Alkali-soluble polyesters and their preparation methods
By preparing alkali-soluble polyester, the problems of performance degradation in physical methods and high energy consumption in chemical methods in PET recycling have been solved, realizing efficient and low-carbon waste polyester recycling and producing high-value chemicals with good water solubility and thermal stability.
Patent Information
- Application Number
- CN202611344341.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-01
- Publication Date
- 2026-11-17
AI Technical Summary
Among existing PET recycling methods, physical methods lead to molecular chain breakage and performance degradation, while chemical methods are energy-intensive and costly, making it difficult to achieve high-quality regeneration. Furthermore, waste PET is difficult to degrade naturally, resulting in serious resource waste.
An alkali-soluble polyester preparation method is adopted, in which waste polyester is reacted with aliphatic diols with 2 to 3 carbon atoms, isophthalic acid-5-sulfonate or its derivatives, and polyethylene glycol within a specific temperature and time range to prepare a water-soluble intermediate product. Subsequently, melt polycondensation is carried out to avoid the high-energy purification process, and ion exchange resin is used for purification.
It achieves efficient and low-carbon recycling of waste polyester, and the product has good water solubility, thermal stability and color, meeting the requirements of high-end applications, reducing energy consumption and material loss, and improving the recycling rate.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention relates to the field of polymeric materials, and more particularly to an alkali-soluble polyester and its preparation method. Background Technology
[0002] Polyester (PET) materials, with their excellent mechanical properties, good barrier properties, and low cost, are widely used in food packaging, textile fibers, films, and engineering plastics, and their production and usage scale are continuously increasing. The resulting waste PET volume is enormous, and its natural degradation is extremely difficult, causing not only serious resource waste but also a significant environmental burden. Therefore, the efficient recycling and resource utilization of waste PET has become a critical issue that the industry urgently needs to address.
[0003] Currently, PET recycling methods are mainly divided into physical and chemical methods. Physical methods employ traditional mechanical PET recycling processes, which are prone to molecular chain breakage, molecular weight reduction, color deterioration, and impurity accumulation during processing. The performance of recycled materials deteriorates significantly, making it difficult to meet the requirements of food contact and high-end products. It can only achieve downgraded, low-value utilization and cannot achieve high-quality closed-loop recycling of PET. Chemical methods often use ethylene glycol alcoholysis to recycle PET. This process uses ethylene glycol to depolymerize waste PET to prepare diethyl terephthalate (BHET). However, this reaction is a reversible equilibrium reaction, requiring a much higher molar ratio of ethylene glycol as raw material, significantly increasing the energy consumption and cost of subsequent product separation and purification.
[0004] CN101955581B discloses a one-step method for preparing water-soluble polyester slurry from waste polyester plastics. This method involves modifying and polycondensing waste polyester fragments, 1,2-propanediol, diethylene glycol, a water-based polyester modifier A, a composite stabilizer, and a catalyst in the same reactor. This process ensures that the main chain of the polyester slurry contains both ester groups and water-soluble groups, making it both water-loving and water-soluble. The method first prepares the water-based polyester modifier A, which requires esterification with an excess of diol and an unsaturated dicarboxylic acid. Then, the double bonds of the raw material are sulfonated with sodium metabisulfite or sodium bisulfite to obtain sulfonated modified polyester. Finally, the prepared water-based polyester modifier A, 1,2-propanediol, diethylene glycol, composite stabilizer, and catalyst are reacted with the waste polyester to prepare the water-soluble polyester slurry. Summary of the Invention
[0005] One object of the present invention is to provide a method for preparing alkali-soluble polyester, which can reduce the amount of ethylene glycol added and prepare polyester with good alkali solubility. Furthermore, it can prepare alkali-soluble polyester with good color and thermal stability.
[0006] Another object of the present invention is to provide an alkali-soluble polyester that has good hue, thermal stability and alkali solubility.
[0007] On one hand, the present invention provides a method for preparing alkali-soluble polyester, comprising the following steps: (1) Waste polyester, aliphatic diols with 2 to 3 carbon atoms, isophthalic acid-5-sulfonate or its derivatives, polyethylene glycol and transesterification catalyst are mixed and reacted at 160 to 240 °C for 1 to 10 h to obtain a water-soluble intermediate product. (2) Dissolve the water-soluble intermediate in water, purify and dry to obtain the purified product; (3) The purified product is mixed with diethyl terephthalate and a polycondensation catalyst, and a melt polycondensation reaction is carried out under the protection of an inert gas to obtain an alkali-soluble polyester.
