Furthermore, the ratio of the organic ammonium salt to the volatile organic solvent is 3 mmol: 6 mL; the volatilization in S3 is carried out under constant temperature conditions, and the temperature of the constant temperature conditions is 30 °C.

[0011] Furthermore, the organic ammonium salt is methylammonium chloride, the terbium salt is terbium trichloride hexahydrate, and the organic-inorganic hybrid terbium-based halide single crystal is MA3TbCl6 single crystal.

[0012] The present invention also provides an organic-inorganic hybrid terbium-based halide single crystal, which is prepared by the above preparation method. The chemical formula of the single crystal is A3TbX6, where A is an organic ammonium ion and X is a halide ion. The size of the single crystal is on the order of centimeters.

[0013] Furthermore, the single crystal is an MA3TbCl6 single crystal with a size of 1.0 cm × 1.0 cm; the photoluminescence quantum yield of the single crystal is 97.61%, and the photoluminescence lifetime is 5.39 ms.

[0014] The present invention also provides a deep ultraviolet photodetector, comprising the above-mentioned organic-inorganic hybrid terbium-based halide single crystal, wherein a MoO3 layer and an Ag electrode are deposited on the polished surface of the single crystal, constituting a metal-semiconductor-metal (MSM) type photodetector. Preferably, the thickness of the MoO3 layer is 5 nm, and the thickness of the Ag electrode is 100 nm.

[0015] This invention also provides the application of the aforementioned deep ultraviolet photodetector in non-destructive testing of biological evidence or anti-counterfeiting identification of biometric fingerprints. It utilizes the difference in characteristic absorption spectra of fingerprints, bloodstains, and sweat in the 235 nm and 285 nm dual-bands to collect photocurrent responses in the 235 nm and 285 nm bands for imaging detection. The anti-counterfeiting identification of biometric fingerprints includes: determining the dual-band state based on whether the photocurrent responses in the 235 nm and 285 nm bands are below a set threshold; if both bands are below the set threshold, it is determined to be a genuine biometric fingerprint; if both bands are above the set threshold, it is determined to be a silicone counterfeit fingerprint; if the 235 nm band is below the set threshold and the 285 nm band is above the set threshold, it is determined to be a gelatin counterfeit fingerprint.

[0016] Compared with the prior art, the present invention has the following beneficial effects: Material system innovation: For the first time, this invention successfully synthesized and prepared centimeter-scale (1.0 × 1.0 cm) organic-inorganic hybrid MA3TbCl6 single crystals using methylammonium chloride (MACl) and terbium trichloride hexahydrate (TbCl3·6H2O) as raw materials through a seed crystal-induced directional evaporation growth process. This fills the gap in the large-size fabrication of this type of terbium-based hybrid single crystal material and provides a new high-quality material option for deep ultraviolet optoelectronic devices.

[0017] Size Advantage: This invention successfully prepared a regular cubic large-size single crystal of 1.0 cm × 1.0 cm through a seed crystal-induced directional evaporation growth process. This breakthrough overcomes the long-standing technical bottleneck of lacking large-area, high-quality single crystals for lanthanide halide materials in deep ultraviolet detection applications. It completely solves the size limitations of traditional processes, which can only obtain micron-sized polycrystalline powders or millimeter-sized easily cracked crystals. It achieves a leapfrog size from polycrystalline powders to large-size single crystals, which can fully meet the stringent requirements of large-area, high-sensitivity deep ultraviolet detection devices for single crystal size and quality.

[0018] Optical performance advantages: The single-crystal PLQY prepared by this invention has a purity of 97.61% and a photoluminescence lifetime of 5.39 ms, indicating that the internal defect density of the crystal is extremely low, non-radiative recombination is significantly suppressed, which is conducive to the efficient transport of photogenerated carriers.

