A process for preparing PET-based high-toughness recycled modified plastics

By constructing a polyurethane elastomer system consisting of waste PET degradation products, soybean oil polyol, polycaprolactone diol, and modified cellulose nanocrystals, the problems of insufficient toughness and weak interfacial bonding of polyurethane elastomers were solved, achieving a balance and stability of material properties with high toughness and high strength.

CN123107033APending Publication Date: 2026-11-17WEINAN KELINLE ENVIRONMENTAL PROTECTION TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611507781.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-28
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In the existing technology, polyurethane elastomers prepared from waste PET degradation products have insufficient toughness, uneven stiffness and toughness, low strength of bio-based polyols, weak interfacial bonding between fillers and matrix, and non-reactive additives affect the stability of the material.

Method used

A polyurethane elastomer system was constructed using waste PET degradation products, soybean oil polyol, polycaprolactone diol, and modified cellulose nanocrystals. Flexible segments were formed by reacting epoxidized soybean oil with itaconic acid, polycaprolactone diol provided crystallinity, cellulose nanocrystals were surface-modified to enhance interfacial compatibility, and gallium indium tin alloy was added to assist in toughening.

Benefits of technology

It achieves a balance between high toughness and high strength, improves the interfacial compatibility and stability of the material, avoids performance fluctuations caused by raw material fluctuations, and enhances the mechanical properties and thermal stability of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123107033A_ABST
    Figure CN123107033A_ABST
Patent Text Reader

Abstract

This invention discloses a process for preparing PET-based high-toughness recycled modified plastics, belonging to the field of polymer material recycling technology, including: raw material preparation, soybean oil polyol synthesis, polycaprolactone diol pretreatment, polyurethane prepolymer preparation, chain extension reaction, elastomer curing, cellulose nanofiber modification, and composite molding. This invention uses waste PET degradation products in conjunction with aromatic amines to construct a composite chain extension system, achieving high-value utilization of recycled resources while avoiding the brittleness defects caused by single recycled components. Furthermore, the design of composite soft segments combining bio-based soybean oil polyol and polycaprolactone diol imparts intrinsic flexibility to the material. Further, the cellulose nanofibers are aminated using a silane coupling agent to enhance chemical bonding with the polyurethane matrix. The introduction of gallium indium tin alloy liquid metal microregions as dynamic stress dissipation centers improves the balance between strength and toughness of the recycled PET-based plastics and increases the compatibility of the filler interface.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of polymer material recycling technology, specifically to a process for preparing PET-based high-toughness recycled modified plastics. Background Technology

[0002] Polyurethane elastomers are widely used in films, coatings, and engineering plastics due to their excellent mechanical properties and wear resistance. With increasing environmental protection requirements, the use of waste polyethylene terephthalate (PET) degradation products as chain extenders to prepare recycled polyurethane materials has become a research hotspot. However, existing technologies for preparing polyurethane elastomers using waste PET degradation products still face the following problems: On the one hand, the molecular chains of waste PET degradation products are relatively rigid and the polar groups are unevenly distributed. When used directly as chain extenders, they have poor compatibility with soft segments, which can easily lead to excessive phase separation within the material, resulting in decreased toughness and insufficient elongation at break. On the other hand, bio-based polyols, such as soybean oil polyols, introduced to improve toughness can enhance flexibility, but their own strength is relatively low, making it difficult to achieve both high toughness and high strength. Moreover, existing modification methods mostly rely on single filler reinforcement, and the interfacial bonding between the filler and the matrix is ​​weak, making it prone to debonding and failure under stress. In addition, some processes add non-reactive additives to adjust viscosity or promote dispersion, which not only increases the difficulty of subsequent removal but may also leave residues that affect the long-term stability of the material.

[0003] Therefore, there is an urgent need to develop a process for preparing PET-based recycled modified plastics that can synergistically improve interfacial compatibility, achieve a balance between rigidity and toughness, and have controllable process control. Summary of the Invention

[0004] To address the aforementioned technical problems, a process for preparing PET-based high-toughness recycled modified plastics is provided, and this technical solution solves the problems described above.

