A polyester-terminated solution-polymerized styrene-butadiene rubber and its preparation method and tread compound
By introducing ester groups at the chain ends of solution-polymerized styrene-butadiene rubber (SSBR) to form hydrogen bonds with the surface of silica, and combining anionic polymerization technology with continuous polymerization, the industrialization problem of SSBR chain end modification technology has been solved, achieving low rolling resistance and high wet skid resistance in high-end tires.
Patent Information
- Application Number
- CN202611004634.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-07
- Publication Date
- 2026-11-17
AI Technical Summary
Existing solution styrene-butadiene rubber (SSBR) chain-end modification technologies are difficult to industrialize, have many side reactions, and cannot meet the performance requirements of high-end tires. In particular, their ability to bond with the surface of silica is insufficient, resulting in high rolling resistance, poor wet skid resistance and wear resistance.
Polyester-terminated solution-polymerized styrene-butadiene rubber (SBR) is used. By introducing ester groups at the chain end to form hydrogen bonds with the silanol groups on the surface of silica, combined with anionic polymerization technology, the ratio of styrene, butadiene, and polyester structural units is controlled to achieve chain end fixation and molecular weight control. Continuous polymerization is then used for large-scale production.
It reduces the number of free chain ends, decreases side reactions, improves the bonding ability between rubber and silica, enhances dispersibility, and achieves green tire performance with low rolling resistance and high wet skid resistance.
Smart Images

Figure CN123106950A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of solution-polymerized styrene-butadiene rubber (SBR), and more specifically, to a polyester-terminated solution-polymerized SBR, its preparation method, and a tread compound. Background Technology
[0002] With the rapid development of the transportation industry, especially the continuous upgrading of the comprehensive performance requirements for tires in new energy commercial vehicles and high-end passenger vehicles, solution polystyrene-butadiene rubber (SSBR), as the core substrate of tire tread, directly determines the key indicators of tires such as low rolling resistance, high wet skid resistance, and wear resistance, making it a core direction for the research and development of high-end green tires. Green tires generally use silica as a reinforcing filler. Silica has a large number of active silanol groups on its surface, while the ends of traditional solution polystyrene-butadiene rubber molecular chains lack specific functional groups, making it impossible to form an effective bond with the silica surface. This results in a large amount of internal friction at the ends of rubber molecules during the dynamic use of the tire, which not only increases tire rolling resistance and vehicle energy consumption but also reduces the wet skid resistance and wear resistance of the tread rubber, making it difficult to meet the performance requirements of high-end tires.
[0003] Anionic polymerization technology, with its characteristics of fast initiation, slow growth, and no spontaneous termination, has become an ideal technical route for the functional modification of SSBR chain ends. It allows the rubber to retain active negative ion centers after polymerization, providing a technical foundation for functional modification of rubber chain ends and possessing potential for industrial scale-up. By adding functional polar monomers at the end of polymerization, functional groups that can interact with silica are grafted onto the ends of rubber molecules, fixing the ends of rubber molecules to the silica surface, effectively reducing internal friction at the molecular ends, and is a core modification method for improving the overall performance of green tires. Currently, the mainstream directions for SSBR chain-end functionalization modification in the industry all revolve around forming chemical bonds with the silanol groups on the surface of silica. For example, by preparing epoxidative functionalization initiators, butadiene and styrene are polymerized to obtain SSBR with double-ended epoxy groups, and covalent bonds are formed by the ring-opening reaction of epoxy groups and silica silanol groups. Other studies have prepared SSBR with double-ended silylethoxy groups through anionic polymerization, and chain-end fixation is achieved by the condensation reaction of silylethoxy groups and silica silanol groups. All of these studies optimize the interfacial bonding between rubber and silica by constructing chemical bonding sites.
[0004] However, existing SSBR chain-end modification technologies still have many technical defects, making it difficult to achieve large-scale industrial applications. For example, patent CN112707994A uses epoxidation functionalization initiator modification technology. Its dedicated initiator synthesis process is complex, purity control is difficult, and production costs are high. Moreover, the industrial preparation technology of the initiator has not yet been broken through, and it is currently only at the laboratory pilot stage, which cannot meet the needs of industrial production. In addition, Dr. Liu Xiao's (2009 doctoral dissertation at Beijing University of Chemical Technology, "Molecular Structure of Energy-Saving SSBR and Design, Preparation, Structure and Performance Study of its Nano-Reinforcing Materials") describes the preparation process of SSBR modified with double-terminated silanyl ethoxy groups. In this process, anionic active species readily undergo side reactions with silanyl ethoxy groups. When the modifier reacts with the active species, while achieving chain-end grafting, a coupling effect also occurs due to the side reactions of silanyl ethoxy groups, leading to the failure of the silanyl ethoxy functional groups. This significantly reduces the subsequent bonding ability between the rubber and the silanyl hydroxyl groups on the silica surface, resulting in poor modification stability. Furthermore, patent CN119899317A uses nitrogen as an initiator for end-capping of rubber molecules, but with only one nitrogen atom at the end, it is difficult to form an effective bond with the silica surface.
[0005] Therefore, existing SSBR chain-end functionalization technologies have shortcomings such as high difficulty in industrialization and numerous side reactions during the preparation process, making it difficult to meet the performance requirements of high-end tires. Summary of the Invention
[0006] One objective of this invention is to provide a polyester-terminated solution-polymerized styrene-butadiene rubber (SBR) and its preparation method. The ester groups at the chain ends of the polyester-terminated SBR form hydrogen bonds with the silanol groups on the surface of silica. These hydrogen bonds reduce the number of free chain ends, decrease side reactions, thereby reducing hysteresis loss, inhibiting filler aggregation, and improving dispersibility, thus lowering the difficulty of industrialization. A second objective of this invention is to provide a tread compound prepared from polyester-terminated solution-polymerized SBR.
