Modified C9 petroleum resin, its preparation method and application, marine protective materials
By constructing a block copolymer structure of C9 petroleum resin and polyester segments of natural antifouling groups, the problems of controlled degradation and continuous release of antifouling activity in marine antifouling coatings were solved, achieving high strength, controlled degradation and environmentally friendly antifouling effects.
Patent Information
- Application Number
- CN202611165202.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-03
- Publication Date
- 2026-11-17
AI Technical Summary
Existing C9 petroleum resins are difficult to degrade in a controlled manner and release antifouling activity in marine antifouling coatings. Furthermore, traditional antifouling agents cause serious environmental pollution, and existing modified resins have failed to effectively combine rigid frameworks with functional degradation fragments.
The structure employs a block copolymer, combining C9 petroleum resin segments with polyester segments containing natural antifouling groups, linked by ester or ether bonds to form ABA or AB type block copolymers. The polyester segments slowly hydrolyze in seawater to release antifouling active substances, maintaining the material's mechanical strength and antifouling effect.
It achieves controllable degradation and continuous release of antifouling activity in materials, possesses excellent mechanical strength and self-polishing antifouling effect, and the degradation products are harmless to the marine environment, thus solving the environmental pollution problem of traditional materials.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] This invention relates to the field of polymer materials technology, specifically to a modified C9 petroleum resin, its preparation method and application, and marine engineering protective materials. Background Technology
[0002] Marine biofouling refers to the phenomenon of marine organisms (such as barnacles, mussels, and algae) attaching and growing on the surfaces of marine engineering facilities such as ships, offshore platforms, and subsea pipelines, seriously affecting the performance and service life of these facilities. Biofouling increases ship drag, leading to increased fuel consumption, reduced speed, accelerated metal corrosion, and shortened equipment maintenance cycles.
[0003] To prevent biofouling, traditional methods primarily rely on antifouling coatings, which inhibit marine organism attachment by adding antifouling agents to the coatings. Traditional antifouling coatings mostly use heavy metal antifouling agents such as organotin and cuprous oxide, which cause serious pollution to the marine ecosystem and have been banned or restricted by the International Maritime Organization (IMO). Although natural antifouling agents have environmental advantages, current technologies for immobilization and slow-release of natural antifouling agents are immature, making it difficult to achieve long-term antifouling effects. Existing biodegradable polyester-based antifouling materials, while environmentally friendly, generally suffer from low mechanical strength, poor seawater resistance, and difficulty in controlling degradation rates. Rapid hydrolysis of polyester segments leads to premature coating failure, while slow degradation fails to achieve effective self-polishing antifouling effects.
[0004] C9 petroleum resin is a thermoplastic resin obtained by polymerization of C9 fraction (boiling range 120-200℃), a byproduct of petroleum cracking. It possesses excellent water resistance, chemical corrosion resistance, and adhesive properties, and is widely used in coatings, inks, and adhesives. In marine antifouling coatings, C9 petroleum resin is often used as a film-forming substance. However, traditional C9 petroleum resins have a simple structure and lack functional groups, making it difficult to meet the dual requirements of biodegradability and antifouling activity for environmentally friendly antifouling coatings.
[0005] Existing C9 petroleum resins lack biodegradability and antifouling activity. For example, a modified petroleum resin preparation method (publication number CN108774296A) improves the overall performance of the resin by introducing functional monomers. However, this modified resin is mainly used in general coatings and is not applied to marine antifouling applications, nor does it possess controlled degradation and antifouling activity release capabilities. Pure petroleum resin-based antifouling coatings are difficult to degrade in marine environments, leading to "coating accumulation" problems with long-term use. Furthermore, petroleum resins themselves do not possess antifouling activity and must rely on external antifouling agents, resulting in rapid agent loss and short-lasting antifouling effects.