[0005] To achieve the above objectives, the technical solution adopted by the present invention is as follows:

[0006] A process for preparing a PET-based high-toughness recycled modified plastic, wherein the process uses waste PET degradation products as chain extenders, and constructs a polyurethane elastomer system by compounding soybean oil polyol, polycaprolactone diol, and modified cellulose nanocrystals. The preparation steps include:

[0007] S1: Raw material preparation. Prepare the following raw materials by weight: epoxidized soybean oil, ethylene glycol, itaconic acid, polycaprolactone diol, isophorone diisocyanate, dibutyltin dilaurate, waste PET degradation products, 3,3'-dichloro-4,4'-diaminodiphenylmethane, 3-aminopropyltriethoxysilane, cellulose nanofibers, gallium indium tin alloy and organic solvents.

[0008] S2: Synthesis of soybean oil polyols: Epoxy soybean oil and ethylene glycol are mixed and itaconic acid is added. After stirring evenly, the mixture is placed in a high-temperature and high-pressure reactor for constant temperature reaction. After cooling, soybean oil polyols are obtained.

[0009] S3: Polycaprolactone diol pretreatment, the polycaprolactone diol is vacuum dehydrated and then cooled for later use.

[0010] S4: Preparation of polyurethane prepolymer: Soybean oil polyol is mixed with pretreated polycaprolactone diol, isophorone diisocyanate is added, the mixture is heated and reacted under nitrogen protection, and a catalyst is added dropwise to continue the reaction to obtain polyurethane elastomer prepolymer.

[0011] S5: Chain extension reaction. Waste PET degradation products are mixed with 3,3'-dichloro-4,4'-diaminodiphenylmethane, vacuum dried, and then dissolved in acetone. The mixture is then added dropwise to the prepolymer while cooling. Acetone is added according to the viscosity of the system to maintain a uniform stirring state and the reaction continues to obtain a viscous solution.

[0012] S6: Elastomer curing: After degassing the viscous solution, it is cast into a film, cured at room temperature, cured in an oven, and the residual solvent is removed by vacuum to obtain a polyurethane elastomer;

[0013] S7: Modified cellulose nanofibers: 3-aminopropyltriethoxysilane was hydrolyzed in an aqueous ethanol solution, followed by the addition of cellulose nanofibers and stirring. The mixture was then washed, centrifuged, and dried to obtain modified cellulose nanofibers.

[0014] S8: Composite molding, the modified cellulose nanocrystals are dispersed in an organic solvent by ultrasonic dispersion treatment, polyurethane elastomer and gallium indium tin alloy are added and stirred to dissolve, after degassing, casting and drying, to obtain PET-based high-toughness recycled modified plastic.

[0015] Preferably, in S1, the raw materials are proportioned by weight as follows: 30 parts of epoxidized soybean oil, 30 parts of ethylene glycol, 0.3 parts of itaconic acid, 29-31 parts of polycaprolactone diol, 32-34 parts of isophorone diisocyanate, 0.5-0.6 parts of dibutyltin dilaurate, 3.9-7.9 parts of waste PET degradation products, 2-5 parts of 3,3'-dichloro-4,4'-diaminodiphenylmethane, 2 parts of 3-aminopropyltriethoxysilane, 1 part of cellulose nanofibers, and 4-10 parts of gallium indium tin alloy.

[0016] Preferably, in step S2, after the epoxy soybean oil, ethylene glycol and itaconic acid are magnetically stirred evenly in a beaker, they are poured into a high-temperature and high-pressure stainless steel reactor and reacted at a constant temperature of 140°C for 2 hours. The reaction endpoint is determined by the acid value dropping to ≤5mgKOH / g. After the reaction is completed, the mixture is naturally cooled to room temperature.

[0017] Preferably, in step S3, the vacuum degree of vacuum dehydration is 0.08 MPa, the temperature is 110-120°C, the dehydration time is 3 hours, and the vacuuming is stopped after the dehydration is completed and the temperature is lowered to 50-60°C.

[0018] Preferably, in step S4, the reaction is carried out in a three-necked flask equipped with a polytetrafluoroethylene stirrer and a serpentine condenser. The water bath is heated to 80°C, the stirring speed is set to 250 r / min, the catalyst dibutyltin dilaurate is added dropwise after reacting for 1 hour, and the reaction continues for 2 hours under nitrogen protection throughout.

[0019] Preferably, in step S5, the vacuum degree of vacuum drying is 0.08 MPa, the temperature is 80°C, and the time is 3 hours; the mass of acetone used to dissolve the chain extender is 20%-40% of the mass of the prepolymer, and the total amount of acetone added does not exceed 30% of the mass of the prepolymer.

[0020] Preferably, in step S5, the water bath temperature is controlled at 50°C, the stirring speed is adjusted to 300 r / min, and the reaction continues for 3 hours.