[0008] Through the above steps, waste polyester undergoes functionalization modification simultaneously during alcoholysis, and the product exists directly in the form of water-soluble oligomers, without having to go through the high-energy-consuming purification steps such as recrystallization and molecular distillation in the traditional bis(hydroxyethyl) terephthalate (BHET) monomer pathway. The water solubility of the product provides a process basis for subsequent ion exchange purification, realizing the efficient, low-carbon, and full-component utilization of waste polyester into high-value alkali-soluble polyester.
[0009] In this invention, the reaction temperature in step (1) is 160–240°C, and the reaction time is 1–10 h; preferably 170–220°C, 1–4 h; more preferably 190–220°C, 1–2 h. Within this temperature and time range, waste polyester can be effectively depolymerized and copolymerized with sulfonate monomers and polyethylene glycol, while the number average molecular weight of the water-soluble intermediate is controlled within the target range of 800–4000 g / mol.
[0010] According to some embodiments of the present invention, the number average molecular weight of the water-soluble intermediate is 800–4000 g / mol. When the number average molecular weight of the water-soluble intermediate is less than 800 g / mol, excessive depolymerization occurs, producing more water-insoluble components such as BHET dimers and trimers, leading to a decrease in the waste polyester recovery rate. When the number average molecular weight of the water-soluble intermediate is greater than 4000 g / mol, insufficient depolymerization occurs, and sulfonate monomers and polyethylene glycol cannot be effectively incorporated into the depolymerized product, resulting in poor water solubility of the product, which also leads to a decrease in the waste polyester recovery rate. According to some preferred embodiments of the present invention, the number average molecular weight of the water-soluble intermediate is 1100–2900 g / mol, thus ensuring a higher waste polyester recovery rate.
[0011] According to the preparation method of the present invention, preferably, in step (1), the aliphatic diol is selected from one or more of ethylene glycol and 1,3-propanediol; the isophthalic acid-5-sulfonate or its derivative is selected from one or more of sodium bis(hydroxyethyl) isophthalate-5-sulfonate and sodium isophthalate-5-sulfonate; the transesterification catalyst is selected from one or more of zinc acetate, manganese acetate, potassium carbonate, n-butyl titanate, and isopropyl titanate; and the number average molecular weight of the polyethylene glycol is 200-3000 g / mol. In step (3), the polycondensation catalyst is selected from one or more of the following: antimony glycolate, n-butyl titanate, isopropyl titanate, titanium oxalate, titanium acetate, titanium tetrachloride, and 1,8-diazabicyclo[5.4.0]undec-7-ene (DBU).
[0012] In this invention, the aliphatic diols having 2 to 3 carbon atoms are selected from one or more of ethylene glycol and 1,3-propanediol; preferably ethylene glycol.
[0013] In this invention, isophthalic acid-5-sulfonate or its derivatives are selected from one or more of sodium bis(hydroxyethyl) isophthalate-5-sulfonate and sodium isophthalate-5-sulfonate; preferably, sodium bis(hydroxyethyl) isophthalate-5-sulfonate. After the isophthalic acid-5-sulfonate structural unit is introduced into the polyester backbone, the sulfonate ion group imparts hydrophilicity to the oligomer and significantly improves its dispersion and solubility in aqueous media.
[0014] In this invention, polyethylene glycol (PEG) segments are embedded in the oligomer backbone via ester bonds, which significantly enhances the product's solubility in aqueous media and imparts a certain degree of segmental flexibility to the oligomer. The molecular weight of PEG directly affects the water solubility of the water-soluble intermediates and the quality of the final product. PEG with too low a molecular weight results in short hydrophilic segments in the depolymerization intermediates, leading to poor water solubility and a low waste polyester recovery rate. Conversely, PEG with too high a molecular weight results in poor water solubility of the depolymerization intermediates and a decrease in the melting point and thermal stability of the final synthesized alkali-soluble polyester, affecting subsequent applications such as composite spinning. The number-average molecular weight of PEG can be 200–3000 g / mol; preferably 200–2000 g / mol; more preferably 200–800 g / mol. This ensures a high waste polyester recovery rate, and the resulting alkali-soluble polyester sample is bright white with minimal yellowing, while also possessing excellent thermal stability.
[0015] In this invention, the transesterification catalyst is selected from one or more of zinc acetate, manganese acetate, potassium carbonate, n-butyl titanate, and isopropyl titanate; preferably zinc acetate or potassium carbonate.
[0016] In this invention, the polycondensation catalyst is selected from one or more of antimony glycolate, n-butyl titanate, isopropyl titanate, titanium oxalate, titanium acetate, titanium tetrachloride, and 1,8-diazabicyclo[5.4.0]undec-7-ene; preferably antimony glycolate or n-butyl titanate.