[0007] To achieve the above objectives, the present invention provides a polyester-terminated solution-polymerized styrene-butadiene rubber having the molecular structure shown in Formula I: (I) In Equation I: R1 and R2 are each independently selected from C1-C 20 Straight-chain hydrocarbon groups, C1-C 20 Branched hydrocarbon groups, C1-C containing heteroatoms 20 Straight-chain hydrocarbon groups, C1-C containing heteroatoms 20 One of the branched hydrocarbon groups; The value of 'a' makes the molecular mass of styrene structural units account for 5% to 45% of the total molecular mass; The values of b+c result in butadiene structural units accounting for 55% to 95% of the total molecular mass; The value of d makes the molecular mass of the polyester structural unit account for 0.3% to 5% of the total molecular mass.
[0008] The technical effects achieved by adopting this solution are as follows: the ester groups at the ends of the polyester-terminated solution-polymerized styrene-butadiene rubber (SBR) chain form hydrogen bonds with the silanol groups on the surface of silica, fixing the chain ends to the silica surface, reducing side reactions, and thus lowering the difficulty of industrialization. Furthermore, by controlling the proportion of structural units of styrene, butadiene, and polyester-terminated segments, a synergistic balance between processing performance, mechanical properties, and mechanical properties of the polyester-terminated solution-polymerized SBR is achieved. Specifically, R1 and R2 are each independently and preferentially C1-C5 straight-chain hydrocarbon groups or C1-C5 branched oxygen-containing hydrocarbon groups.
[0009] Furthermore, the ratio of b / (b+c) ranges from 0.3 to 0.8, where b and c represent the number of 1,2- and 1,4-structural units of butadiene in the molecule, respectively. The 1,2-structural units of butadiene contain side chains, which can increase the glass transition temperature of rubber; the 1,4-structural units of butadiene are linear chains, exhibiting good flexibility. Therefore, the control of the 1,2- and 1,4-structural units of butadiene can achieve a balance and customized design of comprehensive properties such as the glass transition temperature, rolling resistance, wet skid resistance, and abrasion resistance of rubber.
[0010] Furthermore, the molecular weight of the polyester-terminated solution-polymerized styrene-butadiene rubber (SBR) is 200,000 to 400,000; the molecular weight distribution of the polyester-terminated solution-polymerized SBR is 1.0 to 3.0. Silica filler exhibits good dispersion in this polyester-terminated solution-polymerized SBR; the surface of silica has a strong bonding ability with this polyester-terminated solution-polymerized SBR. The prepared tread compound has high tensile strength, high rolling resistance, and good wet skid resistance, resulting in a longer tire service life.
[0011] This invention also provides a method for preparing polyester-terminated solution-polymerized styrene-butadiene rubber, specifically comprising: S10. Under anhydrous and oxygen-free conditions, butadiene monomer, styrene monomer, and initiator are added to a solvent to carry out a polymerization reaction to obtain a polymerization reaction solution. S20. Add an end-capping modifier to the polymerization reaction solution to carry out the end-capping reaction, and obtain a solution of solution-polymerized styrene-butadiene rubber with active polyester end-capping modification; S30. Add a terminating agent to the solution polymerized styrene-butadiene rubber solution modified with active polyester end-capping to obtain a solution polymerized styrene-butadiene rubber solution modified with polyester end-capping. S40. After desolventizing and drying the polyester-terminated solution-polymerized styrene-butadiene rubber solution, polyester-terminated solution-polymerized styrene-butadiene rubber is obtained. The end-capping modifier has the molecular structure shown in Formula II: (II) In Equation II: R1 and R2 are each independently selected from C1-C 20 Straight-chain hydrocarbon groups, C1-C 20 Branched hydrocarbon groups, C1-C containing heteroatoms 20 Straight-chain hydrocarbon groups, C1-C containing heteroatoms 20 One of the branched hydrocarbon groups.
[0012] The technical effects achieved by adopting this solution are as follows: Butadiene-styrene copolymer chains are synthesized via active anionic polymerization under anhydrous and oxygen-free conditions. Polyester groups are then introduced at the ends of the active chains using end-capping modifiers. Following termination, desolventizing, and drying treatments, a functionalized solution-polymerized styrene-butadiene rubber product is finally obtained. The strong polarity of the polyester end groups enhances the chemical bonding and dispersion uniformity between the rubber and polar fillers such as silica, thereby improving the mechanical and dynamic properties of the tread rubber. Furthermore, this preparation process is simple, requiring no complex post-modification steps, and is suitable for large-scale continuous production.
[0013] Furthermore, in step S10, a polarity modifier and an activator are added; wherein the polarity modifier includes at least one of tetrahydrofurfuryl ethyl ether, furfuryl propane, ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, N,N,N',N'-tetramethylethylenediamine, pentamethyldiethylenetriamine, and triethylamine; and the activator includes at least one of tetrahydrofuran, diethyl ether, and tetrahydropyran.
[0014] The technical effects achieved by adopting this technical solution are as follows: The purpose of the regulator is to control the random copolymerization of butadiene and styrene monomers and to achieve a highly consistent distribution of styrene-butadiene in each copolymer chain; the purpose of the activator is to improve the reactivity of the initiator and to achieve near-synchronous initiation and growth of molecular chains.
[0015] Furthermore, the polymerization reaction is anionic solution polymerization technology, the polymerization temperature is 20℃~90℃, the polymerization time is 30min~100min, and the polymerization pressure is 0.4MPa~0.6MPa.
[0016] The technical effects achieved by adopting this solution are as follows: By controlling the polymerization temperature between 20℃ and 90℃, the balance between 1,2-addition and 1,4-addition during butadiene chain growth is ensured, preventing deviation due to temperature fluctuations; by controlling the polymerization time between 30min and 100min, a high conversion rate of over 95% is ensured in the polymerization reaction; and by controlling the polymerization pressure between 0.4MPa and 0.6MPa, the stability and homogeneity of the liquid-phase polymerization system are guaranteed, while avoiding equipment investment and safety hazards caused by excessive pressure, ensuring that the polymerization system remains in a homogeneous and stable reaction state.
