A novel highly adaptable polyurethane ink binder, its preparation method and application
Polyurethane ink binders were prepared by bulk synthesis and gradient temperature controlled segmented reaction process, which solved the problems of flammability, explosiveness and environmental pollution of traditional solvent methods, and achieved high applicability and anti-blocking properties, making them suitable for the field of green flexible packaging.
Patent Information
- Application Number
- CN202611527093.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-29
- Publication Date
- 2026-11-17
AI Technical Summary
Existing polyurethane ink binders use solvent methods in their synthesis, which leads to flammability, explosiveness, environmental pollution, and inconvenience in transportation. Furthermore, they lack compatibility with PET and BOPP films.
Polyurethane ink binder was prepared by bulk synthesis. By introducing multi-branched polyester soft segments, branched isocyanate hard segments, and short alkyl end-capped structures, combined with a gradient temperature-controlled segmented reaction process, high-temperature crosslinking was avoided. Triethylenediamine and triethylamine were used as a composite catalyst to form a low-temperature chain extension and end-capping process, followed by baking to close the loop, resulting in a polyurethane resin with a low softening point and good solubility in environmentally friendly solvents.
A polyurethane ink binder with high applicability and good anti-blocking properties has been developed. It is safe and environmentally friendly in production, convenient in transportation and storage, and has good affinity with PET and BOPP films.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] This invention belongs to the field of green flexible packaging technology, specifically a novel polyurethane ink binder, especially a polyurethane ink binder with high applicability, good anti-blocking properties, and convenient transportation, and further discloses its preparation method and application. Background Technology
[0002] The field of green flexible packaging technology refers to flexible packaging technologies applied in food packaging, pharmaceutical packaging, and other fields. It commonly uses food-grade materials, such as food-grade PET and BOPP films, and environmentally friendly ester and alcohol solvents for the inks. Commonly used ink binder resins are generally environmentally friendly chlorinated polypropylene and polyurethane resins. Polyurethane resin, in particular, has become the main binder resin due to its excellent performance and wide applicability, offering advantages such as virtually no odor after film formation and adjustable hardness. However, currently, almost all polyurethane ink binders in China are synthesized using solvent methods, which has certain drawbacks. Firstly, the solvents are generally flammable and explosive, posing a safety risk; secondly, solvent evaporation into the air also causes environmental pollution. Summary of the Invention
[0003] To address the aforementioned problems, the present invention aims to provide a novel, highly adaptable polyurethane ink binder and its preparation method. This binder is synthesized using a bulk synthesis method, without the use of solvents, and exhibits a wide distribution of rigid ester bonds, urethane bonds, and branched structures, demonstrating good affinity with both PET and BOPP films. Therefore, it possesses characteristics not found in traditional polyurethane ink binders, such as high adaptability and good anti-blocking properties, and also features safe production, environmental friendliness, and convenient transportation.
[0004] In order to achieve the above-mentioned objectives of the present invention, the following technical solution is adopted: In a first aspect, the present invention provides a novel highly adaptable polyurethane ink binder, prepared from raw materials comprising the following parts by weight: 100 parts of polyester polyol; 11.1-22.2 parts of diisocyanate; Diol chain extenders: 2.3-6.5 parts; 0.5-0.8 parts of capping agent; 0.3 parts catalyst; The polyester polyol mentioned therein is an adipic acid-type polyester polyol with more branches, and a number average molecular weight of 550-650, preferably 600, including one of poly(3-methyl-1,5-pentanediol adipate) polyol (a polyester polyol synthesized by polycondensation reaction of adipic acid and 3-methyl-1,5-pentanediol), poly(2-methyl-1,3-propanediol adipate), and poly(neopentanediol adipate) polyol (commonly known as poly(neopentanediol adipate), a polyester polyol obtained by polycondensation reaction of adipic acid and neopentanediol). The diisocyanate is an isophorone diisocyanate with a branched molecular structure, and there is no compound of linear aliphatic diisocyanates. The diol chain extender is one of neopentyl glycol, dipropylene glycol, or 2-methyl-1,3-propanediol, which have relatively many branches in their molecular structure.
[0005] Preferably, the capping agent is a C2-C8 saturated monoalkyl alcohol, selected from ethanol, butanol, n-octanol, and isooctanol; Preferably, the catalyst is a tertiary amine composite catalytic system composed of triethylenediamine and triethylamine, wherein the mass ratio of triethylenediamine to triethylamine is 1:0.5 to 1:2.