[0017] According to the preparation method of the present invention, preferably, the mass ratio of the waste polyester to the aliphatic diol is 1:(0.15-3.5); the mass ratio of the waste polyester to the isophthalic acid-5-sulfonate or its derivative is 1:(0.1-0.5); the mass ratio of the waste polyester to the polyethylene glycol is 1:(0.1-8); and the mass ratio of the waste polyester to the transesterification catalyst is 1:(0.005-0.03).
[0018] According to some embodiments of the present invention, the mass ratio of the waste polyester to the aliphatic diol is 1:(0.3-3.5); the mass ratio of the waste polyester to the isophthalic acid-5-sulfonate or its derivative is 1:(0.3-0.5); the mass ratio of the waste polyester to the polyethylene glycol is 1:(0.3-1.2); and the mass ratio of the waste polyester to the transesterification catalyst is 1:(0.005-0.03).
[0019] According to some preferred embodiments of the present invention, the mass ratio of the waste polyester to the aliphatic diol is 1:(0.3-1); the mass ratio of the waste polyester to the isophthalic acid-5-sulfonate or its derivative is 1:(0.3-0.5); the mass ratio of the waste polyester to the polyethylene glycol is 1:(0.3-1.2); the mass ratio of the waste polyester to the transesterification catalyst is 1:(0.005-0.01); the mass ratio of the purified product to the diethyl terephthalate is 1:(0.3-0.5); and the mass ratio of the purified product to the polycondensation catalyst is 1:(0.0001-0.0005). The alkali-soluble polyester prepared in this way exhibits good alkali solubility, color, and thermal stability.
[0020] According to the preparation method of the present invention, preferably, in step (2), the mass ratio of the waste polyester to water is 1:(5-30), and the dissolution temperature is 40-90℃.
[0021] According to some preferred embodiments of the present invention, the mass ratio of water added to waste polyester is 1:(10-20), and the dissolution temperature is 40-50°C. This results in a high yield of purified product, and the prepared alkali-soluble polyester exhibits good color and thermal stability.
[0022] According to the preparation method of the present invention, preferably, in step (2), the drying is carried out in a thin film evaporator with an absolute pressure of 30 to 100 mbar and a jacket temperature of 50 to 70°C.
[0023] In some preferred embodiments, the absolute pressure in step (2) is 50-70 mbar and the jacket temperature is 50-60°C.
[0024] According to the preparation method of the present invention, preferably, in step (3), the melt polycondensation is carried out at 250-290°C and 0.01-1 mbar absolute pressure.
[0025] In this invention, melt polycondensation is carried out at 250–290°C and 0.01–1 mbar absolute pressure; preferably, an inert gas (such as nitrogen) is first released to remove air from the system, and then the temperature is raised to 260–270°C and reacted at 0.01–0.6 mbar absolute pressure until the motor stirring power reaches a predetermined value.
[0026] In this invention, purification includes one or more of filtration, ion exchange purification, electrodialysis, and salting out; preferably filtration and ion exchange purification.
[0027] According to the preparation method of the present invention, preferably, in step (2), the purification includes the following steps: 1) filtration to obtain filtrate; 2) treatment of the filtrate with ion exchange resin.
[0028] According to the preparation method of the present invention, preferably, step 2) is carried out at 40-70°C for 1-6 hours, and the ion exchange resin includes chelating ion exchange resin and / or cation exchange resin.
[0029] In this invention, ion exchange resin selectively adsorbs metal cations in the filtrate through an ion exchange mechanism, achieving efficient removal of various metal ions such as antimony, lead, cadmium, iron, and copper, as well as catalysts. The ion exchange resin is selected from one or more of chelating ion exchange resins and cation exchange resins; preferably, it is selected from one or more of iminodiacetic acid chelating resins, aminophosphonic acid chelating resins, polyamine chelating resins, strong acid cation exchange resins, and weak acid cation exchange resins; more preferably, it is selected from one or more of iminodiacetic acid chelating resins, strong acid cation exchange resins, and weak acid cation exchange resins. The ion exchange treatment is carried out at 40–70°C for 1–6 hours, preferably at 40–50°C for 2–4 hours.
[0030] On the other hand, the present invention also provides an alkali-soluble polyester prepared according to the above-described preparation method.
[0031] According to the present invention, the alkali-soluble polyester preferably has an L value of 84-96 and a b value of 1.9-4.7 as measured according to GB / T14190-2017 "Test Method for Fiber Grade Polyester (PET) Chips"; and its 5% mass thermogravimetric temperature is not lower than 336°C.
[0032] According to some preferred embodiments of the present invention, the alkali-soluble polyester produced by the present invention, measured according to GB / T14190-2017 "Test Method for Fiber Grade Polyester (PET) Chips", has an L value of 84-96 and a b value of 1.9-4.7; its 5% mass thermogravimetric temperature is not lower than 336℃. This alkali-soluble polyester has the characteristics of low metal content, low terminal carboxyl group content, good color, and excellent thermal stability. After treatment in a 1wt% NaOH alkaline solution at 90℃ for 2 hours, the alkali loss value is greater than 98%, which can meet the quality requirements of high-end applications such as alkali-soluble yarn sizing agents, adhesives, and coatings.