[0017] Further, the solvent includes at least one of cyclohexane, n-hexane, cyclopentane, n-heptane, benzene, toluene, and ethylbenzene; and / or the terminator includes at least one of phenol, methanol, ethanol, o-methylphenol, and p-methylphenol; and / or the initiator includes at least one of n-butyllithium and sec-butyllithium.
[0018] The technical effects achieved by adopting this solution are as follows: The solvent selected is at least one of cyclohexane, n-hexane, cyclopentane, n-heptane, benzene, toluene, and ethylbenzene. These solvents are all non-polar or weakly polar hydrocarbon solvents, exhibiting good compatibility with butadiene and styrene monomers, as well as solution-polymerized styrene-butadiene rubber. They do not participate in anionic polymerization reactions, providing a stable reaction environment for the active chain ends, and each solvent has a moderate boiling point. This facilitates efficient recovery through distillation or vaporization in subsequent solvent removal processes, combining process safety and economy. The terminator is at least one of phenol, methanol, ethanol, o-methylphenol, and p-methylphenol. The active hydrogen in the terminator can rapidly undergo a protonation reaction with the active carbon anion, instantly terminating chain growth and completely deactivating all residual active centers, thus inactivating the anionic active species. The initiator is at least one of n-butyllithium or sec-butyllithium. n-Butyllithium and sec-butyllithium have good solubility in non-polar solvents, rapid initiation speed, and controllable quantitative distribution, allowing for precise calculation of the target molecular weight based on their dosage.
[0019] Furthermore, the temperature of the end-capping reaction is -70℃ to 40℃, the time of the end-capping reaction is 1h to 3h, and the pressure of the end-capping reaction is 0.4MPa to 0.6MPa.
[0020] The technical effects achieved by adopting this solution are as follows: Because end-capping agents are prone to side reactions at high temperatures, leading to the deactivation of anionic active species, controlling the end-capping temperature between -70℃ and 40℃ effectively inhibits non-target side reactions between the ester groups and the active chain ends in the end-capping agent; controlling the end-capping time between 1h and 3h ensures an end-capping rate of over 90%; and controlling the end-capping pressure between 0.4MPa and 0.6MPa ensures the stability and homogeneity of the liquid-phase polymerization system while avoiding equipment investment and safety hazards caused by excessive pressure, keeping the polymerization system in a homogeneous and stable reaction state.
[0021] Furthermore, the preparation method of polyester-terminated solution-polymerized styrene-butadiene rubber adopts a continuous polymerization method, wherein the continuous polymerization method is carried out by a reactor group of 2 to 5 reactors connected in series.
[0022] The technical effects achieved by adopting this technical solution are as follows: By using a continuous polymerization method with 2 to 5 reactors connected in series, each reactor has an independently set temperature, and the initiation, growth, end-capping, and termination steps are spatially separated. This effectively avoids the accumulation of temperature rise and local overheating caused by the exothermic polymerization in a single reactor, and realizes the staged control and continuous production of the polymerization process, providing a stable and controllable process path for large-scale continuous industrial production.
[0023] The present invention also provides a tread compound, wherein the raw material of the tread compound includes polyester-terminated solution-polymerized styrene-butadiene rubber as described above, or polyester-terminated solution-polymerized styrene-butadiene rubber prepared by the preparation method of polyester-terminated solution-polymerized styrene-butadiene rubber as described above.
[0024] The technical effects achieved by adopting this technical solution are as follows: The tread compound uses polyester-terminated solution-polymerized styrene-butadiene rubber and silica as core raw materials. The polyester groups at the chain ends can form strong hydrogen bonds with the silanol groups on the surface of silica, which effectively inhibits the agglomeration of silica during mixing and vulcanization, and enables it to be uniformly dispersed in polyester-terminated solution-polymerized styrene-butadiene rubber, thereby achieving a green tire with low rolling resistance and high wet skid resistance. Attached Figure Description
[0025] The above and / or additional aspects and advantages of the present invention will become apparent and readily understood from the description of the embodiments taken in conjunction with the following drawings, in which: Figure 1 The polymerization reaction mechanism is described in the embodiments of this application; Figure 2 The end-capping reaction mechanism is described in the embodiments of this application. Detailed Implementation
[0026] To make the above-mentioned objectives, features, and advantages of the present invention more apparent and understandable, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0027] Embodiments of the present invention provide a polyester-terminated solution-polymerized styrene-butadiene rubber having a molecular structure as shown in Formula I: (I) In Equation I: R1 and R2 are each independently selected from C1-C 20 Straight-chain hydrocarbon groups, C1-C 20 Branched hydrocarbon groups, C1-C containing heteroatoms 20 Straight-chain hydrocarbon groups, C1-C containing heteroatoms 20One of the branched hydrocarbon groups; wherein the heteroatom is selected from one or more of oxygen, nitrogen, phosphorus and silicon.
[0028] The value of 'a' makes the molecular mass of styrene structural units account for 5% to 45% of the total molecular mass; The values of b+c result in butadiene structural units accounting for 55% to 95% of the total molecular mass; The value of d results in the molecular weight of the polyester structural unit accounting for 0.3% to 5% of the total molecular weight; a represents the number of styrene structural units in the molecule; b and c represent the number of 1,2- and 1,4- structural units of butadiene in the molecule, respectively; d represents the number of polyester structural units formed by the end-capping modifier in the molecule. Generally, the content of the modifier should not be too high, as too much will lead to a decrease in material performance.
[0029] Preferably, R1 and R2 are each independently selected from C1-C5 straight-chain hydrocarbon groups or C1-C5 branched oxygen-containing hydrocarbon groups, the molecular weight of the styrene structural unit accounts for 15-30% of the total molecular weight, the molecular weight of the butadiene structural unit accounts for 70-85% of the total molecular weight, and the molecular weight of the polyester structural unit accounts for 0.3-5% of the total molecular weight.