[0006] In existing technologies, the rigid framework of resins is difficult to effectively combine with functional degradable fragments, resulting in materials that cannot achieve controlled degradation and synergistic antifouling functions while maintaining mechanical strength. How to construct a molecular structure that combines high strength, controlled degradation, and continuous release of antifouling activity is a pressing technical challenge in the field of marine antifouling materials. Summary of the Invention
[0007] The first technical problem to be solved by the present invention is to provide a modified C9 petroleum resin that effectively combines a rigid resin skeleton with a functional degradable antifouling material, in light of the current state of the prior art.
[0008] The second technical problem to be solved by the present invention is to provide a method for preparing the above-mentioned modified C9 petroleum resin, in view of the current state of the prior art.
[0009] The third technical problem to be solved by the present invention is to provide an application of the above-mentioned modified C9 petroleum resin in light of the current state of the prior art.
[0010] The fourth technical problem to be solved by the present invention is to provide a marine protective material using the above-mentioned modified C9 petroleum resin, in view of the current state of the prior art.
[0011] The technical solution adopted by the present invention to solve the first technical problem mentioned above is as follows: a modified C9 petroleum resin is a block copolymer, comprising C9 petroleum resin segments and polyester segments containing natural antifouling groups, wherein the natural antifouling groups of the polyester segments are derived from capsaicin derivatives or vanillin derivatives.
[0012] Preferably, the block copolymer comprises an ABA-type triblock or an AB-type diblock structure, wherein A is a C9 petroleum resin segment and B is a polyester segment containing natural antifouling groups.
[0013] ABA triblock: Two C9 petroleum resin segments (A) are located at both ends, with a functional polyester segment (B) in the middle. This structure gives the material better physical crosslinking points and entanglement networks, resulting in superior mechanical properties; degradation occurs in the middle B segment, while the A segments at both ends maintain structural integrity, achieving surface degradation without overall strength loss; AB diblock: Synthesizing is simpler, suitable for scenarios with slightly lower mechanical performance requirements. Users can choose different structures according to their target application scenarios (high strength required for marine coatings, long-term sustained release required for fixed platforms).
[0014] Preferably, the number average molecular weight of the C9 petroleum resin segments is 1000-5000. When it is below 1000, the rigidity is insufficient; when it is above 5000, the melt viscosity is too high, making it difficult to undergo polycondensation reaction with the polyester segments.
[0015] The number average molecular weight of the polyester segments is 2000-8000. When it is below 2000, the degradation is too fast (coating failure in <6 months); when it is above 8000, the degradation is too slow (no self-polishing in >2 years), and the anti-fouling effect decreases.
[0016] The number average molecular weight of the block copolymer is 5,000-20,000: if the molecular weight is too low, the film-forming property is poor; if it is too high, the solubility becomes poor and the coating application is difficult.
[0017] Preferably, the capsaicin derivative is at least one of capsaicin, dihydrocapsaicin, or nonanoyl vanillin; the vanillin derivative is at least one of vanillin, ethyl vanillin, or isovandrin. Using naturally derived capsaicin or vanillin derivatives as the antifouling active group, the product undergoes slow-release hydrolysis in seawater, avoiding pollution of the marine ecosystem by heavy metal antifouling agents. The degradation products are non-toxic and comply with the environmental requirements of the International Maritime Organization.
[0018] Preferably, the polyester segments have ester bonds or ether bonds. Ester bonds release antifouling groups through hydrolysis in seawater; the hydrolysis rate is synchronized with the degradation rate of the polyester segments, achieving release upon degradation. Capsaicin derivatives contain phenolic hydroxyl groups, which can form ester bonds with carboxyl groups. Ether bonds have higher chemical stability than ester bonds and are suitable for scenarios requiring a slower release rate.