[0033] Compared with the prior art, the beneficial effects of the present invention are: (1) This invention introduces isophthalic acid-5-sulfonate or its derivatives and water-soluble components such as polyethylene glycol, along with a small amount of ethylene glycol and controlled reaction conditions, to directionally alcoholyze waste polyester into water-soluble intermediates, instead of the traditional BHET monomers. This approach reduces the amount of ethylene glycol used and improves the atom economy of the reaction system, achieving a purified product yield of >97%. Furthermore, the intermediates exist directly as water-soluble oligomers, avoiding the high-energy-consuming and high-loss purification steps such as recrystallization and molecular distillation required in traditional methods, thus eliminating material losses during the purification process. This process not only significantly improves the overall recovery rate of waste polyester but also effectively reduces energy consumption and waste generation, achieving efficient, low-carbon, and full-component utilization from waste polyester to high-value chemicals.
[0034] (2) This invention involves the directional alcoholysis of waste polyester into water-soluble intermediates, which are then directly adsorbed using ion exchange resin to remove metal ions introduced from the processing, use, and catalysts of the waste polyester. This purification method is simple to operate and does not require the introduction of exogenous additives such as polycarboxylic acid chelating agents or organophosphonic acid compounds that may contaminate the products. It solves the core problem of the difficulty in effectively removing metal ions in the prior art, while avoiding the risk of secondary contamination of the product by chelating agent components. The metal content in the alkali-soluble polyester produced by ion exchange treatment is reduced to 23-298 ppm. This low metal content can effectively reduce the catalytic effect of metal ions on the thermal degradation of polymers, enabling the product to maintain stable color and mechanical properties during high-temperature processing and long-term use.
[0035] (3) In this invention, polyethylene glycol is added, which can synergistically exert a hydrophilic effect with isophthalic acid-5-sulfonate or its derivatives to form a stable water-soluble intermediate. Further, the number average molecular weight of polyethylene glycol is preferably 200-2000 g / mol, more preferably 200-800 g / mol, so as to balance the yield of the purified product, the color of the alkali-soluble polyester, the thermal stability and the alkali solubility.
[0036] (4) The alkali-soluble polyester of the present invention has good hue (L value 84-96, b value 1.9-4.7) and thermal stability (5% thermal weight loss temperature ≥336℃). The alkali loss value after treatment in 1wt% NaOH alkaline solution at 90℃ for 2 hours is greater than 98%, which can meet the quality requirements of low metal content, low color difference and high heat resistance in high-end application scenarios such as alkali-soluble yarn sizing, adhesives and coatings. Detailed Implementation
[0037] The present invention will be further described below with reference to specific embodiments, but the scope of protection of the present invention is not limited thereto.
[0038] The testing method is described below: (1) Number-average molecular weight determination of water-soluble intermediates: The molecular weight of the obtained water-soluble oligomers was determined by gel permeation chromatography (GPC). An Infinity Lab Meso Pore 3μm column was used with tetrahydrofuran as the mobile phase at a flow rate of 1mL / min. Polystyrene (PSt) standard was used as the standard for calibration. The column temperature was 40℃ and the test time was 30min.
[0039] (2) Yield of purified product: First, using diethyl terephthalate as a reference, a series of standard solutions of known concentrations were prepared with tetrahydrofuran. The absorbance was measured at 254 nm using a UV-Vis spectrophotometer, and an absorbance-concentration standard working curve was plotted. The purified product was dissolved in tetrahydrofuran to prepare a sample solution of 0.01 mg / mL. The absorbance at 254 nm was measured using a UV-Vis spectrophotometer. Based on the standard working curve, the amount of benzene ring in the sample solution was calculated. Then, the amount of substance of isophthalic acid-5-sulfonate or its derivatives is calculated based on the mass of isophthalic acid-5-sulfonate or its derivatives. Each molecule of isophthalic acid-5-sulfonate or its derivatives contains one benzene ring. Therefore, the amount of substance of isophthalic acid-5-sulfonate or its derivatives is the amount of substance of the benzene ring in isophthalic acid-5-sulfonate or its derivatives. Then, the amount of benzene rings in the waste polyester is calculated based on the amount of waste polyester fed into the waste polyester, which is calculated as 1 mol of benzene rings per 192g of waste polyester. Finally, calculate according to the following formula: Yield (%) = (Amount of benzene ring in sample solution - Amount of benzene ring in isophthalic acid-5-sulfonate or its derivative) ÷ Amount of benzene ring in waste polyester × 100%.