[0030] The ester groups at the chain ends of polyester-terminated solution-polymerized styrene-butadiene rubber (SBR) can form strong hydrogen bonds with the silanol groups on the surface of silica. These hydrogen bonds reduce the number of free chain ends, thereby reducing hysteresis loss, inhibiting filler aggregation, and improving dispersibility. Furthermore, by controlling the proportion of styrene, butadiene, and polyester-terminated chain segments in the structural units, a synergistic balance between processing properties, mechanical properties, and performance characteristics of polyester-terminated solution-polymerized SBR was achieved.
[0031] In some embodiments of this application, the ratio of b / (b+c) is between 0.3 and 0.8, where b and c are the quantities of 1,2- and 1,4-structural units of butadiene in the molecule, respectively. The 1,2-structural units of butadiene contain side chains, which can increase the glass transition temperature of rubber; the 1,4-structural units of butadiene are linear chains, exhibiting good flexibility. Therefore, the regulation of the 1,2- and 1,4-structural units of butadiene can achieve a balance and customized design of comprehensive properties such as the glass transition temperature, rolling resistance, wet slip resistance, and abrasion resistance of rubber. Preferably, the ratio of b / (b+c) is between 0.45 and 0.75.
[0032] In some embodiments of this application, the molecular weight of the polyester-terminated solution-polymerized styrene-butadiene rubber (SBR) is 200,000 to 400,000; the molecular weight distribution of the polyester-terminated solution-polymerized SBR is 1.0 to 3.0. Silica filler has a good dispersion effect in this polyester-terminated solution-polymerized SBR; the surface of silica has a strong bonding ability with the polyester-terminated solution-polymerized SBR. The prepared tread rubber has high tensile strength, high rolling resistance, and good wet skid resistance, resulting in a longer tire service life. Preferably, the molecular weight of the polyester-terminated solution-polymerized SBR is 250,000 to 350,000; the molecular weight distribution of the polyester-terminated solution-polymerized SBR is 1.05 to 2.3.
[0033] Embodiments of the present invention also provide a method for preparing polyester-terminated solution-polymerized styrene-butadiene rubber, specifically comprising: S10. Under anhydrous and oxygen-free conditions, butadiene monomer, styrene monomer, and initiator are added to a solvent to carry out a polymerization reaction, yielding a polymerization reaction solution; the polymerization reaction mechanism is as follows: Figure 1 As shown; S20. Add an end-capping modifier to the polymerization reaction solution to carry out the end-capping reaction, obtaining an active polyester end-capped styrene-butadiene rubber solution; the end-capping reaction mechanism is as follows: Figure 2 As shown; S30. Add a terminating agent to the solution polymerized styrene-butadiene rubber solution modified with active polyester end-capping to obtain a solution polymerized styrene-butadiene rubber solution modified with polyester end-capping. S40. After desolventizing and drying the polyester-terminated solution-polymerized styrene-butadiene rubber solution, polyester-terminated solution-polymerized styrene-butadiene rubber is obtained. The end-capping modifier has the molecular structure shown in Formula II: (II) In Equation II: R1 and R2 are each independently selected from C1-C 20 Straight-chain hydrocarbon groups, C1-C 20 Branched hydrocarbon groups, C1-C containing heteroatoms 20 Straight-chain hydrocarbon groups, C1-C containing heteroatoms 20 One of the branched hydrocarbon groups. Preferably, R1 and R2 are each independently selected from C1-C5 straight-chain hydrocarbon groups or C1-C5 branched oxygen-containing hydrocarbon groups. The heteroatom is selected from one or more of oxygen, nitrogen, phosphorus and silicon.
[0034] In the preparation of a polyester-terminated solution-polymerized styrene-butadiene rubber (SBR), butadiene-styrene copolymer chains are synthesized by active anionic polymerization under anhydrous and oxygen-free conditions. Polyester groups are then introduced at the ends of the active chains using a terminator. Following termination, desolventizing, and drying, a functionalized modified SBR product is obtained. The strong polarity of the polyester end groups enhances the chemical bonding and dispersion uniformity between the rubber and polar fillers such as silica, thereby improving the mechanical and dynamic properties of the tread rubber. Furthermore, this preparation process is simple, requiring no complex post-modification steps, and is suitable for large-scale continuous production. Anhydrous and oxygen-free conditions are achieved by introducing nitrogen or argon gas as a protective gas into the reaction system.
[0035] Before the end-capping modifier participates in the reaction, it is soaked in molecular sieve. The main purpose of soaking the molecular sieve is to remove water molecules. Since water easily forms hydrogen bonds with the end-capping modifier, the molecular sieve soaking time is relatively long so that the water can be fully removed.
[0036] In some embodiments of this application, a polarity modifier and an activator are added in step S10. The polarity modifier includes at least one of tetrahydrofurfuryl ethyl ether, furfuryl propane, ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, N,N,N',N'-tetramethylethylenediamine, pentamethyldiethylenetriamine, and triethylamine. The activator includes at least one of tetrahydrofuran, diethyl ether, and tetrahydropyran. The purpose of the modifier is to control the random copolymerization of butadiene and styrene monomers, achieving a highly consistent styrene-butadiene distribution in each copolymer chain. The purpose of the activator is to enhance the reactivity of the initiator, achieving near-synchronous initiation and growth of the molecular chains. The amount of modifier used is 50 ppm to 500 ppm; preferably, the amount of modifier used is 100 ppm to 200 ppm.
[0037] In some embodiments of this application, the polymerization reaction is anionic solution polymerization, the polymerization temperature is 20℃~90℃, the polymerization time is 30min~100min, and the polymerization pressure is 0.4MPa~0.6MPa. By controlling the polymerization temperature at 20℃~90℃, the balance between 1,2-addition and 1,4-addition during butadiene chain growth is ensured, preventing shifts due to temperature fluctuations. By controlling the polymerization time at 30min~100min, a high conversion rate of over 95% is ensured. By controlling the polymerization pressure at 0.4MPa~0.6MPa, the stability and homogeneity of the liquid-phase polymerization system are guaranteed, while avoiding equipment investment and safety hazards caused by excessive pressure, ensuring the polymerization system remains in a homogeneous and stable reaction state. Preferably, the polymerization temperature is 35℃-60℃.
