Based on Zn 2+ -Self-healing polyurea conductive elastomers with carboxyl coordination crosslinking, their preparation methods and applications

The method of preparing self-healing polyurea-based conductive elastomers by Zn2+-carboxyl coordination crosslinking solves the problem of insufficient mechanical strength and self-healing ability of flexible sensing materials under large deformation, realizes the application of high strain and long life sensing materials, and has excellent antibacterial properties and biocompatibility.

CN123107030APending Publication Date: 2026-11-17EASTERN LIAONING UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611204160.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-10
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing flexible sensing materials suffer from insufficient mechanical strength, poor cyclic stability, or limited self-healing ability under large deformations, making it difficult to simultaneously meet the comprehensive requirements of high strain, long lifespan, and multi-scenario application.

Method used

A self-healing polyurea-based conductive elastomer was prepared using a Zn2+-carboxyl coordination crosslinking method. The polyurea prepolymer was synthesized by polypropylene glycol bis(2-aminopropyl ether) and isophorone diisocyanate. After chain extension by adding 3,5-diaminobenzoic acid, a dynamic metal coordination crosslinking network was formed with zinc chloride solution. An ionic liquid was added to construct a continuous ion transport channel.

Benefits of technology

It achieves a synergistic improvement in mechanical properties and self-healing properties, and the material has excellent antibacterial properties and biocompatibility, making it suitable for flexible wearable sensors and health monitoring devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123107030A_ABST
    Figure CN123107030A_ABST
Patent Text Reader

Abstract

This application provides a Zn-based 2+ Self-healing polyurea-based conductive elastomers with carboxyl coordination crosslinking, their preparation methods, and applications: Polyurea prepolymers were synthesized using polypropylene glycol bis(2-aminopropyl ether) and isophorone diisocyanate as raw materials. Then, 3,5-diaminobenzoic acid was introduced as a functional chain extender to provide carboxyl coordination sites. Finally, zinc chloride solution was added, and the elastomer was crosslinked with Zn... 2+ A high-strength metal-coordinated crosslinking network is constructed through dynamic coordination with carboxyl groups. Finally, ionic liquid 1-ethyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide is added to construct a continuous ion transport channel, thus obtaining a conductive elastomer. The conductive elastomer provided in this application possesses excellent mechanical properties, efficient self-healing properties, stable ion conductivity, broad-spectrum antibacterial properties, and good biocompatibility, making it suitable for applications such as flexible wearable sensors, human motion monitoring devices, and health monitoring devices.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application belongs to the field of flexible sensing materials technology, and particularly relates to a Zn-based... 2+ -Self-healing polyurea-based conductive elastomers with carboxyl coordination crosslinking, their preparation methods and applications. Background Technology

[0002] Flexible sensors, as core components of next-generation intelligent healthcare and human-computer interaction systems, possess unique advantages such as stretchability and conformability, enabling them to dynamically conform to human skin and even soft tissue surfaces. They demonstrate irreplaceable application value in personalized health management, early disease screening, telemedicine, and sports rehabilitation. Flexible sensors used to acquire physiological signals require materials with good stretchability, stable conductivity, and sensitive response to strain or pressure changes. In recent years, various polymeric conductive elastomers have been used to construct flexible sensors; however, these materials often suffer from insufficient mechanical strength, poor cyclic stability, or limited self-healing capabilities under large deformations, making it difficult to simultaneously meet the comprehensive requirements of high strain, long lifespan, and multi-scenario application.

[0003] Self-healing performance and mechanical properties are two core indicators for evaluating the overall performance of self-healing flexible sensing materials, directly determining the device's service life, reliability, and adaptability to various application scenarios. However, there is an inherent trade-off between the two: achieving high-strength material properties requires the construction of a stable network structure based on strong dynamic bonds, but the reversible reconstruction of strong dynamic bonds often requires harsh external conditions (such as high temperature or specific pH environments), limiting self-healing efficiency; while achieving high self-healing efficiency usually relies on the rapid dissociation and reconstruction of weak dynamic bonds, but its loose network structure significantly reduces the material's mechanical strength, making it difficult to meet the structural stability and load-bearing capacity requirements of flexible sensors in practical applications. Therefore, breaking this "seesaw" effect and achieving a synergistic improvement in self-healing efficiency and mechanical properties is a key challenge in the preparation of high-performance self-healing flexible sensing materials. Summary of the Invention

[0004] This application is made in view of the above-mentioned issues, and its purpose is to provide a polyurea-based conductive elastomer that has excellent mechanical properties, high efficiency self-healing ability, stable conductivity and good biocompatibility, which is of great significance for promoting the application of flexible sensors in wearable health monitoring, human-computer interaction and other fields.

[0005] The first aspect of this application provides a Zn-based... 2+ A method for preparing a self-healing polyurea-based conductive elastomer with carboxyl coordination crosslinking includes the following steps: S1. Synthesis of polyurea elastomers (PDU) containing carboxyl side groups: Polypropylene glycol bis(2-aminopropyl ether) and isophorone diisocyanate were dissolved separately in organic solvents. Under a dry nitrogen atmosphere at room temperature, isophorone diisocyanate solution was added dropwise to the polypropylene glycol bis(2-aminopropyl ether) solution. The mixture was stirred continuously under a dry nitrogen atmosphere at room temperature to carry out a prepolymerization reaction, yielding an isocyanate-terminated polyurea prepolymer. 3,5-Diaminobenzoic acid was added to the isocyanate-terminated polyurea prepolymer as a chain extender to carry out a chain extension reaction. The entire reaction was carried out under a dry nitrogen atmosphere at room temperature. After the reaction was completed, the polyurea elastomer containing carboxyl side groups was obtained by solution casting and drying, denoted as PDU.

[0006] S2, Zn 2+ Synthesis of carboxyl-coordinated crosslinked polyurea elastomer (PDUZn): The polyurea elastomer containing carboxyl side groups was dissolved in an organic solvent, and then a zinc chloride solution was added. The mixture was stirred and mixed thoroughly at room temperature under a dry nitrogen atmosphere to allow the Zn... 2+ Zn undergoes a coordination crosslinking reaction with the carboxyl groups on the molecular chains of polyurea elastomers containing carboxyl side groups; after the reaction is complete, Zn is obtained by solution casting and drying. 2+ -Carboxyl-coordinated crosslinked polyurea elastomer; S3. Synthesis of polyurea-based conductive elastomer (PDUZn-IL): Zn 2+ -Carboxyl-coordinated crosslinked polyurea elastomer was dissolved in an organic solvent, then an ionic liquid was added, and the mixture was stirred and mixed evenly at room temperature under a dry nitrogen atmosphere. After solution casting and drying, a Zn-based product was obtained. 2+ -Self-healing polyurea conductive elastomer with carboxyl coordination crosslinking.

[0007] In any embodiment, the molar ratio of polypropylene glycol bis(2-aminopropyl ether), isophorone diisocyanate, and 3,5-diaminobenzoic acid is 1:(1.5-2.5):(0.5-1); the organic solvent is at least one of N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, or N-methylpyrrolidone.

[0008] In any embodiment, during the coordination crosslinking reaction, the amount of zinc chloride solution added satisfies the requirement that the -COOH and Zn groups in the polyurea elastomer molecular chain containing carboxyl side groups... 2+ The molar ratio is (1:2) to (6:1); the amount of ionic liquid added is Zn 2+ -5 wt% to 40 wt% of the carboxyl-coordinated crosslinked polyurea elastomer.

[0009] In any embodiment, the prepolymerization reaction takes 4 to 12 hours, and the chain extension reaction takes 4 to 12 hours.

[0010] In any embodiment, the drying temperature is 50–70°C.

[0011] A second aspect of this application also provides a Zn-based... 2+ The self-healing polyurea-based conductive elastomer with α-carboxyl coordination crosslinking was obtained by the above preparation method.

[0012] In any embodiment, the number-average molecular weight of the polypropylene glycol bis(2-aminopropyl ether) is 400–2000 g·mol⁻¹. -1 The ionic liquid is 1-ethyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide.

[0013] In any embodiment, the molar ratio of polypropylene glycol bis(2-aminopropyl ether), isophorone diisocyanate, and 3,5-diaminobenzoic acid is 1:(1.5-2.5):(0.5-1).

[0014] In any embodiment, the organic solvent is at least one of N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, or N-methylpyrrolidone.

[0015] A third aspect of this application provides a Zn-based 2+ Applications of self-healing polyurea conductive elastomers with carboxyl coordination crosslinking in the preparation of flexible wearable sensors, human motion monitoring devices, or health monitoring devices.

