A method for preparing high specific capacity lithium-sulfur cathode material
By using a pressing and desulfurization roasting process under closed conditions, combined with a mixed atmosphere of inert gas and oxygen-containing gas, the problems of cycle performance degradation and exhaust gas treatment of lithium-sulfur battery cathode materials were solved, achieving efficient utilization of elemental sulfur and improvement of electrochemical performance.
Patent Information
- Application Number
- CN202611006236.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-07
- Publication Date
- 2026-11-17
AI Technical Summary
Traditional lithium-sulfur battery carbon-sulfur composite cathode materials suffer from cycle performance degradation and coulombic efficiency reduction due to the dissolution of lithium polysulfides in the electrolyte. Furthermore, the uncertainty of the sulfidation reaction process leads to poor product consistency, safety hazards, and difficulties in exhaust gas treatment.
The sulfurization reaction is carried out under closed conditions using a tableting process. A mixed atmosphere of inert gas and a small amount of oxygen-containing gas is used, and the reaction pressure is controlled at 0.5~4 MPa. Subsequently, desulfurization roasting is carried out to remove excess elemental sulfur and form porous organic matter to improve the sulfur grafting rate and utilization rate.
It improves the stability of the sulfidation reaction and product consistency, reduces tail gas treatment pressure, reduces the risk of equipment blockage, enhances electrochemical performance and the utilization rate of elemental sulfur, and reduces production costs.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention belongs to the field of chemical power source technology, specifically relating to a method for preparing a high specific capacity lithium-sulfur cathode material. Background Technology
[0002] In recent years, with the continuous expansion of energy storage demand, energy storage technologies with higher energy density, longer lifespan, and higher safety have become the focus of research and development. Lithium-sulfur batteries, with their high theoretical specific energy (2600 Wh / kg), low price, and environmental friendliness, have received increasing attention and research, becoming the best candidate to replace lithium-ion batteries. However, the carbon-sulfur composite cathode materials used in traditional lithium-sulfur batteries face a series of problems, such as cycle performance degradation, decreased coulombic efficiency, and safety issues related to lithium dendrite pulverization caused by the dissolution of long-chain lithium polysulfides (Li2Sn, 4≤n≤8) in the electrolyte. These problems are the main reasons why they have not yet been commercialized.
[0003] Organic sulfides, such as sulfurized polyacrylonitrile (SPAN), are sulfur cathode materials based on a "solid-solid" conversion mechanism that can effectively circumvent the "shuttle effect" of polysulfides, showing great potential in practical applications. Currently, their synthesis processes are mostly carried out under normal or slightly negative pressure conditions. During the reaction, the inert protective gas carries away sublimated sulfur, resulting in low sulfur utilization. Simultaneously, excessive sulfur feedstock significantly impacts preparation efficiency, while sulfur recovery and hydrogen sulfide treatment substantially increase costs. Furthermore, the resulting cathode material contains unreacted sulfur, leading to poor cycle performance. In addition, the sublimated sulfur produced during the reaction is discharged with the exhaust gas, condensing into a solid upon encountering low-temperature pipelines, making cleaning difficult and prone to causing pipeline blockage, affecting experimental progress and posing safety hazards. The sulfurization reaction process is uncertain (incomplete or excessive reaction), resulting in poor consistency of SPAN products; and the entire process cannot be monitored.
[0004] This application is submitted in order to address the aforementioned issues. Summary of the Invention
[0005] The purpose of this invention is to provide a method for preparing high-specific-capacity lithium-sulfur cathode materials to overcome the shortcomings of existing technologies. This method can reduce the amount of sulfur added, reduce the pressure of tail gas treatment, and improve the electrochemical performance of the product, thus having significant advantages.
[0006] The objective of this invention is achieved through the following technical solution: This application provides a method for preparing a high-specific-capacity lithium-sulfur cathode material, comprising the following steps: S1. A linear carbon chain polymer is mixed with elemental sulfur and compressed into tablets. Then, a vulcanization reaction is carried out under closed conditions and a protective atmosphere, wherein the protective atmosphere is mainly composed of inert gas and contains a small amount of oxygen-containing gas. The reaction pressure is controlled at 0.5~4 MPa to obtain a vulcanized polymer. S2. The sulfurized polymer is desulfurized and roasted under inert gas protection to remove excess elemental sulfur and obtain a pure sulfurized polymer.
[0007] Preferably, the linear carbon chain polymer in step S1 is selected from one or more of polyacrylonitrile, polybutadiene, styrene-butadiene rubber, polyethylene, polypropylene, or polyacrylic acid.