[0038] In some embodiments of this application, the solvent includes at least one selected from cyclohexane, n-hexane, cyclopentane, n-heptane, benzene, toluene, and ethylbenzene; and / or the terminator is phenol; and / or the initiator includes at least one selected from n-butyllithium and sec-butyllithium. The solvents selected are at least one selected from cyclohexane, n-hexane, cyclopentane, n-heptane, benzene, toluene, and ethylbenzene. These solvents are all non-polar or weakly polar hydrocarbon solvents, which have good compatibility with butadiene and styrene monomers and solution-polymerized styrene-butadiene rubber. They do not participate in anionic polymerization reactions, can provide a stable reaction environment for the active chain ends, and each solvent has a moderate boiling point. This design facilitates efficient recovery via distillation or steam purification in subsequent solvent removal processes, combining process safety and economy. The terminator includes at least one of phenol, methanol, ethanol, o-methylphenol, and p-methylphenol. The active hydrogen in the terminator rapidly protonates the activated carbon anion, instantly terminating chain growth and completely deactivating all residual active centers, thus inactivating the anionic active species. The initiator is at least one of n-butyllithium or sec-butyllithium. Both n-butyllithium and sec-butyllithium exhibit good solubility in non-polar solvents, rapid initiation, and controllable quantitative initiation, allowing for precise calculation of the target molecular weight based on their dosage. Preferably, the solvent is one or two of cyclohexane, cyclopentane, benzene, and toluene; the modifier is tetrahydrofurfuryl ethyl ether or furfuryl propane.
[0039] In some embodiments of this application, the end-capping reaction temperature is -70℃ to 40℃, the end-capping reaction time is 1h to 3h, and the end-capping reaction pressure is 0.4MPa to 0.6MPa. Since the end-capping agent is prone to side reactions at higher temperatures, leading to the deactivation of anionic active species, controlling the end-capping temperature at -70℃ to 40℃ effectively suppresses non-target side reactions between the ester groups and the active chain ends in the end-capping agent. Controlling the end-capping time to 1h to 3h ensures an end-capping rate of over 90%. Controlling the end-capping pressure to 0.4MPa to 0.6MPa ensures the stability and homogeneity of the liquid-phase polymerization system while avoiding equipment investment and safety hazards caused by excessive pressure, keeping the polymerization system in a homogeneous and stable reaction state. Preferably, the end-capping temperature is -70℃ to 0℃.
[0040] In some embodiments of this application, the preparation method of polyester-terminated solution-polymerized styrene-butadiene rubber employs a continuous polymerization method, wherein the continuous polymerization is carried out using a reactor group of 2 to 5 reactors connected in series. By using a continuous polymerization method with 2 to 5 reactors connected in series, each reactor has its own independently set temperature, and the initiation, growth, termination, and other steps are spatially separated. This effectively avoids the accumulation of temperature rise and local overheating caused by the exothermic polymerization within a single reactor, achieving staged control and continuous production of the polymerization process, and providing a stable and controllable process path for large-scale industrial continuous production. Preferably, three-reactor and four-reactor continuous polymerization are used.
[0041] Embodiments of the present invention also provide a tread compound, the raw materials of which include polyester-terminated solution-polymerized styrene-butadiene rubber as described above, or polyester-terminated solution-polymerized styrene-butadiene rubber prepared by the preparation method of polyester-terminated solution-polymerized styrene-butadiene rubber as described above. This tread compound uses polyester-terminated solution-polymerized styrene-butadiene rubber and silica as core raw materials. The polyester groups at the chain ends can form strong hydrogen bonds with the silanol groups on the surface of silica, effectively inhibiting the agglomeration of silica during mixing and vulcanization, allowing it to be uniformly dispersed in the polyester-terminated solution-polymerized styrene-butadiene rubber, thereby achieving a green tire with low rolling resistance and high wet skid resistance.
[0042] Example 1 Example 1 provides a method for preparing polyester-terminated solution-polymerized styrene-butadiene rubber, employing a four-reactor continuous polymerization process. Styrene and butadiene copolymerization is completed in the first and second reactors, the end-capping reaction is completed in the third reactor, and the termination reaction is completed in the fourth reactor. The specific steps include: S1. Under a nitrogen atmosphere, under anhydrous and oxygen-free conditions, add 6L of toluene solvent to a 10L reactor; then add 150g of styrene monomer, 140ppm of polarity modifier bis(tetrahydrofuran)propane and 100ppm of activator tetrahydrofuran to the reactor; add 450g of butadiene monomer and raise the temperature of the reactor to 40℃. S2. Add 5 mL of butyllithium (concentration of 0.6 mol / L) to the reactor to initiate the copolymerization of styrene monomer and butadiene monomer. During the polymerization process, a large amount of heat is released, which raises the temperature of the reactor. Circulating water is used to control the temperature of the reactor to be maintained within the range of 35℃~65℃. The reaction time is 50 min. The pressure inside the reactor is maintained at 0.4 MPa~0.6 MPa to obtain the polymerization reaction solution. S3. The polymerization reaction solution is transferred to the third reactor, which is cooled rapidly to -40°C using liquid nitrogen. 18 g of methyl methacrylate monomer that has been soaked in molecular sieves for one week is added to carry out the end-capping reaction for 2 hours. The temperature of the third reactor is maintained between -40°C and -30°C. The pressure inside the third reactor is maintained between 0.4 MPa and 0.6 MPa to obtain a solution of solution-polymerized styrene-butadiene rubber modified with active polyester end-capping. S4. Transfer the solution polymerized styrene-butadiene rubber solution modified with active polyester end capping to the fourth reactor, add phenol terminator to the fourth reactor to deactivate the anionic activity, and obtain the solution polymerized styrene-butadiene rubber solution modified with polyester end capping. S5. The solution polymerized styrene-butadiene rubber (SBR) with polyester end-capping is slowly poured into methanol. After phase separation precipitation and solvent removal, and drying in a vacuum oven, the polyester end-capped SBR is obtained.