[0021] Preferably, in step S6, the degassing process involves a vacuum degree of 0.08 MPa, a temperature of 50°C, and a time of 15 minutes; after casting into a glass culture dish to form a film, the film is cured at room temperature for 1-2 days, then cured in an oven at 60-70°C for 48 hours, and finally the residual solvent is removed by vacuum extraction at 80°C for 2 hours.

[0022] Preferably, in step S7, the volume ratio of ethanol to water is 8:2, the pH is adjusted to 3.5-4.5 with acetic acid, cellulose nanocrystals are added after hydrolysis at room temperature for 30 minutes, magnetic stirring is continued for 3 hours, the mixture is washed 3-5 times, the precipitate is collected by centrifugation, and dried for 3 hours.

[0023] Preferably, in step S8, the organic solvent is a ternary mixed solvent of N,N-dimethylformamide, dimethyl sulfoxide, and toluene, with a volume ratio of (3-5):(2-4):(1-3). The modified cellulose nanocrystals are first ultrasonically dispersed in dimethyl sulfoxide for 120 minutes, and then other organic solvents are added. The amount of polyurethane elastomer added is 25 parts by weight, and the amount of modified cellulose nanocrystals added is 2 parts by weight. The mixture is mechanically stirred and dissolved at 60°C for 120 minutes, and after degassing, it is dried in an oven at 60°C for 2-3 days.

[0024] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0025] 1. Soybean oil polyol synthesized by reacting epoxidized soybean oil with itaconic acid provides flexible segments and branched structure, while polycaprolactone diol imparts crystallinity and strength. The two are combined to form a polyurethane matrix with appropriate separation of soft and hard segment microphases. Waste PET degradation products are combined with 3,3'-dichloro-4,4'-diaminodiphenylmethane as a chain extender. This not only utilizes the rigidity of PET segments to improve the modulus, but also enhances the hydrogen bonding between hard segments through the aromatic amine structure, avoiding the brittleness problem caused by a single rigid chain extender, so that the material has both high elongation at break and tensile strength.

[0026] 2. 3-Aminopropyltriethoxysilane is used to modify the surface of cellulose nanofibers to graft amino functional groups onto their surface. These amino groups can react in situ with the isocyanate groups in the polyurethane prepolymer during the S8 composite molding process to form a chemical bonding interface. This effectively overcomes the problems of poor compatibility and easy agglomeration and debonding between unmodified cellulose nanofibers and the polyurethane matrix. As a result, stress can be efficiently transferred with low addition amount, further improving the toughness and strength of the material.

[0027] 3. By placing the gallium indium tin alloy in the S8 composite molding step rather than the modification stage, we can avoid its oxidation and deactivation in the acidic hydrolysis environment. This ensures that it is uniformly dispersed in the polyurethane matrix in the form of liquid metal micro-regions. Without interfering with the early polymerization reaction, the droplet deformation energy dissipation mechanism can be used to assist in toughening, while also providing a basis for the potential thermal or electrical conductivity of the material.

[0028] 4. By limiting key control points such as the acid value at the end of the S2 reaction, the acetone replenishment ratio in S5 / S6, and the ternary solvent ratio in S9, the problems of incomplete synthesis of bio-based polyols, local gelation of chain extension reaction, and uncontrollable separation of composite film-forming phases are effectively solved, making the entire preparation process have good industrial applicability and quality consistency, and avoiding significant performance fluctuations due to raw material fluctuations or operational deviations. Attached Figure Description

[0029] Figure 1 This is a flowchart illustrating the preparation steps of the present invention. Detailed Implementation

[0030] The following description is intended to disclose the invention and enable those skilled in the art to implement it. The preferred embodiments described below are merely examples, and other obvious variations will occur to those skilled in the art.

[0031] Unless otherwise specified, all raw materials used in the preparation of PET-based high-toughness recycled modified plastics in this invention are commercially available; all instruments used in the tests are conventional laboratory instruments, and the testing standards comply with industry norms.