[0016] Compared with the prior art, this application has the following beneficial effects: 1. The preparation process is simple and can be completed at room temperature. It does not require complicated procedures or harsh reaction conditions, which not only reduces production costs but also facilitates large-scale preparation.

[0017] 2. Achieve synergistic breakthroughs in mechanical properties and self-healing performance. By optimizing the molar ratio of coordinating groups to transition metal ions, the industry pain point of difficulty in simultaneously achieving both mechanical properties and repair efficiency in self-healing materials is addressed.

[0018] 3. It possesses both excellent antibacterial properties and biocompatibility. The membrane-breaking effect of the imidazole cation in the ionic liquid enables the material to achieve an inhibition rate of over 99% against both Escherichia coli and Staphylococcus aureus, and it has no significant cytotoxicity to human skin fibroblasts, meeting the safety requirements for wearable devices in long-term contact with human skin.

[0019] 4. Wide range of applications. This material can accurately monitor the movement of multiple joints in the human body and weak physiological signals such as pulse and respiration, as well as accurately identify the movement state. It has broad application prospects in the fields of flexible wearable sensors, human motion monitoring devices, and health monitoring devices. Attached Figure Description

[0020] Figure 1 This application is based on Zn 2+ Synthetic route diagram of self-healing polyurea conductive elastomer with carboxyl coordination crosslinking.

[0021] Figure 2 The infrared spectra of the conductive elastomers prepared in Examples 1 to 3 of this application are shown.

[0022] Figure 3 The stress-strain curves are for the conductive elastomers prepared in Examples 1 to 3 of this application.

[0023] Figure 4 The relative resistance-time response diagram (a) and the comparison diagram of the standard factor (b) of the PDUZn0.5-20IL conductive elastomer sample prepared for Example 2 of this application under different strain ranges are shown.

[0024] Figure 5 The image shows the joint sensing signal of the PDUZn0.5-20IL conductive elastomer sample prepared in Example 2 of this application; where a is the electrical signal response of finger joint bending, b is the electrical signal response of wrist joint bending, c is the electrical signal response of knee joint bending, and d is the electrical signal response of elbow joint bending.

[0025] Figure 6 The images show the micro-motion sensing signals of the PDUZn0.5-20IL conductive elastomer sample prepared in Example 2 of this application; where a is the electrical signal response diagram of pulse fluctuation, b is the electrical signal response diagram of respiration, c is the electrical signal response diagram of pressing the internationally recognized SOS emergency code, and d is the electrical signal response diagram of writing "Fire".

[0026] Figure 7 The diagrams show the self-healing properties of the PDUZn0.5-xIL conductive elastomer series samples prepared in Examples 1 to 3 of this application; where a is the mechanical self-healing property diagram and b is the electrical self-healing property diagram.

[0027] Figure 8 The antibacterial properties and biocompatibility of the PDUZn0.5-20IL conductive elastomer sample prepared in Example 2 of this application are shown in the figure. Detailed Implementation

[0028] The following detailed description, with appropriate reference to the accompanying drawings, discloses the Zn-based method of this application. 2+- Embodiments of self-healing polyurea-based conductive elastomers with carboxyl coordination crosslinking, their preparation methods, and applications. However, unnecessary detailed descriptions may be omitted. For example, detailed descriptions of well-known matters and repetitive descriptions of practically identical structures may be omitted. This is to avoid unnecessarily lengthy descriptions and to facilitate understanding by those skilled in the art. Furthermore, the accompanying drawings and the following description are provided to enable those skilled in the art to fully understand this application and are not intended to limit the subject matter of the claims.

[0029] The "range" disclosed in this application is defined by a lower limit and an upper limit. A given range is defined by selecting a lower limit and an upper limit, which define the boundaries of a particular range. Ranges defined in this way can include or exclude endpoints and can be arbitrarily combined; that is, any lower limit can be combined with any upper limit to form a range. For example, if ranges of 60-120 and 80-110 are listed for a specific parameter, it is expected that ranges of 60-110 and 80-120 are also included. Furthermore, if minimum range values ​​of 1 and 2 are listed, and if maximum range values ​​of 3, 4, and 5 are listed, then the following ranges are all expected: 1-3, 1-4, 1-5, 2-3, 2-4, and 2-5. In this application, unless otherwise stated, the numerical range "ab" represents a shortened representation of any combination of real numbers between a and b, where a and b are real numbers. For example, the numerical range "0-5" indicates that all real numbers between "0-5" have been listed in this article; "0-5" is simply a shortened representation of these numerical combinations. Furthermore, when a parameter is stated as an integer ≥2, it is equivalent to disclosing that the parameter is, for example, an integer such as 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0030] Unless otherwise specified, all embodiments and optional embodiments of this application can be combined to form new technical solutions.

[0031] Unless otherwise specified, all technical features and optional technical features of this application may be combined to form new technical solutions.

[0032] Unless otherwise specified, all steps in this application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or it may include steps (b) and (a) performed sequentially. For example, the mention that the method may also include step (c) indicates that step (c) may be added to the method in any order. For example, the method may include steps (a), (b), and (c), or it may include steps (a), (c), and (b), or it may include steps (c), (a), and (b), etc.

[0033] Unless otherwise specified, the terms "comprising" and "including" as used in this application can be open-ended or closed-ended. For example, "comprising" and "including" can mean that other components not listed may also be included, or that only the listed components may be included.

[0034] Unless otherwise specified, the term "or" is inclusive in this application. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, the condition "A or B" is satisfied by any of the following conditions: A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).

[0035] To overcome the "seesaw" effect between self-healing performance and mechanical properties, and to achieve a synergistic improvement in both self-healing efficiency and mechanical performance, this application aims to prepare high-performance self-healing flexible sensing materials. This application utilizes metal-ligand coordination bonds as a type of dynamically reversible non-covalent interaction, providing a technical path to address the aforementioned challenges. Essentially, ligands such as carboxyl, amino, and hydroxyl groups provide lone pairs of electrons to transition metal ions with empty orbitals, forming a dynamic coordination network. This unique coordination mechanism endows the material with significant advantages: on the one hand, the strength of the coordination bonds can be precisely controlled by adjusting the type of metal ion, ligand structure, and coordination environment, potentially finding a balance between the mechanical stability brought by strong bonding and the self-healing activity conferred by weak bonding; on the other hand, the dynamic reversibility of the coordination bonds enables damage self-repair through bond dissociation-reconstruction processes. Furthermore, polyurea, a widely used polymer material, is introduced, possessing excellent mechanical properties such as good molecular structure designability, superior elasticity, and outstanding fracture toughness. Polyurea-based conductive elastomers prepared using polyurea as the matrix and ionic liquid as the conductive medium show broad application potential in the field of flexible electronics.

[0036] However, research has found that existing polyurea-based conductive elastomers mostly rely on hydrogen bonding or physical entanglement to maintain their three-dimensional network structure, resulting in relatively insufficient mechanical strength and fatigue resistance. They are prone to irreversible damage under high strain or cyclic loading conditions. While there have been attempts to introduce metal coordination into polyurea systems in existing technologies, these are mostly limited to a single crosslinking mode, failing to fully utilize the synergistic effect of metal coordination, hydrogen bonding, and ion conduction, making it difficult to simultaneously optimize mechanical properties, self-healing efficiency, and conductivity. This application synthesizes a polyurea prepolymer using polypropylene glycol bis(2-aminopropyl ether) and isophorone diisocyanate as raw materials; then, 3,5-diaminobenzoic acid is introduced to provide carboxyl coordination sites, and then zinc chloride solution is added, through Zn... 2+A high-strength metal-coordinated crosslinking network is constructed through dynamic coordination with carboxyl groups. Finally, a continuous ion transport channel is built by combining with an ionic liquid, resulting in a conductive elastomer with high mechanical strength, high self-healing efficiency, and stable ionic conductivity. This application significantly enhances the self-healing ability and structural stability of the material by introducing a metal-coordinated network while maintaining the excellent mechanical properties of the polyurea matrix.