[0043] Example 2 Example 2 provides a method for preparing polyester-terminated solution-polymerized styrene-butadiene rubber, employing a four-reactor continuous polymerization process. Styrene and butadiene copolymerization is completed in the first and second reactors, the end-capping reaction is completed in the third reactor, and the termination reaction is completed in the fourth reactor. The specific steps include: S1. Under nitrogen atmosphere and in an anhydrous and oxygen-free condition, add 6L of toluene solvent to a 10L reactor; then add 30g of styrene monomer, 130ppm of polarity modifier bis(tetrahydrofuran)propane and 100ppm of activator tetrahydrofuran to the reactor; add 570g of butadiene monomer and raise the temperature of the reactor to 20.2℃. S2. Add 6 mL of butyllithium (concentration of 0.6 mol / L) to the reactor to initiate the copolymerization of styrene monomer and butadiene monomer. During the polymerization process, a large amount of heat is released, which raises the temperature of the reactor. Circulating water is used to control the temperature of the reactor to be maintained within the range of 20℃~65℃. The reaction time is 100 min. The pressure inside the reactor is maintained at 0.4 MPa~0.6 MPa to obtain the polymerization reaction solution. S3. The polymerization reaction solution is transferred to the third reactor, which is cooled rapidly to -69.4°C using liquid nitrogen. 2 grams of methyl methacrylate monomer that has been soaked in molecular sieves for one week are added to carry out the end-capping reaction for 2 hours. The temperature of the third reactor is maintained between -70°C and -50°C. The pressure inside the third reactor is maintained between 0.4 MPa and 0.6 MPa to obtain a solution of active polyester end-capped modified styrene-butadiene rubber. S4. Transfer the solution polymerized styrene-butadiene rubber solution modified with active polyester end capping to the fourth reactor, add phenol terminator to the fourth reactor to deactivate the anionic activity, and obtain the solution polymerized styrene-butadiene rubber solution modified with polyester end capping. S5. The solution polymerized styrene-butadiene rubber (SBR) with polyester end-capping is slowly poured into methanol. After phase separation precipitation and solvent removal, and drying in a vacuum oven, the polyester end-capped SBR is obtained.
[0044] Example 3 Example 3 provides a method for preparing polyester-terminated solution-polymerized styrene-butadiene rubber, employing a four-reactor continuous polymerization process. Styrene and butadiene copolymerization is completed in the first and second reactors, the end-capping reaction is completed in the third reactor, and the termination reaction is completed in the fourth reactor. The specific steps include: S1. Under a nitrogen atmosphere and in an anhydrous and oxygen-free environment, add 6 L of cyclohexane solvent to a 10 L reactor; then add 270 g of styrene monomer, 370 ppm of polarity modifier N,N,N',N'-tetramethylethylenediamine and 100 ppm of activator tetrahydrofuran; add 330 g of butadiene monomer, and raise the temperature of the reactor to 89.6 °C. S2. Add 4.2 mL of butyllithium (concentration of 0.6 mol / L) to the reactor to initiate the copolymerization of styrene monomer and butadiene monomer. During the polymerization process, a large amount of heat is released, which raises the temperature of the reactor. Circulating water is used to control the temperature of the reactor to be maintained within the range of 85℃~110℃. The reaction time is 30 min. The pressure inside the reactor is maintained at 0.4 MPa~0.6 MPa to obtain the polymerization reaction solution. S3. The polymerization reaction solution is transferred to the third reactor, which is cooled rapidly to 39.5°C using liquid nitrogen. 30 g of methyl methacrylate monomer that has been soaked in molecular sieves for one week is added to carry out the end-capping reaction for 2 h. The temperature of the third reactor is maintained between 30°C and 50°C. The pressure inside the third reactor is maintained between 0.4 MPa and 0.6 MPa to obtain a solution of active polyester end-capped modified styrene-butadiene rubber. S4. Transfer the solution polymerized styrene-butadiene rubber solution modified with active polyester end capping to the fourth reactor, add phenol terminator to the fourth reactor to deactivate the anionic activity, and obtain the solution polymerized styrene-butadiene rubber solution modified with polyester end capping. S5. The solution polymerized styrene-butadiene rubber (SBR) with polyester end-capping is slowly poured into methanol. After phase separation precipitation and solvent removal, and drying in a vacuum oven, the polyester end-capped SBR is obtained.
[0045] Example 4 Example 4 provides a method for preparing polyester-terminated solution-polymerized styrene-butadiene rubber, employing a four-reactor continuous polymerization process. Styrene and butadiene copolymerization is completed in the first and second reactors, the end-capping reaction is completed in the third reactor, and the termination reaction is completed in the fourth reactor. The specific steps include: S1. Under a nitrogen atmosphere and in an anhydrous and oxygen-free environment, add a mixed solvent of 3L xylene and 3L n-pentane to a 10L reactor; then add 150g styrene monomer, 110ppm pentamethyldiethylenetriamine (a polarity modifier), and 100ppm tetrahydrofuran (an activator) to the reactor; add 450g butadiene monomer and raise the temperature of the reactor to 55°C. S2. Add 5 mL of butyllithium (concentration of 0.6 mol / L) to the reactor to initiate the copolymerization of styrene monomer and butadiene monomer. During the polymerization process, a large amount of heat is released, which raises the temperature of the reactor. Circulating water is used to control the temperature of the reactor to be maintained within the range of 55℃~80℃. The reaction time is 50 min. The pressure inside the reactor is maintained at 0.4 MPa~0.6 MPa to obtain the polymerization reaction solution. S3. The polymerization reaction solution is transferred to the third reactor, which is cooled rapidly to -20°C using liquid nitrogen. 18 g of methyl methacrylate monomer that has been soaked in molecular sieves for one week is added to carry out the end-capping reaction for 2 hours. The temperature of the third reactor is maintained between -30°C and -10°C. The pressure inside the third reactor is maintained between 0.4 MPa and 0.6 MPa to obtain a solution of solution-polymerized styrene-butadiene rubber modified with active polyester end-capping. S4. Transfer the solution polymerized styrene-butadiene rubber solution modified with active polyester end capping to the fourth reactor, add phenol terminator to the fourth reactor to deactivate the anionic activity, and obtain the solution polymerized styrene-butadiene rubber solution modified with polyester end capping. S5. The solution polymerized styrene-butadiene rubber (SBR) with polyester end-capping is slowly poured into methanol. After phase separation precipitation and solvent removal, and drying in a vacuum oven, the polyester end-capped SBR is obtained.