[0019] Breakthrough in ultraviolet detection: The deep ultraviolet photodetector constructed based on this invention, using a single crystal, achieves responsivity of up to 4.13 A / W (235 nm) and 5.94 A / W (285 nm); with a specific detectivity of 1.18 × 10⁻⁶. 12 Jones (235 nm) and 1.56 × 10 12 Jones (285 nm) achieves performance far superior to various deep ultraviolet detectors based on solution preparation or doping modification in existing literature, and is on the same order of magnitude as reported wide-bandgap semiconductor detectors. This invention utilizes a low-cost solution processing strategy to successfully achieve highly sensitive deep ultraviolet detection without the need for high-temperature epitaxial growth, breaking through the technical bottlenecks of high cost and small area of ​​traditional high-performance detectors.

[0020] Applications of multi-evidence non-destructive testing and spectral anti-counterfeiting identification: Utilizing the difference in characteristic absorption spectra between the 235 nm and 285 nm dual-bands, high-resolution in-situ non-destructive imaging of various types of evidence such as fingerprints, bloodstains, and sweat can be achieved, enabling rapid initial screening without complex preprocessing. Simultaneously, based on the characteristic absorption spectra of endogenous components such as proteins, lipids, and sweat in the deep ultraviolet band of fingerprint residues, an intrinsic spectral anti-counterfeiting identification mechanism is established, which can effectively distinguish between genuine biological fingerprints and counterfeit fingerprints made of silicone, gelatin, etc., providing a reliable technical means for high-security criminal investigation evidence collection and biometric anti-counterfeiting authentication. Attached Figure Description

[0021] Figure 1 This is an experimental flowchart of the preparation method of the present invention; Figure 2 The growth results and luminescence pattern of the single crystal of this invention are shown. Figure 3 This is a schematic diagram of the device structure of the deep ultraviolet photodetector of the present invention; Figure 4 The figures show the crystal growth results under different conditions according to the present invention; Figure 5 This is an XRD comparison image of the single crystal of this invention; Figure 6 This is an optical characterization diagram of the single crystal of the present invention; Figure 7 This is a test diagram showing the detection performance of the deep ultraviolet photodetector of this invention; Figure 8 Comparison of the ultraviolet absorption spectra of three typical physical evidences: fingerprints, blood, and sweat; Figure 9 Comparison of simulated ultraviolet images of three types of physical evidence at 235 nm and 285 nm wavelengths; Figure 10 The image shows the results of the photocurrent response threshold and true value discrimination for dual-band biometric fingerprint anti-counterfeiting identification. Figure 11 This is a simulated ultraviolet imaging comparison of the results of dual-band biometric fingerprint anti-counterfeiting identification. Detailed Implementation

[0022] The present invention will be further described in detail below with reference to the accompanying drawings and embodiments. The following embodiments use MA3TbCl6 as a typical example. The principle of the seed crystal-induced directional evaporation growth process described in the following embodiments is as follows: By introducing a seed crystal, a preferential deposition interface with a low nucleation energy barrier is provided. The solute is arranged in an orderly manner on the surface of the seed crystal and continuously consumes the solute in the solution, so that the supersaturation of the system is always maintained below the critical value for homogeneous nucleation, thereby effectively suppressing spontaneous nucleation. At the same time, the lattice structure on the surface of the seed crystal plays a template guiding role, and the solute grows epitaxially layer by layer along the exposed crystal face of the seed crystal to achieve centimeter-scale A3TbX6 single crystals.