[0006] The binder of this invention is a low-temperature pulverizable solid polyurethane resin, in which multiple branched polyester soft segments, branched isocyanate hard segments, and short alkyl end caps are introduced into the molecular chain. The synergistic regulation of soft and hard segments enables the resin to have a low softening point, high anti-blocking properties, and environmentally friendly solvent solubility (alcohol esters), making it suitable for benzene-free and ketone-free green flexible packaging ink systems with high environmental friendliness.
[0007] Secondly, the present invention provides a method for preparing a novel highly adaptable polyurethane ink binder, comprising the following steps: (a) Prepolymer synthesis stage: Heat polyester polyol to 80±5℃, add diisocyanate at once, stir homogenously and then gradually increase the temperature to 110~120℃ (first increase to 70-80℃, react for 0.5 hours, then increase to 110-120℃), and maintain the temperature for 4~6 hours for prepolymerization to prepare highly branched polyurethane prepolymer; (b) Low-temperature chain extension and end-capping stage: The high-branched polyurethane prepolymer is naturally cooled to 70±5℃, and diol chain extender and end-capping agent are added simultaneously. After stirring evenly, the temperature is raised to 85±5℃ at a constant rate, and the chain extension and end-capping are carried out at a constant temperature for 1~2 hours to complete the initial growth and end-capping of molecular chains. (c) Catalytic ring-closing baking stage: The material is cooled to 70±5℃ and stirred for 0.5h. The catalyst is added and stirred rapidly for 10min. After the material is discharged at low temperature and quickly, it is spread on a tray and baked at 80~100℃ in the absence of air for 8~12h to complete the ring-closing reaction of the residual NCO in the molecular chain and obtain a solid resin. (d) Post-processing stage: The solid resin is naturally cooled to room temperature, coarsely crushed and then ultra-finely ground to obtain powdered polyurethane ink binder.
[0008] This invention adopts a segmented process of "low-temperature chain extension and end-capping followed by baking and closed-loop production", which avoids excessive cross-linking and local gel agglomeration caused by traditional one-step high-temperature reaction. The finished product can be pulverized at room temperature, and there is no need for organic solvent dilution during discharge, with no solvent discharge throughout the process.
[0009] Thirdly, the present invention provides an application of a novel highly adaptable polyurethane ink binder in the preparation of polyurethane green flexible packaging inks.
[0010] Beneficial effects: 1. Innovative Branched Synergistic Structure: For the first time, a three-in-one molecular structure of "multi-branched polyester soft segment + branched IPDI hard segment + alkyl end cap" is defined, clearly demonstrating the composite effect brought about by the synergy of soft and hard segments (anti-blocking, easy solubility in environmentally friendly solvents (alcohol esters), and low softening point). The multi-branched synergistic structure, combined with ester groups and urethane groups (synthesized polyurethane resins contain a large number of ester bonds and urethane bonds, which have very strong cohesive force and hydrogen bonding force, resulting in excellent anti-blocking performance), is highly similar to the structure of flexible packaging substrates such as BOPP and PET, giving the binder good adaptability and good adhesion to both non-polar substrates such as BOPP and highly polar substrates such as PET. 2. Innovation in composite catalytic system: The single catalyst is replaced with a triethylenediamine / triethylamine composite system to precisely control the two-stage chain extension reaction rate and avoid local excessive cross-linking.
[0011] 3. Innovation in preparation process (1) Unique segmented chain extension + post-discharge baking closed-loop process: Traditional polyurethane resins are all reacted at high temperature in the reactor throughout the process, with a wide molecular weight distribution, which makes them very easy to gel and clump locally. This scheme first completes the chain extension and end-capping at low temperature, and then discharges the material into the oven for post-curing process, baking closed loop, step-by-step chain extension reaction, narrow and uniform molecular weight distribution, completely avoiding gelation. At the same time, no solvent is involved in the synthesis throughout the process, which is in line with the direction of green chemical industry. Compared with the solvent-based resins synthesized by traditional methods, its production is relatively safe, does not pollute the environment, and is more convenient for transportation and storage.
[0012] (2) The gradient temperature control stepwise reaction logic is clear, and each temperature and time corresponds to the molecular chain regulation target, and the process steps are non-obvious.