[0046] Example 5 Example 1 provides a method for preparing polyester-terminated solution-polymerized styrene-butadiene rubber, employing a four-reactor continuous polymerization process. Styrene and butadiene copolymerization is completed in the first and second reactors, the end-capping reaction is completed in the third reactor, and the termination reaction is completed in the fourth reactor. The specific steps include: S1. Under a nitrogen atmosphere and in an anhydrous and oxygen-free environment, add a mixed solvent of 4.8 L cyclohexane and 1.2 L n-hexane to a 10 L reactor; then add 150 g of styrene monomer, 230 ppm of polarity modifier diethylene glycol dimethyl ether, and 100 ppm of activator tetrahydrofuran; add 450 g of butadiene monomer, and raise the temperature of the reactor to 40 °C. S2. Add 5 mL of butyllithium (concentration of 0.6 mol / L) to the reactor to initiate the copolymerization of styrene monomer and butadiene monomer. During the polymerization process, a large amount of heat is released, which raises the temperature of the reactor. Circulating water is used to control the temperature of the reactor to be maintained within the range of 35℃~65℃. The reaction time is 50 min. The pressure inside the reactor is maintained at 0.4 MPa~0.6 MPa to obtain the polymerization reaction solution. S3. The polymerization reaction solution is transferred to the third reactor, which is cooled rapidly to 10°C using liquid nitrogen. 18 g of methyl methacrylate monomer that has been soaked in molecular sieves for one week is added to carry out the end-capping reaction for 2 hours. The temperature of the third reactor is maintained between 0°C and 20°C. The pressure inside the third reactor is maintained between 0.4 MPa and 0.6 MPa to obtain a solution of active polyester end-capped modified styrene-butadiene rubber. S4. Transfer the solution polymerized styrene-butadiene rubber solution modified with active polyester end capping to the fourth reactor, add phenol terminator to the fourth reactor to deactivate the anionic activity, and obtain the solution polymerized styrene-butadiene rubber solution modified with polyester end capping. S5. The solution polymerized styrene-butadiene rubber (SBR) with polyester end-capping is slowly poured into methanol. After phase separation precipitation and solvent removal, and drying in a vacuum oven, the polyester end-capped SBR is obtained.
[0047] The obtained polyester-terminated solution-polymerized styrene-butadiene rubber was subjected to structural analysis using NMR and GPC. The main analyses included styrene content, butadiene content, acrylate content, butadiene 1,2-structure content, molecular weight, and their distribution, as shown in Table 1.
[0048] The solution-polymerized styrene-butadiene rubber of Comparative Example 1 was not end-capped; the solution-polymerized styrene-butadiene rubber of Comparative Example 2 was commercial SSBR2550.
[0049] Table 1. Performance characterization results of polyester-terminated solution-polymerized styrene-butadiene rubber The present invention also describes the preparation of tire tread compounds by compounding and vulcanizing the solution-polymerized styrene-butadiene rubbers of Examples 1-5 and Comparative Examples 1-2. The method for preparing the tread compounds is as follows: Set the temperature of the Hack internal mixer to 55°C and the speed to 50 rpm. First, put SSBR and environmentally friendly aromatic oil into the mold cavity and mix for 2 minutes. Then, add silica to the internal mixer mold cavity in four batches. Then, add the remaining silica, stearic acid, zinc oxide, antioxidant, and coupling agent into the internal mixer and mix for 5 minutes to ensure thorough mixing. Heat the Hack internal mixer to 150°C and adjust the speed to 25 rpm to heat-treat the compound for 5 minutes. Discharge the compound and cool it to room temperature. Finally, sulfur and accelerator were added to the rubber compound on a two-roll mill, and the compound was sheeted nine times to ensure thorough mixing of the components. The rubber compound samples were then tested using a rotorless vulcanizer to obtain vulcanization curves. The optimal vulcanization time for each sample was determined from these curves. Finally, tread rubber performance test samples were prepared using different molds.
[0050] Examples 6-10 are tread compounds compounded with solution-polymerized styrene-butadiene rubber (SBR) modified with polyester end-capping as described in Examples 1-5 of this invention; Comparative Example 3 is a tread compound compounded with solution-polymerized SBR without end-capping modification; Comparative Example 4 is a tread compound compounded with commercially available SSBR2550; the compounding formulations of Examples 6-10 and Comparative Examples 3-4 are shown in Table 2. The performance characterization results of Examples 6-10 and Comparative Examples 3-4 are shown in Table 3. Since commercially available SSBR2550 is an oil-extended SSBR, consistent with the addition of 26 grams of aromatic oil in Comparative Examples 3 and 3, no further aromatic oil was added during compounding.
[0051] Table 2. Compound formulations for Examples 6-10, Comparative Examples 3, and Comparative Example 4 Table 3 Performance characterization results of Example 2, Comparative Example 3, and Comparative Example 4 The Payne effect reflects the dispersion effect of silica filler in the rubber matrix; the smaller the value, the better the dispersion effect. The Payne effect values of Examples 6-10 are significantly lower than those of Comparative Examples 3 and 4, indicating that the filler dispersion effect of polyester-terminated solution-polymerized styrene-butadiene rubber is significantly improved.
[0052] The reinforcing factor is the ratio of 300 constant elongation to 100 constant elongation. It reflects the bonding ability between the rubber and the silica surface. The larger the reinforcing factor, the stronger the bonding ability. The reinforcing factors of Examples 6-10 are higher than those of Comparative Examples 3 and 4, indicating that the polyester-terminated solution-polymerized styrene-butadiene rubber has a stronger bonding ability with silica.