[0023] Example 1 This embodiment demonstrates the fabrication of MA3TbCl6 single crystal and corresponding deep ultraviolet optoelectronic devices. The experimental procedure for crystal growth is as follows: Figure 1 As shown, the steps are as follows: solution preparation: place the raw material in a sample vial; stir at 40 ℃ and 500 rpm until the solution is clear; after filtration, add a seed crystal to the freshly filtered precursor solution; seal the container with a perforated sealing film, and grow a single crystal at 30 ℃ using a slow evaporation method. The specific steps are as follows: S1: Preparation of the precursor solution. The organic ammonium ion A can be selected from at least one of methylammonium ion, ethylammonium ion, and propanemonium ion. In this embodiment, A is preferably methylammonium ion, and the corresponding organic ammonium salt is methylammonium chloride (CH3NH3Cl, abbreviated as MACl, 99.99%); the halide ion X is selected from Cl... - ,Br - and I - Any one of them may be used, and in this embodiment, X is preferably Cl. - The corresponding terbium salt is terbium trichloride hexahydrate (TbCl3·6H2O, 99.9%). 3 mmol of methylammonium chloride and 1 mmol of terbium trichloride hexahydrate were mixed, i.e., the molar ratio of organic ammonium salt to terbium salt was 3:1; dissolved in 6 mL of a volatile organic solvent, in this embodiment anhydrous ethanol, with a volume ratio of organic ammonium salt to volatile organic solvent of 3 mmol:6 mL; stirred at 40 °C for half an hour until completely dissolved, forming a transparent precursor solution. This solution was then rapidly filtered through a 0.45 μm PTFE filter to remove impurities, yielding a transparent precursor solution.

[0024] S2: Preparation and screening of seed crystals. The filtered precursor solution was sealed with a perforated sealing film and then statically evaporated and crystallized at room temperature. Crystals with smooth surfaces, regular morphology, and no cracks were screened as seed crystals for subsequent directional growth.

[0025] S3: Seed crystal-induced directional evaporation growth. The selected seed crystals are carefully placed into a freshly filtered precursor solution. The volume ratio of seed crystal to precursor solution can be within the range of 1:50 to 1:2000, depending on the actual size of the seed crystal. The solution is then sealed again with a perforated sealing film and placed under constant temperature conditions to maintain slow solvent evaporation, inducing directional growth of the solute. In this embodiment, the constant temperature is 30 °C. During the growth process, the solute is orderly arranged on the surface of the seed crystal and grows epitaxially layer by layer along the exposed crystal plane of the seed crystal, obtaining an organic-inorganic hybrid terbium-based halide single crystal with the general chemical formula A3TbX6. In this embodiment, it is an MA3TbCl6 single crystal.

[0026] Device fabrication: The MA3TbCl6 single crystal obtained in this embodiment was polished to obtain a crystal with a smooth surface; then, MoO3 and Ag electrodes were sequentially thermally evaporated and deposited on the wafer surface using a mask to construct a metal-semiconductor-metal (MSM) photodetector. The device structure is as follows. Figure 3 As shown: A polished MA3TbCl6 single crystal is used as the substrate, and Ag electrodes are set on the left and right sides of the substrate surface respectively. A MoO3 transition layer is set between the Ag electrode and the single crystal surface (shown as a thin layer below the electrode in the figure). The thickness of the MoO3 layer is 5 nm, and the thickness of the Ag electrode is 100 nm.

[0027] Example 2 This example serves as a counterexample to investigate the effect of the raw material molar ratio on crystal growth. The precursor solution preparation, seed crystal screening, and seed crystal-induced directional evaporation growth were performed according to the same steps S1-S3 as in Example 1. The only difference from Example 1 is that in S1, 2 mmol of methylammonium chloride (MACl) and 1 mmol of terbium trichloride hexahydrate (TbCl3·6H2O) were mixed, i.e., the molar ratio of organic ammonium salt to terbium salt was 2:1, and dissolved in 6 mL of anhydrous ethanol. The remaining process steps and parameters were the same as in Example 1.

[0028] Example 3 This example serves as a counterexample to investigate the effect of solvent dosage on crystal growth. The precursor solution preparation, seed crystal screening, and seed crystal-induced directional evaporation growth were performed according to the same steps S1-S3 as in Example 1. The only difference from Example 1 is that in S1, 3 mmol of methylammonium chloride (MACl) and 1 mmol of terbium trichloride hexahydrate (TbCl3·6H2O) were dissolved in 12 mL of anhydrous ethanol, i.e., the ratio of organic ammonium salt to volatile organic solvent was 3 mmol:12 mL. The remaining process steps and parameters were the same as in Example 1.