[0019] The technical solution adopted by the present invention to solve the second technical problem mentioned above is as follows: A method for preparing the above-mentioned modified C9 petroleum resin includes the following steps:
[0020] (1) Preparation of C9 petroleum resin oligomers with terminal hydroxyl or terminal carboxyl groups;
[0021] (2) Preparation of natural antifouling monomers containing natural antifouling groups: esterification reaction of capsaicin derivatives or vanillin derivatives with dicarboxylic acid under the action of acid catalyst, or acyl chloride reaction of capsaicin derivatives or vanillin derivatives with dicarboxylic acid chloride under the action of acid binder, to obtain natural antifouling monomers containing natural antifouling groups.
[0022] (3) Preparation of modified C9 petroleum resin:
[0023] (3.1) Prepare the raw materials according to the following mass proportions: 100 parts of C9 petroleum resin oligomer with terminal hydroxyl or terminal carboxyl groups, 30-70 parts of natural antifouling monomer (preferably 40-60 parts), 60-100 parts of diacid, 40-80 parts of diol, and 0.01-0.5 parts of catalyst.
[0024] (3.2) Mix the above raw materials and carry out melt polycondensation reaction under the action of catalyst. The reaction temperature is 180-240℃, the reaction time is 2-6 hours, and the vacuum degree is 50-500Pa to obtain modified C9 petroleum resin.
[0025] When the amount of natural antifouling monomer is less than 30 parts, the antifouling effect is insufficient (coverage rate >25% in 6 months). When the amount is more than 70 parts, the resin becomes more brittle and the adhesion decreases. The molar ratio of diacid to diol should be controlled at 1:1.05-1:1.2 (with a slight excess of alcohol) to ensure complete polycondensation reaction.
[0026] Preferably, the preparation method of the terminal hydroxyl C9 petroleum resin oligomer in step (1) is as follows: 100 parts of C9 petroleum resin, 15-25 parts of ethylene glycol, 3-8 parts of p-toluenesulfonic acid catalyst, and toluene solvent are mixed evenly to form a mixture, the solid content of the mixture is 20%, and the mixture is reacted for 3-6 hours under anhydrous and oxygen-free conditions at 70-90°C.
[0027] Preferably, the preparation method of the carboxyl-terminated C9 petroleum resin oligomer in step (1) is as follows: 100 parts of C9 petroleum resin and 8-15 parts of benzoyl peroxide are mixed evenly in an organic solvent according to the mass fraction, and reacted at 110-130℃ for 6-10 hours in an oxygen atmosphere with an oxygen flow rate of 50-100 mL / min.
[0028] Preferably, the dicarboxylic acid in step (3) is at least one of terephthalic acid, isophthalic acid, adipic acid, and sebacic acid; the diol is at least one of ethylene glycol, propylene glycol, butanediol, and hexanediol; the catalyst is at least one of tetrabutyl titanate, zinc acetate, and antimony trioxide, and the amount of catalyst used is 0.01-0.5% of the total mass of the reactants.
[0029] The technical solution adopted by this invention to solve the third technical problem mentioned above is: an application of the modified C9 petroleum resin, which is used to prepare marine protective materials. Marine protective coatings can be marine antifouling coatings or marine antifouling coating materials. The differences between marine antifouling coatings and marine antifouling coating materials are as follows:
[0030]
[0031] The technical solution adopted by the present invention to solve the fourth technical problem mentioned above is as follows: a marine protective material includes the following components and their mass fractions: 20-40 parts of modified C9 petroleum resin, 30-50 parts of organic solvent, 10-30 parts of pigments and fillers, and 1-5 parts of additives.
[0032] The organic solvent is at least one of xylene, toluene, and butyl acetate; the pigment and filler is at least one of iron oxide red, titanium dioxide, talc, and calcium carbonate; and the additive is at least one of dispersant, leveling agent, and defoamer.
[0033] Pigments and fillers comprise pigments and fillers. Pigments (iron oxide red / titanium dioxide) provide hiding power and rust prevention; fillers (talc / calcium carbonate) increase coating thickness and sandability, reducing costs. Dispersants (such as BYK-163): prevent pigment / filler agglomeration, ensuring uniform dispersion in the resin. Leveling agents (such as BYK-333): reduce surface tension of the coating, eliminating brush marks and orange peel, resulting in a smooth coating. Defoamers (such as BYK-052): eliminate air bubbles generated during mixing and application, preventing pinhole defects in the coating.
