A phosphorus-containing copper porphyrin flame retardant, its preparation method and its application
By integrating phosphorus-containing copper porphyrin flame retardants at the molecular level, the problem of mechanical property degradation under high addition levels of epoxy resin flame retardants has been solved, achieving high efficiency in flame retardancy and self-extinguishing properties under low addition levels, thus improving the flame retardant safety and mechanical properties of epoxy resin.
Patent Information
- Application Number
- CN202611447831.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-17
- Publication Date
- 2026-11-17
AI Technical Summary
Existing epoxy resin flame retardants suffer from mechanical property degradation at high addition levels and limited efficiency of single flame retardant elements. Furthermore, traditional flame retardants release toxic substances during combustion or require high addition levels.
A phosphorus-containing copper porphyrin flame retardant is used. Through the coordination of copper ions with the nitrogen atom in the center of the porphyrin ring, and the interaction of phosphorus elements with amino groups through hydrogen bonds, a PN-Cu synergistic flame retardant system is constructed to achieve molecular-level integration. The preparation method includes steps such as dissolution, reaction, and post-treatment.
Achieving high-efficiency flame retardancy in epoxy resin composites with low addition amounts, exhibiting good self-extinguishing properties during combustion, reduced heat release rate, increased char residue, and maintained mechanical properties, aligning with the development trend of environmentally friendly flame-retardant materials.
Smart Images

Figure CN123106722A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of flame-retardant polymer materials technology, specifically relating to a phosphorus-containing copper porphyrin flame retardant, its preparation method, and its application. Background Technology
[0002] Epoxy resin, as the most widely used thermosetting polymer material, is widely used in electronic packaging, building materials, aerospace and other fields due to its excellent mechanical properties, adhesive properties and chemical stability. However, bisphenol A type epoxy resin has a limiting oxygen index of only 19%-21%, which makes it a flammable material. When burned, it releases a large amount of heat and toxic fumes, posing a serious fire hazard. Therefore, it must be modified to be flame-retardant.
[0003] Among existing epoxy resin flame retardants, halogenated flame retardants have high flame retardant efficiency, but they release toxic and carcinogenic substances when burning and have been restricted by regulations in many countries; inorganic flame retardants such as aluminum hydroxide and magnesium hydroxide require a high addition amount of 40%-60% or more to meet the standards, which will seriously degrade the mechanical properties of epoxy resin; ordinary organophosphorus flame retardants have problems such as insufficient thermal stability and migration and precipitation, and the efficiency of a single flame retardant element is limited.
[0004] Porphyrin compounds possess a rigid macrocyclic conjugated structure and excellent thermal stability. The central nitrogen atom can coordinate with metal ions, catalyzing char formation and enhancing the graphitization of the char layer at high temperatures, making them highly promising flame-retardant framework materials. However, existing porphyrin-based flame retardants are mostly modified with a single metal or element, lacking sufficient multi-element synergistic effects, and their flame-retardant efficiency still has room for improvement. Therefore, developing a multi-element synergistic high-efficiency flame retardant based on a porphyrin framework to achieve synergistic improvement in flame retardancy and mechanical properties at low addition levels is a technical problem to be solved in this field. Summary of the Invention
[0005] To address the shortcomings of existing technologies, the present invention aims to provide a phosphorus-containing copper porphyrin flame retardant, its preparation method, and its application. By integrating phosphorus, nitrogen, and copper flame retardant elements at the molecular level, it achieves efficient synergistic flame retardancy through condensed phases, while avoiding the problem of severe mechanical property degradation under high addition levels of traditional flame retardants. This improves flame retardant safety while maintaining good mechanical properties.
[0006] To achieve the above-mentioned objectives, the present invention adopts the following technical solution: A phosphorus-containing copper porphyrin flame retardant comprises a porphyrin ring skeleton, copper ions coordinated to the central nitrogen atom of the porphyrin ring, and phosphorus-containing groups bonded to the porphyrin ring structure; wherein the copper ions form a coordinate bond with the central nitrogen atom of the porphyrin ring, and the phosphorus element exists in the porphyrin structure through hydrogen bonding between the phosphate ester group and the amino group, constructing a PN-Cu synergistic flame retardant system, the chemical structural formula of which is as follows: .