[0037] In one embodiment of this application, a Zn-based method is proposed. 2+ A method for preparing a self-healing polyurea-based conductive elastomer with carboxyl coordination crosslinking includes the following steps: S1. Synthesis of polyurea elastomers (PDU) containing carboxyl side groups: Polypropylene glycol bis(2-aminopropyl ether) and isophorone diisocyanate were dissolved separately in organic solvents. Under a dry nitrogen atmosphere at room temperature, isophorone diisocyanate solution was added dropwise to the polypropylene glycol bis(2-aminopropyl ether) solution. The mixture was stirred continuously at room temperature to carry out a prepolymerization reaction, yielding an isocyanate-terminated polyurea prepolymer. 3,5-Diaminobenzoic acid was added to the isocyanate-terminated polyurea prepolymer as a chain extender to carry out a chain extension reaction. The entire reaction was carried out at room temperature under a dry nitrogen atmosphere. After the reaction was completed, the polyurea elastomer containing carboxyl side groups was obtained by solution casting and drying, denoted as PDU. S2, Zn 2+ Synthesis of carboxyl-coordinated crosslinked polyurea elastomer (PDUZnx): The polyurea elastomer containing carboxyl side groups was dissolved in an organic solvent, then added to a zinc chloride solution, and stirred until homogeneous under a dry nitrogen atmosphere at room temperature, so that Zn 2+ Zn undergoes a coordination crosslinking reaction with the carboxyl groups on the molecular chains of polyurea elastomers containing carboxyl side groups; after the reaction is complete, Zn is obtained by solution casting and drying. 2+ -Carboxyl-coordinated crosslinked polyurea elastomer; S3. Synthesis of polyurea-based conductive elastomer (PDUZnx-yIL): Zn 2+ -Carboxyl-coordinated crosslinked polyurea elastomer was dissolved in an organic solvent, then an ionic liquid was added, and the mixture was stirred and mixed evenly at room temperature under a dry nitrogen atmosphere. After solution casting and drying, a Zn-based product was obtained. 2+ -Self-healing polyurea conductive elastomer with carboxyl coordination crosslinking.

[0038] This application relates to a Zn-based 2+- A self-healing polyurea-based conductive elastomer with carboxyl coordination crosslinking. First, a polyurea prepolymer was synthesized using polypropylene glycol bis(2-aminopropyl ether) and isophorone diisocyanate as raw materials. Second, 3,5-diaminobenzoic acid was used as a chain extender; its two amino groups reacted with the terminal isocyanate groups of the prepolymer, introducing carboxyl side groups into the polyurea backbone, resulting in a polyurea elastomer containing carboxyl side groups. Then, a zinc chloride solution was added to the polyurea elastomer containing carboxyl side groups. 2+ A dynamic metal-coordinated crosslinking network is formed by coordinating with the carboxyl groups on the molecular chain of a polyurea elastomer containing carboxyl side groups. Finally, the ionic liquid 1-ethyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide is introduced into the above coordination network system, and a conductive elastomer is obtained by solution casting and drying. This elastomer has good mechanical properties, self-healing properties, sensing properties, antibacterial properties and biocompatibility, and is suitable for flexible wearable sensors, human motion monitoring devices and health monitoring devices.

[0039] In this application, the -COOH group in the polyurea molecular chain can react with Zn. 2+ Coordination occurs, and this coordination effectively modulates the interaction strength between molecular chains, thus significantly affecting the mechanical properties of polyurea elastomers. Moderate coordination enhances the degree of cross-linking between molecular chains, improving the rigidity and toughness of the material, while excessive coordination may lead to molecular chain aggregation, resulting in a decrease in the material's mechanical properties. This application achieves this through systematic optimization of the relationship between -COOH and Zn... 2+ The molar ratio was optimized to achieve the optimal mechanical properties of the material.

[0040] This application selects zinc chloride as the coordination crosslinking agent, utilizing Zn 2+ A cross-linked network is constructed through dynamic coordination between Zn and the carboxyl side groups on the polyurea molecular chain. 2+ The coordination bond energy with the carboxyl group is approximately 104-134 kJ / mol, representing a weak but abundant coordination interaction. Its strength is sufficient to improve the material's mechanical properties, and it also possesses excellent dynamic reversibility. In comparison, Fe... 3+ Cu 2+ When metal ions have excessively strong coordination with carboxyl groups, they easily form kinetically inert rigid networks, resulting in brittle materials that are difficult to self-heal at room temperature; Ca 2+ Mg 2+ Na + When the coordination ability between metal ions and carboxyl groups is too weak, effective cross-linking cannot be formed, resulting in insufficient mechanical strength of the material. Furthermore, Zn... 2+ It possesses biological functional properties such as low toxicity and broad-spectrum antibacterial activity. It has no significant toxicity to human skin fibroblasts. When synergistically combined with ionic liquids, it has an antibacterial rate of over 99% against Escherichia coli and Staphylococcus aureus. It is particularly suitable for scenarios where wearable devices are in long-term contact with human skin.

[0041] The introduction of ionic liquids not only significantly enhances the ionic conductivity of the material but also endows it with excellent antibacterial activity. The positively charged imidazole groups in ionic liquids can interact electrostatically with the negatively charged components on bacterial cell membranes, disrupting their integrity by forming channels in the cell membrane and causing leakage of cytoplasmic contents, thus achieving broad-spectrum and highly effective killing of Escherichia coli and Staphylococcus aureus.

[0042] This application utilizes polyurea covalent networks and Zn 2+ The synergistic construction of a carboxyl dynamic coordination network and an ionic liquid ion conduction network forms a structure integrating triple physical cross-linking and ion transport. Among them, the polyurea covalent backbone provides basic mechanical load-bearing capacity; Zn... 2+ -The dynamic coordination bonds of the carboxyl groups can undergo reversible dissociation and recombination under external forces, achieving energy dissipation and self-repair of damage; the ionic liquid forms continuous ion transport channels in the network, endowing the material with stable electrical conductivity. The synergistic effect of these three mechanisms enables the material to maintain excellent mechanical properties while possessing both efficient self-healing capabilities and stable sensing functions.

[0043] The realization of the above-mentioned triple network synergy requires the following key control conditions: First, the polyurea covalent backbone must maintain a linear topological structure, forming a linear polymer without irreversible chemical cross-links through polymerization, so as to ensure that the molecular chain segments have the necessary degrees of freedom of movement when subjected to force, for Zn 2+ - The dynamic dissociation and recombination of carboxyl coordination bonds and the diffusion rearrangement of ionic liquids provide the structural basis; secondly, the density of carboxyl coordination sites needs to be moderate, determined by the amount of 3,5-diaminobenzoic acid used. If the density is too low, Zn... 2+ The sparse coordination crosslinking network results in insufficient mechanical reinforcement and self-healing driving force; excessive density leads to excessive aggregation of rigid benzene ring hard segments, increasing material brittleness; thirdly, Zn 2+ The molar ratio of Zn to carboxyl groups needs to be within a dynamic equilibrium range (1:2 to 6:1), and the coordination crosslinking density needs to be sufficient to form a through-network to bear the load, while also being able to undergo reversible dissociation-recombination under thermal stimulation to achieve damage repair. Excess Zn 2+ This will lead to excessive cross-linking or ion cluster aggregation, while too little will result in an incomplete coordination network; fourth, the ionic liquid content needs to be between the percolation threshold and the network destruction threshold (5 wt%–40 wt%) to ensure the formation of continuous ion channels, while avoiding damage to the polyurea hydrogen bond network and Zn. 2+ - Excessive disruption of the carboxyl coordination network; fifth, all three components need to be uniformly dispersed at the molecular scale, relying on the co-dissolution with strongly polar aprotic solvents and a gentle drying process to ensure Zn 2+ Uniform coordination and uniform distribution of ionic liquids avoid local phase separation or network defects.

[0044] x represents the molar amount of ZnCl2 solution added, and y represents the amount of ionic liquid added in the form of Zn²⁺. + -Carboxyl-coordinated crosslinked polyurea elastomer mass percentage.

[0045] In some embodiments, the molar ratio of polypropylene glycol bis(2-aminopropyl ether), isophorone diisocyanate, and 3,5-diaminobenzoic acid is 1:(1.5-2.5):(0.5-1); the organic solvent is at least one of N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, or N-methylpyrrolidone.

[0046] In some embodiments, during the coordination crosslinking reaction, the amount of zinc chloride solution added satisfies the relationship between -COOH and Zn in the polyurea elastomer molecular chain containing carboxyl side groups. 2+ The molar ratio is (1:2) to (6:1); the amount of ionic liquid added is Zn 2+ -5 wt% to 40 wt% of the carboxyl-coordinated crosslinked polyurea elastomer.

[0047] If the ratio is higher than 6:1 (Zn) 2+ Insufficient Zn content results in sparse coordination crosslinking points, hindering the formation of an effective metal coordination network, limiting the improvement in mechanical strength, and insufficient self-healing driving force; if the ratio is less than 1:2 (Zn 2+ Excessive free Zn 2+ It cannot be fully coordinated by carboxyl groups, and is prone to forming ion clusters or precipitates, leading to internal defects, phase separation and deterioration of mechanical properties in the material.