[0029] Example 4 This example compares the morphology of the products obtained in Examples 1 to 3 and characterizes the phase and optical properties of the single crystal obtained in Example 1.

[0030] Comparison of growth results: Figure 2 The image shows the growth results and emission patterns of the single crystal obtained in Example 1. The left image is a photograph of the single crystal placed on red graph paper under sunlight (the scale bar in the image is 1 cm). The crystal is semi-transparent and regularly cubic. The right image is a photograph under ultraviolet light with a wavelength of 365 nm. The crystal as a whole exhibits uniform and bright green emission, with a corresponding emission wavelength of 548 nm. Figure 4 These are photographs of crystals obtained under different conditions, with the top row showing photographs taken under sunlight and the bottom row showing photographs taken under 365 nm ultraviolet light. Figure 4 (a) is the initial crystal obtained by evaporation and crystallization in Example 1 (the photo includes a millimeter scale). The crystal size is on the order of millimeters, the morphology is regular, and it emits green light under ultraviolet light, which is the seed crystal obtained by screening. Figure 4 (d) is a large single crystal obtained by seed crystal induced growth in Example 1. The crystal is placed on graph paper and is in a regular cubic shape with a size of 1.0 × 1.0 cm. Under ultraviolet light, it emits bright and uniform green light, indicating that under this condition, regular and uniformly luminescent centimeter-sized MA3TbCl6 single crystals were obtained by volatilization growth.

[0031] Figure 4(b) The product obtained in Example 2 (with millimeter scale in the photo) is irregularly lumpy and emits green light under ultraviolet light, but it is not a single crystal. This is because the molar ratio of methylammonium chloride to terbium trichloride hexahydrate deviates from the stoichiometric ratio of 3:1, and the system cannot form a stable supersaturated crystal state. After a long period of solvent evaporation, only lumpy substances precipitate at the bottom of the container, and single crystals cannot grow. Figure 4 (c) The product obtained in Example 3 (with millimeter scale in the photo) consists of several small crystal fragments approximately 2 mm in size, which exhibit green luminescence under ultraviolet light. This is because the solvent volume is significantly increased, the solution concentration is extremely low, and the supersaturation is insufficient, resulting in an extremely low nucleation rate and extremely slow crystal growth. Ultimately, only very small crystal fragments can be precipitated, making it impossible to obtain single crystals with centimeter-sized crystals. Comparing the results of Examples 1-3, it can be seen that only when the molar ratio of organic ammonium salt to terbium salt in step S1 is 3:1, and the ratio of organic ammonium salt to volatile organic solvent is not less than 3 mmol: 6 mL, can high-quality single crystals with centimeter-sized crystals be obtained.

[0032] Phase and crystal quality analysis: Figure 5 The powder X-ray diffraction (XRD) pattern of the prepared centimeter-sized MA3TbCl6 single crystal is shown. The horizontal axis represents the 2θ diffraction angle (unit: degree, range 10°~38°), and the vertical axis represents the diffraction intensity (unit: au). The blue spectral lines at the top are the measured diffraction pattern of MA3TbCl6, and the main characteristic diffraction peaks are labeled with their corresponding crystal planes (202), (010), (111), (201), (402), and (213). The purple spectral lines at the bottom are the standard diffraction pattern calculated by the single crystal structure simulation. The measured diffraction peak pattern and the simulated standard diffraction pattern are in high agreement. The characteristic diffraction peaks are sharp and there are no obvious impurity phase peaks, proving that the obtained product is pure phase MA3TbCl6 and has excellent crystal quality.