[0013] The present invention has been described in detail above; however, the above embodiments are merely illustrative in nature and are not intended to limit the invention. Furthermore, this document is not limited to the foregoing prior art or the invention itself, or to any theory described in the following embodiments. Detailed Implementation
[0014] The present invention will be further described below with reference to the embodiments. It should be noted that the following embodiments are provided for illustrative purposes only and do not constitute a limitation on the scope of protection of the present invention.
[0015] Unless otherwise specified, the raw materials, reagents, and methods used in the embodiments are all conventional raw materials, reagents, and methods in the art.
[0016] Example 1: The preparation method of the novel polyurethane ink binder described in this embodiment includes: (a) Prepolymerization reaction: Take 100g of poly(3-methyl-1,5-pentanediol) with an average molecular weight of 600 according to the formula and heat it to 75°C. Then add 11.1g of isophorone diisocyanate and stir to mix. First, raise the temperature to 75°C and react for 0.5 hours, then raise the temperature to 120°C and react for 4 hours. (b) Preliminary chain extension polymerization reaction: After the prepolymerization reaction is completed, turn off the heating and turn on the reflux water to cool the material to 65°C. Take 2.3g of neopentyl glycol and 0.5g of ethanol and add them to the reaction mixture in step (a). Stir evenly and then heat the mixture to 80°C at a constant rate to continue the reaction for 1 hour. (c) Baking chain extension polymerization reaction: Cool the reactants to 65°C and stir uniformly for 0.5 hours. Then add 0.3g of catalyst (triethylenediamine:triethylamine = 1:1), stir quickly and evenly (10 minutes), and quickly discharge the material into a tray and bake at 80°C for 8 hours to obtain the block product; (d) The obtained product is cooled and coarsely crushed to obtain the final product.
[0017] Example 2: The preparation method of the novel polyurethane ink binder described in this embodiment includes: (a) Prepolymerization reaction: Take 100g of poly(2-methyl-1,3-propanediol) with an average molecular weight of 600 according to the formula and heat it to 80°C. Then add 16.65g of isophorone diisocyanate and stir to mix. First, raise the temperature to 75°C and react for 0.5 hours, then raise the temperature to 115°C and react for 5 hours. (b) Preliminary chain extension polymerization reaction: After the prepolymerization reaction is completed, turn off the heating and turn on the reflux water to cool the material to 75°C. Take 6.2g of dipropylene glycol and 0.8g of n-octanol and add them to the reaction mixture in step (a). Stir evenly and then heat the mixture to 85°C at a constant rate to continue the reaction for 1.5 hours. (c) Baking chain extension polymerization reaction: Cool the reactants to 70°C and stir uniformly for 0.5 hours. Then add 0.3g of catalyst (triethylenediamine:triethylamine = 1:1), stir quickly and evenly (10 minutes), and quickly discharge the material into a tray and bake at 90°C for 9 hours to obtain the block product; (d) The obtained product is cooled and coarsely crushed to obtain the final product.
[0018] Example 3: The preparation method of the novel polyurethane ink binder described in this embodiment includes: (a) Prepolymerization reaction: Take 100g of poly(adipate-neopentyl glycol) polyol with an average molecular weight of 600 according to the formula and heat it to 75°C. Then add 22.2g of isophorone diisocyanate and stir to mix. First, raise the temperature to 75°C and react for 0.5 hours, then raise the temperature to 110°C and react for 6 hours. (b) Preliminary chain extension polymerization reaction: After the prepolymerization reaction is completed, turn off the heating and turn on the reflux water to cool the material to 68°C. Take 6.5g of 2-methyl-1,3-propanediol and 0.6g of isooctyl alcohol and add them to the reaction material in step (1). Stir evenly and then heat up to 82°C at a constant rate to continue the reaction for 2 hours. (c) Baking chain extension polymerization reaction: Cool the reactants to 68°C and stir uniformly for 0.5 hours. Then add 0.3g of catalyst (triethylenediamine:triethylamine = 1:1), stir quickly and evenly (10 minutes), and quickly discharge the material into a tray and bake at 100°C for 10 hours to obtain the block product; (d) The obtained product is cooled and coarsely crushed to obtain the final product.