[0007] A method for preparing a phosphorus-containing copper porphyrin flame retardant, the method comprising the following steps: S1. Dissolve 5,10,15,20-tetrakis(4-aminophenyl)porphyrin in a mixed solvent to form a mixed solution; S2. Under nitrogen protection, add cuprous diphenyl phosphate to the mixture and stir the reaction at room temperature to obtain the reaction product; S3. The reaction product is post-treated to obtain a phosphorus-containing copper porphyrin flame retardant.
[0008] Furthermore, the molar ratio of 5,10,15,20-tetra(4-aminophenyl)porphyrin to diphenylcopper(II)phosphite is 1:(1-1.2), and the reaction time is 30 min.
[0009] Furthermore, the mixed solvent is a mixed solution of chloroform and acetonitrile, wherein the volume ratio of chloroform to acetonitrile is chloroform:acetonitrile = (1.1-1.3):1.
[0010] Furthermore, the post-processing in S3 includes: removing the solvent under reduced pressure after the reaction is completed, dissolving the crude product in dichloromethane, precipitating it in methanol, centrifuging it, and then drying it under vacuum to obtain the finished product.
[0011] Furthermore, the centrifugation speed is 9100 r / min, the centrifugation time is 5 min; the vacuum drying temperature is 60℃, and the drying time is 24 h.
[0012] A flame-retardant epoxy resin composite material, the composite material comprising bisphenol A type epoxy resin, an amine curing agent, and a phosphorus copper porphyrin flame retardant as described above; the amount of phosphorus copper porphyrin flame retardant added is 2% to 4% of the total mass of epoxy resin and curing agent.
[0013] Furthermore, the amine curing agent includes a 4,4'-diaminodiphenylmethane curing agent.
[0014] Furthermore, the processing method of the flame-retardant epoxy resin composite material includes: obtaining the bisphenol A type epoxy resin (E-51), 4,4'-diaminodiphenylmethane curing agent and phosphorus copper porphyrin flame retardant by gradient thermosetting and cooling demolding; wherein the thermosetting method includes: holding at 150°C for 2 hours, raising the temperature to 180°C and holding for 2 hours, raising the temperature to 200°C and holding for 2 hours, and naturally cooling to room temperature for demolding.
[0015] Application of a phosphorus-containing copper porphyrin flame retardant in the flame retardant modification of epoxy resin.
[0016] Compared with existing pure epoxy resin systems, the present invention has the following advantages: 1. This invention introduces both copper ions and phosphorus-containing groups into the porphyrin ring framework. Infrared spectroscopy confirms successful coordination between copper ions and the central nitrogen atom of the porphyrin ring, while the characteristic absorption peaks of the phosphorus-containing groups are fully preserved, achieving effective integration of phosphorus and copper flame-retardant elements at the molecular level. Adding a small amount of the flame retardant of this invention enables epoxy resin composites to achieve a vertical combustion flame-retardant rating, self-extinguishing after flame removal, with a significantly lower peak heat release rate compared to pure epoxy resin, a reduced total heat release, and a significantly improved char residue rate, demonstrating the remarkable synergistic flame-retardant effect of phosphorus and copper.
[0017] 2. This invention uses cuprous diphenyl phosphate as a phosphorus-copper bifunctional modifier, and the modification of porphyrin can be completed through a one-step coordination reaction. The reaction is carried out at room temperature, without the need for heating or complex equipment, and is simple to operate and suitable for large-scale preparation.
[0018] 3. The flame retardant of this invention does not contain halogens or antimony. Cone calorimetry tests show that the CO and CO2 release rates during the combustion process of the composite material are reduced compared to pure epoxy resin after adding the flame retardant of this invention, and the release of smoke is suppressed to a certain extent, which is in line with the development direction of environmentally friendly flame retardant materials.