[0033] Optical performance test: Under 365 nm ultraviolet light excitation, the crystal photoluminescence exhibits a bright green light. Figure 6 The optical characterization results are for MA3TbCl6 single crystals. Figure 6 (a) Photoluminescence excitation spectrum (PLE, green line in the figure, monitoring emission at 548 nm) and photoluminescence spectrum (PL, purple line in the figure), with the horizontal axis representing wavelength (in nm, range 300–700 nm) and the vertical axis representing intensity (in au). The main excitation peak of the PLE spectrum is located around 280 nm, corresponding to Tb 3+ The 4f→5d transition and ligand-metal charge transfer; the PL spectrum shows Tb under 280 nm excitation.3+ of 5 D4→ 7 F J Characteristic transition emissions, labeled sequentially from shortwave to longwave in the spectrum. 7 F6 (approximately 490 nm) 7 F5 (548 nm, the strongest green characteristic emission peak), 7 F4 (approximately 585 nm) and 7 F3 (approximately 620 nm), with the excitation wavelength λ also marked in the figure. ex =280 nm and emission wavelength λ em =548 nm. Figure 6 (b) shows the time-resolved photoluminescence (TRPL) decay curve of the single crystal. The horizontal axis represents time (unit: ms, range: 0-40 ms), and the vertical axis represents intensity (unit: au, logarithmic coordinate). The green scatter points are measured values, and the purple solid line is the fitted curve. The fitted exciton lifetime τ = 5.39 ms. The figure also indicates that PLQY = 97.61%. The absolute photoluminescence quantum yield (PLQY) test results show that it has an ultra-high PLQY of 97.61%, indicating that nonradiative recombination inside the crystal is greatly suppressed. Figure 6 (c) is the curve of PL intensity of the single crystal placed in air (25 °C) with storage time in the long-term stability test. The horizontal axis is the storage time (unit: days, 1 to 84 days), and the vertical axis is the normalized PL intensity (unit: au). After 84 days, the PL intensity remained at 89.9% of the initial value. Figure 6 (d) shows the change curve of PLQY over time during the corresponding storage process. The horizontal axis represents storage time (in days), and the vertical axis represents PLQY (in %). PLQY slowly decreased from the initial 97.61% to 84.84%. The above results fully demonstrate that the crystal has excellent long-term environmental stability and can meet the stringent requirements for material stability in practical device applications.

[0034] Example 5 This embodiment is a test of the ultraviolet photoelectric response of the deep ultraviolet photodetector obtained in Example 1. The test results are as follows: Figure 7 As shown.

[0035] Figure 7 (a) The current-time (It) response curve of the device under 235 nm ultraviolet light irradiation and a bias voltage of 1.5 V. The horizontal axis represents time (in seconds), and the vertical axis represents current (in nA, ranging from 0 to 40 nA). The optical power density is 1 μW / cm². 2Gradually increase to 200 μW / cm 2 (The numbers in the figure are labeled from top to bottom as 200, 150, 100, 50, 25, and 1 μW / cm) 2 The photocurrent of the device increases in a stepwise manner with the increase of optical power density, and the switching response is stable and reversible. Figure 7 (b) Responsivity R and specific detectivity D at 235 nm The curve shows the change in optical power density, with the horizontal axis representing optical power density (unit: μW / cm²). 2 The left vertical axis represents the responsivity R (unit: A / W, purple spectral line), and the right vertical axis represents the specific detectivity D. (Unit: 10) 12 Jones (blue spectral line); at a light power density of 1 μW / cm² 2 Under the test conditions, the photocurrent responsivity was 4.13 A / W, and the specific detectivity was 1.18 × 10⁻⁶. 12 Jones. Figure 7 (c) 235 nm, 200 μW / cm 2 The single-cycle normalized response curve is shown below. The horizontal axis represents time (in seconds), and the vertical axis represents the normalized current (in au). The green shaded area in the figure indicates the switching ratio η≈10.58, and the rise time t is also marked. r ≈55.33 ms, descent time t d ≈66.04 ms.