[0008] Preferably, the tableting pressure in step S1 is 1~8 MPa.
[0009] Preferably, the oxygen-containing gas content, expressed as its oxygen content, is in a volume ratio of 1 to 5% to the inert gas.
[0010] Preferably, the vulcanization reaction in step S1 is carried out in a closed reactor. The linear carbon chain polymer and the elemental sulfur are pressed into tablets and then loaded into the closed reactor under air conditions. A certain amount of inert gas is then introduced to carry out the vulcanization reaction.
[0011] Preferably, the mass ratio of the linear carbon chain polymer to the elemental sulfur in step S1 is 1:(1.5~4).
[0012] Preferably, the vulcanization reaction temperature in step S1 is 200~500℃ and the time is 0.5~6h.
[0013] Preferably, the desulfurization temperature in step S2 is 150~400℃ and the time is 2~10h.
[0014] Preferably, step S1 uses a pressure monitoring device to detect and adjust the reaction pressure in real time.
[0015] Preferably, the inert gas in step S2 is a free-flowing inert gas.
[0016] Compared with the prior art, this application has the following advantages: This invention enhances the encapsulation of sulfur molecules through a tableting process and increases the partial pressure of sulfur by raising the reaction pressure. A protective gas, including a small amount of oxygen-containing gas, oxidizes the generated hydrogen sulfide in situ into elemental sulfur, which is then recycled in the sulfidation reaction. This promotes the sulfidation reaction in the forward direction, effectively increasing the sulfur grafting rate and sulfur utilization rate, thereby improving the electrochemical performance of the product. Simultaneously, this treatment method optimizes the matching relationship between reaction pressure and sulfur addition, reducing the amount of sulfur added and reaction time, improving process stability and product consistency, reducing the content of sublimated sulfur in the exhaust gas, alleviating exhaust gas treatment pressure, reducing the risk of equipment blockage, reducing production costs, and minimizing sulfur loss. Detailed Implementation
[0017] This application provides a method for preparing a high-specific-capacity lithium-sulfur cathode material, comprising the following steps: S1. A linear carbon chain polymer is mixed with elemental sulfur, compressed into tablets, and subjected to a vulcanization reaction under sealed conditions and a protective atmosphere. The protective atmosphere is mainly composed of inert gas, with a small amount of oxygen-containing gas. The reaction pressure is controlled at 0.5~4 MPa to obtain the vulcanized polymer. The oxygen-containing gas can be oxygen, air, etc. This application uses a linear carbon chain polymer for the vulcanization reaction because linear carbon chains can better undergo grafting reactions with sulfur, and sulfur can form a stable six-membered pyridine ring structure on the carbon chain.
[0018] S2. Then, the sulfurized polymer is desulfurized and roasted under inert gas protection to remove excess elemental sulfur and obtain pure sulfurized polymer.
[0019] Compared with the prior art, the present invention has the following beneficial effects: (1) Before the sulfidation reaction, the present application first uses a tableting method to fix sulfur molecules around the polymer, which is beneficial to the reaction of sulfur vapor and polymer during the sulfidation roasting process; after the reaction consumes sulfur vapor, porous organic matter is formed, and the carbon chain serves as the supporting skeleton of the organic matter, which is more conducive to the shuttle and conduction of lithium ions and improves the electrochemical performance of the product.
[0020] (2) This application uses high pressure for the sulfidation reaction. By increasing the reaction pressure, the partial pressure of sulfur is increased, thereby promoting the forward sulfidation reaction, effectively improving the sulfur grafting rate and the utilization rate of elemental sulfur (sulfur), reducing the proportion of elemental sulfur (sulfur) in the raw materials, shortening the reaction time, effectively reducing the content of sublimated sulfur in the tail gas, alleviating the tail gas treatment pressure, and reducing the risk of equipment blockage. While reducing the proportion of elemental sulfur (sulfur) in the raw materials, it can also effectively increase the sulfur content in the product, thereby improving the electrochemical performance of the product.
[0021] (3) The sulfidation reaction atmosphere of this application contains a small amount of oxygen-containing gas. Elemental sulfur and linear polymer materials begin to dehydrogenate and sulfide at 200°C, producing hydrogen sulfide gas. The small amount of oxygen in the system oxidizes the generated hydrogen sulfide in situ to elemental sulfur and reuses it in the sulfidation reaction. This process not only improves the utilization rate of elemental sulfur, but also promotes the reaction in the forward direction by reducing the H2S gas generated in the reaction. Since elemental sulfur and oxygen need to react at a temperature above 248°C to oxidize elemental sulfur to sulfur dioxide or sulfur trioxide, and hydrogen sulfide in the system will preferentially react with oxygen before elemental sulfur, all the oxygen in the sulfidation roasting process can be used for the oxidation of hydrogen sulfide gas, that is, adding a small amount of oxygen is sufficient to meet the reaction requirements.