[0040] (3) Alkali loss test method: Take 100 mL of 1 wt% NaOH solution and place it in a 90℃ constant temperature water bath for 10 min to equilibrate. Then add 1 g of polyester powder with a particle size of 50-100 mesh to the constant temperature water bath and stir for 2 h. Filter with a 0.45 μm filter membrane and wash with water 3 times. Dry the filter residue in a 100℃ vacuum drying oven for 2 h. After cooling to room temperature, weigh it to obtain the mass of the polyester powder after alkali treatment. Calculate it according to the following formula: Alkali reduction (%) = (1 - mass of polyester powder after alkali treatment) × 100%.
[0041] (4) Thermal stability test: Thermogravimetric analysis (TGA) was used to determine the 5% mass thermal weight loss temperature (Td5%) under nitrogen atmosphere and heating rate of 10℃ / min.
[0042] (5) Metal content test: Inductively coupled plasma (ICP) method was used for determination.
[0043] (6) Color and end carboxyl content test: carried out in accordance with GB / T14190-2017 "Test method for fiber grade polyester (PET) chips".
[0044] In the following examples and comparative examples, unless otherwise stated, the waste polyester used is colorless bottle flakes that have been pulverized; 5-sulfonate isophthalic acid or its derivatives are sodium diethyl 5-sulfonate isophthalic acid; and polyethylene glycol is PEG300.
[0045] Example 1 (1) 1 kg of waste polyester, 0.969 kg of ethylene glycol, 0.463 kg of sodium bis(hydroxyethyl) isophthalate-5-sulfonate, 0.313 kg of polyethylene glycol (PEG300) and 0.010 kg of zinc acetate exchange catalyst were added to the depolymerization reactor and reacted at 220 °C for 1 h to obtain a water-soluble intermediate with a number average molecular weight of 1900 g / mol; (2) Add 10 kg of water to the water-soluble intermediate and heat to 50 °C to dissolve; filter to remove insoluble matter, and treat the filtrate with 0.050 kg of iminodiacetic acid chelating resin at 50 °C for 2 h; then remove water by thin-film evaporator at 60 °C and 70 mbar absolute pressure to obtain purified product (white solid). The yield of purified product was tested to be 99%. (3) Take 1 kg of purified product, 0.479 kg of diethyl terephthalate, and 0.00034 kg of ethylene glycol antimony polycondensation catalyst and add them to a 2.5 L polymerization reactor. Stir evenly, purge with nitrogen three times to remove air from the system, heat to 270 °C and carry out melt polycondensation reaction at an absolute pressure of 0.6 mbar. When the motor stirring power reaches 50 W, the alkali-soluble polyester is discharged.
[0046] Example 2
[0047] Except for the following differences, the remaining steps are the same as in Example 1: In step (1), the reaction time is 2 hours, and the number-average molecular weight of the obtained water-soluble intermediate is 1100 g / mol. The yield of the purified product was tested to be 99%.
[0048] Example 3
[0049] Except for the following differences, the remaining steps are the same as in Example 1: In step (1), the amount of ethylene glycol used is changed to 3.230 kg, and the number average molecular weight of the obtained water-soluble intermediate is 1400 g / mol. The yield of the purified product was tested and found to be 100%.
[0050] Example 4
[0051] Except for the following differences, the remaining steps are the same as in Example 1: In step (1), the amount of ethylene glycol was changed to 0.323 kg, and the reaction was carried out at 220°C for 4 h. The number average molecular weight of the water-soluble intermediate obtained was 2400 g / mol. The yield of the purified product was tested to be 97%.
[0052] Example 5
[0053] Except for the following differences, the remaining steps are the same as in Example 1: In step (2), 0.050 kg of strong acid cation exchange resin was used for treatment for 2 hours. The yield of the purified product was tested to be 99%.
[0054] Example 6
[0055] Except for the following differences, the remaining steps are the same as in Example 1: In step (2), 0.050 kg of weak acid cation exchange resin was used for treatment for 2 hours. The yield of the purified product was tested to be 100%.
[0056] Example 7
[0057] Except for the following differences, the remaining steps are the same as in Example 1: In step (1), the reaction temperature is 170°C and the reaction time is 1 hour, and the number average molecular weight of the obtained water-soluble intermediate is 2900 g / mol. The yield of the purified product was tested to be 98%.
[0058] Example 8
[0059] Except for the following differences, the remaining steps are the same as in Example 1: In step (1), the transesterification catalyst is replaced with potassium carbonate, and the number average molecular weight of the resulting water-soluble intermediate is 2600 g / mol. The yield of the purified product was tested to be 98%.