[0034] Modified C9 petroleum resin is dissolved in an organic solvent, and pigments, fillers, and additives are added to produce marine protective materials. These materials are then coated onto the surfaces of marine engineering facilities such as ships, offshore platforms, and subsea pipelines. In seawater, the polyester segments on the coating surface slowly hydrolyze, releasing natural antifouling active substances to form an antifouling active layer. Simultaneously, the coating surface is continuously renewed, achieving a self-polishing and antifouling effect. The degradation products of the coating are small-molecule organic compounds that are harmless to the marine environment.
[0035] Compared with the prior art, the advantages of the present invention are:
[0036] 1. This invention constructs a block copolymer molecular structure consisting of a rigid main chain backbone and functional degradable side chains, organically combining C9 petroleum resin segments with polyester segments containing natural antifouling groups. The C9 petroleum resin segments serve as the rigid main chain backbone, providing mechanical strength and water resistance; the polyester segments serve as functional degradable side chains, slowly hydrolyzing in seawater to release natural antifouling active substances, thus endowing the material with excellent mechanical strength, controllable degradation performance, and synergistic antifouling function.
[0037] This invention constructs a block copolymer structure combining rigid C9 petroleum resin segments with polyester segments containing natural antifouling groups, achieving an organic combination of a rigid framework and functional degradable segments. This overcomes the contradiction in existing technologies where mechanical strength and degradability are difficult to balance. The rigid C9 petroleum resin segments ensure the mechanical strength and adhesion of the coating, while the flexible polyester segments improve the coating's flexibility. The overall performance is superior to that of pure acrylic resin or pure polyester materials. Furthermore, by adjusting the length, type, and content of natural antifouling monomers in the polyester segments, the self-polishing rate of the resin in seawater can be precisely controlled, matching it with the ship's sailing speed and the coating's design life.
[0038] 2. The modified C9 petroleum resin of the present invention can be used to prepare marine engineering protective materials. Marine engineering facilities can be ships, offshore platforms, subsea pipelines, etc. After the marine engineering protective material is coated on the surface of the marine engineering facility, in the seawater environment, the polyester segments slowly hydrolyze and release natural antifouling active substances (capsaicin derivatives or vanillin derivatives), achieving a self-polishing antifouling effect. At the same time, the degradation products are harmless to the marine environment, solving the problems of environmental pollution and single function of traditional antifouling materials, and opening up a new way for the high-value utilization of C9 petroleum resin.
[0039] 3. This invention uses conventional melt polycondensation equipment, and the process flow is compatible with existing resin production processes, making it easy to promote industrialization. Detailed Implementation
[0040] The present invention will be further described in detail below with reference to specific embodiments. The following embodiments are used to illustrate the present invention, but are not intended to limit the scope of protection of the present invention.
[0041] The C9 petroleum resin mentioned below is a commercially available product. It can be purchased from Zibo Ningsong Chemical Co., Ltd., product brand C9 resin PR-110, or from Qingdao Haifei Chemical Co., Ltd., product brand SY-100 (C9-SY series), or from Fushun Huaxing Petrochemical Co., Ltd., product brand HX-C9-100.
[0042] Capsaicin can be purchased from Nanjing Daosifu Company, with a purity of ≥98% and CAS 404-86-4.
[0043] Vanillin can be purchased from Wuhan Haishan Technology Co., Ltd., with a purity of ≥99% and CAS 121-33-5.