[0032] Raw material parameter description:

[0033] Epoxy soybean oil: epoxy value ≥6.0%, purchased from Henan Liwei Biopharmaceutical Co., Ltd.; Ethylene glycol: analytical grade, purchased from Sinopharm Chemical Reagent Co., Ltd.; Itaconic acid: purity ≥99%, purchased from Shanghai Maclean Biochemical Technology Co., Ltd.; Polycaprolactone diol (PCL-2000): molecular weight 2000 g / mol, hydroxyl value 56±3 mgKOH / g, purchased from Suzhou Hanfeng New Materials Co., Ltd.; Isophorone diisocyanate (IPDI): purity ≥99.5%, purchased from Wanhua Chemical Group Co., Ltd.; Dibutyltin dilaurate: purity ≥98%, purchased from Aladdin Reagent Co., Ltd.; Waste PET degradation products: obtained by purification after alcoholysis of waste mineral water bottles with ethylene glycol. Hydroxyl value 180±10 mg KOH / g, self-made; 3,3'-dichloro-4,4'-diaminodiphenylmethane (MOCA): purity ≥99%, purchased from Jiangsu Suqing Chemical Co., Ltd.; 3-aminopropyltriethoxysilane (KH-550): purity ≥97%, purchased from Nanjing Xiangqian Chemical Co., Ltd.; Cellulose nanocrystals: diameter 5-10 nm, length 100-200 nm, purchased from Guilin Qihong Technology Co., Ltd.; Gallium indium tin alloy: Ga:In:Sn mass ratio 68.5:21.5:10, melting point 10.7℃, purchased from Changsha Xinkang Metal Materials Co., Ltd.; Organic solvents (DMF, DMSO, toluene): all analytical grade, purchased from Tianjin Damao Chemical Reagent Factory.

[0034] Reference Figure 1 As shown, a process for preparing a PET-based high-toughness recycled modified plastic includes:

[0035] Example 1:

[0036] A process for preparing PET-based high-toughness recycled modified plastics involves using waste PET degradation products as chain extenders, and constructing a polyurethane elastomer system by compounding soybean oil polyol, polycaprolactone diol, and modified cellulose nanocrystals. The preparation steps are as follows:

[0037] S1: Raw material preparation. Prepare the following raw materials by weight: 30 parts epoxidized soybean oil, 30 parts ethylene glycol, 0.3 parts itaconic acid, 30 parts polycaprolactone diol, 33 parts isophorone diisocyanate, 0.55 parts dibutyltin dilaurate, 5.9 parts waste PET degradation products, 3.5 parts 3,3'-dichloro-4,4'-diaminodiphenylmethane, 2 parts 3-aminopropyltriethoxysilane, 1 part cellulose nanofibers, and 7 parts gallium indium tin alloy.

[0038] S2: Synthesis of soybean oil polyols: Epoxy soybean oil and ethylene glycol were magnetically stirred evenly in a beaker and then poured into a high-temperature and high-pressure stainless steel reactor. Itaconic acid was added, and the reaction was carried out at a constant temperature of 140°C for 2 hours. The reaction endpoint was determined by the acid value dropping to 4.8 mg KOH / g. After the reaction was completed, the mixture was naturally cooled to room temperature to obtain soybean oil polyols.

[0039] S3: Polycaprolactone diol pretreatment: Place polycaprolactone diol in a vacuum drying oven and dehydrate it for 3 hours under a vacuum of 0.08 MPa and a temperature of 115°C. After dehydration, cool it down to 55°C and stop vacuuming. Set aside for later use.

[0040] S4: Preparation of polyurethane prepolymer: Soybean oil polyol and pretreated polycaprolactone diol were mixed and added to a three-necked flask equipped with a polytetrafluoroethylene stirrer and a serpentine condenser. Isophorone diisocyanate was added. Nitrogen protection was maintained throughout the process. The water bath was heated to 80°C and the stirring speed was set to 250 r / min. After reacting for 1 hour, the catalyst dibutyltin dilaurate was added dropwise, and the reaction was continued for 2 hours to obtain a polyurethane elastomer prepolymer with an NCO content of 5.2%.

[0041] S5: Chain extension reaction. Waste PET degradation products are mixed with 3,3'-dichloro-4,4'-diaminodiphenylmethane and vacuum dried for 3 hours at a vacuum of 0.08 MPa and 80°C. The mixture is then dissolved in acetone at 30% of the prepolymer mass. After cooling to 50°C, the mixture is added dropwise to the prepolymer. The water bath temperature is controlled at 50°C, and the stirring speed is adjusted to 300 r / min. Acetone is added according to the viscosity of the system (total addition is 15% of the prepolymer mass) to maintain a uniform stirring state. The reaction is continued for 3 hours to obtain a viscous solution.