[0060] Example 9
[0061] Except for the following differences, the remaining steps are the same as in Example 1: In step (3), the polycondensation catalyst is replaced with 0.00014 kg of tetrabutyl titanate (i.e., tetrabutyl titanate). The yield of the purified product was tested to be 99%.
[0062] Example 10
[0063] Except for the following differences, the remaining steps are the same as in Example 1: In step (1), isophthalic acid-5-sulfonate or its derivative is replaced with 0.348 kg of sodium isophthalic acid-5-sulfonate, and the number average molecular weight of the resulting water-soluble intermediate is 2200 g / mol. The yield of the purified product was tested to be 99%.
[0064] Example 11
[0065] Except for the following differences, the remaining steps are the same as in Example 1: In step (1), polyethylene glycol was replaced with 2.087 kg of polyethylene glycol (PEG2000), and the number average molecular weight of the resulting water-soluble intermediate was 2900 g / mol. The yield of the purified product was tested to be 99%.
[0066] Example 12
[0067] Except for the following differences, the remaining steps are the same as in Example 1: In step (1), polyethylene glycol was replaced with 0.835 kg of polyethylene glycol (PEG800), and the number average molecular weight of the resulting water-soluble intermediate was 1500 g / mol. The yield of the purified product was tested to be 98%.
[0068] Example 13
[0069] Except for the following differences, the remaining steps are the same as in Example 1: In step (1), polyethylene glycol was replaced with 0.209 kg of polyethylene glycol (PEG200), and the number average molecular weight of the resulting water-soluble intermediate was 1100 g / mol. The yield of the purified product was tested to be 98%.
[0070] Comparative Example 1 (1) Add 1 kg of waste polyester, 6.000 kg of ethylene glycol and 0.010 kg of zinc acetate to the depolymerization reactor and react at 220°C for 2 h; (2) Add 30 kg of water to the mixture and heat to 90 °C to dissolve; filter to remove insoluble matter, and allow the filtrate to cool naturally to room temperature and refrigerate at 4 °C for 24 h; (3) White crystals were obtained by filtration and dried under vacuum at 60°C for 24 hours. According to the yield test method of the purified product, the yield of the product in this comparative example was only 78% (traditional high ethylene glycol dosage + recrystallization route).
[0071] Comparative Example 2 Except for the following differences, the remaining steps were the same as in Example 1: sodium bis(hydroxyethyl) isophthalate-5-sulfonate was not added. The yield of the purified product was tested to be 47%.
[0072] Comparative Example 3 Except for the following differences, the remaining steps were the same as in Example 1: no polyethylene glycol was added. The yield of the purified product was tested to be 36%.
[0073] Comparative Example 4 Except for the following differences, the remaining steps are the same as in Example 1: polyethylene glycol was replaced with 4.174 kg of polyethylene glycol (PEG4000). The yield of the purified product was tested to be 91%.
[0074] Comparative Example 5 Except for the following differences, the remaining steps are the same as in Example 1: In step (2), the ion exchange resin treatment is omitted, and the filtrate is directly evaporated through a membrane to remove water. The yield of the purified product was tested to be 100%.
[0075] The alkali-soluble polyesters prepared in the above examples and comparative examples were tested, and the test results are shown in Table 1.
[0076] Table 1
[0077] In Example 1, PEG300, zinc acetate ester exchange catalyst, and iminodiacetic acid chelating resin were used for purification during the preparation process. The results showed that the yield of the purified product was 99%; the metal content of the alkali-soluble polyester was 212 ppm, the L value was 94, the b value was 2.1, the Td5% was 356℃, and the alkali reduction was 99%.
[0078] In Example 2, the transesterification time was extended to 2 hours. Only the molecular weight of the water-soluble intermediate decreased, while other properties remained basically the same as in Example 1.
[0079] Example 3 increased the amount of ethylene glycol, leading to a deeper degree of alcoholysis and a decrease in the molecular weight of the water-soluble intermediate; the yield of the purified product was 100%; the alkali-soluble polyester exhibited excellent color, thermal stability, and alkali solubility. Example 4 reduced the amount of ethylene glycol, resulting only in a slight decrease in the yield of the purified product to 97%, while the other properties of the alkali-soluble polyester remained good. This demonstrates that the present invention can produce alkali-soluble polyesters with good color, thermal stability, and alkali solubility in a high yield even with reduced ethylene glycol usage.
[0080] In Example 5, a strongly acidic cation exchange resin was used, achieving a purification product yield of 99%. The metal content of the alkali-soluble polyester was 229 ppm, and the color, thermal weight loss, and alkali reduction were all good. In Example 6, a weakly acidic cation exchange resin was used, achieving a purification product yield of 100%. The metal content of the alkali-soluble polyester increased to 298 ppm, higher than in Examples 1 and 5. Note: Weakly acidic cation exchange resins can also achieve purification with excellent product yields, but their metal removal ability is weaker than chelating resins and strongly acidic cation exchange resins, resulting in higher metal residues.