[0044] Example 1
[0045] A method for preparing modified C9 petroleum resin with capsaicin derivatives as natural antifouling groups includes the following steps:
[0046] Step 1: Preparation of C9 petroleum resin oligomers with terminal hydroxyl groups:
[0047] 100g of commercially available C9 petroleum resin (softening point 90-110℃, number-average molecular weight approximately 2000) was dissolved in 500mL of toluene. 5g of p-toluenesulfonic acid was added as a catalyst, and the mixture was heated to 85℃ under nitrogen protection. Then, 20g of ethylene glycol was slowly added dropwise, and the reaction was allowed to proceed for 5 hours. After the reaction was complete, the mixture was cooled to room temperature, neutralized with saturated sodium carbonate solution, washed with water until neutral, and vacuum dried to obtain 115g of C9 petroleum resin oligomer with terminal hydroxyl groups. The hydroxyl value was determined to be 45mgKOH / g, and the number-average molecular weight was 2500.
[0048] Step 2: Preparation of natural antifouling monomers containing capsaicin groups:
[0049] Take 50g of commercially available capsaicin (purity ≥98%), dissolve it in 200mL of dichloromethane, add 40g of adipic acid and 1g of p-toluenesulfonic acid, heat to reflux, and react for 6 hours. After the reaction is complete, cool to room temperature, wash with saturated sodium bicarbonate solution, wash with water until neutral, remove the solvent by rotary evaporation, and dry under vacuum to obtain 78g of natural antifouling monomer containing capsaicin groups.
[0050] Step 3: Preparation of modified C9 petroleum resin:
[0051] 100g of the C9 petroleum resin oligomer with terminal hydroxyl groups prepared in step 1, 50g of the natural antifouling monomer containing capsaicin groups prepared in step 2, 80g of terephthalic acid, 60g of ethylene glycol, and 0.3g of tetrabutyl titanate were added to a reactor equipped with a stirrer, a nitrogen protection device, and a vacuum system. Under nitrogen protection, the temperature was raised to 180℃ and stirred for 1 hour; then the temperature was raised to 220℃ and reacted for 2 hours; finally, the reaction was carried out at 230℃ under a vacuum of 200 Pa for 3 hours. After the reaction was completed, the mixture was cooled to room temperature, pulverized, and 240g of a pale yellow solid product was obtained, which is the modified C9 petroleum resin.
[0052] The number-average molecular weight of the modified C9 petroleum resin was 15,000 and the molecular weight distribution index was 1.9, as determined by gel permeation chromatography. The glass transition temperature was 55℃ and the softening point was 105℃, as determined by differential scanning calorimetry.
[0053] Example 2
[0054] A method for preparing modified C9 petroleum resin with vanillin derivatives as natural antifouling groups includes the following steps:
[0055] Step 1: Preparation of C9 petroleum resin oligomers with terminal carboxyl groups:
[0056] 100g of C9 petroleum resin (same as in Example 1) was dissolved in 400mL of xylene, and 10g of benzoyl peroxide was added. The mixture was heated to 120℃ and oxygen was introduced for oxidation reaction for 8 hours. After the reaction was completed, the mixture was cooled to room temperature, methanol was added to precipitate the resin, filtered, and vacuum dried to obtain 95g of C9 petroleum resin oligomer with terminal carboxyl groups. The acid value was determined to be 38mgKOH / g, and the number average molecular weight was 3000.
[0057] Step 2: Preparation of natural antifouling monomers containing vanillin groups
[0058] 60g of commercially available vanillin (purity ≥99%) was dissolved in 150mL of pyridine and cooled to 0℃ in an ice bath. 50g of adipic acid chloride was slowly added dropwise. After the addition was complete, the temperature was raised to room temperature, and the reaction was allowed to proceed for 12 hours. After the reaction was complete, the mixture was acidified to pH=2 with dilute hydrochloric acid, extracted with ethyl acetate, washed with saturated brine, dried over anhydrous sodium sulfate, and the solvent was removed by rotary evaporation. The mixture was then dried under vacuum to obtain 85g of an antifouling monomer containing vanillin groups. Pyridine acted as an acid-binding agent to neutralize the byproduct HCl, and adipic acid chloride provided an acyl chloride group, which underwent nucleophilic substitution with the phenolic hydroxyl group of vanillin to form an ester bond.