[0048] If the ionic liquid is added at a concentration below 5 wt%, it disperses in an island-like pattern within the polyurea three-dimensional network, failing to form a continuous ionic conductive pathway. This results in excessively low conductivity and insufficient sensing sensitivity. Simultaneously, the plasticizing effect is weak, the glass transition temperature decreases only slightly, molecular chain mobility is limited, and the self-repair rate decreases significantly. Furthermore, the imidazole cation concentration is insufficient to effectively disrupt bacterial cell membranes, leading to substandard antibacterial performance. If the addition concentration exceeds 40 wt%, the anions and cations in the ionic liquid act as hydrogen-bonding competitive ligands, inhibiting the hydrogen bond cross-linking network between polyurea molecular chains and the Zn... 2+ The destructive effect of the carboxyl coordination network is too severe, resulting in a sharp decrease in physical crosslinking density, a significant reduction in tensile strength and modulus, and insufficient material load-bearing capacity. At the same time, excessive ionic liquid may exceed the swelling capacity limit of the polyurea network, leading to phase separation, exudation, or surface stickiness, which deteriorates dimensional stability and long-term service reliability.

[0049] In some embodiments, the prepolymerization reaction takes 4 to 12 hours, and the chain extension reaction takes 4 to 12 hours.

[0050] If the prepolymerization reaction time is too short, the monomer conversion rate will be insufficient, resulting in a low molecular weight of the isocyanate-terminated prepolymer and subsequent stoichiometric mismatch in chain extension. If the time is too long, the prepolymer viscosity will be too high, and the isocyanate groups will easily undergo side reactions with water or urea bonds, leading to network defects. If the chain extension reaction time is too short, the reaction between 3,5-diaminobenzoic acid and the prepolymer will be incomplete, resulting in insufficient introduction of carboxyl side groups and subsequent Zn... 2+ The coordination network is sparse; if the reaction time is too long, the hard segments of the formed urea bonds will undergo biuret side reactions with the residual isocyanate groups, resulting in excessive cross-linking of the network and increased brittleness of the material. Within this time range, the prepolymerization reaction can be ensured to be sufficient and the chain extension reaction to be complete, while suppressing side reactions, thus achieving the controllable synthesis of high molecular weight linear polyurea.

[0051] In some embodiments, the drying temperature is 50–70°C.

[0052] In one embodiment of this application, a Zn-based method is proposed. 2+ The self-healing polyurea-based conductive elastomer with α-carboxyl coordination crosslinking was obtained by the above preparation method.

[0053] Polypropylene glycol bis(2-aminopropyl ether) is used as a flexible soft segment raw material. Its terminal amino groups react with the isocyanate groups of isophorone diisocyanate at room temperature to form an isocyanate-terminated polyurea prepolymer without the need for additional catalysts. In this prepolymer, the polypropylene glycol bis(2-aminopropyl ether) segment acts as a flexible soft segment, giving the material excellent ductility and low-temperature flexibility; the isophorone diisocyanate provides a rigid hard segment, reacting with the amino group to form urea bonds, giving the material mechanical strength and structural stability. Terminal amino polyethers are chosen instead of terminal hydroxyl polyethers because polyurea chemistry is inherently dependent on the amine-isocyanate reaction. Terminal amino groups have higher reactivity and can complete polymerization at room temperature without a catalyst, fundamentally avoiding the foaming defects caused by the need for catalysts and environmental moisture interference in the traditional polyurethane system due to the terminal hydroxyl route.

[0054] 3,5-Diaminobenzoic acid was selected as the single chain extender. The amino groups at both ends of its molecule participate in the polymerization of the polyurea backbone, achieving chain growth. Simultaneously, the carboxyl side groups (-COOH) in the molecule are introduced into the polyurea backbone, providing a pathway for subsequent Zn polymerization. 2+ Coordination crosslinking provides the necessary reaction sites. This design accomplishes both chain extension and functionalization simultaneously with a single molecule, eliminating the need for multiple chain extenders. This application does not use the binary chain extender 4,4'-diaminodiphenyl disulfide containing dynamic disulfide bonds and 1,4-cyclohexanedimethylamine containing an alicyclic structure because neither of these chain extenders contains a carboxyl group and therefore cannot react with Zn. 2+ Coordination reactions occur, preventing the construction of the core Zn in this application. 2+-Carboxyl dynamic coordination crosslinking network; and the above binary system belongs to the dynamic disulfide bond self-healing technology route, whose self-healing mechanism is fundamentally different from the metal coordination crosslinking mechanism of this application, and the two are irreplaceable.

[0055] Ionic liquids in polyurea matrices need to reach a percolation threshold to form continuous ion transport channels, giving the material stable ionic conductivity. At the same time, their anions and cations interact competitively with urea bonds and soft segment ether oxygen atoms on the polyurea molecular chain to exert a plasticizing effect, reduce the glass transition temperature, and enhance the mobility of molecular chain segments, thereby accelerating the self-healing process. In addition, imidazole cations endow the material with broad-spectrum antibacterial properties.

[0056] In some embodiments, the number-average molecular weight of the polypropylene glycol bis(2-aminopropyl ether) is 400–2000 g·mol⁻¹. -1 The ionic liquid is 1-ethyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide.

[0057] If the molecular weight is lower than 400 g·mol -1 If the soft segment chain length is too short, it cannot form an effective flexible phase region, resulting in excessive material rigidity, a significant decrease in elongation at break, and loss of elastomer characteristics; if the molecular weight is higher than 2000 g·mol⁻¹, the material will be too stiff. -1 Excessive dilution of the relative content of hard segments and insufficient physical crosslinking density lead to decreased tensile strength, poor dimensional stability, and difficulty in solution casting for film formation. Within this range, a good microphase separation structure can be formed between the soft segments and the urea bond hard segments, enabling the material to maintain excellent ductility and low-temperature flexibility while possessing sufficient mechanical strength and structural stability.

[0058] In some embodiments, the molar ratio of polypropylene glycol bis(2-aminopropyl ether), isophorone diisocyanate, and 3,5-diaminobenzoic acid is 1:(1.5-2.5):(0.5-1).

[0059] When polypropylene glycol bis(2-aminopropyl ether) is prepolymerized with isophorone diisocyanate, it is necessary to ensure a moderate excess or near-stoichiometry of isocyanate groups to form terminal isocyanate-based prepolymers. If the isophorone diisocyanate ratio is below 1.5, there are insufficient isocyanate groups, preventing the formation of terminal isocyanate-based prepolymers, reducing chain extension efficiency, and resulting in insufficient molecular weight. If it is above 2.5, there is an excessive amount of free isophorone diisocyanate monomer, and the chain extender preferentially reacts with it to form smaller molecules, leading to a decrease in the degree of polymerization. 3,5-Diaminobenzoic acid, as a chain extender, has its proportion determining the density of carboxyl side groups and the content of rigid hard segments. If the proportion is below 0.5, there are insufficient carboxyl coordination sites, affecting subsequent Zn... 2+The coordination crosslinking network is sparse, resulting in limited mechanical reinforcement. If the ratio is higher than 1, the proportion of rigid benzene ring hard segments is too high, which increases the brittleness of the material, reduces the elongation at break, and deteriorates the solution processing performance.

[0060] In some embodiments, the organic solvent is at least one of N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, or N-methylpyrrolidone.

[0061] All solvents are highly polar aprotic solvents with high dielectric constants and large dipole moments, which can simultaneously and effectively dissolve polyurea prepolymer, 3,5-diaminobenzoic acid, zinc chloride, and ionic liquids, ensuring that the reaction takes place in a homogeneous solution. More importantly, the above solvents can react with Zn through carbonyl oxygen or sulfoxide oxygen. 2+ Coordination solvation occurs, causing Zn 2+ Uniform dispersion to ensure subsequent Zn 2+ - Uniformity of carboxyl coordination crosslinking. The solvent molecules mentioned above do not contain active hydrogen, are chemically stable, and will not undergo side reactions with isocyanate groups under room temperature polymerization conditions, fundamentally avoiding foaming, chain termination, and stoichiometric mismatch problems. In addition, the boiling points of the solvents are in the range of 153-202℃, forming a reasonable gradient with the subsequent drying temperature of 50-70℃, ensuring the stable retention of the solvent during the reaction stage while facilitating complete removal through gentle heating during the drying stage. If protic solvents containing active hydrogen (such as water and alcohols) are used, the active hydrogen in the solvent molecules will react violently with the isocyanate groups, leading to uncontrolled polymerization, foaming of the material, and deterioration of mechanical properties. If weakly polar aprotic solvents (such as toluene and hexane) are used, polyurea, ionic liquids, and zinc chloride cannot be effectively dissolved, and phase separation occurs in the system, making it difficult to carry out homogeneous polymerization and solution casting. If highly volatile solvents (such as diethyl ether and acetone) are used, they evaporate too quickly at room temperature, making it impossible to maintain the stable homogeneous environment required for the polymerization reaction, and easily leading to uneven local concentrations and excessively wide molecular weight distribution.