[0042] S6: Elastomer curing: The viscous solution is degassed for 15 minutes under a vacuum of 0.08 MPa and a temperature of 50°C, then cast into a glass petri dish to form a film. It is cured at room temperature for 1.5 days, then cured in an oven at 65°C for 48 hours, and finally the residual solvent is removed by vacuum at 80°C for 2 hours to obtain the polyurethane elastomer.

[0043] S7: Modified cellulose nanofibers: 3-aminopropyltriethoxysilane was added to an ethanol-water aqueous solution with a volume ratio of 8:2. The pH was adjusted to 4.0 with acetic acid. After hydrolysis at room temperature for 30 minutes, cellulose nanofibers were added and magnetic stirring was continued for 3 hours. The mixture was washed 4 times and the precipitate was collected by centrifugation. The precipitate was dried at 60°C for 3 hours to obtain modified cellulose nanofibers.

[0044] S8: Composite molding. The organic solvent used is a ternary mixed solvent of N,N-dimethylformamide, dimethyl sulfoxide, and toluene, with a volume ratio of 4:3:2. First, the modified cellulose nanocrystals are ultrasonically dispersed in dimethyl sulfoxide for 120 minutes, and then N,N-dimethylformamide and toluene are added. 25 parts by weight of polyurethane elastomer, 2 parts by weight of modified cellulose nanocrystals, and 7 parts by weight of gallium indium tin alloy are added. The mixture is mechanically stirred and dissolved at 60°C for 120 minutes. After degassing, it is cast into a polytetrafluoroethylene mold and dried in an oven at 60°C for 2.5 days to obtain PET-based high-toughness recycled modified plastic.

[0045] Example 2:

[0046] A preparation process for a PET-based high-toughness recycled modified plastic, comprising the following steps:

[0047] S1: Raw material preparation. Prepare the following raw materials by weight: 30 parts epoxidized soybean oil, 30 parts ethylene glycol, 0.3 parts itaconic acid, 29 parts polycaprolactone diol, 32 parts isophorone diisocyanate, 0.5 parts dibutyltin dilaurate, 3.9 parts waste PET degradation products, 2 parts 3,3'-dichloro-4,4'-diaminodiphenylmethane, 2 parts 3-aminopropyltriethoxysilane, 1 part cellulose nanofibers, and 4 parts gallium indium tin alloy.

[0048] S2: Synthesis of soybean oil polyols, same as in Example 1, with an endpoint acid value of 5.0 mg KOH / g;

[0049] S3: Polycaprolactone diol pretreatment, vacuum dehydration temperature is 110℃, other parameters are the same as in Example 1;

[0050] S4: Preparation of polyurethane prepolymer, same as in Example 1, to obtain a polyurethane elastomer prepolymer with an NCO content of 5.0%;

[0051] S5: Chain extension reaction, the mass of acetone used to dissolve the chain extender is 20% of the mass of the prepolymer, the total amount of acetone added is 10% of the mass of the prepolymer, and the other parameters are the same as in Example 1;

[0052] S6: Elastomer curing, room temperature curing for 1 day, oven curing temperature is 60℃, other parameters are the same as in Example 1;

[0053] S7: Cellulose nanofibers were modified, the pH of the ethanol aqueous solution was adjusted to 3.5, the washing was performed 3 times, and the other parameters were the same as in Example 1;

[0054] S8: Composite molding, with a ternary mixed solvent volume ratio of 3:2:1, ultrasonic dispersion time of 120 minutes, drying time of 2 days, and other parameters the same as in Example 1, to obtain PET-based high-toughness recycled modified plastic.

[0055] Example 3:

[0056] A preparation process for a PET-based high-toughness recycled modified plastic, comprising the following steps:

[0057] S1: Raw material preparation. Prepare the following raw materials by weight: 30 parts epoxidized soybean oil, 30 parts ethylene glycol, 0.3 parts itaconic acid, 31 parts polycaprolactone diol, 34 parts isophorone diisocyanate, 0.6 parts dibutyltin dilaurate, 7.9 parts waste PET degradation products, 5 parts 3,3'-dichloro-4,4'-diaminodiphenylmethane, 2 parts 3-aminopropyltriethoxysilane, 1 part cellulose nanofibers, and 10 parts gallium indium tin alloy.