[0019] 4. Cross-sectional morphology analysis shows that after adding the flame retardant of the present invention, the cross-section of the composite material changes from the smooth cleavage surface of pure epoxy resin to a tough fracture feature with tearing edges and river-like stripes. The pores are reduced and the pore walls are thickened. While improving the flame retardant performance, it maintains good mechanical properties and overcomes the technical defect of severe mechanical property deterioration under high addition of traditional flame retardants. Attached Figure Description
[0020] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0021] Figure 1 The prepared phosphorus-containing copper porphyrin flame retardant and its predicted Fourier transform infrared spectrum are shown. Figure 2 Scanning electron microscope image of CuT flame retardant powder; Figure 3 The thermogravimetric (TG) versus differential thermogravimetric (DTG) curves of CuT flame retardant; Figure 4 Thermogravimetric curve of EP-4CuT composite material; Figure 5 This is a cross-sectional scanning electron microscope image of the EP-0CuT and EP-4CuT composite material. Figure 6 EDS elemental surface scan of the EP-0CuT and EP-4CuT composite material; Figure 7 The graph shows the heat release rate (HRR) versus total heat release (THR) curves of the EP-CuT composite material. Figure 8 The graph shows the combustion CO generation rate (COP) and CO2 generation rate (CO2P) curves of the EP-CuT composite material. Detailed Implementation
[0022] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention are described clearly and completely. Obviously, the described embodiments are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0023] A phosphorus-containing copper porphyrin flame retardant, Cu-TAPP (hereinafter referred to as CuT), is obtained by a coordination reaction between 5,10,15,20-tetratetra(4-aminophenyl)porphyrin (TAPP) and diphenyl copper phosphate (Cu(DPP)2). Copper ions form coordinate bonds with the nitrogen atom at the center of the porphyrin ring, and phosphorus exists in the porphyrin structure through hydrogen bonding between the phosphate ester group and the amino group, achieving molecular-level integration of phosphorus and copper flame retardant elements. Its chemical structural formula is as follows: .
[0024] This flame retardant mainly relies on the condensation mechanism to achieve its flame retardant effect: phosphorus can catalyze the dehydration of the epoxy resin matrix into char at high temperatures, and copper can effectively promote the graphitization of the char layer, ultimately forming a dense, continuous and stable protective char layer, which effectively blocks the transfer of heat and oxygen during combustion, achieving PN-Cu multi-element molecular-level synergistic flame retardancy.
[0025] The preparation method of the above-mentioned phosphorus-containing copper porphyrin flame retardant includes the following steps: 5,10,15,20-tetra(4-aminophenyl)porphyrin was dissolved in a chloroform-acetonitrile mixture under high-purity nitrogen atmosphere and stirred until completely dissolved. Diphenyl copper phosphate was slowly added while maintaining a nitrogen atmosphere and stirring continuously at room temperature. After the reaction was completed, the solvent was removed by vacuum distillation. The crude product was dissolved in dichloromethane, precipitated in methanol, centrifuged, and dried under vacuum to obtain a dark red powder containing copper porphyrin flame retardant.
[0026] The mass ratio of 5,10,15,20-tetra(4-aminophenyl)porphyrin to diphenylcopper(II)phosphate was 0.78:0.82, which corresponds to a molar ratio of approximately 1:1.05, falling within the range of 1:(1-1.2). The reaction time was 30 min; the centrifugation speed was 9100 r / min, and the centrifugation time was 5 min; the vacuum drying temperature was 60 °C, and the drying time was 24 h.
[0027] A flame-retardant epoxy resin composite material is prepared by a gradient thermosetting process from bisphenol A type epoxy resin (E-51), 4,4'-diaminodiphenylmethane curing agent and the above-mentioned phosphorus-containing copper porphyrin flame retardant; the amount of flame retardant added is 2% and 4%, respectively, corresponding to sample numbers EP-2CuT and EP-4CuT, and the pure epoxy resin sample without added flame retardant is numbered EP-0CuT.
[0028] The gradient thermosetting process is as follows: heat at 150℃ for 2 hours, heat up to 180℃ for 2 hours, heat up to 200℃ for 2 hours, and then let it cool naturally to room temperature before demolding.