[0062] Example The following describes embodiments of this application. The embodiments described below are exemplary and are only used to explain this application, and should not be construed as limiting this application. Where specific techniques or conditions are not specified in the embodiments, they are performed according to the techniques or conditions described in the literature in this field or according to the product instructions. Reagents or instruments used, unless otherwise specified, are all conventional products that can be obtained commercially.

[0063] Example 1 A Zn-based 2+ The preparation method of the self-healing polyurea-based conductive elastomer with carboxyl coordination crosslinking is as follows: S1. Synthesis of polyurea elastomers (PDU) containing carboxyl side groups: In this embodiment, polypropylene glycol bis(2-aminopropyl ether) PPG2000 (number average molecular weight M) was weighed. n ≈2000 g·mol -1 1 g (0.5 mmol) of N,N-dimethylformamide (DMF) was added to a 100 mL reaction flask with a 2 mm standard glass ground joint, and 10 mL of anhydrous N,N-dimethylformamide (DMF) was added. The mixture was stirred until the raw material was completely dissolved. Then, 10 mL of anhydrous DMF solution containing isophorone diisocyanate (IPDI, 1 mmol) was added dropwise to the PPG2000 solution. After the addition was complete, the reaction mixture was stirred continuously at room temperature for 6 h. Subsequently, 3,5-diaminobenzoic acid (DABA, 0.5 mmol) was added to the system, and the reaction was stirred for another 6 h. The entire reaction was carried out at room temperature under a dry nitrogen atmosphere. After the reaction was completed, the resulting polyurea solution was cast into a polytetrafluoroethylene (PTFE) mold using a solution casting method. The solution was cured at 60 °C and the residual solvent DMF was completely removed, finally yielding a polyurea elastomer containing carboxyl side groups, denoted as PDU.

[0064] The purpose of this step is to prepare a flexible polyurea elastomer containing carboxyl side groups, which will be used in the subsequent construction of Zn. 2+ - The carboxyl-based dynamic coordination network provides coordination sites. PPG2000, as a flexible soft segment, imparts excellent ductility and low-temperature flexibility to the material; IPDI, as a rigid hard segment, provides mechanical strength and structural stability; the two amino groups on the DABA molecule react with the isocyanate groups at the prepolymer end, introducing carboxyl side groups into the polyurea backbone, which is crucial for the formation of Zn. 2+ The coordination and crosslinking sites are crucial. The preferred molar ratio of PPG2000 to IPDI is 1:2 to ensure that both ends of the prepolymer are isocyanate groups, facilitating subsequent chain extension reactions. The amount of DABA added is 1.0 times the molar amount of PPG2000 (i.e., 0.5 mmol) to ensure a moderate grafting density of carboxyl side groups: if there is too little DABA, there will be insufficient carboxyl coordination sites, resulting in a low crosslinking density and difficulty in forming an effective metal coordination network; if there is too much DABA, the proportion of rigid hard segments in the system will be too high, reducing the flexibility of the material.

[0065] S2, Zn 2+ Synthesis of carboxyl-coordinated crosslinked polyurea elastomer (PDUZn0.5): In this embodiment, the PDU obtained from S1 was dissolved in 20 mL of DMF, and then mixed with a ZnCl2 solution (0.5 mmol / L). The mixture was stirred thoroughly at room temperature under a dry nitrogen atmosphere to allow the ZnCl2 solution to settle. 2+ The solution was uniformly dispersed and coordinated with the carboxyl groups in the PDU. The solution was then poured into a PTFE mold and vacuum dried at 60 °C to remove the solvent and complete crosslinking, yielding Zn. 2+-Carboxyl-coordinated crosslinked polyurea elastomer, named PDUZn0.5.

[0066] S3. Synthesis of polyurea-based conductive elastomer (PDUZn0.5-10IL): In this embodiment, the PDUZn0.5 (1.4 g) elastomer obtained in S2 was added to 40 mL of DMF and magnetically stirred until dissolved. Then, 10 wt% (0.2 g) of the ionic liquid [EMIM][TFSI] was added to the solution, and stirring was continued for 30 min at room temperature and under a dry nitrogen atmosphere to ensure uniform mixing. The mixture was then poured into a PTFE mold, and the solvent was evaporated at 60 °C to obtain the conductive elastomer, named PDUZn0.5-10IL.

[0067] Example 2 A Zn-based 2+ The preparation method of the carboxyl-coordinated crosslinked self-healing polyurea conductive elastomer is the same as steps S1 and S2 in Example 1, except that: S3. Synthesis of polyurea-based conductive elastomer (PDUZn0.5-20IL): In this embodiment, the PDUZn0.5 (1.4 g) elastomer obtained in S2 was added to 40 mL of DMF and magnetically stirred until dissolved. Then, 20 wt% (0.3 g) of the ionic liquid [EMIM][TFSI] was added to the solution, and stirring was continued for 30 min at room temperature and under a dry nitrogen atmosphere to ensure uniform mixing. The mixture was then poured into a PTFE mold, and the solvent was evaporated at 60 °C to obtain the conductive elastomer, named PDUZn0.5-20IL.

[0068] Example 3 A Zn-based 2+ The preparation method of the carboxyl-coordinated crosslinked self-healing polyurea conductive elastomer is the same as steps S1 and S2 in Example 1, except that: S3. Synthesis of polyurea-based conductive elastomer (PDUZn0.5-30IL): In this embodiment, the PDUZn0.5 (1.4 g) elastomer obtained in S2 was added to 40 mL of DMF and magnetically stirred until dissolved. Then, 30 wt% (0.6 g) of the ionic liquid [EMIM][TFSI] was added to the solution, and stirring was continued for 30 min at room temperature and under a dry nitrogen atmosphere to ensure uniform mixing. The mixture was then poured into a PTFE mold, and the solvent was evaporated at 60 °C to obtain a conductive elastomer, named PDUZn0.5-30IL.

[0069] Example 4 A Zn-based2+ The method for preparing the carboxyl-coordinated crosslinked self-healing polyurea conductive elastomer differs from step S1 in Example 2 only in that: S2, Zn 2+ Synthesis of carboxyl-coordinated crosslinked polyurea elastomer (PDUZn0.25): In this embodiment, the PDU obtained from S1 was dissolved in 20 mL of DMF, and then mixed with a ZnCl2 solution (0.25 mmol / L). The mixture was stirred thoroughly at room temperature under a dry nitrogen atmosphere to allow the ZnCl2 solution to settle. 2+ The solution was uniformly dispersed and coordinated with the carboxyl groups in the PDU. The solution was then poured into a PTFE mold and vacuum dried at 60 °C to remove the solvent and complete crosslinking, yielding Zn. 2+ -Carboxyl-coordinated crosslinked polyurea elastomer, named PDUZn0.25.

[0070] S3. Synthesis of polyurea-based conductive elastomer (PDUZn0.25-20IL): In this embodiment, the PDUZn0.25 (1.4 g) elastomer obtained in S2 was added to 40 mL of DMF and magnetically stirred until dissolved. Then, 20 wt% (0.3 g) of the ionic liquid [EMIM][TFSI] was added to the solution, and stirring was continued for 30 min at room temperature and under a dry nitrogen atmosphere to ensure uniform mixing. The mixture was then poured into a PTFE mold, and the solvent was evaporated at 60 °C to obtain the conductive elastomer, named PDUZn0.25-20IL.

[0071] Example 5 A Zn-based 2+ The preparation method of the carboxyl-coordinated crosslinked self-healing polyurea conductive elastomer is the same as step S1 in Example 2, except that: In this embodiment, the PDU obtained from S1 was dissolved in 20 mL of DMF, and then mixed with a ZnCl2 solution (0.75 mmol / L). The mixture was stirred thoroughly at room temperature under a dry nitrogen atmosphere to allow the ZnCl2 solution to settle. 2+ The solution was uniformly dispersed and coordinated with the carboxyl groups in the PDU. The solution was then poured into a PTFE mold and vacuum dried at 60 °C to remove the solvent and complete crosslinking, yielding Zn. 2+ -Carboxyl-coordinated crosslinked polyurea elastomer, named PDUZn1.