[0058] S2: Synthesis of soybean oil polyols, same as in Example 1, with an endpoint acid value of 4.5 mg KOH / g;

[0059] S3: Polycaprolactone diol pretreatment, vacuum dehydration temperature is 120℃, other parameters are the same as in Example 1;

[0060] S4: Preparation of polyurethane prepolymer, same as in Example 1, to obtain a polyurethane elastomer prepolymer with an NCO content of 5.4%;

[0061] S5: Chain extension reaction, the mass of acetone used to dissolve the chain extender is 40% of the mass of the prepolymer, the total amount of acetone added is 25% of the mass of the prepolymer, and the other parameters are the same as in Example 1;

[0062] S6: Elastomer curing, room temperature curing for 2 days, oven curing temperature is 70℃, other parameters are the same as in Example 1;

[0063] S7: Cellulose nanofibers were modified, the pH of the ethanol aqueous solution was adjusted to 4.5, the washing was performed 5 times, and the other parameters were the same as in Example 1;

[0064] S8: Composite molding, with a ternary mixed solvent volume ratio of 5:4:3, ultrasonic dispersion time of 120 minutes, drying time of 3 days, and other parameters the same as in Example 1, to obtain PET-based high-toughness recycled modified plastic.

[0065] Comparative Example 1:

[0066] Without adding modified cellulose nanofibers, the other raw materials and preparation process are the same as in Example 1; specifically, in S8, only 25 parts of polyurethane elastomer and 7 parts of gallium indium tin alloy are added, no modified cellulose nanofibers are added, the amount of ternary mixed solvent is reduced accordingly, and the other steps remain unchanged.

[0067] Comparative Example 2:

[0068] Unmodified cellulose nanofibers were used instead of modified cellulose nanofibers, and the remaining raw materials and preparation process were the same as in Example 1; specifically, the following adjustments were made: in S7, no silane coupling agent modification treatment was performed, and the original cellulose nanofibers were directly used for composite molding in S8, while the remaining steps remained unchanged.

[0069] Comparative Example 3:

[0070] Without adding gallium indium tin alloy, the other raw materials and preparation process are the same as in Example 1; specifically, in S8, only 25 parts of polyurethane elastomer and 2 parts of modified cellulose nanofibers are added, without adding gallium indium tin alloy, and the other steps remain unchanged.

[0071] Performance testing

[0072] Mechanical property testing

[0073] Standards: Tensile strength and elongation at break shall be tested according to GB / T1040.3-2006, dumbbell-shaped specimen, tensile rate 50 mm / min; tear strength shall be tested according to GB / T529-2008, right-angled specimen.

[0074] Indicators: tensile strength (MPa), elongation at break (%), tear strength (kN / m).

[0075] Thermal stability and microstructure testing

[0076] Standard: Thermogravimetric analysis (TGA) was performed under a nitrogen atmosphere with a heating rate of 10 °C / min to 600 °C; cross-sectional morphology was observed using scanning electron microscopy (SEM) with an accelerating voltage of 5 kV.

[0077] Indicators: Initial decomposition temperature Td5% (°C), carbon residue rate at 600°C (%), and qualitative evaluation of cross-sectional roughness.

[0078] Table 1. Mechanical property test results

[0079]

[0080] Table 2 Thermal stability test results

[0081]

[0082] As shown in the table above, the PET-based high-toughness recycled modified plastics prepared in Examples 1-3 all exhibited tensile strengths ≥26.2 MPa, elongation at break ≥542%, and tear strength ≥39.8 kN / m, demonstrating the synergistic toughening and strengthening effects of waste PET chain extenders, composite soft segments, modified cellulose nanocrystals, and gallium indium tin alloy. Among them, Example 3 showed the best mechanical properties due to its higher content of waste PET degradation products and gallium indium tin alloy.

[0083] Comparative Example 1, lacking modified cellulose nanofibers, lacked chemical bonding interfaces and rigid reinforcement points, resulting in a significant decrease in tensile strength and elongation at break. Comparative Example 2, using unmodified cellulose nanofibers, exhibited poor compatibility with the polyurethane matrix due to surface hydroxyl agglomeration, with obvious debonding visible in the SEM cross-section. Its mechanical properties were lower than those of the Example but better than those of Comparative Example 1. Comparative Example 3, lacking gallium indium tin alloy, retained the reinforcing effect of nanofibers but lacked the energy dissipation mechanism of liquid metal droplet deformation, resulting in an elongation at break that was approximately 11% lower than that of Example 1, further confirming the necessity of each core component and process.

[0084] Comprehensive testing standards: The mechanical properties, thermal stability, microstructure and solvent residue of all products in the embodiments and comparative examples of this invention are tested in accordance with the general testing standards for plastics and polyurethane elastomers, with unified testing equipment, test environment and judgment criteria to ensure that all test data are true and comparable.