[0029] A method for processing a flame-retardant epoxy resin composite material involves a gradient thermosetting process using bisphenol A type epoxy resin (E-51), a 4,4'-diaminodiphenylmethane curing agent, and a phosphorus copper porphyrin flame retardant. The thermosetting process includes: holding at 150°C for 2 hours, raising the temperature to 180°C and holding for 2 hours, raising the temperature to 200°C and holding for 2 hours, and then naturally cooling to room temperature for demolding. Specific Implementation
[0030] Example 1: Preparation of phosphorus-containing copper porphyrin flame retardant: Weigh 0.78 g of 5,10,15,20-tetra(4-aminophenyl)porphyrin into a 250 mL three-necked flask, add a mixed solvent of 120 mL chloroform and 100 mL acetonitrile, purge with high-purity nitrogen, and stir until the monomer is completely dissolved. After the system temperature stabilizes at room temperature, slowly add 0.82 g of cuprous diphenyl phosphate, maintain the nitrogen atmosphere, and stir the reaction at room temperature for 30 min. The solution color gradually changes from dark red to dark purplish-red.
[0031] After the reaction was complete, the solvent was evaporated from the reaction solution under reduced pressure at 40℃ to obtain a dark purple-red crude product. 30 mL of dichloromethane was added to the crude product to dissolve it completely, followed by the slow addition of 100 mL of methanol. After ultrasonic dispersion for 20 min, the mixture was centrifuged at 9100 r / min for 5 min, the supernatant was discarded, and the lower solid layer was collected. The solid was dried in a vacuum drying oven at 60℃ for 24 h to obtain a dark red powdery copper porphyrin phosphorus flame retardant, denoted as CuT.
[0032] Example 2: Preparation of EP-2CuT flame-retardant epoxy resin composite material: Weigh 23.48g of bisphenol A type epoxy resin E-51 and 5.95g of 4,4'-diaminodiphenylmethane curing agent according to a 1:1 molar ratio of active hydrogen to epoxy groups (the amount of curing agent was adjusted according to the epoxy equivalent and amine hydrogen equivalent to maintain a 1:1 molar ratio of epoxy groups to amine hydrogen). Then, 0.67g of CuT flame retardant prepared in Example 1 (added at 2% of the total mass of the system) and 4,4'-diaminodiphenylmethane curing agent were placed in an oven preheated to 150°C and heated. After mixing evenly, the mixture was mixed with bisphenol A type epoxy resin E-51 and heated to melt and stir for about 1 minute to form a homogeneous viscous liquid. The mixture was poured into a polytetrafluoroethylene mold preheated to 150°C and cured according to the following procedure: 150°C for 2 hours, 180°C for 2 hours, and 200°C for 2 hours. After curing, the material is naturally cooled to room temperature and then demolded to obtain a flame-retardant epoxy resin composite material, denoted as EP-2CuT.
[0033] Example 3: Preparation of EP-4CuT flame-retardant epoxy resin composite material: The steps are basically the same as in Example 2, except that the CuT flame retardant addition is 4% of the total mass of the system, corresponding to 1.35g of CuT flame retardant. Based on the epoxy equivalent and amine hydrogen equivalent, the amount of curing agent is adjusted to 5.63g. The resulting sample is designated as EP-4CuT.
[0034] Comparative Example 1: Preparation of pure epoxy resin sample: The steps are basically the same as in Example 2, except that CuT flame retardant is not added and the amount of curing agent is 6.27g. The resulting pure epoxy resin sample is designated as EP-0CuT.
[0035] The above-described embodiments and comparative samples were subjected to structural characterization and performance testing, and the results are as follows: like Figure 1 The Fourier transform infrared spectroscopy results show that the NH stretching vibration peak of TAPP (3350 cm⁻¹) is significantly weakened after the reaction, and the product peak is at 1650 cm⁻¹. ⁻1 The characteristic absorption peak of Cu-N coordination bond appears nearby; at the same time, the characteristic peaks of P=O (1200 cm⁻¹) and POC (960 cm⁻¹) in Cu(DPP)₂ are completely retained in the product, confirming that the copper ion is successfully coordinated with the nitrogen atom in the center of the porphyrin ring, and that phosphorus and copper elements are effectively introduced into the target product. like Figure 2 As shown in the image, scanning electron microscopy reveals that CuT powder consists of agglomerates composed of numerous fine particles. The particles are irregularly distributed in a mixture of rod-shaped, needle-shaped, and block-shaped forms, without any obvious specific crystal form, exhibiting the agglomeration phenomenon common in powder materials.