[0072] S3. Synthesis of polyurea-based conductive elastomer PDUZn1-20IL: In this embodiment, the PDUZn0.5 (1.4 g) elastomer obtained in S2 was added to 40 mL of DMF and magnetically stirred until dissolved. Then, 20 wt% (0.3 g) of the ionic liquid [EMIM][TFSI] was added to the solution, and stirring was continued for 30 min at room temperature and under a dry nitrogen atmosphere to ensure uniform mixing. The mixture was then poured into a PTFE mold, and the solvent was evaporated at 60 °C to obtain the conductive elastomer, named PDUZn1-20IL.

[0073] The instruments and characterization methods used are as follows: (1) Infrared spectroscopy (FT-IR): The test was performed using a Spectrum Fourier transform infrared spectrometer from PerkinElmerg, USA. The wavelength range of the absorption spectrum scan was 500 cm⁻¹. -1 -4000cm -1 .

[0074] (2) Scanning electron microscopy (SEM) and energy dispersive X-ray spectroscopy (EDS): The surface morphology of the sample was observed using the Quattro S scanning electron microscope from Thermo Fisher Scientific, and elemental surface scanning analysis was performed in conjunction with EDS.

[0075] (3) Mechanical property testing: The mechanical properties were tested using a CMT6103 electronic universal testing machine from Meters Industrial Systems. The samples were prepared using a dumbbell-shaped polytetrafluoroethylene mold of national standard type I. The tensile rate during the test was 50 mm·min. -1 By plotting stress as the Y-axis and strain as the X-axis, the stress-strain curve of the conductive elastomer can be obtained.

[0076] (4) Sensing performance testing: The tests were conducted using the CHI760E electrochemical workstation from Shanghai Chenhua Instruments Co., Ltd. When testing the conductivity and sensing performance of the conductive elastomer sample, the conductive elastomer was prepared into a 30mm diameter using a polytetrafluoroethylene mold. 15mm The electrode is 3mm in size, secured at both ends with double-ended alligator clips. The other end of the alligator clips is connected to an electrochemical workstation. The IT mode is selected to record the strain current change of the conductive elastomer, and the strain sensing signal is represented by the relative resistance change (ΔR / R0). The resistance (R, Ω) is calculated using the following formula:

[0077] In the formula, Voltage (V) applied to the electrochemical workstation. The current (A) of the conductive elastomer.

[0078] The change in relative resistance is calculated using the following formula:

[0079] In the formula, R is the resistance value of the conductive elastomer when strain is applied, and R0 is the initial resistance value of the conductive elastomer.

[0080] The sensitivity of a flexible sensor assembled from conductive elastomers is typically measured by the normalization factor (GF), which is calculated using the following formula.

[0081]

[0082] In the formula This represents the change in relative resistance. The strain applied to the conductive elastomer includes the applied force.

[0083] (5) Self-healing test of mechanical properties: The test was conducted using a CMT6103 electronic universal testing machine from MTES Industrial Systems. After the sample was completely cut with a scalpel, the two cut surfaces were immediately and completely bonded together. The sample was placed at room temperature for a period of time to allow it to self-heal, and then the self-healing efficiency was tested using the universal testing machine. Self-healing efficiency ( It can be calculated using the following formula.

[0084]

[0085] In the formula The fracture strength or elongation at break after self-healing is considered. This represents the breaking strength or elongation at break of the original conductive elastomer.

[0086] (6) Self-healing test of conductivity: The test was conducted using the CHI760E electrochemical workstation of Shanghai Chenhua Instrument Co., Ltd. Both ends of the sample were fixed with double-ended alligator clip electrodes, and the other end of the alligator clip electrodes was connected to the electrochemical workstation. The it mode was selected to record the current change of the conductive elastomer. The sample was completely cut off by an insulated plastic blade. After waiting for a period of time, the cut surfaces were put back together. After the current stabilized, the current recovery time was recorded.

[0087] Examples 1 to 5 of this application all yielded high-strength, high-self-healing-efficiency Zn-based materials. 2+ -Self-healing polyurea-based conductive elastomers with carboxyl coordination crosslinking are described below, using conductive elastomers obtained in Examples 1-3 (with different ionic liquid contents) and conductive elastomers obtained in Examples 2, 4, and 5 (with different Zn content). 2+ Taking the content as an example, the specific research methods and results are as follows: like Figure 1 As shown, this application is based on Zn 2+The synthesis of self-healing polyurea-based conductive elastomers with carboxyl coordination crosslinking is divided into three stages: synthesis of polyurea elastomers (PDU) containing carboxyl side groups, Zn... 2+ - Construction of carboxyl-coordinated crosslinked polyurea elastomer PDUZnx, and its composite and crosslinking with ionic liquids.

[0088] First, isocyanate-terminated polyurea prepolymers were synthesized via a prepolymerization reaction using PPG2000 and IPDI. Then, DABA was used as a chain extender; its two amino groups reacted with the isocyanate-terminated groups of the prepolymer, introducing carboxyl side groups into the polyurea backbone. The addition of DABA simultaneously introduced carboxyl functional groups into the system, facilitating subsequent Zn synthesis. 2+ Coordination crosslinking provides reaction sites. Finally, ZnCl2 is mixed with PDU, Zn 2+ It coordinates with the carboxyl groups on the PDU chain to form a dynamic metal coordination crosslinking network; the introduction of ionic liquids [EMIM][TFSI] forms continuous ion transport channels in the network.

[0089] The study found that achieving the desired effect at each stage of the above synthetic route requires strict control of the following key factors: First, the prepolymerization reaction must be carried out stepwise. PPG2000 must first react fully with IPDI to form a prepolymer with terminal isocyanate groups before introducing DABA for chain extension, in order to ensure the activity of the prepolymer end groups and the statistical distribution of DABA on the main chain. Second, the amount of DABA must be matched with the end groups of the prepolymer. The amino groups at both ends react with the terminal isocyanate groups to uniformly introduce carboxyl side groups into the polyurea main chain. Insufficient DABA will result in sparse carboxyl sites, while excessive DABA will result in excessive aggregation of rigid hard segments. Third, ZnCl2 must be added after the polyurea chain construction is completed. After the DABA chain extension reaction is sufficient and a polyurea elastomer with carboxyl side groups is formed, ZnCl2 is then introduced. 2+ Coordination crosslinking occurs, preventing Zn 2+ Fourth, Zn interferes with the polymerization reaction during the prepolymerization stage; 2+ The molar ratio of the ionic liquid to the carboxyl group must be within a dynamic equilibrium range (1:2 to 6:1) to ensure that the coordination crosslinking density is sufficient to bear the load and also possesses reversible dissociation activity; fifth, the ionic liquid must be added after the coordination network has formed, and molecular-level uniform dispersion should be achieved through solution blending to avoid mixing with Zn. 2+ Competition for coordination or localized enrichment may occur; sixth, the entire process must be carried out at room temperature, in a dry nitrogen atmosphere, and in a strongly polar aprotic solvent to suppress side reactions of the isocyanate groups and ensure the Zn 2+ Uniform dissolution with ionic liquids.

[0090] Figure 1 In the enlarged illustration on the right, solid lines represent the polyurea covalent backbone, dashed lines represent hydrogen bonds between carboxyl groups and between carboxyl groups and polyurea segments, and dots and nodes correspond to Zn. 2+Coordination and crosslinking with carboxyl groups. Under external force, the polyurea covalent chain provides the basic load-bearing capacity, the hydrogen bond network preferentially breaks to dissipate energy, while Zn... 2+ -Carboxyl coordination bonds can undergo reversible dissociation and recombination, achieving stress release and structural reconstruction; when the external force is removed or the crack closes, the remaining carboxyl / Zn 2+ Hydrogen bond interactions re-establish cross-linking points, restoring conductive pathways and mechanical networks, thereby endowing conductive elastomers with high strength, high elongation, and self-healing capabilities.