[0081] Example 7: The transesterification temperature was lowered to 170°C. As the temperature decreased, the transesterification rate decreased and the molecular weight of the intermediate product increased. The yield of the purified product was 98%. The alkali-soluble polyester exhibited excellent performance.
[0082] In Example 8, the transesterification catalyst was replaced with potassium carbonate, and the yield of the purified product was 98%; the metal content of the alkali-soluble polyester was 213 ppm, and other properties were excellent.
[0083] In Example 9, the polycondensation catalyst was replaced with tetrabutyl titanate, and the metal content of the alkali-soluble polyester was only 23 ppm; however, the color of the alkali-soluble polyester deteriorated slightly: L value was 84, b value was 4.7; Td5% value was 354℃, and alkali reduction was 99%. Note: Tetrabutyl titanate, as a polycondensation catalyst, can yield alkali-soluble polyesters with low metal content; however, it easily causes yellowing of the alkali-soluble polyester, increasing the b value and deteriorating the color; antimony glycolate has a significantly better color advantage than the tetrabutyl titanate catalyst.
[0084] Example 10 reduced the amount of isophthalic acid-5-sulfonate or its derivatives, and the yield of the purified product was 99%; the properties of the alkali-soluble polyester were similar to those of Example 1.
[0085] In Example 11, PEG300 was replaced with PEG2000, and the yield of the purified product was 99%; the Td5% of the alkali-soluble polyester decreased to 336°C; the L value was 88, the b value was 3.1, and the hue deteriorated slightly; the alkali reduction was 98%, a slight decrease. Increasing the molecular weight of PEG to 2000, although the product could be prepared, reduced the thermal stability of the alkali-soluble polyester, slightly decreased its alkali solubility, and slightly deteriorated its hue. In Example 12, PEG300 was replaced with PEG800, and the yield of the purified product was 98%; the Td5% of the alkali-soluble polyester was 353°C; the L value was 94, the b value was 2.6, and the alkali reduction was 99%. In Example 13, PEG300 was replaced with PEG200, and the yield of the purified product was 98%; the Td5% of the alkali-soluble polyester was 358°C; the L value was 95, the b value was 2.0, and the alkali reduction was 98%. It is noted that the number average molecular weight of PEG in this invention is preferably 200-2000 g / mol, more preferably 200-800 g / mol, which results in excellent yield of purified product, color of alkali-soluble polyester, thermal stability and alkali solubility.
[0086] Comparative Example 1, without the addition of isophthalic acid-5-sulfonate or its derivatives, and PEG, used conventional ethylene glycol alcoholysis and recrystallization purification, resulting in a product yield of only 78%. This process has a low recycling rate of waste polyester, high energy consumption, and low added value of the product.
[0087] Comparative Example 2, without the addition of isophthalic acid-5-sulfonate or its derivatives, yielded a purified product of 47%; the Td5% of the obtained polyester was 372℃; the L value was 96, the b value was 2.4, and the alkali reduction was 28%. Comparative Example 3, without the addition of PEG, yielded a purified product of only 36%, and the alkali reduction of the obtained polyester was only 41%; lacking the synergistic hydrophilic effect of PEG, the water-soluble intermediate had extremely poor water solubility, resulting in a very low purification yield; furthermore, the alkali solubility of the final alkali-soluble polyester decreased significantly, with an alkali reduction of only 41%. Comparative Examples 2 and 3 demonstrate that isophthalic acid-5-sulfonate or its derivatives and PEG are indispensable, and the synergistic effect of PEG and isophthalic acid-5-sulfonate or its derivatives is key to the water-soluble intermediate and high alkali reduction.
[0088] Comparative Example 4 replaced PEG300 with PEG4000. The water solubility of the water-soluble intermediate decreased, resulting in a purified product yield of 91%; the Td5% of the alkali-soluble polyester also decreased significantly to 322℃; the L value was 85, the b value was 3.5, and the hue deteriorated.
[0089] Comparative Example 5 omitted the ion exchange resin purification step. The yield of the purified product was 100%; the metal content of the alkali-soluble polyester was as high as 2614 ppm; the color was severely deteriorated, with an L value of 73 and a b value of 8.4; the Td5% value was 346℃. This indicates that the ion exchange resin purification step is indispensable, as it can be used to remove transesterification metal catalysts from water-soluble intermediates, and helps to improve the color and thermal stability of alkali-soluble polyesters.