[0019] Example 4: The preparation method of the novel polyurethane ink binder described in this embodiment includes: (a) Prepolymerization reaction: Take 100g of poly(3-methyl-1,5-pentanediol) with an average molecular weight of 600 according to the formula and heat it to 85°C. Then add 13.875g of isophorone diisocyanate and stir to mix. First, raise the temperature to 75°C and react for 0.5 hours, then raise the temperature to 112°C and react for 4.5 hours. (b) Preliminary chain extension polymerization reaction: After the prepolymerization reaction is completed, turn off the heating and turn on the reflux water to cool the material to 75°C. Take 4.7g of dipropylene glycol and 0.75g of butanol and add them to the reaction mixture in step (a). Stir evenly and then heat the mixture to 90°C at a constant rate to continue the reaction for 1 hour. (c) Baking chain extension polymerization reaction: Cool the reactants to 75°C and stir uniformly for 0.5 hours. Then add 0.3g of catalyst (triethylenediamine:triethylamine = 1:1), stir quickly and evenly (10 minutes), and quickly discharge the material into a tray and bake at 85°C for 11 hours to obtain the block product; (d) The obtained product is cooled and coarsely crushed to obtain the final product.
[0020] Example 5: The preparation method of the novel polyurethane ink binder described in this embodiment includes: (a) Prepolymerization reaction: Take 100g of poly(2-methyl-1,3-propanediol) with an average molecular weight of 600 according to the formula and heat it to 81°C. Then add 19.425g of isophorone diisocyanate and stir to mix. First, raise the temperature to 75°C and react for 0.5 hours, then raise the temperature to 118°C and react for 5.5 hours. (b) Preliminary chain extension polymerization reaction: After the prepolymerization reaction is completed, turn off the heating and turn on the reflux water to cool the material to 72°C. Take 5.1g of 2-methyl-1,3-propanediol and 0.7g of n-octanol and add them to the reaction mixture in step (a). Stir evenly and then heat the mixture to 88°C at a constant rate to continue the reaction for 2 hours. (c) Baking chain extension polymerization reaction: Cool the reactants to 72°C and stir uniformly for 0.5 hours. Then add 0.3g of catalyst (triethylenediamine:triethylamine = 1:1), stir quickly and evenly (10 minutes), and quickly discharge the material into a tray and bake at 95°C for 12 hours to obtain the block product; (d) The obtained product is cooled and coarsely crushed to obtain the final product.
[0021] Comparative Example 1: The difference between this comparative example and Example 1 is that the poly(3-methyl-1,5-pentanediol adipate) polyol is replaced with poly(1,4-butanediol adipate) diol (PBA).
[0022] Comparative Example 2: The difference between this comparative example and Example 1 is that the prepolymerization reaction did not use a gradient temperature increase.
[0023] Test case To test product performance, this invention also discloses a solid polyurethane resin dissolution formulation and a formulation for a green flexible packaging ink based on a polyurethane system.
[0024] The polyurethane resins prepared in Examples 1-5 and Comparative Examples 1-2 were first dissolved into polyurethane solutions according to the solid polyurethane resin dissolution formulations shown in Table 1. Then, the solutions were printed using a laboratory gravure printing machine according to the green flexible packaging formulations of the polyurethane system shown in Table 2, and the relevant properties were tested.
[0025] Table 1 shows the solid polyurethane resin dissolution formulation.
[0026] The green flexible packaging ink formulations listed in Table 2
[0027] First, the primary material was prepared and ground using a gyratory mill. After grinding for 2 hours, a secondary material was added and dispersed for 30 minutes to obtain the ink. Proof printing was performed using a laboratory gravure printing press, and the relevant performance was tested.
[0028] Adhesion testing was conducted according to GB / T 13217.7. Anti-blocking performance was tested using the hot-pressing method according to GB / T 13217.8-2009, applying 2000g pressure at 50℃ for 2 hours. Because conventional products involve solvent dilution reactions during production, storage and transportation are handled as Class A flammable and explosive materials, requiring the use of hazardous materials vehicles. This not only increases costs but also poses safety hazards such as leaks. The evaluation methods for safety, environmental friendliness, and ease of transportation and storage are based on whether the product is a hazardous chemical and a Class A flammable and explosive material.
[0029] Table 3 shows the ink adhesion test results.
[0030] As shown in the table above, the ink binder prepared using this invention exhibits excellent adhesion and superior anti-blocking properties. Since it eliminates the traditional solvent synthesis method, there is no solvent release during the production process, resulting in superior safety and environmental friendliness. It also greatly facilitates transportation and storage. Ink manufacturers can dissolve this product before ink preparation, avoiding safety and environmental issues associated with transportation and storage.
[0031] The testing methods for the obtained inks are as follows: GB / T 2024-2012 Gravure printing composite inks for plastic films; GB / T 13217.4-2008 Test method for viscosity of liquid ink; GB / T 13217.6-2008 Test method for tinting strength of liquid inks.