[0091] The factors contributing to the aforementioned triple network synergistic response are as follows: First, the polyurea covalent backbone must maintain a linear topology, forming a linear polymer without irreversible chemical crosslinks through polymerization, providing the necessary degrees of freedom for molecular chain segments. If irreversible crosslinks are introduced into the backbone, the dynamic response of hydrogen bonds and coordination bonds will be frozen, and the stress transfer and energy dissipation mechanisms will fail. Second, the hydrogen bond network must form a reasonable bond energy level difference. A difference in energy levels must be maintained between strong hydrogen bonds between urea bonds and weak hydrogen bonds between carboxyl groups / soft segments / ionic liquids, so that weak hydrogen bonds preferentially break and dissipate energy under external force, while strong hydrogen bonds maintain the integrity of the network framework. If the hydrogen bond network strength is uniform, all hydrogen bonds will break simultaneously under stress, resulting in brittle failure rather than ductile dissipation. Third, Zn 2+ -Carboxyl coordination bonds must possess moderate bond energy and exchange rate, and their strength must be sufficient to provide physical crosslinking load under static conditions, while also being capable of reversible dissociation-recombination under thermal stimulation; if the coordination bond is too strong (e.g., Fe), it will cause damage. 3+ If the group is too weak (e.g., Ca), it cannot dissociate at room temperature, and self-repair requires stringent conditions; if it is too weak (e.g., Ca), it cannot dissociate at room temperature. 2+ -Carboxyl groups), therefore, cannot be effectively supported. Fourth, the ionic conductivity channels of the ionic liquid must be interlocked with the mechanical network topology, achieving synchronous response of mechanical deformation and ion migration through uniform dispersion at the molecular level; if the ionic liquid is only physically attached to the surface, the conductivity channels cannot be synchronously rebuilt during mechanical network repair. Fifth, the repair conditions must match the network dynamics. This application uses heat treatment at 40℃ for 10 h, which is consistent with the Zn... 2+ The dissociation-reorganization kinetics of the carboxyl coordination bond are matched with the plasticizing effect of the ionic liquid, ensuring that hydrogen bonds and coordination bonds synergistically drive interface reconstruction.

[0092] Figure 2 The following are the infrared spectra of the conductive elastomers prepared in Examples 1 to 3. The FTIR spectroscopy results clearly confirm the successful synthesis of PDU: after polymerization, IPDI reaches a concentration at 2260 cm⁻¹. -1 -NCO characteristic peak, DABA 3200cm -1 The complete disappearance of the -NH2 absorption peak indicates that the monomer's active group has fully participated in the reaction; simultaneously, the PDU absorption peak at 3320 cm⁻¹... -1 1650 cm -11550cm -1 The presence of a characteristic absorption peak for the urea group confirms the successful formation of the urea bond. Additionally, Zn... 2+ After coordination with the polyurea chain segment, the absorption peaks of the characteristic functional groups of polyurea underwent a systematic redshift (shift towards lower wavenumbers): among which, the characteristic peak of the NH stretching vibration of the urea group (3200–3400 cm⁻¹) was significantly redshifted. -1 ), characteristic peak of C=O stretching vibration (1600~1700 cm⁻¹) -1 ) and the characteristic peak of NH bending vibration (1500~1550 cm) -1 Both exhibited significant low wavenumber shifts. This phenomenon can be attributed to the N and O atoms of the urea group in the polyurea segment acting as electron donors, transferring electrons to Zn. 2+ The empty orbitals provide lone pairs of electrons to form coordinate bonds. After ionic liquid doping, all samples retained the characteristic absorption peaks of polyurea, including the peak at 3300 cm⁻¹. -1 The NH stretching vibration peak at 2900 cm⁻¹ -1 CH stretching vibration peak at 1650 cm⁻¹ -1 The C=O stretching vibration peak at 3300 cm⁻¹ indicates that the introduction of the ionic liquid did not disrupt the basic chemical structure of the matrix. With increasing ionic liquid content, the peak at 3300 cm⁻¹... -1 The intensity of the NH characteristic peak gradually decreases, the peak shape broadens, and it shifts slightly to lower wavenumbers. This is because the ionic liquid anions and cations form competitive hydrogen bonds with the polyurea segments, disrupting the original strong intermolecular hydrogen bond network of polyurea and reducing the NH bond constant. This provides a structural basis for improving the material's free volume and ion transport efficiency. (At 1000–1600 cm⁻¹) -1 The fingerprint area, 1500–1600 cm -1 The region gradually exhibits characteristic peaks of C=N and C=C skeletal stretching vibrations of ionic liquid cations (such as imidazole rings), and the absorption peak intensity significantly increases with increasing ionic liquid content, directly confirming the successful loading and uniform dispersion of the ionic liquid in the matrix; 1000–1200 cm⁻¹ -1 The splitting of the CN / CO skeleton vibration peaks in the region and the appearance of new shoulder peaks indicate that there is a strong hydrogen bond interaction between the ionic liquid and the polyurea polar groups, which stabilizes the internal structure of the composite material.

[0093] Figure 3The stress-strain curves of the conductive elastomers prepared in Examples 1 to 3 are shown. Experimental results show that with the continuous increase of ionic liquid (IL) addition, the effective hydrogen bond crosslinking density between polyurea molecular chains continuously decreases, and the constraint effect of physical crosslinking points on molecular chain segment slippage weakens, which is directly reflected in a decrease in mechanical strength macroscopically. Specifically, when the IL addition is 10 wt%, the tensile strength of the PDUZn0.5-10IL sample reaches 6.0 MPa, and the elongation at break is approximately 1300%; when the IL addition is increased to 20 wt%, the tensile strength of the PDUZn0.5-20IL sample is 4.2 MPa, with a corresponding elongation at break of approximately 1100%; even when the IL addition is further increased to 30 wt%, the PDUZn0.5-30IL sample still maintains a tensile strength of 2.9 MPa and an elongation at break of 850%, maintaining excellent tensile ductility and a certain mechanical load-bearing capacity.

[0094] Figure 4 The relative resistance-time response (RRT) of the PDUZn0.5-20IL conductive elastomer sample prepared in Example 2 under different strain ranges is shown in Figure a (Figure a) and the comparison of the normalization factor (GF) is shown in Figure b (Figure b). As the strain of the conductive elastomer increases from 100% to 200%, the relative resistance increases from an average of 300% to an average of 720%. Within the test strain range of 0–200%, the GF value of this sample exhibits good linear response characteristics, with its GF value stabilizing at around 4.0. This result indicates that the sensor possesses excellent and stable linear sensing response capability over a wide strain range, and can meet the detection requirements of different strain amplitudes.

[0095] Figure 5 The images show the joint sensing signal diagrams of the PDUZn0.5-20IL conductive elastomer sample prepared in Example 2. Figure a shows the electrical signal response of finger joint bending, figure b shows the electrical signal response of wrist joint bending, figure c shows the electrical signal response of knee joint bending, and figure d shows the electrical signal response of elbow joint bending. Experimental results show that the PDUZn0.5-20IL-based flexible sensor can generate a rapid and sensitive electrical signal response to multi-angle gradual bending movements of the finger joints. Its signal changes can accurately match changes in the joint movement amplitude, achieving precise sensing of subtle finger joint movements. For reciprocating flexion and extension movements of the wrist, elbow, and knee joints, the sensor can also output stable and regular dynamic response curves without signal drift, amplitude attenuation, or other abnormal phenomena. This indicates that the PDUZn0.5-20IL conductive elastomer can well adapt to the sensing needs of joint movements in multiple parts of the human body and has excellent real-time human motion monitoring performance.

[0096] Figure 6The micro-motion sensing signal diagrams of the PDUZn0.5-20IL conductive elastomer sample prepared in Example 2 are shown in Figure a. Figure a shows the electrical signal response diagram of pulse fluctuations. It can be seen that the electrical signal output by the sensor can form a periodic response that is completely synchronized with the human pulse, accurately capturing subtle changes in pulse fluctuations without signal delay or baseline drift. Figure b shows the electrical signal response diagram of respiration. The results show that the sensor has good response sensitivity to normal respiratory rhythms and can stably capture the signal changes caused by each breath, fully meeting the practical application requirements of long-term respiratory monitoring. Figure c shows the electrical signal response diagram of the internationally recognized SOS emergency code compression. The results show that the sensor produces a clear electrical response to the specific compression sequence corresponding to SOS, with not only fast response speed but also high signal recognition, enabling stable transmission of silent distress signals. Figure d shows the electrical signal response when writing "Fire". This sensor can produce a sensitive and stable electrical response to different strokes and different pressure during the writing process. The signals corresponding to different writing actions are significantly different, and the writing trajectories of different English letters can be clearly distinguished.