[0053] The higher the tensile strength, the stronger the tread compound's adaptability to harsh environments, indicating that the tread compound prepared from polyester-terminated solution-polymerized styrene-butadiene rubber has a stronger adaptability to harsh environments.
[0054] Compression heat generation is a method for characterizing rolling resistance. It simulates the dynamic deformation of the tire during use, which causes internal friction in the material (internal friction is the cause of rolling resistance), resulting in an increase in material temperature. The higher the compression heat generation temperature, the greater the rolling resistance. The compression heat generation values of Examples 6-10 are significantly lower than those of Comparative Examples 3 and 4, indicating that the tread rubber prepared by polyester end-capped solution-polymerized styrene-butadiene rubber has lower rolling resistance.
[0055] The loss factor at 5.0℃ reflects the wet skid resistance of the tread compound. A higher loss factor at low temperatures indicates stronger molecular mobility and better wet skid resistance. This suggests that the tread compound prepared from polyester-terminated solution-polymerized styrene-butadiene rubber exhibits the best wet skid resistance.
[0056] Akron wear is a core indicator of tire performance, and wear performance directly affects tire lifespan. Lower tire wear generally indicates a longer tire lifespan. This suggests that the tread compound prepared from polyester-terminated solution-polymerized styrene-butadiene rubber has a longer lifespan.
[0057] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them; although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A polyester-terminated, solution-polymerized styrene-butadiene rubber characterized in that, The polyester-terminated solution-polymerized styrene-butadiene rubber has the molecular structure shown in Formula I: (Ⅰ) In formula I: R1, R2are each independently selected from one of a linear hydrocarbon group C1-C 20 alkyl, a branched hydrocarbon group C1-C 20 alkyl, a branched hydrocarbon group C1-C 20 alkyl, a branched hydrocarbon group C1-C 20 alkyl, a branched hydrocarbon group C1-C The value of 'a' makes the molecular mass of styrene structural units account for 5% to 45% of the total molecular mass; The values of b+c result in butadiene structural units accounting for 55% to 95% of the total molecular mass; The value of d makes the molecular mass of the polyester structural unit account for 0.3% to 5% of the total molecular mass.
2. The polyester-terminated solution-polymerized styrene-butadiene rubber according to claim 1, characterized in that, b / (b+c) is between 0.3 and 0.
8.
3. The polyester-terminated solution-polymerized styrene-butadiene rubber according to claim 1, characterized in that, The molecular weight of the polyester-terminated solution-polymerized styrene-butadiene rubber is 200,000 to 400,000. The molecular weight distribution of the polyester-terminated solution-polymerized styrene-butadiene rubber is in the range of 1.0 to 3.
0.
4. A process for the preparation of a polyester-terminated solution-polymerized styrene-butadiene rubber, characterized in that The preparation method specifically includes: S10. Under anhydrous and oxygen-free conditions, butadiene monomer, styrene monomer, and initiator are added to a solvent to carry out a polymerization reaction to obtain a polymerization reaction solution. S20. Add an end-capping modifier to the polymerization reaction solution to carry out an end-capping reaction, and obtain a solution of solution-polymerized styrene-butadiene rubber with active polyester end-capping modification; S30. Add a terminating agent to the solution polymerized styrene-butadiene rubber solution modified with active polyester end-capping to obtain a solution polymerized styrene-butadiene rubber solution modified with polyester end-capping. S40. After desolventizing and drying the polyester-terminated solution-polymerized styrene-butadiene rubber solution, polyester-terminated solution-polymerized styrene-butadiene rubber is obtained. The end-capping modifier has the molecular structure shown in Formula II: (Ⅱ) In formula II: R1, R2are each independently selected from one of a linear hydrocarbon group C1-C 20 a branched hydrocarbon group C1-C 20 a branched hydrocarbon group C1-C 20 a branched hydrocarbon group C1-C 20 a branched hydrocarbon group C1-C 5. The production method according to claim 4, characterized by, In step S10, a polarity modifier and an activator are added; The polarity modifier includes at least one of tetrahydrofurfuryl ethyl ether, furfuryl propane, ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, N,N,N',N'-tetramethylethylenediamine, pentamethyldiethylenetriamine, and triethylamine. The activator includes at least one of tetrahydrofuran, diethyl ether, and tetrahydropyran.
6. The preparation method according to claim 4, characterized in that, The polymerization reaction is anionic solution polymerization, the polymerization temperature is 20℃~90℃, the polymerization time is 30min~100min, and the polymerization pressure is 0.4MPa~0.6MPa.
7. The preparation method according to claim 4, characterized in that, The solvent includes at least one selected from cyclohexane, n-hexane, cyclopentane, n-heptane, benzene, toluene, and ethylbenzene; and / or The terminator includes at least one of phenol, methanol, ethanol, o-methylphenol, and p-methylphenol; and / or The initiator includes at least one of n-butyllithium and sec-butyllithium.
8. The preparation method according to claim 4, characterized in that, The end-capping reaction temperature is -70℃ to 40℃, the end-capping reaction time is 1h to 3h, and the end-capping reaction pressure is 0.4MPa to 0.6MPa.
9. The preparation method according to claim 4, characterized in that, The preparation method employs a continuous polymerization method, which uses a reactor group consisting of 2 to 5 reactors connected in series.
10. A tread compound, characterized in that: The raw materials include polyester-terminated solution-polymerized styrene-butadiene rubber according to any one of claims 1 to 3, or the raw materials include polyester-terminated solution-polymerized styrene-butadiene rubber prepared by the preparation method according to any one of claims 4 to 9.
Citation Information
Patent Citations
Double-end multifunctional solution polymerized styrene-butadiene rubber, composite material of double-end multifunctional solution polymerized styrene-butadiene rubber and white carbon black, and preparation method of composite material
CN119899317A