[0036] Figure 7 (d) shows the It response curve of the device under 285 nm ultraviolet light irradiation and a bias voltage of 1.5 V. The horizontal axis represents time (in seconds), and the vertical axis represents current (in nA, ranging from 0 to 100 nA). The optical power density is also 1 μW / cm². 2 Gradually increase to 200 μW / cm 2 . Figure 7 (e) Responsivity R and specific detectivity D at 285 nm With optical power density (0~1500 μW / cm) 2 The curve showing the change in the coordinate axis is set the same as the curve showing the change in the coordinate axis. Figure 7 (b); at an optical power density of 1 μW / cm² 2 Under the test conditions, the photocurrent responsivity was 5.94 A / W, and the specific detectivity was 1.56 × 10⁻⁶. 12 Jones. Figure 7 (f) is 285 nm, 200 μW / cm 2 The single-cycle normalized response curve is shown below, with an on / off ratio η≈81.20 and a rise time t. r≈41.75 ms, descent time t d The time is approximately 56.60 ms, indicating that it is suitable for real-time monitoring of ultraviolet light intensity.

[0037] Using a single crystal as the core component of an ultraviolet photodetector, its photocurrent response under different ultraviolet light intensities was tested. The results show that the detector possesses a good linear response range and high sensitivity, making it suitable for application in the field of ultraviolet light detection.

[0038] Example 6 This embodiment demonstrates an application of non-destructive imaging detection for multiple pieces of evidence. Figure 8 This is a comparison of the ultraviolet absorption spectra of three typical physical evidences: fingerprints, blood, and sweat. The horizontal axis represents wavelength (in nm, ranging from 250 to 450 nm), and the vertical axis represents absorbance (in au). The three curves in the figure represent squalene (green curve, corresponding to the lipid component in fingerprints), bloodstain (dark curve), and artificial sweat (cyan curve), respectively. The inset on the right is a schematic diagram of the deep ultraviolet absorption layer of the skin, which shows the distribution of sebum and sweat in the skin surface.

[0039] Fingerprint (squalene + sweat): Since the main components include lipids such as squalene and trace amounts of sweat, it exhibits obvious characteristic absorption at 235 nm (corresponding to lipid / protein absorption) and also has a certain absorption response at 285 nm, but the overall intensity and peak shape are significantly different from pure sweat.

[0040] Blood (protein): The absorption spectrum is mainly contributed by hemoglobin and protein peptide bonds. It exhibits strong dual-band characteristic absorption signals at 235 nm (corresponding to peptide bond characteristic absorption) and 285 nm, and the overall absorbance is high.

[0041] Artificial sweat: The absorption spectrum characteristics are mainly attributed to the uric acid component in sweat. It exhibits a strong and single characteristic absorption peak at 285 nm, while the absorbance at 235 nm is extremely low.

[0042] Figure 9 This is a comparison of simulated ultraviolet images of three types of evidence at 235 nm and 285 nm wavelengths. The three columns represent fingerprints, bloodstains, and sweat, respectively, with the top row showing 235 nm at 200 μW / cm². 2 The imaging results are shown below, downlink at 285 nm @ 200 μW / cm. 2Imaging results (optical power density uniformly set at 200 μW / cm²) 2 Each sub-image has the X axis (mm) and Y axis (mm) as the horizontal axis. The color mark on the right represents the detector's photocurrent (A). The darker the color mark, the lower the photocurrent response at that location, indicating stronger absorption of ultraviolet light by the corresponding evidence. It can be seen that at the 235nm band, fingerprints show a complete fingerprint outline, bloodstains show a clear splatter distribution, while sweat shows almost no response. At the 285nm band, both fingerprints and bloodstains are clearly imaged, and sweat also shows a clear distribution pattern. That is, the 235nm band has high reactivity for protein / lipid-rich fingerprints and bloodstains, but almost no response to sweat; while the 285nm band has high reactivity for both sweat (uric acid component) and bloodstains (protein). This dual-band orthogonal imaging result provides a clear physical basis for the multi-evidence nondestructive testing of this invention.