[0097] Figure 7 Figure 1 shows the self-healing performance of the PDUZn0.5-xIL conductive elastomer series samples prepared in Examples 1 to 3 of this application. Figure 2a shows the mechanical self-healing performance. When the ionic liquid content increases from 0 wt% to 30 wt%, the mechanical repair efficiency of the conductive elastomer samples remains at an excellent level of over 90%, and the repair efficiency gradually increases with the increase of ionic liquid content. This is because the self-healing performance of the system has a significant component dependence; the self-healing efficiency of the material is significantly positively correlated with the amount of ionic liquid doping, that is, the higher the amount of ionic liquid doping, the better the self-healing efficiency of the material. Figure b shows the electrical self-healing performance of the PDUZn0.5-20IL sample in Example 2. At the moment the sample is completely cut off, the resistance jumps abruptly. This is because after the physical fracture of the sample, the internal conductive path is completely interrupted, which leads to a sharp increase in resistance. When the two fracture surfaces are precisely aligned and bonded, the sample resistance drops rapidly within 300ms, quickly recovering to the initial resistance level before the damage. Moreover, the resistance after repair is not significantly different from the initial value, and no significant residual resistance or signal drift phenomenon is observed, demonstrating excellent electrical reversible recovery capability.

[0098] Figure 8The graph shows the antibacterial properties and biocompatibility of the PDUZn0.5-20IL conductive elastomer sample prepared in Example 2. In Figure a, a large number of dense colony-forming units (CFUs) appeared in the culture dishes corresponding to both the control group and the PDU sample, indicating that the pure polyurea substrate itself has extremely low inherent antibacterial activity and almost no antibacterial ability. With the gradual introduction of functional components, the number of colonies in the culture dishes showed a clear gradient decreasing trend: the number of colonies in the PDUZn0.5 group was significantly lower than that in the control group. This is because Zn... 2+ As a low-toxicity and highly effective inorganic antibacterial component, it exhibits broad-spectrum antibacterial inhibitory activity against both *Escherichia coli* and *Staphylococcus aureus*. In Figure b, the bacterial survival rate in both the control group and the pure PDU group was 100%, showing no significant antibacterial activity. The PDUZn0.5 group showed inhibition rates of approximately 85% and 87% against *Escherichia coli* and *Staphylococcus aureus*, respectively, demonstrating a certain level of antibacterial ability. The PDUZn0.5-20IL group achieved inhibition rates exceeding 99% against both strains, with an inhibition rate as high as 99.3% against *Escherichia coli* and 99.1% against *Staphylococcus aureus*. This result further confirms that the composite material possesses excellent broad-spectrum antibacterial properties. The effect of PDUZn0.5-20IL conductive elastomer on the viability of human skin fibroblasts was investigated using the CCK-8 assay. Figure c shows that after incubation of human skin fibroblasts with extracts at concentrations of 6.25 mg / mL and 12.25 mg / mL for 24 h, the relative viability of the cells was not significantly different from the control group, and remained above 95%. This indicates that the conductive elastomer material has excellent biocompatibility and can fully meet the safety requirements for long-term contact between wearable devices and human skin, providing biosafety assurance for its practical application.

[0099] This application develops a Zn-based... 2+ A self-healing polyurea-based conductive elastomer with carboxyl coordination crosslinking is prepared using a simple process involving a polyurea covalent network and Zn... 2+ The triple synergy of the carboxyl dynamic coordination network and the ionic liquid ion conduction network achieves simultaneous optimization of mechanical strength, self-healing efficiency, conductivity, and biocompatibility. This material has significant application prospects in human motion monitoring, health diagnosis, rehabilitation therapy, and human-computer interaction.

[0100] It should be noted that this application is not limited to the above-described embodiments. The above embodiments are merely examples, and any embodiments with the same structure and effect as the technical concept within the scope of this application are included in the technical scope of this application. Furthermore, various modifications that can be conceived by those skilled in the art to the embodiments, and other ways of constructing by combining some of the constituent elements of the embodiments, without departing from the spirit of this application, are also included in the scope of this application.

Claims

1. based on Zn 2+ - process for the preparation of carboxyl-coordinately crosslinked self-healing polyurea-based conductive elastomers, characterized in that, Includes the following steps: S1. Synthesis of polyurea elastomers (PDU) containing carboxyl side groups: Polypropylene glycol bis(2-aminopropyl ether) and isophorone diisocyanate were dissolved separately in organic solvents. Under a dry nitrogen atmosphere at room temperature, isophorone diisocyanate solution was added dropwise to the polypropylene glycol bis(2-aminopropyl ether) solution. The mixture was stirred continuously at room temperature to carry out a prepolymerization reaction, yielding an isocyanate-terminated polyurea prepolymer. 3,5-Diaminobenzoic acid was added to the isocyanate-terminated polyurea prepolymer as a chain extender to carry out a chain extension reaction. The entire reaction was carried out at room temperature under a dry nitrogen atmosphere. After the reaction was completed, the polyurea elastomer containing carboxyl side groups was obtained by solution casting and drying, denoted as PDU. S2, Zn 2+ Synthesis of carboxylate-coordinating cross-linked polyurea elastomers (PDUZn): PDU is dissolved in an organic solvent, then zinc chloride solution is added, the mixture is stirred uniformly at room temperature under dry nitrogen atmosphere, and Zn 2+ carboxyl groups on the molecular chain of PDU to form a coordination crosslinking reaction; after the reaction is completed, solution casting and drying are performed to obtain Zn 2+ carboxyl coordination crosslinking polyurea elastomer; S3. Synthesis of polyurea-based conductive elastomer (PDUZn-IL): Zn 2+ - carboxylate coordination cross-linked polyurea elastomer is dissolved in an organic solvent, then an ionic liquid is added, and the mixture is stirred uniformly at room temperature under a dry nitrogen atmosphere, solution casting, drying, to obtain a Zn 2+ - carboxylate coordination cross-linked self-repairing polyurea-based conductive elastomer.

2. The Zn-based alloy according to claim 1, wherein the Zn-based alloy contains 0.0001 to 0.1% of Mg. 2+ Process for the preparation of carboxyl-coordinately crosslinked self-healing polyurea-based conductive elastomers, characterized in that, The number average molecular weight of the polypropylene glycol bis(2- aminopropyl ether) is 400 to 2000 g·mol -1 .

3. The Zn-based alloy according to claim 1, wherein the Zn-based alloy contains 0.0001 to 0.1% of Mg. 2+ Process for the preparation of carboxyl-coordinately crosslinked self-healing polyurea-based conductive elastomers, characterized in that, The ionic liquid is 1-ethyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide.

4. The Zn-based alloy according to claim 1, wherein the Zn-based alloy contains 0.0001 to 0.1% of Mg. 2+ Process for the preparation of carboxyl-coordinately crosslinked self-healing polyurea-based conductive elastomers, characterized in that, The molar ratio of polypropylene glycol bis(2-aminopropyl ether), isophorone diisocyanate, and 3,5-diaminobenzoic acid is 1:(1.5-2.5):(0.5-1).

5. The Zn-based alloy according to claim 1, wherein the Zn-based alloy contains 0.0001 to 0.1% of Mg. 2+ Process for the preparation of carboxyl-coordinately crosslinked self-healing polyurea-based conductive elastomers, characterized in that, The organic solvent is at least one of N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, or N-methylpyrrolidone.

6. The Zn-based [system / mechanism] according to claim 1 2+ A method for preparing a self-healing polyurea-based conductive elastomer with α-carboxyl coordination crosslinking, characterized in that... In the coordination crosslinking reaction, the amount of zinc chloride solution added satisfies the molar ratio of -COOH in the molecular chain of the polyurea elastomer containing carboxyl side groups to Zn 2+ is (1:2)~(6:1).

7. The Zn-based alloy according to claim 1, wherein the Zn-based alloy contains 0.0001 to 0.1% of Mg. 2+ Process for the preparation of carboxyl-coordinately crosslinked self-healing polyurea-based conductive elastomers, characterized in that, The amount of the ionic liquid added is 0.1 to 10 wt% of Zn 2+ - 5 wt% to 40 wt% of the mass of the carboxyl-coordinated cross-linked polyurea elastomer.

8. The Zn-based [system / mechanism] according to claim 1 2+ A method for preparing a self-healing polyurea-based conductive elastomer with α-carboxyl coordination crosslinking, characterized in that... The prepolymerization reaction takes 4 to 12 hours, and the chain extension reaction takes 4 to 12 hours.

9. Based on Zn 2+ A self-healing polyurea-based conductive elastomer with carboxyl-coordinated crosslinking, characterized in that... The conductive elastomer obtained by the preparation method according to any one of claims 1-8.

10. Based on Zn 2+ The application of self-healing polyurea-based conductive elastomers with carboxyl coordination crosslinking is characterized by... The conductive elastomer described in claim 9 is used to prepare flexible wearable sensors, human motion monitoring devices, or health monitoring devices.