[0059] Step 3: Melt polycondensation reaction
[0060] 95g of the C9 petroleum resin oligomer with terminal carboxyl groups prepared in step 1, 60g of the natural antifouling monomer containing vanillin groups prepared in step 2, 70g of isophthalic acid, 55g of butanediol, and 0.4g of zinc acetate were added to a reaction vessel. Under nitrogen protection, the temperature was raised to 190℃ and the reaction was stirred for 1.5 hours; then the temperature was raised to 230℃ and the reaction was carried out for 2.5 hours; finally, the reaction was carried out at 240℃ under a vacuum of 150 Pa for 3.5 hours. After the reaction was completed, the mixture was cooled to room temperature, pulverized, and 220g of a light brown solid product, namely the modified C9 petroleum resin, was obtained.
[0061] The modified C9 petroleum resin was determined to have a number-average molecular weight of 18,000, a molecular weight distribution index of 2.0, a glass transition temperature of 60℃, and a softening point of 110℃.
[0062] Example 3
[0063] Preparation and performance testing of marine protective materials:
[0064] Marine protective material: 100g of the modified C9 petroleum resin prepared in Example 1 was dissolved in 200g of xylene, and 20g of iron oxide red pigment, 10g of talc, 5g of dispersant (BYK-163), 3g of leveling agent (BYK-333), and 2g of defoamer (BYK-052) were added. After stirring at high speed for 2 hours, the mixture was ground to a fineness of ≤30μm to obtain the marine protective material.
[0065] The preparation method of marine engineering protective materials is as follows: First, the modified C9 petroleum resin is dissolved in the solvent xylene, then pigments, fillers and additives are added, and the mixture is stirred to make the material evenly dispersed. Then, the material is ground until the fineness is ≤30μm, large particles are filtered out, and the material is packaged.
[0066] Coating preparation: Marine protective material was coated on the surface of a sandblasted steel plate with a dry film thickness of 150 μm and cured at room temperature (25±2℃) for 7 days.
[0067] The performance test methods and results of the above coatings are as follows:
[0068]
[0069] The antifouling effect test of the marine siding was conducted in accordance with the national standard GB / T 5370 "Test Method for Shallow Sea Immersion of Antifouling Paint Samples". The samples were hung on floating rafts in the sea areas of Qingdao and Xiamen, and the biofouling situation was observed and recorded regularly.
[0070] The gravimetric method involves immersing the coated sample in artificial seawater for a certain period of time, then removing it, drying it to constant weight, and calculating the percentage of the mass difference before and after immersion relative to the initial mass, which is the degradation weight loss rate. The HPLC method (high performance liquid chromatography) involves filtering the seawater sample through a 0.45 μm filter membrane and injecting it into an HPLC analyzer. A C18 column is used, with methanol-water as the mobile phase. The capsaicin concentration is determined under a UV detector (the maximum absorption wavelength of capsaicin is approximately 280 nm), and quantification is performed using the external standard method.
[0071] Environmental safety assessment: Ecotoxicity tests were conducted on the degradation products of the coating. The results showed that the median lethal concentration (LC50) of the degradation products for marine microalgae (Dunaliella salina), copepods (Dichroa febrifuga), and fish (zebrafish) was greater than 100 mg / L, which falls under the "practically non-toxic" category according to the chemical classification standards, indicating that the degradation products are safe for the marine environment.