[0032] The application performance test results of the ink are shown in Table 4 below, with the comparative sample as a control.
[0033] Table 4 shows the stability test results of the inks.
[0034] Table 4 shows the following: 1. The initial viscosity of the ink used for printing, using the resin of Comparative Example 1, was 21.5 seconds. This viscosity is relatively high because: 1. The pigment dispersion ability of Comparative Example 1 resin is not as good as the grinding effect of the novel polyurethane pigment dispersion resin of this invention; 2. Comparative Example 1 resin is more sensitive to alcohols in the ink system, hence the higher ink viscosity. 2. After one month, the stability of the ink prepared with Comparative Example 1 resin is significantly worse than that of the novel polyurethane pigment dispersion resin of this invention. This is because the pigment encapsulation effect of Comparative Example 1 resin is poor, and the pigment has agglomerated, thus increasing the ink viscosity. 3. The tinting strength of the inks in Examples 1-5 is significantly better than that of Comparative Example 1. This is because the dispersion effect of the novel polyurethane dispersion resin of this invention is better than that of Comparative Example 1 resin, the pigment particle size is lower, the pigment particle size per unit area is smaller, and the distribution is more uniform, thus resulting in better tinting strength.
[0035] The above embodiments are merely illustrative of the technical solutions of the present invention and are not intended to limit it. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features therein, without departing from the spirit and substance defined by the claims of the present invention; and such modifications or substitutions are still within the scope defined by the claims of the present invention.
Claims
1. A novel highly adaptable polyurethane ink binder, characterized in that, It is prepared from the following raw materials in parts by weight: 100 parts of polyester polyol; 11.1-22.2 parts of diisocyanate; Diol chain extenders, 2.3-6.5 parts; 0.5-0.8 parts of capping agent; 0.3 parts catalyst; The polyester polyol mentioned above is an adipic acid type polyester polyol with a number average molecular weight of 550-650. The diisocyanate is isophorone diisocyanate; The diol chain extender is one of neopentyl glycol, dipropylene glycol, and 2-methyl-1,3-propanediol.
2. The novel highly adaptable polyurethane ink binder according to claim 1, characterized in that, The polyester polyol is one of poly(3-methyl-1,5-pentanediol adipate), poly(2-methyl-1,3-propanediol adipate), and poly(neopentanediol adipate).
3. The novel highly adaptable polyurethane ink binder according to claim 1, characterized in that, The capping agent is a C2~C8 saturated monoalkyl alcohol.
4. The novel highly adaptable polyurethane ink binder according to claim 3, characterized in that, The capping agent is one of ethanol, butanol, n-octanol, and isooctanol.
5. The novel highly adaptable polyurethane ink binder according to claim 1, characterized in that, The catalyst is a mixture of triethylenediamine and triethylamine, with a mass ratio of 1:0.5 to 1:
2.
6. A method for preparing a novel highly adaptable polyurethane ink binder according to any one of claims 1-5, characterized in that, Includes the following steps: (a) Prepolymer synthesis stage: Take polyester polyol and heat it to 80±5℃, add diisocyanate at one time, stir homogenously and then gradually heat it to 110~120℃, and perform a constant temperature prepolymerization reaction for 4~6h to prepare a highly branched polyurethane prepolymer. (b) Low-temperature chain extension and end-capping stage: The high-branched polyurethane prepolymer is naturally cooled to 70±5℃, and diol chain extender and end-capping agent are added simultaneously. After stirring evenly, the temperature is raised to 85±5℃ at a constant rate, and the chain extension and end-capping are carried out at a constant temperature for 1~2 hours to complete the initial growth and end-capping of molecular chains. (c) Catalytic ring-closing baking stage: The material is cooled to 70±5℃ and stirred for 0.5h. The catalyst is added and stirred rapidly for 10min. After the material is discharged at low temperature and quickly, it is spread on a tray and baked at 80~100℃ in the absence of air for 8~12h to complete the ring-closing reaction of the residual NCO in the molecular chain and obtain a solid resin. (d) Post-processing stage: The solid resin is naturally cooled to room temperature, coarsely crushed and then ultra-finely ground to obtain powdered polyurethane ink binder.
7. The application of the novel highly adaptable polyurethane ink binder according to any one of claims 1-5 in the preparation of polyurethane flexible packaging inks.