[0022] (4) The method provided in this application is simple to operate, easy to industrialize, and the product prepared has high capacitance and good cycle stability.
[0023] Preferably, the linear carbon chain polymer in step S1 is selected from one or more of polyacrylonitrile, polybutadiene, styrene-butadiene rubber, polyethylene, polypropylene, or polyacrylic acid.
[0024] Preferably, the tableting pressure in step S1 is 1~8 MPa. Within this pressure range, the linear carbon chain polymer and elemental sulfur can be fully mixed and contacted to obtain sheets of suitable density or other shaped materials such as spheres.
[0025] Preferably, the mixed material formed by compression is in the shape of a sphere or cylinder. If it is a cylinder, the diameter is generally no more than 3 cm and the thickness is no more than 3 cm.
[0026] Preferably, the vulcanization reaction in step S1 is carried out in a closed reactor. The linear carbon chain polymer and elemental sulfur are pressed into tablets and then loaded into the closed reactor under air conditions. Then, a certain amount of inert gas is introduced to carry out the vulcanization reaction. That is, when the closed reactor of this application is loaded, no vacuum is drawn to remove the air inside, nor is inert gas used for gas replacement, so that air remains in the reactor to oxidize part of the elemental sulfur.
[0027] Preferably, the oxygen-containing gas content, expressed as its oxygen content, is 1-5% by volume to the inert gas. This oxygen content range is sufficient to oxidize H2S without excessively affecting the normal sulfidation reaction.
[0028] As mentioned above, by using tableting, increasing the vulcanization reaction pressure, and using a small amount of air or oxygen in the reaction atmosphere, the utilization rate of elemental sulfur is improved and the amount of elemental sulfur used is reduced. Preferably, the mass ratio of linear carbon chain polymer to elemental sulfur in step S1 is 1:(1.5~4).
[0029] Preferably, the vulcanization reaction temperature in step S1 is 200~500℃, and the time is 0.5~6h. Under these temperature conditions, elemental sulfur and linear carbon chain polymers can fully undergo the vulcanization reaction. As those skilled in the art will understand, when the vulcanization reaction pressure and temperature are high, the reaction time can be appropriately shortened; when the vulcanization reaction pressure and temperature are low, the reaction time can be appropriately extended.
[0030] As those skilled in the art will understand, the desulfurization temperature and time are sufficient to allow unreacted elemental sulfur to sublimate and remove elemental sulfur from the product, while also avoiding any adverse effects on the structure of the sulfidation reaction products. Preferably, the desulfurization temperature in step S2 is 150~400℃, and the time is 2~10h.
[0031] Preferably, step S1 uses a pressure monitoring device to detect and adjust the reaction pressure in real time. As the reaction proceeds, the amount of gaseous sulfides generated decreases, and the pressure drops. A certain amount of inert gas is then introduced to maintain the reaction pressure.
[0032] Preferably, in step S2, the inert gas is a fluid inert gas, which can promptly remove the sublimated elemental sulfur.
[0033] As will be understood by those skilled in the art, the inert gas may be nitrogen, helium, argon, etc.
[0034] Example 1 Linear carbon chain polymer polybutadiene and elemental sulfur were mixed uniformly at a mass ratio of 1:4 and pressed into sheets under a pressure of 4 MPa. The sheets were then placed in a sealed reaction furnace under air conditions, and a certain amount of nitrogen was introduced to ensure that the oxygen content of the mixed gas was 3% of the nitrogen content. The temperature was raised to 400℃ for a vulcanization reaction, and the reaction time was 3 hours. The reaction pressure was controlled at 2.5 MPa. During the reaction, the pressure inside the furnace was recorded and adjusted in real time through a pressure monitoring device to keep the pressure at around 2.5 MPa, thus obtaining the vulcanized polymer. (2) The sulfurized polymer obtained by the reaction was desulfurized and roasted under the protection of flowing nitrogen. The reaction temperature was controlled at 300℃ and the reaction time was 4h to remove excess sulfur and obtain pure sulfurized polymer. (3) Test the electrochemical performance of the pure vulcanized polymer and calculate the sulfur recovery rate of the tail gas to be 30%.