[0085] Mechanical property testing: Tensile strength and elongation at break were tested according to GB / T1040.3-2006 "Determination of tensile properties of plastics - Part 3: Test conditions for films and sheets", using dumbbell-shaped specimens and a tensile rate of 50 mm / min; tear strength was tested according to GB / T529-2008 "Determination of tear strength of vulcanized rubber or thermoplastic rubber (trouser-shaped, right-angled and crescent-shaped specimens)", using right-angled specimens, recording the maximum force value and calculating the tear strength per unit thickness.

[0086] Thermal stability and microstructure testing: Thermogravimetric analysis (TGA) was performed according to GB / T33047.1-2016 "Determination of Thermal Decomposition Products of Plastic Polymers". The temperature was increased to 600℃ at 10℃ / min under a nitrogen atmosphere, and the initial decomposition temperature Td5% and the char residue at 600℃ were recorded. Scanning electron microscopy (SEM) was performed according to JY / T0584-2020 "General Rules for Analysis Methods of Scanning Electron Microscopy". The sample cross-section was imaged under an accelerating voltage of 5kV after gold sputtering treatment to qualitatively evaluate the cross-sectional roughness, filler dispersion state and interfacial bonding.

[0087] Solvent residue detection: According to GB / T23986-2009 "Determination of Volatile Organic Compounds (VOCs) in Paints and Varnishes by Gas Chromatography", the residual amounts of acetone, DMF, DMSO and toluene were determined by headspace sampling-gas chromatography. The total solvent residue was characterized by mass fraction, and ≤0.5% was considered qualified.

[0088] Sensory evaluation: Ten professionals with experience in polymer material applications were selected to conduct blind evaluations and score the samples according to three indicators: surface smoothness, transparency uniformity, and tactile flexibility (each with a maximum score of 10 points). The final result is the average score of the 10 people, which is used to help verify the consistency between the material molding quality and the user experience.

[0089] The foregoing has shown and described the basic principles, main features, and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The embodiments and descriptions in the specification are merely principles of the invention. Various changes and modifications can be made to the invention without departing from its spirit and scope, and all such changes and modifications fall within the scope of the claimed invention. The scope of protection claimed by the appended claims and their equivalents is defined.

Claims

1. A preparation process for PET-based high-toughness recycled modified plastic, characterized in that, The preparation process uses waste PET degradation products as chain extenders to construct a polyurethane elastomer system by compounding soybean oil polyol, polycaprolactone diol, and modified cellulose nanocrystals. The preparation steps include: S1: Raw material preparation. Prepare the following raw materials by weight: epoxidized soybean oil, ethylene glycol, itaconic acid, polycaprolactone diol, isophorone diisocyanate, dibutyltin dilaurate, waste PET degradation products, 3,3'-dichloro-4,4'-diaminodiphenylmethane, 3-aminopropyltriethoxysilane, cellulose nanofibers, gallium indium tin alloy and organic solvents. S2: Synthesis of soybean oil polyols: Epoxy soybean oil and ethylene glycol are mixed and itaconic acid is added. After stirring evenly, the mixture is placed in a high-temperature and high-pressure reactor for constant temperature reaction. After cooling, soybean oil polyols are obtained. S3: Polycaprolactone diol pretreatment, the polycaprolactone diol is vacuum dehydrated and then cooled for later use. S4: Preparation of polyurethane prepolymer: Soybean oil polyol is mixed with pretreated polycaprolactone diol, isophorone diisocyanate is added, the mixture is heated and reacted under nitrogen protection, and a catalyst is added dropwise to continue the reaction to obtain polyurethane elastomer prepolymer. S5: Chain extension reaction. Waste PET degradation products are mixed with 3,3'-dichloro-4,4'-diaminodiphenylmethane, vacuum dried, and then dissolved in acetone. The mixture is then added dropwise to the prepolymer while cooling. Acetone is added according to the viscosity of the system to maintain a uniform stirring state and the reaction continues to obtain a viscous solution. S6: Elastomer curing: After degassing the viscous solution, it is cast into a film, cured at room temperature, cured in an oven, and the residual solvent is removed by vacuum to obtain a polyurethane elastomer; S7: Modified cellulose nanofibers: 3-aminopropyltriethoxysilane was hydrolyzed in an aqueous ethanol solution, followed by the addition of cellulose nanofibers and stirring. The mixture was then washed, centrifuged, and dried to obtain modified cellulose nanofibers. S8: Composite molding, the modified cellulose nanocrystals are dispersed in an organic solvent by ultrasonic dispersion treatment, polyurethane elastomer and gallium indium tin alloy are added and stirred to dissolve, after degassing, casting and drying, to obtain PET-based high-toughness recycled modified plastic.