[0036] In Fourier transform infrared spectroscopy, the amino N-H stretching vibration peak (approximately 3350 cm⁻¹) showed a significant low wavenumber shift, peak broadening, and intensity decrease after the reaction, confirming the formation of intermolecular hydrogen bonds between the phosphate ester group and the amino group. In this system, copper ions form strong coordination bonds with the nitrogen atoms of the porphyrin ring to fix the metal sites, while phosphorus-containing groups are enriched in the porphyrin periphery system through hydrogen bonding between the phosphate ester and the amino group. During the epoxy resin curing stage (high temperature of 150-200℃), although some hydrogen bonds can undergo reversible dissociation, the strong coordination framework of copper porphyrin remains stable, and the phosphorus-containing groups are still bound to the periphery of the porphyrin molecule. At the same time, the curing crosslinking forms a three-dimensional network structure, and the steric hindrance further inhibits the migration and precipitation of phosphorus-containing components, preventing small molecules from migrating out and ensuring the stability of the flame retardant properties of the composite material.
[0037] Thermal stability properties: such as Figure 3 As shown, the CuT flame retardant has a 5% thermal decomposition temperature of 275℃ and a char residue rate of 59.39% at 800℃, exhibiting good thermal stability and charring ability; Figure 4 As shown, the EP-4CuT composite material has a carbon residue rate of 23.7% at 800℃ compared to pure EP, demonstrating excellent catalytic carbonization effect.
[0038] The flame retardancy rating, mechanical properties and combustion behavior of the composite material samples prepared in Examples 2-3 and Comparative Example 1 were tested, and the results are summarized in Table 1.
[0039] Table 1 Performance test results of EP-0CuT, EP-2CuT and EP-4CuT composite materials Component Name Example 2 Example 3 Comparative Example 1 Flame retardant parts 2 4 0 Vertical flammability rating V2 V0 No grade Tensile strength (MPa) 46.4±5.1 47.3±4.6 43.5±4.5 Elongation at break (%) 7.2±4.3 7.5±4.8 9.8±4.7 <![CDATA[Peak heat release rate (kW / m 2 )]]> 626.4 599.0 912.6 <![CDATA[Total heat release (MJ / m 2 )]]> 48.2 46.6 49.3 Flame retardant performance: In the vertical burning test, pure EP burned continuously until completely burned without self-extinguishing; EP-2CuT reached V2 level, showing a certain flame retardant effect; EP-4CuT self-extinguished within 20 seconds after two ignitions, reaching V0 level and exhibiting obvious self-extinguishing characteristics. Figure 7 As shown in the HRR curve morphology, pure EP rapidly increases its heat release rate to a single peak after ignition, indicating concentrated heat release; while the HRR curve of EP-4CuT tends to be flatter overall, with the peak appearing time significantly delayed, indicating that the flame retardant exerts an inhibitory effect in the early stages of combustion, slowing down the thermal decomposition process of the resin matrix; cone calorimetry shows that the peak heat release rate of EP-4CuT is significantly lower than that of pure EP, with the total heat release decreasing to 46.6 MJ / m². The CO and CO2 generation rate curves are shown below. Figure 8 As shown, the generation rates of both gases after adding CuT are lower than those of pure EP during the entire combustion process, effectively suppressing flue gas release and significantly improving fire safety.
[0040] Mechanical morphology analysis: such as Figure 5As shown in the cross-sectional SEM, pure EP exhibits typical brittle fracture with a smooth fracture surface and large pores. After adding CuT, the material fracture surface shows a large number of tearing ridges and river-like striations, the pore size decreases, the pore wall thickens, the fracture mode changes to ductile fracture, and the energy dissipation capacity is significantly improved.