[0090] As demonstrated in Examples 1-13, the preparation method of this invention can fully recycle waste polyester with a relatively low amount of ethylene glycol, producing a high-value-added alkali-soluble polyester. The alkali-soluble polyester of this invention features low metal content, low terminal carboxyl group content, good color, and high thermal stability. Furthermore, after treatment in a 1 wt% NaOH alkali solution at 90°C for 2 hours, the alkali reduction value is greater than 98%, meeting the quality requirements of low metal content, low color difference, and high heat resistance for high-end applications such as alkali-soluble yarn sizing agents, adhesives, and coatings.
[0091] All aspects, embodiments, and features of this invention should be considered illustrative in all respects and not limiting of the invention; the scope of the invention is defined only by the claims. Other embodiments, modifications, and uses will become apparent to those skilled in the art without departing from the spirit and scope of the invention as claimed.
[0092] In the preparation method of this invention, the order of the steps is not limited to the listed order. For those skilled in the art, variations in the order of the steps without creative effort are also within the scope of protection of this invention. Furthermore, two or more steps or actions can be performed simultaneously.
[0093] Finally, it should be noted that the specific embodiments described herein are merely illustrative examples of the invention and are not intended to limit the implementation of the invention. Those skilled in the art can make various modifications or additions to the described specific embodiments or use similar methods to replace them; it is neither necessary nor possible to exemplify all embodiments here. However, these obvious variations or modifications derived from the essential spirit of the invention still fall within the scope of protection of the invention, and interpreting them as any additional limitation would contradict the spirit of the invention.
Claims
1. A method for preparing an alkali-soluble polyester, characterized in that, Includes the following steps: (1) Waste polyester, aliphatic diols with 2 to 3 carbon atoms, isophthalic acid-5-sulfonate or its derivatives, polyethylene glycol and transesterification catalyst are mixed and reacted at 160 to 240 °C for 1 to 10 h to obtain a water-soluble intermediate product. (2) Dissolve the water-soluble intermediate in water, purify and dry to obtain the purified product; (3) The purified product is mixed with diethyl terephthalate and a polycondensation catalyst, and a melt polycondensation reaction is carried out under the protection of an inert gas to obtain an alkali-soluble polyester.
2. The preparation method according to claim 1, characterized in that, In step (1), the aliphatic diol is selected from one or more of ethylene glycol and 1,3-propanediol; the isophthalic acid-5-sulfonate or its derivative is selected from one or more of sodium bis(hydroxyethyl) isophthalate-5-sulfonate and sodium isophthalate-5-sulfonate; the transesterification catalyst is selected from one or more of zinc acetate, manganese acetate, potassium carbonate, n-butyl titanate, and isopropyl titanate; and the number average molecular weight of the polyethylene glycol is 200-3000 g / mol. In step (3), the polycondensation catalyst is selected from one or more of antimony glycol, n-butyl titanate, isopropyl titanate, titanium oxalate, titanium acetate, titanium tetrachloride, and 1,8-diazabicyclo[5.4.0]undec-7-ene.
3. The preparation method according to claim 2, characterized in that, The mass ratio of the waste polyester to the aliphatic diol is 1:(0.15-3.5); the mass ratio of the waste polyester to the isophthalic acid-5-sulfonate or its derivative is 1:(0.1-0.5); the mass ratio of the waste polyester to the polyethylene glycol is 1:(0.1-8); and the mass ratio of the waste polyester to the transesterification catalyst is 1:(0.005-0.03).
4. The preparation method according to claim 1, characterized in that, In step (2), the mass ratio of the waste polyester to water is 1:(5-30), and the dissolution temperature is 40-90℃.
5. The preparation method according to claim 1, characterized in that, In step (2), the drying is carried out in a thin-film evaporator with an absolute pressure of 30 to 100 mbar and a jacket temperature of 50 to 70°C.
6. The preparation method according to claim 1, characterized in that, In step (3), the melt polycondensation is carried out at 250-290°C and 0.01-1 mbar absolute pressure.
7. The preparation method according to any one of claims 1 to 6, characterized in that, In step (2), the purification includes the following steps: 1) Filter to obtain filtrate; 2) The filtrate is treated with ion exchange resin.
8. The preparation method according to claim 7, characterized in that, Step 2) The process is carried out at 40-70°C for 1-6 hours, wherein the ion exchange resin includes chelating ion exchange resin and / or cation exchange resin.
9. An alkali-soluble polyester, characterized in that, It is prepared according to any one of claims 1 to 8.
10. The alkali-soluble polyester according to claim 9, characterized in that, The alkali-soluble polyester has an L value of 84–96 and a b value of 1.9–4.7; its 5% mass thermal weight loss temperature is not lower than 336℃.
Citation Information
Patent Citations
Water-soluble polyester slurry prepared from waste polyester plastics and preparation method thereof