[0043] Example 7 This embodiment demonstrates a dual-band biometric fingerprint anti-counterfeiting identification application. Figure 10 The image shows the results of the photocurrent response threshold and the true value discrimination for dual-band biometric fingerprint anti-counterfeiting identification. Figure 10 (a) 235 nm @ 200 μW / cm 2 Photocurrent histograms of four types of samples—clean substrate, genuine fingerprint, silicone fake fingerprint, and gelatin fake fingerprint—are presented. The vertical axis represents current (in nA, ranging from 0 to 30 nA). The orange dashed line in the figure represents the judgment threshold of 2.0 × 10⁻⁶. -8 A. Each column is marked with a status indicator (photocurrent above the threshold is recorded as 1, and below the threshold is recorded as 0). Figure 10 (b) 285 nm @ 200 μW / cm 2 The following are the corresponding bar charts for the four samples, with the vertical axis representing current (unit: nA, range 0–60 nA), and the judgment threshold being 3.4 × 10⁻⁶. -8 A; Figure 10 (c) is a dual-band truth table, where the Category column represents the sample category, I 235 nm with I 285 nm The two columns list the state determination results of the four samples at 235 nm and 285 nm, respectively. The numbers in the cells represent the state bits, and the corresponding criteria are in parentheses (e.g., "" indicates that the photocurrent of the sample is higher than 2.0 × 10⁻⁶). -8 Threshold A): Clean substrate is 11, genuine biometric fingerprint is 00, silicone fake fingerprint is 11, and gelatin fake fingerprint is 01. Based on this, a clear identification logic can be established: Genuine bio-fingerprint: Because it contains both protein / lipid (235 nm absorption) and sweat uric acid (285 nm absorption), it exhibits strong absorption in both wavelengths, resulting in a decrease in photocurrent. The dual-wavelength state is determined to be 00.

[0044] Silicone fingerprint: Because it does not contain any biological absorption components, it has no obvious absorption characteristics in both wavelengths, the photocurrent remains high, and the dual-wavelength state is judged as 11.

[0045] Gelatin pseudofingerprint: Because it contains a polypeptide backbone but has a very low content of aromatic amino acids and does not contain uric acid, it only shows absorption at 235 nm (state 0) and no absorption at 285 nm (state 1). The dual-band state is determined to be 01.

[0046] The dual-band current threshold discrimination logic clearly demonstrates the effectiveness of the anti-counterfeiting mechanism of this invention. By combining the orthogonal response states of 235nm and 285nm, it can accurately distinguish between genuine biometric fingerprints and counterfeit fingerprints made of different materials, greatly improving the reliability of biometric anti-counterfeiting identification.

[0047] Figure 11 This is a simulated ultraviolet imaging comparison of dual-band biometric fingerprint anti-counterfeiting identification results. The three columns represent genuine fingerprints (Genuine), silicone counterfeit fingerprints, and gelatin counterfeit fingerprints, respectively. The top row is 235 nm @ 200 μW / cm². 2 The imaging results are shown below, downlink at 285 nm @ 200 μW / cm. 2 The imaging results are shown below; each sub-image has X (unit: mm) on the horizontal axis and Y (unit: mm) on the vertical axis. The color mark on the right represents the photocurrent (unit: A). In the silicone counterfeit fingerprint sub-image, the fingerprint pressing area is marked with a blue dashed ellipse. Real fingerprints, due to the presence of both lipids (235 nm absorption) and sweat (285 nm absorption), exhibit clear patterns in both wavelengths; silicone fingerprints, lacking biological components, show no response in either wavelength; gelatin fingerprints, containing only protein, only image at the 235 nm wavelength, showing no response at 285 nm. This result directly confirms the dual-band anti-counterfeiting logic of this invention.