[0041] Elemental distribution analysis: such as Figure 6 As shown, the EDS surface scan results indicate that P, N, and Cu elements are uniformly distributed on the cross-section of the EP-4CuT composite material, and no obvious areas of element enrichment or deficiency were observed. This suggests that the phosphorus-containing copper porphyrin flame retardant has good dispersion uniformity in the epoxy resin matrix, which is beneficial for the flame retardant elements to play a synergistic role in the combustion process.
[0042] It should be noted that, in this document, relational terms such as "first" and "second" are used only to distinguish one entity or operation from another, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Furthermore, the terms "comprising," "including," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such a process, method, article, or apparatus. Without further limitations, an element defined by the phrase "comprising one..." does not exclude the presence of other identical elements in the process, method, article, or apparatus that includes said element.
[0043] The above embodiments are only used to illustrate the technical solutions of the present invention, and are not intended to limit it. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some of the technical features. Such modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A phosphorus-containing copper porphyrin flame retardant, characterized in that, The flame retardant comprises a porphyrin ring skeleton, copper ions coordinated to the nitrogen atom at the center of the porphyrin ring, and phosphorus-containing groups bonded to the porphyrin ring structure; wherein, the copper ions form a coordination bond with the nitrogen atom at the center of the porphyrin ring, and the phosphorus element exists in the porphyrin structure through hydrogen bonding between the phosphate ester group and the amino group, constructing a PN-Cu synergistic flame retardant system, the chemical structural formula of which is as follows: 。 2. A method for preparing a phosphorus-containing copper porphyrin flame retardant, characterized in that, The method includes the following steps: S1. Dissolve 5,10,15,20-tetrakis(4-aminophenyl)porphyrin in a mixed solvent to form a mixed solution; S2. Under nitrogen protection, add cuprous diphenyl phosphate to the mixture and stir the reaction at room temperature to obtain the reaction product; S3. The reaction product is post-treated to obtain a phosphorus-containing copper porphyrin flame retardant.
3. The preparation method of a phosphorus-containing copper porphyrin flame retardant according to claim 2, characterized in that, The molar ratio of 5,10,15,20-tetra(4-aminophenyl)porphyrin to diphenylcopper(II)phosphite was 1:(1-1.2), and the reaction time was 30 min.
4. The preparation method of a phosphorus-containing copper porphyrin flame retardant according to claim 2, characterized in that, The mixed solvent is a mixed solution of chloroform and acetonitrile, wherein the volume ratio of chloroform to acetonitrile is chloroform:acetonitrile = (1.1-1.3):
1.
5. The method for preparing a phosphorus-containing copper porphyrin flame retardant according to claim 2, characterized in that, The post-processing in S3 includes: removing the solvent under reduced pressure after the reaction, dissolving the crude product in dichloromethane, precipitating it in methanol, centrifuging it, and then drying it under vacuum to obtain the finished product.
6. The method for preparing a phosphorus-containing copper porphyrin flame retardant according to claim 5, characterized in that, The centrifugation speed was 9100 r / min, and the centrifugation time was 5 min; the vacuum drying temperature was 60℃, and the drying time was 24 h.
7. A flame-retardant epoxy resin composite material, characterized in that, The composite material includes bisphenol A type epoxy resin, amine curing agent, and phosphorus copper porphyrin flame retardant as described in claim 1; the amount of phosphorus copper porphyrin flame retardant added is 2% to 4% of the total mass of epoxy resin and curing agent.
8. The flame-retardant epoxy resin composite material according to claim 7, characterized in that, The amine curing agent includes 4,4'-diaminodiphenylmethane curing agent.
9. The flame-retardant epoxy resin composite material according to claim 7, characterized in that, The processing method of the flame-retardant epoxy resin composite material includes: bisphenol A type epoxy resin (E-51), 4,4'-diaminodiphenylmethane curing agent and the phosphorus copper porphyrin flame retardant as described in claim 1, which are obtained by gradient thermosetting, cooling and demolding; wherein the thermosetting method includes: holding at 150°C for 2 hours, raising the temperature to 180°C and holding for 2 hours, raising the temperature to 200°C and holding for 2 hours, and naturally cooling to room temperature for demolding.
10. The application of the phosphorus-containing copper porphyrin flame retardant as described in claim 1 in the flame retardant modification of epoxy resin.