2. The preparation process of PET-based high-toughness recycled modified plastic according to claim 1, characterized in that: In S1, the raw materials are proportioned by weight as follows: 30 parts of epoxidized soybean oil, 30 parts of ethylene glycol, 0.3 parts of itaconic acid, 29-31 parts of polycaprolactone diol, 32-34 parts of isophorone diisocyanate, 0.5-0.6 parts of dibutyltin dilaurate, 3.9-7.9 parts of waste PET degradation products, 2-5 parts of 3,3'-dichloro-4,4'-diaminodiphenylmethane, 2 parts of 3-aminopropyltriethoxysilane, 1 part of cellulose nanofibers, and 4-10 parts of gallium indium tin alloy.

3. The preparation process of PET-based high-toughness recycled modified plastic according to claim 1, characterized in that: In step S2, epoxidized soybean oil, ethylene glycol, and itaconic acid are magnetically stirred evenly in a beaker and then poured into a high-temperature and high-pressure stainless steel reactor. The reactor is kept at a constant temperature of 140°C for 2 hours. The reaction endpoint is determined by the acid value dropping to ≤5mgKOH / g. After the reaction is completed, the reactor is allowed to cool naturally to room temperature.

4. The preparation process of PET-based high-toughness recycled modified plastic according to claim 1, characterized in that: In step S3, the vacuum degree of vacuum dehydration is 0.08 MPa, the temperature is 110-120℃, the dehydration time is 3 hours, and the vacuuming is stopped after the dehydration is completed and the temperature is lowered to 50-60℃.

5. The preparation process of PET-based high-toughness recycled modified plastic according to claim 1, characterized in that: In step S4, the reaction is carried out in a three-necked flask equipped with a polytetrafluoroethylene stirrer and a serpentine condenser. The water bath is heated to 80°C, and the stirring speed is set to 250 r / min. After reacting for 1 hour, the catalyst dibutyltin dilaurate is added dropwise, and the reaction continues for 2 hours under nitrogen protection throughout.

6. The preparation process of PET-based high-toughness recycled modified plastic according to claim 1, characterized in that: In step S5, the vacuum degree of vacuum drying is 0.08 MPa, the temperature is 80°C, and the time is 3 hours; the mass of acetone used to dissolve the chain extender is 20%-40% of the mass of the prepolymer, and the total amount of acetone added does not exceed 30% of the mass of the prepolymer.

7. The preparation process of PET-based high-toughness recycled modified plastic according to claim 6, characterized in that: In step S5, the water bath temperature is controlled at 50°C, the stirring speed is adjusted to 300 r / min, and the reaction continues for 3 hours.

8. The preparation process of PET-based high-toughness recycled modified plastic according to claim 1, characterized in that: In step S6, the degassing process is performed at a vacuum level of 0.08 MPa, a temperature of 50°C, and a time of 15 minutes. After casting the film onto a glass culture dish, it is cured at room temperature for 1-2 days, then cured in an oven at 60-70°C for 48 hours, and finally the residual solvent is removed by vacuum extraction at 80°C for 2 hours.

9. The preparation process of PET-based high-toughness recycled modified plastic according to claim 1, characterized in that: In step S7, the volume ratio of ethanol to water is 8:

2. The pH is adjusted to 3.5-4.5 with acetic acid. After hydrolysis at room temperature for 30 minutes, cellulose nanocrystals are added, and magnetic stirring is continued for 3 hours. The mixture is washed 3-5 times, centrifuged to collect the precipitate, and dried for 3 hours.

10. The preparation process of PET-based high-toughness recycled modified plastic according to claim 1, characterized in that: In step S8, the organic solvent is a ternary mixed solvent of N,N-dimethylformamide, dimethyl sulfoxide, and toluene, with a volume ratio of (3-5):(2-4):(1-3). The modified cellulose nanocrystals are first ultrasonically dispersed in dimethyl sulfoxide for 120 minutes, and then other organic solvents are added. The amount of polyurethane elastomer added is 25 parts by weight, and the amount of modified cellulose nanocrystals added is 2 parts by weight. The mixture is mechanically stirred and dissolved at 60°C for 120 minutes, and after degassing, it is dried in an oven at 60°C for 2-3 days.