[0035] Example 2 Linear carbon chain polymer polyacrylic acid and elemental sulfur were mixed uniformly at a mass ratio of 1:2 and pressed into sheets under a pressure of 8 MPa. The sheets were then placed in a sealed reaction furnace under air conditions, and a certain amount of nitrogen was introduced to ensure that the mass ratio of oxygen to nitrogen in the mixed gas was 5%. The temperature was raised to 200℃ for vulcanization reaction, and the reaction time was 6 hours. The reaction pressure was controlled at 0.5 MPa. During the reaction, the pressure inside the furnace was recorded and adjusted in real time through a pressure monitoring device to keep the pressure at around 0.5 MPa, thus obtaining the vulcanized polymer. (2) The sulfurized polymer obtained by the reaction was desulfurized and roasted under the protection of flowing nitrogen. The reaction temperature was controlled at 150℃ and the reaction time was 10h to remove excess sulfur and obtain pure sulfurized polymer. (3) Test the electrochemical performance of the pure vulcanized polymer and calculate the sulfur recovery rate of the tail gas to be 10%.
[0036] Example 3 Linear carbon chain polymer polyacrylonitrile was mixed with elemental sulfur at a mass ratio of 1:1.5 and pressed into sheets under a pressure of 1 MPa. The sheets were then placed in a sealed reaction furnace under air conditions, and a certain amount of nitrogen was introduced to ensure that the oxygen content of the mixed gas was 1% of the nitrogen content. The temperature was raised to 360℃ for a vulcanization reaction, and the reaction time was 2.5 hours. The reaction pressure was controlled at 1.5 MPa. During the reaction, the pressure inside the furnace was recorded and adjusted in real time through a pressure monitoring device to keep the pressure at around 1.5 MPa, thus obtaining the vulcanized polymer. (2) The sulfurized polymer obtained by the reaction was desulfurized and roasted under the protection of flowing nitrogen. The reaction temperature was controlled at 270℃ and the reaction time was 6h to remove excess sulfur and obtain pure sulfurized polymer. (3) Test the electrochemical performance of the pure sulfurized polymer and calculate the sulfur recovery rate of the tail gas to be 5%.
[0037] Example 4 (1) The linear carbon chain polymer polyacrylonitrile and elemental sulfur are mixed evenly at a mass ratio of 1:3 and pressed into sheets under a pressure of 2 MPa. The sheets are then placed in a sealed reaction furnace under air conditions. A certain amount of nitrogen is then introduced to ensure that the mass ratio of oxygen to nitrogen in the mixed gas is 2%. The temperature is raised to 500℃ for vulcanization reaction, and the reaction time is 0.5 h. The reaction pressure is controlled at 4 MPa. During the reaction, the pressure inside the furnace is recorded and adjusted in real time through a pressure monitoring device to keep the pressure at around 4 MPa, thus obtaining the vulcanized polymer. (2) The sulfurized polymer obtained by the reaction was desulfurized and roasted under the protection of flowing nitrogen. The reaction temperature was controlled at 400℃ and the reaction time was 2h to remove excess sulfur and obtain pure sulfurized polymer. (3) Test the electrochemical performance of the pure vulcanized polymer and calculate the sulfur recovery rate of the tail gas to be 20%.
[0038] Comparative Example 1 (1) The linear carbon chain polymer polyacrylonitrile and elemental sulfur were mixed evenly at a mass ratio of 1:3. The reaction pressure was controlled at atmospheric pressure, and other experimental conditions were the same as in Example 4 to obtain a pure sulfurized polymer. (2) Test the electrochemical performance of the pure sulfurized polymer and calculate the sulfur recovery rate of the tail gas to be 65%.
[0039] Comparative Example 2 (1) The linear carbon chain polymer polyacrylonitrile and elemental sulfur were mixed evenly at a mass ratio of 1:3. The mixture was directly vulcanized and calcined as powder without being pressed into tablets. Other experimental conditions were the same as in Example 4 to obtain a pure vulcanized polymer. (2) Test the electrochemical performance of the pure vulcanized polymer and calculate the sulfur recovery rate of the tail gas to be 30%.
[0040] Comparative Example 3 (1) The linear carbon chain polymer polyacrylonitrile and elemental sulfur were mixed evenly at a mass ratio of 1:3 and loaded into a sealed reaction furnace under inert gas protection to ensure that the oxygen content in the reaction furnace was 0%. Other experimental conditions were the same as in Example 4 to obtain a pure sulfurized polymer. (2) Test the electrochemical performance of the pure vulcanized polymer and calculate the sulfur recovery rate of the tail gas to be 50%.