[0072] Example 4
[0073] Effect of different polyester segment lengths on degradation rate
[0074] Following the method of Example 1, by adjusting only the amounts of diacid and diol in step 3, while keeping 100g of C9 petroleum resin oligomer with terminal hydroxyl groups, 50g of natural antifouling monomer containing capsaicin groups, and 0.3g of tetrabutyl titanate catalyst constant in step 3, and only changing the total amount of terephthalic acid and ethylene glycol, three modified C9 petroleum resins with different polyester segment lengths were prepared (other conditions were the same):
[0075] Sample A: 50g terephthalic acid, 38g ethylene glycol (total feed amount 88g), target polyester segment Mn approximately 2000;
[0076] Sample B: 80g terephthalic acid, 60g ethylene glycol (total feed amount 140g), which is the formulation of Example 1, with a polyester segment Mn of approximately 4000;
[0077] Sample C: 120g terephthalic acid, 90g ethylene glycol (total feed 210g), with a target polyester segment Mn of approximately 7000. Three modified C9 petroleum resins with different polyester segment lengths were prepared (other conditions were the same). Marine protective materials were prepared using the three modified C9 petroleum resins according to the formulation and process of Example 3, and degradation tests were conducted. The results are as follows:
[0078]
[0079] The results show that the degradation rate of the resin can be effectively controlled by adjusting the polyester chain segment length, thereby meeting the antifouling life requirements of different application scenarios (such as ships and fixed platforms).
[0080] Example 5
[0081] The effect of different natural antifouling monomer contents on antifouling effect
[0082] Following the method of Example 1, in step 3, the amount of capsaicin-containing natural antifouling monomer added was varied (30g, 50g, and 70g respectively, with other conditions remaining unchanged) to prepare three types of modified C9 petroleum resins, and the biofouling coverage of the slate in actual seabed was tested after 6 months. Results: When the amount of natural antifouling monomer added was 30g, the biofouling coverage after 6 months was 25%; when the amount of natural antifouling monomer added was 50g, the coverage was <10%; and when the amount of natural antifouling monomer added was 70g, the coverage was <5%. Considering both antifouling effect and mechanical properties, the preferred amount of antifouling monomer added was 20-30wt% of the total resin.
[0083] Comparative Example 1:
[0084] Preparation and performance testing of marine protective materials:
[0085] Marine protective material: Dissolve 100g of unmodified C9 petroleum resin (i.e., commercially available C9 petroleum resin) from Example 1 in 200g of xylene, add 20g of iron oxide red pigment, 10g of talc, 5g of dispersant (BYK-163), 3g of leveling agent (BYK-333), and 2g of defoamer (BYK-052), stir at high speed for 2 hours, and grind until the fineness is ≤30μm to obtain marine protective material.
[0086] The preparation method of marine engineering protective materials is as follows: first, C9 petroleum resin is dissolved in xylene solvent, then pigments, fillers and additives are added, and the mixture is stirred to make the material evenly dispersed. Then, the material is ground until the fineness is ≤30μm, large particles are filtered out, and then packaged.
[0087] Coating preparation: Marine protective material was coated on the surface of a sandblasted steel plate with a dry film thickness of 150 μm and cured at room temperature (25±2℃) for 7 days.
[0088] Test results: The coating's adhesion (Grade 1) and hardness (2H) were comparable to those of Example 3; however, its antifouling performance was poor, and barnacles, mussels, and other fouling organisms attached to it after one month of immersion; the coating hardly degraded in seawater, and after six months of immersion, the weight loss rate was less than 1%, failing to achieve a self-polishing and antifouling effect; no antifouling active substances such as capsaicin were detected in seawater.
[0089] In summary, this invention successfully prepared a biodegradable, antifouling modified C9 petroleum resin by constructing a block copolymer structure of C9 petroleum resin segments and polyester segments containing natural antifouling groups. This resin retains the film-forming properties and mechanical strength of C9 petroleum resin while also possessing controllable degradation and natural antifouling activity, achieving synergistic optimization of material properties and environmental protection / antifouling capabilities. This opens up new avenues for the high-value utilization of C9 petroleum resin.
Claims
1. A modified carbon nine petroleum resin characterized by: It is a block copolymer containing C9 petroleum resin segments and polyester segments containing natural antifouling groups, wherein the natural antifouling groups of the polyester segments are derived from capsaicin derivatives or vanillin derivatives.