Claims

1. A method for preparing organic-inorganic hybrid terbium-based halide single crystals, characterized in that, Includes the following steps: S1: Dissolve the organic ammonium salt and terbium salt in a volatile organic solvent, filter after dissolution to obtain a transparent precursor solution; S2: After sealing the precursor solution with a perforated sealing film, statically evaporate and crystallize it, and select crystals with smooth surface, regular morphology and no cracks as seed crystals; S3: The filtered precursor solution is placed in a container containing the seed crystal, covered with a perforated sealing film, and slowly evaporated, so that the solute is arranged in an orderly manner on the surface of the seed crystal and grows epitaxially layer by layer along the exposed crystal face of the seed crystal to obtain an organic-inorganic hybrid terbium-based halide single crystal; the general chemical formula of the organic-inorganic hybrid terbium-based halide single crystal is A3TbX6, where A is an organic ammonium ion and X is a halide ion.

2. The preparation method according to claim 1, characterized in that, The organic ammonium ion A is selected from at least one of methylammonium ion, ethylammonium ion and propanemonium ion, and the halide ion X is selected from at least one of Cl-, Br- and I-; the molar ratio of the organic ammonium salt to the terbium salt is 3:

1.

3. The preparation method according to claim 1, characterized in that, The volume ratio of the seed crystal to the precursor solution in S3 is 1:50 to 1:2000.

4. The preparation method according to claim 1, characterized in that, The volatile organic solvent is anhydrous ethanol; the dissolution in S1 is to stir at 40 °C for half an hour until completely dissolved, and the filtration is to filter through a 0.45 μm PTFE filter.

5. The preparation method according to claim 1, characterized in that, The ratio of the organic ammonium salt to the volatile organic solvent is 3 mmol: 6 mL; the volatilization in S3 is carried out under constant temperature conditions, and the temperature of the constant temperature conditions is 30 °C.

6. The preparation method according to any one of claims 1-5, characterized in that, The organic ammonium salt is methylammonium chloride, the terbium salt is terbium trichloride hexahydrate, and the organic-inorganic hybrid terbium-based halide single crystal is MA3TbCl6 single crystal.

7. An organic-inorganic hybrid terbium-based halide single crystal, characterized in that, The single crystal is prepared by the preparation method according to any one of claims 1-6, wherein the general chemical formula of the single crystal is A3TbX6, where A is an organic ammonium ion and X is a halide ion; the size of the single crystal is on the order of centimeters.

8. The organic-inorganic hybrid terbium-based halide single crystal according to claim 7, characterized in that, The single crystal is an MA3TbCl6 single crystal with a size of 1.0 cm × 1.0 cm; the photoluminescence quantum yield of the single crystal is 97.61%, and the photoluminescence lifetime is 5.39 ms.

9. A deep ultraviolet photodetector, characterized in that, The invention includes the organic-inorganic hybrid terbium-based halide single crystal as described in claim 7 or 8, wherein the polished surface of the single crystal is coated with a MoO3 layer and an Ag electrode to form a metal-semiconductor-metal (MSM) type photodetector.

10. The application of the deep ultraviolet photodetector as described in claim 9 in non-destructive testing of biological evidence or anti-counterfeiting identification of biometric fingerprints, characterized in that, The biometric fingerprint anti-counterfeiting identification method utilizes the difference in characteristic absorption spectra of fingerprints, bloodstains, and sweat in the 235 nm and 285 nm dual-bands to collect photocurrent responses in the 235 nm and 285 nm bands for imaging detection. The method includes: determining the dual-band status based on whether the photocurrent responses in the 235 nm and 285 nm bands are lower than a set threshold; if both bands are lower than the set threshold, it is determined to be a genuine biometric fingerprint; if both bands are higher than the set threshold, it is determined to be a silicone counterfeit fingerprint; if the 235 nm band is lower than the set threshold and the 285 nm band is higher than the set threshold, it is determined to be a gelatin counterfeit fingerprint.