[0041] The performance indicators of the products from the above cases are shown in Table 1: Table 1 Indicator Test Results
[0042] The above data show that the sulfur recovery rate of the tail gas of the cathode material prepared by the method of this application is between 5% and 30%, the specific capacity of the 0.2C cycle is 720 to 740 mAh / g, and the number of cycles under 1C is 368 to 390.
[0043] Comparative Example 1, due to its atmospheric pressure sulfurization roasting, had a low sulfur partial pressure, resulting in low sulfur utilization. The sulfur recovery rate in the tail gas increased by 45% compared to Example 4. The prepared cathode material, due to its low sulfur content, experienced a 150 mAh / g decrease in 0.2C secondary discharge specific capacity. Comparative Example 2 employed an unpressed process for sulfurization roasting, with the remaining conditions identical to Example 4. Due to the reduced contact area between sulfur and the polymer, the sulfur recovery rate in the tail gas increased by 10%, the sulfur grafting rate decreased, and the 0.2C secondary discharge specific capacity decreased by 140 mAh / g. Comparative Example 3 underwent sulfurization roasting under an oxygen-free inert gas environment, with the remaining reaction conditions the same as Example 4. It was observed that sulfur mostly escaped in the form of hydrogen sulfide, leading to a 30% increase in tail gas sulfur recovery and a decrease in sulfur utilization. The resulting product had a 160 mAh / g decrease in 0.2C secondary discharge specific capacity.
[0044] Although preferred embodiments of the invention have been described, those skilled in the art, upon learning the basic inventive concept, can make other changes and modifications to these embodiments. Therefore, the appended claims are intended to be interpreted as including both the preferred embodiments and all changes and modifications falling within the scope of the invention. Clearly, those skilled in the art can make various alterations and modifications to the invention without departing from its spirit and scope. Thus, if these modifications and modifications of the invention fall within the scope of the claims and their equivalents, the invention is also intended to include these modifications and modifications.
Claims
1. A method for preparing a high-specific-capacity lithium-sulfur cathode material, characterized in that, Includes the following steps: S1. A linear carbon chain polymer is mixed with elemental sulfur and compressed into tablets. Then, a vulcanization reaction is carried out under closed conditions and a protective atmosphere, wherein the protective atmosphere is mainly composed of inert gas and contains a small amount of oxygen-containing gas. The reaction pressure is controlled at 0.5~4 MPa to obtain a vulcanized polymer. S2. The sulfurized polymer is desulfurized and roasted under inert gas protection to remove excess elemental sulfur and obtain a pure sulfurized polymer.
2. The method for preparing the high specific capacity lithium-sulfur cathode material as described in claim 1, characterized in that, The linear carbon chain polymer mentioned in step S1 is selected from one or more of polyacrylonitrile, polybutadiene, styrene-butadiene rubber, polyethylene, polypropylene, or polyacrylic acid.
3. The method for preparing the high specific capacity lithium-sulfur cathode material as described in claim 1, characterized in that, The tableting pressure in step S1 is 1~8 MPa.
4. The method for preparing the high specific capacity lithium-sulfur cathode material as described in claim 1, characterized in that, The oxygen-containing gas content, expressed as its oxygen content, is in a volume ratio of 1 to 5% to the inert gas.
5. The method for preparing the high specific capacity lithium-sulfur cathode material as described in claim 1, characterized in that, The vulcanization reaction in step S1 is carried out in a closed reactor. The linear carbon chain polymer and the sulfur are pressed into tablets and then loaded into the closed reactor under air conditions. A certain amount of inert gas is then introduced to carry out the vulcanization reaction.
6. The method for preparing the high specific capacity lithium-sulfur cathode material as described in claim 1, characterized in that, The mass ratio of the linear carbon chain polymer to the elemental sulfur in step S1 is 1:(1.5~4).
7. The method for preparing the high specific capacity lithium-sulfur cathode material as described in claim 1, characterized in that, The vulcanization reaction in step S1 is carried out at a temperature of 200~500℃ for 0.5~6h.
8. The method for preparing the high specific capacity lithium-sulfur cathode material as described in claim 1, characterized in that, The desulfurization temperature in step S2 is 150~400℃, and the time is 2~10h.
9. The method for preparing the high specific capacity lithium-sulfur cathode material as described in claim 1, characterized in that, Step S1 uses a pressure monitoring device to detect and adjust the reaction pressure in real time.
10. The method for preparing the high specific capacity lithium-sulfur cathode material as described in claim 1, characterized in that, The inert gas used in step S2 is a free-flowing inert gas.