2. The modified carbon nine petroleum resin according to claim 1, characterized in that: The block copolymer comprises an ABA-type triblock or an AB-type diblock structure, wherein A is a C9 petroleum resin segment and B is a polyester segment containing natural antifouling groups.
3. The modified carbon nine petroleum resin according to claim 1, characterized in that: The number-average molecular weight of the C9 petroleum resin segments is 1000-5000, the number-average molecular weight of the polyester segments is 2000-8000, and the number-average molecular weight of the block copolymer is 5000-20000.
4. The modified carbon nine petroleum resin according to claim 1, characterized in that: The capsaicin derivative is at least one of capsaicin, dihydrocapsaicin, or nonanoyl vanillin; the vanillin derivative is at least one of vanillin, ethyl vanillin, or isovillin.
5. The modified carbon nine petroleum resin according to claim 4, characterized in that: The polyester segments have ester bonds or ether bonds.
6. A method for producing the modified carbon nine petroleum resin according to any one of claims 1 to 4, characterized by, Includes the following steps: (1) Preparation of C9 petroleum resin oligomers with terminal hydroxyl or terminal carboxyl groups; (2) Preparation of natural antifouling monomers containing natural antifouling groups: esterification reaction of capsaicin derivatives or vanillin derivatives with dicarboxylic acid under the action of acid catalyst, or acyl chloride reaction of capsaicin derivatives or vanillin derivatives with dicarboxylic acid chloride under the action of acid binder to obtain natural antifouling monomers. (3) Preparation of modified C9 petroleum resin: (3.1) Prepare the raw materials according to the following mass proportions: 100 parts of C9 petroleum resin oligomer, 30-70 parts of natural antifouling monomer, 60-100 parts of dicarboxylic acid, 40-80 parts of diol, and 0.01-0.5 parts of catalyst; (3.2) Mix the raw materials from step (3.1) evenly and carry out a melt polycondensation reaction under the action of a catalyst. The reaction temperature is 180-240℃, the reaction time is 2-6 hours, and the vacuum degree is 50-500Pa to obtain modified C9 petroleum resin.
7. The method of claim 6, wherein: In step (1), the preparation method of the C9 petroleum resin oligomer with terminal hydroxyl groups is as follows: 100 parts of C9 petroleum resin, 15-25 parts of ethylene glycol, 3-8 parts of p-toluenesulfonic acid catalyst, and toluene solvent are mixed evenly to form a mixture, and the mixture is reacted for 3-6 hours under anhydrous and oxygen-free conditions at 70-90°C. In step (1), the preparation method of the C9 petroleum resin oligomer with terminal carboxyl groups is as follows: 100 parts of C9 petroleum resin and 8-15 parts of benzoyl peroxide are mixed evenly in an organic solvent according to the mass fraction, and reacted at 110-130℃ for 6-10 hours in an oxygen atmosphere with an oxygen flow rate of 50-100mL / min.
8. The preparation method according to claim 6, characterized in that, In step (3), the dicarboxylic acid is at least one of terephthalic acid, isophthalic acid, adipic acid, and sebacic acid; the diol is at least one of ethylene glycol, propylene glycol, butanediol, and hexanediol; and the catalyst is at least one of tetrabutyl titanate, zinc acetate, and antimony trioxide.
9. Use of the modified carbon nine petroleum resin according to any one of claims 1 to 4, characterized in that, This modified C9 petroleum resin is used to prepare marine protective materials.
10. A marine protective material, characterized by, It comprises the following components and their mass fractions: 20-40 parts of the modified C9 petroleum resin as described in any one of claims 1 to 4, 30-50 parts of organic solvent, 10-30 parts of pigments and fillers, and 1-5 parts of additives; The organic solvent is at least one of xylene, toluene, and butyl acetate; the pigment and filler is at least one of iron oxide red, titanium dioxide, talc, and calcium carbonate; and the additive is at least one of dispersant, leveling agent, and defoamer.
Citation Information
Patent Citations
Fire alarm
CA121335A
Preparation method of modified petroleum resin
CN108774296A